Fluorine-containing polyimide foam material and preparation method thereof

By using fluoropolyimide precursors and functional additives, polyimide foam materials with low dielectric constant and good hydrophobic properties are prepared, which solves the increase in thermal conductivity and dielectricity of traditional materials under high humidity conditions. The problem of poor constants achieves temperature resistance, flame retardant, hydrophobic and high wave transmission performance, which is suitable for a variety of application needs.

CN119081115APending Publication Date: 2024-12-06CHANGZHOU TIANSHENG NEW MATERIALS RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411349961.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-26
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Traditional polyimide foam materials have increased thermal conductivity under high humidity conditions, and their dielectric constant and hydrophobic properties are poor, which cannot meet the needs of wave-transmitting materials.

Method used

Using fluorine-containing polyimide acid precursor, a polyimide foam material with low dielectric constant and good hydrophobic properties is prepared by combining fluorine-containing aromatic dianhydride and fluorine-containing diamine, and then mechanically foamed. Foaming process and optimize functional additive composition to improve the mechanical properties and chemical stability of the material.

Benefits of technology

While maintaining high temperature and high oxygen index performance, it prepares temperature-resistant, flame-retardant, hydrophobic, and high wave-transmitting polyimide foam materials, which meet the requirements of low dielectric constant and good hydrophobic performance of traditional materials, and is suitable for harsh and harsh Application in the environment.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of fluorine-containing polyimide foam materials, in particular to a fluorine-containing polyimide foam material and a preparation method thereof. The fluorine-containing polyimide foam material comprises the following substances in parts by weight: 80-120 parts of a fluorine-containing polyimide acid precursor; and 3-12 parts of a functional auxiliary agent. The fluorine-containing polyimide acid precursor is selected as a main raw material of the fluorine-containing polyimide foam material, and the fluorine-containing polyimide foam material has a low dielectric constant and good hydrophobic performance by utilizing the high electron-withdrawing characteristic of fluorine atoms, so that the original high temperature resistance and high oxygen index performance of polyimide foam are maintained; the polyimide foam with temperature resistance, flame retardance, hydrophobicity and high wave transmission is prepared, so that the requirements of low dielectric constant and good hydrophobicity of a traditional polyimide foam material are effectively met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fluorine-containing polyimide foam materials, in particular to a fluorine-containing polyimide foam material and a preparation method thereof. Background Art

[0002] With the rapid development of the economy, especially the rapid development of emerging industries such as lithium batteries, consumer electronics, 5G, and civil drones, the demand for new materials is also increasing. Polyimide (PI) foam plastics are an advanced functional polymer material with the characteristics of radiation resistance, low density, flame retardancy, high and low temperature resistance, sound absorption and noise reduction, and heat insulation.

[0003] Fluorinated PI foam has outstanding heat resistance, and its maximum long-term operating temperature can reach over 300°C. With the rapid development of downstream application fields, further requirements are put forward for the functions and performance of polyimide. On the one hand, with the rapid development of the 5G industry, the demand for wave-transmitting materials is gradually increasing. On the other hand, due to the high open porosity of traditional polyimide foam, the thermal conductivity coefficient increases seriously under high humidity conditions. Lithium batteries, aerospace, etc. have also put forward different functional requirements for polyimide foam. Therefore, how to find a more suitable polyimide foam material, further broaden its functionality, and solve the needs and problems existing in the above-mentioned applications has become one of the focuses of widespread attention of many R&D manufacturers and front-line researchers.

[0004] With respect to the above-mentioned related technologies, the inventors found that the existing polyimide foam materials have poor dielectric constant and hydrophobic properties and cannot meet the demand for polyimide foam materials as wave-transmitting materials. Summary of the invention

[0005] In order to improve the above technical problems, the present application provides a fluorine-containing polyimide foam material and a preparation method thereof.

[0006] A fluorinated polyimide foam material and a preparation method thereof, using the following technical scheme: A fluorine-containing polyimide foam material comprises the following substances in parts by weight: 80-120 parts of fluorinated polyimide acid precursor; Functional additives 3-12 parts.

