Spacecraft protection cover composite material and preparation method thereof

By using high-temperature-resistant modified resins and inorganic fiber additives in spacecraft protective cover composite materials, the problem of insufficient performance of the material under high temperature and impact is solved, and higher high temperature and impact resistance is achieved, satisfying modern spacecraft demand.

CN119081269AInactive Publication Date: 2024-12-06BEIJING AXICOMB NEW MATERIAL
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411470086.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-21
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The spacecraft protective cover composite material has insufficient high temperature resistance, mechanical strength and impact resistance under the impact of space debris, which is difficult to meet the needs of modern spacecraft.

Method used

Using a composite material formula, including ultra-high molecular weight polyethylene, high temperature-resistant modified resin and inorganic fiber additives, the compact chain is formed through the click reaction of polyphenylene sulfide and silazane structure and the organic modification of basalt fibers. Material with excellent thermal stability improves the material's high temperature and impact resistance.

Benefits of technology

It significantly improves the high-temperature resistance and impact resistance of spacecraft protective cover composite materials, so that they can operate stably in high-temperature environments and are not easily damaged under impact of micrometeorites and space debris, meeting the needs of use in various environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081269A_ABST
    Figure CN119081269A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of high polymer materials, and discloses a spacecraft protective cover composite material and a preparation method thereof, the spacecraft protective cover composite material comprises the following raw materials: ultra-high molecular weight polyethylene, maleic anhydride grafted polyethylene, high temperature resistant modified resin, an inorganic fiber additive, an antioxidant, a plasticizer, a lubricant and an ultraviolet absorbent; the high-temperature-resistant modified resin is prepared, and the inorganic fiber additive participates in the preparation process of the spacecraft protective cover composite material, so that the prepared spacecraft protective cover composite material has excellent high-temperature resistance, mechanical strength and impact resistance; the composite material can stably exist in a high-temperature environment, is not easy to damage under the high-speed impact of micrometeorite and space debris, can meet the use requirements in various environments, and has long service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polymer materials, and in particular to a composite material for a spacecraft protective cover and a preparation method thereof. Background Art

[0002] A spacecraft is an aircraft that operates in space according to the laws of celestial mechanics and performs specific tasks such as exploring, developing, and utilizing space and celestial bodies. Most spacecraft operate within the solar system and are important tools for people to conduct space exploration, scientific experiments, communication and navigation, and earth observation. Due to the particularity of the operating environment, spacecraft are easily affected by a variety of complex environments when performing their missions. For example, high temperature environments may cause deformation and failure of spacecraft materials. The impact of space debris may cause damage or breakage of the spacecraft, causing the spacecraft to lose its function and causing immeasurable losses. Therefore, in order to protect spacecraft, spacecraft protection covers came into being.

[0003] With the continuous advancement of science and technology, traditional aircraft protective covers made of single materials such as metal and ceramics have become difficult to meet the urgent needs of today's spacecraft protective covers for lightweight, high strength, high temperature resistance and impact resistance due to their heavy weight and limited performance. Therefore, composite materials have gradually become the mainstream choice for spacecraft protective covers due to their light weight and strong designability. However, when in use, spacecraft not only need to withstand extreme high temperature environments, but also need to resist the impact of micrometeorites and space debris. Ordinary composite materials still have insufficient mechanical strength, high temperature resistance and impact resistance when facing such extreme use environments. Therefore, the development of higher performance composite materials for spacecraft protective covers has become an urgent problem to be solved. Summary of the invention

[0004] The purpose of the present invention is to provide a composite material for a spacecraft protective cover and a preparation method thereof, which solves the problem that the high temperature resistance, mechanical strength and impact resistance of ordinary composite materials for spacecraft protective covers need to be improved.

[0005] The purpose of the present invention can be achieved by the following technical solutions: A composite material for a spacecraft protective cover comprises the following raw materials in parts by weight: 80-90 parts of ultra-high molecular weight polyethylene, 15-25 parts of maleic anhydride grafted polyethylene, 25-35 parts of high temperature resistant modified resin, 12-15 parts of inorganic fiber additives, 2-5 parts of antioxidants, 3-5 parts of plasticizers, 2-3 parts of lubricants, and 1-3 parts of ultraviolet absorbers; the high temperature resistant modified resin is prepared by taking polyphenylene sulfide as a polymer skeleton and introducing silazane and phenylboronic acid pinacol ester structures into the structure; the inorganic fiber additive is prepared by organically modifying basalt fiber and introducing a polyether structure on the surface of basalt fiber.

