Ultrahigh molecular weight polyethylene modified polypropylene and preparation method thereof
By adding ultra-high molecular weight polyethylene and other modifiers to polypropylene materials, the problem of insufficient toughness and ultraviolet aging resistance of polypropylene materials is solved, and modified polypropylene materials with excellent performance are prepared, suitable for pharmaceutical packaging materials and medical care instrument.
Patent Information
- Application Number
- CN202411334067.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-12-06
AI Technical Summary
Polypropylene materials are prone to scratching and degradation of performance in pharmaceutical packaging materials and medical devices due to poor toughness, unsmooth surface, poor friction resistance and poor UV aging resistance.
Use ultra-high molecular weight polyethylene, linear low-density polyethylene, compatibility agents, lubricants, antioxidants and anti-UV absorbers to prepare modified polypropylene materials through specific mixing and processing processes to improve their toughness and surface Smoothness and anti-UV aging properties.
Modified polypropylene materials significantly improve toughness and friction resistance, reduce surface wear, enhance resistance to ultraviolet rays, and extend the service life of parts.
Smart Images

Figure SMS_2 
Figure SMS_3 
Figure SMS_4
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of polypropylene, in particular to polypropylene modified with ultra-high molecular weight polyethylene and a preparation method thereof. Background Art
[0002] Polypropylene is a thermoplastic resin made by polymerization of propylene, referred to as PP. It is a white waxy material with a transparent and light appearance and a melting point of up to 167°C. It is one of the five commonly used general-purpose plastics with properties such as light specific gravity and high impact resistance. Polypropylene is divided into three types according to the arrangement of methyl groups: isotactic polypropylene, atactic polypropylene and syndiotactic polypropylene. It is non-toxic, odorless, low in density, high in heat resistance, non-absorbent, and good in electrical insulation. It is widely used in the production of fiber products, medical equipment, automobiles, chemical containers and other products. It is also used in the packaging of food and medicines. It has been widely used in the field of industrial production, and tens of millions of tons are consumed worldwide each year.
[0003] At present, in the field of pharmaceutical packaging materials, especially spray pumps or certain medical devices, many parts are made of ordinary polypropylene injection molding and then assembled together. Some movable parts often need to rotate or rotate, or move up and down or left and right. Because ordinary polypropylene has poor toughness, rough and dry surface, and poor friction resistance, the surface of parts made of polypropylene is either easily scratched, or two or more polypropylene parts that move against each other are difficult to rotate. At the same time, some polypropylene medical devices have been used for a long time. After being exposed to natural light, sunlight and other light sources, the surface of the white plastic parts gradually turns yellow and ages, and the performance deteriorates.
[0004] Therefore, it is necessary to modify the polypropylene material to improve the toughness, surface smoothness, friction resistance and UV aging resistance of polypropylene products. Summary of the invention
[0005] In view of the above-mentioned shortcomings of the prior art, the purpose of the present invention is to provide a polypropylene modified with ultra-high molecular weight polyethylene and a preparation method thereof, so as to solve the problems in the prior art that the polypropylene has poor toughness, a rough and dry surface, poor friction resistance, and poor resistance to aging and yellowing.
[0006] To achieve the above objectives and other related objectives, the present invention is achieved through the following technical solutions.
[0007] The first aspect of the present invention is to provide a polypropylene modified with ultra-high molecular weight polyethylene, comprising the following raw materials in parts by weight: 40-80 parts of polypropylene, 5-20 parts of ultra-high molecular weight polyethylene, 1-10 parts of linear low density polyethylene, 1-5 parts of a compatibilizer, 1-5 parts of a lubricant, 1-5 parts of a processing base oil, 1-2 parts of an antioxidant, and 1-5 parts of an anti-ultraviolet absorber.