[0007] Through the above technical scheme, the present application selects a fluorinated polyimide acid precursor as the main raw material of a fluorinated polyimide foam material, utilizing the high electron-withdrawing properties of fluorine atoms, which has a low dielectric constant and good hydrophobic properties. While maintaining the original high temperature resistance and high oxygen index properties of the polyimide foam, a polyimide foam that is heat-resistant, flame-retardant, hydrophobic, and highly wave-transparent is prepared, thereby effectively meeting the requirements of traditional polyimide foam materials for low dielectric constant and good hydrophobic properties.

[0008] Furthermore, the fluorine-containing polyimide acid precursor is prepared by prepolymerization of fluorine-containing aromatic dianhydride and fluorine-containing diamine.

[0009] Through the above technical scheme, the present application optimizes the raw materials of the fluorinated polyimide acid precursor, and ensures the unique properties of the polyimide acid precursor by combining the fluorinated aromatic dianhydride with the fluorinated diamine. This combination not only improves the hydrophobicity of the material, but also enhances the mechanical properties and chemical stability of the material, making it suitable for use in harsh environments. At the same time, the prepolymerization reaction can effectively control the molecular weight and structure, thereby affecting the performance of the final product, ensuring the uniformity and consistency of the foam material, and providing a good foundation for subsequent processing and application.

[0010] Further, the fluorine-containing diamine includes one or more of 4,4'-oxybis[3-(trifluoromethyl)aniline], 4,4'-oxybis[3-(oxytrifluoromethyl)aniline], 4,4'-oxybis[3-fluoroaniline], 2-(trifluoromethyl)-1,4-p-phenylenediamine, 2-(oxytrifluoromethyl)-1,4-p-phenylenediamine, 2-fluoro-1,4-p-phenylenediamine, 2,2'-bis(trifluoromethyl)diaminobiphenyl, 2,2'-bis(oxytrifluoromethyl)diaminobiphenyl and 2,2'-bis(fluoro)diaminobiphenyl.

[0011] Furthermore, in the preparation process of the fluorinated polyimide acid precursor, the molar ratio of the fluorinated aromatic dianhydride to the fluorinated diamine is (1.01-1.05):1.

[0012] Furthermore, the functional additives include a thickener and a foam stabilizer.

[0013] Furthermore, the thickener includes one or more of bentonite, magnesium silicate, hydroxyethyl cellulose, and hydroxypropyl methyl cellulose.

[0014] Furthermore, the foam stabilizer includes one or more of DC193, DC197, DC5000, DC5598, L560, L580, AK8805, SF8427, KY-6035, HK-314, GT-320, B4900, and B8123.

[0015] This application optimizes the composition of functional additives. The thickener after optimizing the composition can effectively increase the viscosity of the foam, making the bubbles more stable during the formation process and preventing the bubbles from merging and bursting; while the foam stabilizer can form a film on the liquid interface to further enhance the structural stability of the foam. These functional additives work together to make the obtained foam material have excellent compressive strength and long service life, which is suitable for high-demand application fields.

[0016] In a second aspect, the present application provides a method for preparing a fluorinated polyimide foam material, using the following technical solution; A method for preparing a fluorinated polyimide foam material comprises the following steps: A fluorine-containing aromatic dianhydride and a fluorine-containing diamine are placed in a solvent, and subjected to prepolymerization treatment to obtain a fluorine-containing polyamic acid precursor; Then, add the fluorinated polyimide acid precursor and thickener into the stirrer, stir and thicken, then heat the foam stabilizer and continue stirring; After the stirring is completed, an inert gas is introduced into the stirrer while stirring to form a foam body, the foam body is poured into a mold, the mold is placed in a drying room for gradient heating, and finally high-temperature curing is performed to prepare the fluorinated polyimide foam material.

[0017] Furthermore, in the prepolymerization treatment, the prepolymerization time is 2 to 24 hours, and the prepolymerization temperature is 0° C. to 200° C.

[0018] Furthermore, it is characterized in that the inert gas includes one or more of carbon dioxide, nitrogen and helium.

[0019] The technical solution of this application uses a mechanical foaming process and a formula ratio to control the speed of the foaming reaction and the curing reaction, which greatly improves the production efficiency and consistency of production compared with the traditional physical and chemical foaming method. It also improves the quality and utilization rate of thin polyimide foam.