[0006] Furthermore, the antioxidant is any one of antioxidant 1010, antioxidant 626, and antioxidant 5057; the plasticizer is any one of diisononyl phthalate, castor oil, and epoxidized soybean oil; the lubricant is any one of paraffin, white oil, and polyethylene wax; the ultraviolet absorber is any one of ultraviolet absorber UV-1300, ultraviolet absorber UV-1577, and ultraviolet absorber UV-928.

[0007] Furthermore, the preparation method of the high temperature resistant modified resin comprises the following steps: S1: placing polyphenylene sulfide in toluene, stirring and mixing thoroughly, adding methyl vinyl dichlorosilane and benzoin dimethyl ether to react under ultraviolet light for 1-1.5 hours, and collecting the product after reduced pressure distillation to obtain modified polyphenylene sulfide; S2: Place modified polyphenylene sulfide and 4-aminophenylboronic acid pinacol ester in tetrahydrofuran, introduce nitrogen, add triethylamine, raise the temperature to 55-60°C and react for 3-5h, collect the product after reduced pressure distillation, and obtain a high temperature resistant modified resin.

[0008] In this scheme, under the action of benzoin dimethyl ether and ultraviolet radiation, the mercapto group in the polyphenylene sulfide structure and the alkenyl group in the methylvinyl dichlorosilane structure undergo a click reaction to obtain modified polyphenylene sulfide, and then under the action of triethylamine, the silicon chlorine in the modified polyphenylene sulfide structure reacts with the amino group in the 4-aminophenylboronic acid pinacol ester structure to obtain a high-temperature resistant modified resin. The high-temperature resistant modified resin uses polyphenylene sulfide as a polymer skeleton, and its molecular structure is formed by alternating arrangement of highly polar sulfur atoms and benzene rings, and has a tight and stable chain structure, so that it can effectively resist thermal expansion and thermal decomposition at high temperatures, and has excellent high-temperature resistance and mechanical properties. Methylvinyldichlorosilane containing a chlorosilane structure is chemically bonded into the polymer skeleton, and then the amino group in the 4-aminophenylboronic acid pinacol ester structure is used to react with chlorosilane, and the silicon atom and the nitrogen atom are connected by a covalent bond to form a silicon-nitrogen bond, thereby further improving the high temperature resistance of the polymer skeleton. At the same time, the phenylboronic acid pinacol ester structure in its structure has excellent thermal stability. Therefore, adding this high temperature resistant modified resin to the preparation process of the spacecraft protective cover composite material can effectively improve the high temperature resistance of the spacecraft protective cover composite material, so that it can operate safely and stably in a high temperature environment and have a long service life.

[0009] Furthermore, in step S1, the number average molecular weight of the polyphenylene sulfide is 4000-5000.

[0010] Furthermore, in step S1, the irradiance of the ultraviolet light is 2-3 mw / cm 2 .

[0011] Furthermore, the preparation method of the inorganic fiber additive comprises the following steps: SS1: Place basalt fiber in deionized water, ultrasonically disperse for 10-15 minutes, add acryloyl chloride and accelerator, react at room temperature for 6-8 hours, filter, wash, and vacuum dry to obtain modified basalt fiber; SS2: Place the modified basalt fiber in N,N-dimethylformamide, ultrasonically disperse for 15-20 minutes, add polyvinyl alcohol monoallyl ether and initiator, heat to 60-70°C and react for 5-6 hours, filter, wash and vacuum dry to obtain inorganic fiber additive.

[0012] In this scheme, under the action of the promoter, the hydroxyl groups on the surface of the basalt fiber react with the acyl chloride groups in the structure of acryloyl chloride, and double bonds are introduced on the surface of the basalt fiber to obtain modified basalt fiber. Then, under the action of the initiator, the double bonds on the surface of the modified basalt fiber react with the double bonds in the structure of polyvinyl alcohol monoallyl ether to obtain an inorganic fiber additive. This inorganic fiber additive is organically modified on the surface of the basalt fiber, which can effectively enhance the dispersibility of the basalt fiber in the spacecraft protective cover matrix material. Due to the hydroxyl groups in its structure, it has good compatibility with the spacecraft protective cover matrix material, which can effectively enhance the mechanical strength of the matrix material. In addition, the large number of ether bonds in its structure can effectively enhance the toughness of the matrix material, improve its impact resistance, make it not easy to be damaged, and play a more excellent protective role.

[0013] Furthermore, in step SS1, the accelerator is pyridine.

[0014] Furthermore, in step SS2, the initiator is any one of benzoyl peroxide and diisopropylbenzene peroxide.

[0015] A method for preparing a composite material for a spacecraft protective cover comprises the following preparation steps: Step 1: placing ultra-high molecular weight polyethylene, maleic anhydride grafted polyethylene, high temperature resistant modified resin, inorganic fiber additive, antioxidant, plasticizer, lubricant, and ultraviolet absorber in a high-speed mixer, setting the speed to 200-300 r / min, and fully mixing for 1-1.5 hours to obtain a mixture; Step 2: Place the mixture in a twin-screw extruder, set the screw speed to 300-500r / min, the temperature of each zone is: zone 1 temperature is 170-190°C, zone 2 temperature is 190-210°C, zone 3 temperature is 210-230°C, zone 4 temperature is 190-210°C, and the extrusion temperature is 160-180°C; melt-extrude and granulate, and obtain a spacecraft protective cover composite material after cooling.

[0016] Beneficial effects of the present invention: The present invention prepares high-temperature resistant modified resins and inorganic fiber additives in the preparation process of the spacecraft protective cover composite material, so that the prepared spacecraft protective cover composite material has excellent high-temperature resistance, mechanical strength and impact resistance, can stably exist in a high-temperature environment and is not easily damaged by high-speed impacts of micrometeorites and space debris, can meet the use requirements in a variety of environments, and has a long service life.

[0017] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0019] Figure 1 This is a thermal weight loss curve of basalt fiber, modified basalt fiber and inorganic fiber additive in the embodiment of the present invention. DETAILED DESCRIPTION

[0020] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] The preparation methods of the high temperature resistant modified resin and inorganic fiber additive in the following embodiments and comparative examples of the present invention are as follows: 1. Preparation of high temperature resistant modified resin S1: 3 g of polyphenylene sulfide with a number average molecular weight of 4000 was placed in 60 ml of toluene, and after thorough mixing, 2.6 g of methylvinyldichlorosilane and 0.6 g of benzoin dimethyl ether were added at 2 mw / cm 2 The reaction was carried out under ultraviolet irradiation for 1 hour, and the product was collected after reduced pressure distillation to obtain modified polyphenylene sulfide; S2: 3.5 g of modified polyphenylene sulfide and 3 g of 4-aminophenylboronic acid pinacol ester were placed in 100 ml of tetrahydrofuran, nitrogen was introduced, 0.2 g of triethylamine was added, the temperature was raised to 55° C. and reacted for 3 h, and the product was collected after reduced pressure distillation to obtain a high temperature resistant modified resin.

[0022] The nitrogen element analysis of modified polyphenylene sulfide and high temperature resistant modified resin using EMA 502 organic element analyzer showed that the modified polyphenylene sulfide structure did not contain nitrogen, while the nitrogen content in the high temperature resistant modified resin structure was 4.9%. This was due to the reaction between the silicon chlorine group in the modified polyphenylene sulfide structure and the amino group in the 4-aminophenylboronic acid pinacol ester structure, which introduced the nitrogen element into the modified polyphenylene sulfide structure.

[0023] 2. Preparation of Inorganic Fiber Additives SS1: 3 g of basalt fiber was placed in 100 ml of deionized water, and after ultrasonic dispersion for 10 min, 2.5 g of acryloyl chloride and 0.1 g of pyridine were added, and the mixture was reacted at room temperature for 6 h. The modified basalt fiber was obtained after filtration, washing, and vacuum drying. SS2: Place 3.5 g of modified basalt fiber in 120 ml of N,N-dimethylformamide, ultrasonically disperse for 15 min, add 3 g of polyvinyl alcohol monoallyl ether and 0.5 g of benzoyl peroxide, heat to 60 ° C and react for 5 h, filter, wash and vacuum dry to obtain the inorganic fiber additive.