[0020] In summary, this application has the following beneficial effects: First, fluorinated polyimide acid precursor is selected as the main raw material of fluorinated polyimide foam material, and the high electron-withdrawing property of fluorine atoms is utilized, which has low dielectric constant and good hydrophobic properties. While maintaining the original high temperature resistance and high oxygen index performance of polyimide foam, a polyimide foam with heat resistance, flame retardancy, hydrophobicity and high wave transmittance is prepared, thereby effectively meeting the requirements of low dielectric constant and good hydrophobic properties of traditional polyimide foam materials.

[0021] Second, the present application preferably selects the raw materials of the fluorinated polyimide acid precursor, and ensures the unique properties of the polyimide acid precursor by combining the fluorinated aromatic dianhydride with the fluorinated diamine. This combination not only improves the hydrophobicity of the material, but also enhances the mechanical properties and chemical stability of the material, making it suitable for use in harsh environments. At the same time, the prepolymerization reaction can effectively control the molecular weight and structure, thereby improving the performance of the final product, ensuring the uniformity and consistency of the foam material, and providing a good foundation for subsequent processing and application.

[0022] Third, the present application has selected the raw materials of the fluorinated polyimide acid precursor, and ensured the unique properties of the polyimide acid precursor by combining the fluorinated aromatic dianhydride with the fluorinated diamine. This combination not only improves the hydrophobicity of the material, but also enhances the mechanical properties and chemical stability of the material, making it suitable for use in harsh environments. At the same time, the prepolymerization reaction can effectively control the molecular weight and structure, thereby affecting the performance of the final product, ensuring the uniformity and consistency of the foam material, and providing a good foundation for subsequent processing and application. DETAILED DESCRIPTION The present application is further described in detail below with reference to the embodiments.

[0023] In the examples of the present application, the raw materials and instruments used are as follows. Unless otherwise specified, the raw materials used in the present application are of analytical grade.

[0024] The present application is further described in detail below with reference to the embodiments.

[0025] Example 1 50 kg of hexafluorodianhydride and 48 kg of 4,4'-oxybis[3-(oxytrifluoromethyl)aniline] were stirred in 100 kg of N,N'-dimethylformamide and heated to 65°C for reaction for 3 hours, and then cooled to room temperature to obtain a fluorinated polyimide acid precursor; First, add 100 kg of fluorinated polyimide acid precursor and 5 kg of bentonite into a stirrer, stir and thicken at a speed of 1000 r / min for 30 min, then add 3 kg of foam stabilizer B4900 at a speed of 2000 r / min for 30 min; After the stirring is completed, nitrogen is introduced into the stirrer while stirring, the stirring speed is 10000r / min, the stirring time is 20min, and foaming is formed into a foam body, the foam body is poured into a mold, and the mold is placed in a drying room for gradient heating, that is, reacting at 80°C for 2h, then reacting at 150°C for 2h, and finally curing at 250°C for 2h to obtain a fluorinated polyimide foam material.

[0026] Example 2 50 parts of hexafluorodianhydride and 12 parts of 2-(oxytrifluoromethyl)-1,4-p-phenylenediamine were stirred in 50 parts of dimethyl sulfoxide and heated to 50°C for reaction for 3 hours, and then cooled to room temperature to obtain a fluorinated polyimide acid precursor; First, add 100 parts of fluorinated polyimide acid precursor and 3 parts of hydroxyethyl cellulose into a stirrer, stir and thicken at a stirring speed of 1000 r / min for 40 min, then add 5 parts of foam stabilizer DC5000 at a stirring speed of 3000 r / min for 40 min; After the stirring is completed, nitrogen is introduced into the stirrer while stirring, the stirring speed is 15000r / min, the stirring time is 30min, and foaming is formed into a foam body, the foam body is poured into a mold, and the mold is placed in a drying room for gradient heating, that is, treated at 100°C for 1h, then treated at 180°C for 1h, and finally cured at 230°C for 2h to obtain a fluorinated polyimide foam material.

[0027] Example 3 50 parts of hexafluorodianhydride and 12 parts of 2-(oxytrifluoromethyl)-1,4-p-phenylenediamine were stirred in 50 parts of dimethyl sulfoxide and heated to 50°C for reaction for 3 hours, and then cooled to room temperature to obtain a fluorinated polyimide acid precursor; First, add 100 parts of fluorinated polyimide acid precursor and 3 parts of hydroxyethyl cellulose into a stirrer, stir and thicken at a stirring speed of 1000 r / min for 40 min, then add 5 parts of foam stabilizer DC5000 at a stirring speed of 3000 r / min for 40 min; After the stirring is completed, nitrogen is introduced into the stirrer while stirring, the stirring speed is 15000r / min, the stirring time is 30min, and foaming is formed into a foam body, the foam body is poured into a mold, and the mold is placed in a drying room for gradient heating, that is, treated at 100°C for 1h, then treated at 180°C for 1h, and finally cured at 230°C for 2h to obtain a fluorinated polyimide foam material.