[0024] The basalt fiber, modified basalt fiber and inorganic fiber additives were subjected to thermogravimetric analysis. Figure 1 It can be seen that the final mass retention rate of basalt fiber is 96.2%, and the lost part is caused by the thermal decomposition of the crystalline water in the structure; the final mass retention rate of modified basalt fiber is 51.5%, and the lost part is caused by the thermal decomposition of acryloyl chloride grafted on its surface; the final mass retention rate of inorganic fiber additives is 25.8%, and the lost part is caused by the thermal decomposition of organic matter grafted on its surface.

[0025] Example 1 Preparation of composite materials for spacecraft protective cover Step 1: Place 80 parts of ultra-high molecular weight polyethylene, 15 parts of maleic anhydride grafted polyethylene, 25 parts of high temperature resistant modified resin, 12 parts of inorganic fiber additive, 2 parts of antioxidant 1010, 3 parts of diisononyl phthalate, 2 parts of paraffin wax, and 1 part of ultraviolet absorber UV-1300 in a high-speed mixer, set the speed to 200 r / min, and mix thoroughly for 1 hour to obtain a mixture; Step 2: Place the mixture in a twin-screw extruder, set the screw speed to 300r / min, the temperature of each zone is: zone 1 temperature is 170°C, zone 2 temperature is 190°C, zone 3 temperature is 210°C, zone 4 temperature is 190°C, and the extrusion temperature is 160°C; melt-extrude and granulate, and obtain the spacecraft protective cover composite material after cooling.

[0026] Example 2 Preparation of composite materials for spacecraft protective cover Step 1, 85 parts of ultra-high molecular weight polyethylene, 20 parts of maleic anhydride grafted polyethylene, 30 parts of high temperature resistant modified resin, 13 parts of inorganic fiber additive, 3 parts of antioxidant 626, 4 parts of castor oil, 2.5 parts of white oil, and 2 parts of ultraviolet absorber UV-1577 are placed in a high-speed mixer, the speed is set to 250r / min, and the mixture is fully mixed for 1.2h to obtain a mixture; Step 2: Place the mixture in a twin-screw extruder, set the screw speed to 400r / min, the temperature of each zone is: zone 1 temperature is 180°C, zone 2 temperature is 200°C, zone 3 temperature is 220°C, zone 4 temperature is 200°C, and the extrusion temperature is 170°C; melt-extrude and granulate, and obtain the spacecraft protective cover composite material after cooling.

[0027] Example 3 Preparation of composite materials for spacecraft protective cover Step 1: Place 90 parts of ultra-high molecular weight polyethylene, 25 parts of maleic anhydride grafted polyethylene, 35 parts of high temperature resistant modified resin, 15 parts of inorganic fiber additive, 5 parts of antioxidant 5057, 5 parts of epoxy soybean oil, 3 parts of polyethylene wax, and 3 parts of ultraviolet absorber UV-928 in a high-speed mixer, set the speed to 300 r / min, and mix thoroughly for 1.5 hours to obtain a mixture; Step 2: Place the mixture in a twin-screw extruder, set the screw speed to 500r / min, the temperature of each zone is: zone 1 temperature is 190°C, zone 2 temperature is 210°C, zone 3 temperature is 230°C, zone 4 temperature is 210°C, and the extrusion temperature is 180°C; melt-extrude and granulate, and obtain the spacecraft protective cover composite material after cooling.

[0028] Comparative Example 1 Preparation of composite materials for spacecraft protective cover Step 1, 85 parts of ultra-high molecular weight polyethylene, 20 parts of maleic anhydride grafted polyethylene, 13 parts of inorganic fiber additives, 3 parts of antioxidant 626, 4 parts of castor oil, 2.5 parts of white oil, and 2 parts of ultraviolet absorber UV-1577 are placed in a high-speed mixer, the speed is set to 250r / min, and the mixture is fully mixed for 1.2h to obtain a mixture; Step 2: Place the mixture in a twin-screw extruder, set the screw speed to 400r / min, the temperature of each zone is: zone 1 temperature is 180°C, zone 2 temperature is 200°C, zone 3 temperature is 220°C, zone 4 temperature is 200°C, and the extrusion temperature is 170°C; melt-extrude and granulate, and obtain the spacecraft protective cover composite material after cooling.

[0029] Comparative Example 2 Preparation of composite materials for spacecraft protective cover Step 1, 85 parts of ultra-high molecular weight polyethylene, 20 parts of maleic anhydride grafted polyethylene, 30 parts of high temperature resistant modified resin, 3 parts of antioxidant 626, 4 parts of castor oil, 2.5 parts of white oil, and 2 parts of ultraviolet absorber UV-1577 are placed in a high-speed mixer, the speed is set to 250r / min, and the mixture is fully mixed for 1.2h to obtain a mixture; Step 2: Place the mixture in a twin-screw extruder, set the screw speed to 400r / min, the temperature of each zone is: zone 1 temperature is 180°C, zone 2 temperature is 200°C, zone 3 temperature is 220°C, zone 4 temperature is 200°C, and the extrusion temperature is 170°C; melt-extrude and granulate, and obtain the spacecraft protective cover composite material after cooling.

[0030] Comparative Example 3 Preparation of composite materials for spacecraft protective cover Step 1, 85 parts of ultra-high molecular weight polyethylene, 20 parts of maleic anhydride grafted polyethylene, 30 parts of modified polyphenylene sulfide, 13 parts of inorganic fiber additives, 3 parts of antioxidant 626, 4 parts of castor oil, 2.5 parts of white oil, and 2 parts of ultraviolet absorber UV-1577 are placed in a high-speed mixer, the speed is set to 250r / min, and the mixture is fully mixed for 1.2h to obtain a mixture; Step 2: Place the mixture in a twin-screw extruder, set the screw speed to 400r / min, the temperature of each zone is: zone 1 temperature is 180°C, zone 2 temperature is 200°C, zone 3 temperature is 220°C, zone 4 temperature is 200°C, and the extrusion temperature is 170°C; melt-extrude and granulate, and obtain the spacecraft protective cover composite material after cooling.

[0031] Comparative Example 4 Preparation of composite materials for spacecraft protective cover Step 1, 85 parts of ultra-high molecular weight polyethylene, 20 parts of maleic anhydride grafted polyethylene, 30 parts of high temperature resistant modified resin, 13 parts of modified basalt fiber, 3 parts of antioxidant 626, 4 parts of castor oil, 2.5 parts of white oil, and 2 parts of ultraviolet absorber UV-1577 are placed in a high-speed mixer, the speed is set to 250r / min, and the mixture is fully mixed for 1.2h to obtain a mixture; Step 2: Place the mixture in a twin-screw extruder, set the screw speed to 400r / min, the temperature of each zone is: zone 1 temperature is 180°C, zone 2 temperature is 200°C, zone 3 temperature is 220°C, zone 4 temperature is 200°C, and the extrusion temperature is 170°C; melt-extrude and granulate, and obtain the spacecraft protective cover composite material after cooling.

[0032] Performance Testing The composite materials for spacecraft protection covers prepared in Examples 1 to 2 and Comparative Examples 1 to 4 were made into samples that met the specifications. The samples were subjected to a tensile strength test according to the reference standard GB / T1040-2006 to determine the mechanical strength of the samples. The samples were subjected to a Vicat softening temperature test according to the reference standard GB / T1633-2000 to determine the high temperature resistance of the samples. The samples were subjected to an impact strength test according to the reference standard GB / T1043.1-2008 to determine the impact resistance of the samples. The specific test results are shown in the following table: Tensile strength / MPa Vicat softening temperature / ℃ Impact strength / kJ / mm2 Example 1 44.5 149 19.0 Example 2 44.7 150 19.2 Example 3 44.2 147 18.9 Comparative Example 1 35.3 121 17.9 Comparative Example 2 36.9 142 14.2 Comparative Example 3 42.4 134 18.0 Comparative Example 4 42.3 144 16.6 It can be seen from the above table that the samples prepared in Examples 1 to 3 all have excellent high temperature resistance, mechanical strength and impact resistance. In the sample prepared in Comparative Example 1, no high temperature resistant modified resin was added, and the high temperature resistance was general. In the sample prepared in Comparative Example 2, no inorganic fiber additive was added, the mechanical strength was not high, and the impact resistance was poor. In the sample prepared in Comparative Example 3, modified polyphenylene sulfide was directly added without adding high temperature resistant modified resin, and the high temperature resistance was not as good as that of the embodiment. In the sample prepared in Comparative Example 4, modified basalt fiber was directly added without adding inorganic fiber additives, and the impact resistance needs to be improved.

[0033] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0034] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the scope defined by the concept of the invention, they should all fall within the protection scope of the present invention.