[0028] It should be noted that the fluorine-containing diamines used in the present application include, but are not limited to, one or more of 4,4'-oxybis[3-(trifluoromethyl)aniline], 4,4'-oxybis[3-(oxytrifluoromethyl)aniline], 4,4'-oxybis[3-fluoroaniline], 2-(trifluoromethyl)-1,4-p-phenylenediamine, 2-(oxytrifluoromethyl)-1,4-p-phenylenediamine, 2-fluoro-1,4-p-phenylenediamine, 2,2'-bis(trifluoromethyl)diaminobiphenyl, 2,2'-bis(oxytrifluoromethyl)diaminobiphenyl and 2,2'-bis(fluoro)diaminobiphenyl.

[0029] The thickener used in the present application includes, but is not limited to, one or more of bentonite, magnesium silicate, hydroxyethyl cellulose, and hydroxypropyl methyl cellulose.

[0030] The foam stabilizers used in this application include but are not limited to one or more of DC193, DC197, DC5000, DC5598, L560, L580, AK8805, SF8427, KY-6035, HK-314, GT-320, B4900, and B8123.

[0031] Comparative Example 1 1) Use phthalic anhydride and diaminodiphenylmethane (4,4'-diaminodiphenylmethane) as monomers. At room temperature, add 4,4'-diaminodiphenylmethane (1.98 g, 10 mmol) into a 50 mL three-necked flask and introduce nitrogen, and dissolve it in dimethyl sulfoxide (23.59 g) under stirring at 300 rpm. Once 4,4'-diaminodiphenylmethane is dissolved, add phthalic anhydride (2.18 g, 10 mmol). Stir the reaction in a nitrogen atmosphere for 12 hours, and polymerize to obtain a light yellow polyamic acid solution.

[0032] 2) At 25° C., emulsifier F127 (0.1 g, the content of the emulsifier in phase A is 5 wt%) and dehydrating agent acetic anhydride (0.568 mL) were dissolved in 2 mL of the above polyamic acid solution, added to a 50 mL round-bottom flask, and nitrogen was continuously introduced, and mixed under mechanical stirring until the emulsifier was completely dissolved, as phase A (i.e., continuous phase). 8 mL of tetradecane was used as the dispersed phase (the volume fraction of the dispersed phase in the polyamic acid non-aqueous emulsion was 75%), and the dispersed phase was dripped into the continuous phase dropwise under mechanical stirring at 300 rpm, until the dispersed phase was completely dripped off, stirring was continued for 5 minutes to obtain the polyamic acid non-aqueous emulsion, and then a dehydration catalyst pyridine (0.484 mL) was added to obtain the polyimide non-aqueous emulsion.

[0033] 3) The polyimide non-aqueous emulsion was transferred into a glass mold and sealed, and the mold was placed at 40°C for gelation for 12 hours, and the obtained block-shaped porous material was replaced with ethanol and water for 24 hours, respectively, and then freeze-dried (cold trap temperature -80°C, sample temperature -20°C) for 24 hours to obtain a polyimide foamed material.

[0034] Performance Testing The performance of the fluorinated polyimide foam materials prepared in Examples 1-3 was tested: Tensile strength: tested according to standard GB / T 8812.2-2007; Thermal conductivity: Tested according to standard GB / T 42919.1-2023; Oxygen index: tested according to standard GB / T 2406.1-2008; The details are shown in Table 1 below: Table 1 Performance test table project <![CDATA[Density / kg / m 3 > Tensile strength / kPa Thermal conductivity / W(m·K) Oxygen index / % Water contact angle / ° Example 1 13 60 0.040 37.5 115 Example 2 15 80 0.040 36 121 Example 3 18 92 0.041 38.3 125 Comparative Example 1 12 55 0.042 32 98 From the results of the above Examples 1-3, Comparative Example 1 and Table 1, it can be found that the present application selects a fluorinated polyimide acid precursor as the main raw material for a fluorinated polyimide foam material, utilizing the high electron-withdrawing properties of fluorine atoms, having a low dielectric constant and good hydrophobic properties, while maintaining the original high temperature resistance and high oxygen index properties of the polyimide foam, to prepare a heat-resistant, flame-retardant, hydrophobic, and highly wave-transparent polyimide foam, thereby effectively meeting the requirements of low dielectric constant and good hydrophobic properties of traditional polyimide foam materials.