Claims

1. A composite material for a spacecraft protective cover, It is characterized in that The invention comprises the following raw materials in parts by weight: 80-90 parts of ultra-high molecular weight polyethylene, 15-25 parts of maleic anhydride grafted polyethylene, 25-35 parts of high temperature resistant modified resin, 12-15 parts of inorganic fiber additive, 2-5 parts of antioxidant, 3-5 parts of plasticizer, 2-3 parts of lubricant and 1-3 parts of ultraviolet absorber; the high temperature resistant modified resin is prepared by taking polyphenylene sulfide as a polymer skeleton and introducing silazane and phenylboronic acid pinacol ester structures into the structure; the inorganic fiber additive is prepared by organically modifying basalt fiber and introducing a polyether structure on the surface of basalt fiber.

2. A composite material for a spacecraft protective cover according to claim 1, It is characterized in that The antioxidant is any one of antioxidant 1010, antioxidant 626, and antioxidant 5057; the plasticizer is any one of diisononyl phthalate, castor oil, and epoxidized soybean oil; the lubricant is any one of paraffin, white oil, and polyethylene wax; the ultraviolet absorber is any one of ultraviolet absorber UV-1300, ultraviolet absorber UV-1577, and ultraviolet absorber UV-928.

3. The composite material for a spacecraft protective cover according to claim 1, It is characterized in that The preparation method of the high temperature resistant modified resin comprises the following steps: S1: placing polyphenylene sulfide in toluene, stirring and mixing thoroughly, adding methyl vinyl dichlorosilane and benzoin dimethyl ether to react under ultraviolet light for 1-1.5 hours, and collecting the product after reduced pressure distillation to obtain modified polyphenylene sulfide; S2: Place modified polyphenylene sulfide and 4-aminophenylboronic acid pinacol ester in tetrahydrofuran, introduce nitrogen, add triethylamine, raise the temperature to 55-60°C and react for 3-5h, collect the product after reduced pressure distillation, and obtain a high temperature resistant modified resin.

4. A composite material for a spacecraft protective cover according to claim 3, It is characterized in that In step S1, the number average molecular weight of the polyphenylene sulfide is 4000-5000.

5. The composite material for a spacecraft protective cover according to claim 3, It is characterized in that In step S1, the irradiance of the ultraviolet light is 2-3 mw / cm 2 .

6. The composite material for a spacecraft protective cover according to claim 1, It is characterized in that The preparation method of the inorganic fiber additive comprises the following steps: SS1: Place basalt fiber in deionized water, ultrasonically disperse for 10-15 minutes, add acryloyl chloride and accelerator, react at room temperature for 6-8 hours, filter, wash, and vacuum dry to obtain modified basalt fiber; SS2: Place the modified basalt fiber in N,N-dimethylformamide, ultrasonically disperse for 15-20 minutes, add polyvinyl alcohol monoallyl ether and initiator, heat to 60-70°C and react for 5-6 hours, filter, wash and vacuum dry to obtain inorganic fiber additive.

7. A composite material for a spacecraft protective cover according to claim 6, It is characterized in that In step SS1, the accelerator is pyridine.

8. The composite material for a spacecraft protective cover according to claim 6, It is characterized in that In step SS2, the initiator is any one of benzoyl peroxide and diisopropylbenzene peroxide.

9. A method for preparing the composite material for a spacecraft protective cover as claimed in claim 1, It is characterized in that The method comprises the following preparation steps: Step 1: placing ultra-high molecular weight polyethylene, maleic anhydride grafted polyethylene, high temperature resistant modified resin, inorganic fiber additive, antioxidant, plasticizer, lubricant, and ultraviolet absorber in a high-speed mixer, setting the speed to 200-300 r / min, and fully mixing for 1-1.5 hours to obtain a mixture; Step 2: Place the mixture in a twin-screw extruder, set the screw speed to 300-500r / min, the temperature of each zone is: zone 1 temperature is 170-190°C, zone 2 temperature is 190-210°C, zone 3 temperature is 210-230°C, zone 4 temperature is 190-210°C, and the extrusion temperature is 160-180°C; melt-extrude and granulate, and obtain a spacecraft protective cover composite material after cooling.

Citation Information

Patent Citations

  • Antistatic colorful reflective fabric reflective coating and preparation method thereof

    CN116949823A

  • Super-tough PE composite material and preparation method thereof

    CN118126433A

  • Polyphenylenesulfide composition for powder coating

    US5272185A