[0035] The present invention has been described in detail above in conjunction with specific implementations and exemplary examples, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, a variety of equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.

[0036] All publications, patent applications, patents and other references mentioned in this specification are incorporated herein by reference. Unless otherwise defined, all technical and scientific terms used in this specification have the meanings conventionally understood by those skilled in the art. In the event of a conflict, the definition in this specification shall prevail.

[0037] When this specification uses the prefix "well-known to those skilled in the art", "prior art" or similar terms to introduce materials, substances, methods, steps, devices or components, etc., the objects introduced by the prefix cover those commonly used in the art when this application is filed, but also include those that are not commonly used at present but will become recognized in the art as being suitable for similar purposes.

[0038] In the context of the present specification, any matters or items not mentioned are directly applicable to those known in the art without any changes except those explicitly stated.

Claims

1. A fluorinated polyimide foam material, characterized in that: The composition includes the following materials in parts by weight: 80-120 parts of fluorinated polyimide acid precursor; Functional additives 3-12 parts.

2. A fluorinated polyimide foam material according to claim 1, characterized in that: The fluorine-containing polyimide acid precursor is prepared by prepolymerization of fluorine-containing aromatic dianhydride and fluorine-containing diamine.

3. A fluorinated polyimide foam material according to claim 2, characterized in that: The fluorine-containing diamine includes one or more of 4,4'-oxybis[3-(trifluoromethyl)aniline], 4,4'-oxybis[3-(oxytrifluoromethyl)aniline], 4,4'-oxybis[3-fluoroaniline], 2-(trifluoromethyl)-1,4-p-phenylenediamine, 2-(oxytrifluoromethyl)-1,4-p-phenylenediamine, 2-fluoro-1,4-p-phenylenediamine, 2,2'-bis(trifluoromethyl)diaminobiphenyl, 2,2'-bis(oxytrifluoromethyl)diaminobiphenyl and 2,2'-bis(fluoro)diaminobiphenyl.

4. The fluorinated polyimide foam material according to claim 2, characterized in that: In the preparation process of the fluorinated polyimide acid precursor, the molar ratio of the fluorinated aromatic dianhydride to the fluorinated diamine is (1.01-1.05):

1.

5. The fluorinated polyimide foam material according to claim 1, characterized in that: The functional assistants include thickeners and foam stabilizers.

6. The fluorinated polyimide foam material according to claim 5, characterized in that: The thickener includes one or more of bentonite, magnesium silicate, hydroxyethyl cellulose, and hydroxypropyl methyl cellulose.

7. The fluorinated polyimide foam material according to claim 5, characterized in that: The foam stabilizer includes one or more of DC193, DC197, DC5000, DC5598, L560, L580, AK8805, SF8427, KY-6035, HK-314, GT-320, B4900, and B8123.

8. The method for preparing a fluorinated polyimide foam material according to any one of claims 1 to 7, characterized in that: The method comprises the following preparation steps: A fluorine-containing aromatic dianhydride and a fluorine-containing diamine are placed in a solvent, and subjected to prepolymerization treatment to obtain a fluorine-containing polyamic acid precursor; Then, add the fluorinated polyimide acid precursor and thickener into the stirrer, stir and thicken, then heat the foam stabilizer and continue stirring; After the stirring is completed, an inert gas is introduced into the stirrer while stirring to form a foam body, the foam body is poured into a mold, the mold is placed in a drying room for gradient heating, and finally high-temperature curing is performed to prepare the fluorinated polyimide foam material.

9. The method for preparing a fluorinated polyimide foam material according to claim 8, characterized in that: The prepolymerization time in the prepolymerization treatment is 2 to 24 hours, and the prepolymerization temperature is 0° C. to 200° C.

10. The method for preparing a fluorine-containing polyimide foam material according to claim 8, characterized in that: The inert gas includes one or more of carbon dioxide, nitrogen and helium.