[0008] The second aspect of the present invention is to provide a method for preparing polypropylene modified with ultra-high molecular weight polyethylene, comprising the following steps:
[0009] (1) mixing ultra-high molecular weight polyethylene and processing base oil to obtain pretreated ultra-high molecular weight polyethylene;
[0010] (2) mixing polypropylene, linear low-density polyethylene, a compatibilizer, a lubricant, an antioxidant and an anti-ultraviolet absorber to obtain a mixture, adding the pretreated ultra-high molecular weight polyethylene obtained in step (1) to the mixture, stirring to obtain a mixture;
[0011] (3) melt-extruding the mixture obtained in step (2) to obtain a plastic strip;
[0012] (4) Cooling and pelletizing the plastic strips obtained in step (3) to obtain modified polypropylene particles.
[0013] As described above, the polypropylene modified with ultra-high molecular weight polyethylene and the preparation method thereof of the present invention have the following beneficial effects:
[0014] (1) The present invention utilizes ultra-high molecular weight polyethylene and lubricants to improve the lubricity of the polypropylene material surface and the toughness of the polypropylene material;
[0015] (2) The present invention adopts a conical twin-screw extruder for extrusion granulation, and the modified polypropylene obtained thereby has better comprehensive properties.
[0016] (3) The present invention adopts raw materials such as polypropylene, ultra-high molecular weight polyethylene, linear low-density polyethylene, compatibilizer and lubricant, adjusts and optimizes these raw materials, and adjusts the processing technology at the same time. The obtained modified polypropylene material has uniform mixing, good toughness and excellent comprehensive mechanical properties. DETAILED DESCRIPTION
[0017] In order to make the purpose of the invention, technical solutions and beneficial technical effects of the present invention clearer, the present invention is further described in detail below in conjunction with embodiments. People familiar with this technology can easily understand other advantages and effects of the present invention from the contents disclosed in this specification.
[0018] The modified polypropylene prepared by the present invention is mixed with raw materials such as ultra-high molecular weight polyethylene, linear low density polyethylene, processing lubricant, antioxidant, and anti-ultraviolet absorber, so that the modified polypropylene prepared has good friction resistance, good toughness, and good anti-ultraviolet aging performance; the surface of the parts manufactured by the present invention is smooth, has good friction resistance, is not easy to be scratched, and two or more polypropylene parts that move relative to each other are also difficult to rotate. When the parts made of modified polypropylene are exposed to ultraviolet rays, light aging and oxidation may occur, thereby causing the friction resistance of the surface of the parts to decrease, and at the same time, affecting the toughness of the parts, resulting in a decrease in the toughness of the parts. Therefore, the present application adds an anti-ultraviolet absorber to cooperate with the ultra-high molecular weight polyethylene, thereby improving the anti-ultraviolet performance on the premise of improving the friction resistance of the modified polypropylene. In addition, the modified polypropylene prepared by the present invention has high friction resistance, and after being subjected to friction, the surface wear is small, which helps to maintain the integrity of the product surface and the effectiveness of the anti-ultraviolet agent. Therefore, the present application improves the friction resistance and toughness of the modified polypropylene on the premise of improving the anti-ultraviolet property of the modified polypropylene, so as to facilitate the improvement of the use effect of the modified polypropylene.
[0019] The extended part of this application and the effect description of the extended part, including but not limited to subsequent data analysis, mechanism description, etc.
[0020] The first aspect of the present invention is to provide a polypropylene modified with ultra-high molecular weight polyethylene, comprising the following raw materials in parts by weight: 40-80 parts of polypropylene, 5-20 parts of ultra-high molecular weight polyethylene, 1-10 parts of linear low density polyethylene, 1-5 parts of a compatibilizer, 1-5 parts of a lubricant, 1-5 parts of a processing base oil, 1-2 parts of an antioxidant, and 1-5 parts of an anti-ultraviolet absorber.
[0021] The present invention mainly solves the problems that the surface of common polypropylene materials and products made of common polypropylene materials is not smooth, dry, and has poor friction resistance, and the surface of parts made of polypropylene is either easily scratched, or two or more polypropylene parts that move relative to each other are difficult to rotate. At the same time, it solves the problem that UHMWPE ultra-high molecular weight polyethylene is difficult to extrude and modify; at the same time, it solves the problem that polypropylene is easily degraded, aged, and yellowed.
[0022] The invention adopts ultra-high molecular weight polyethylene to modify polypropylene. The ultra-high molecular weight polyethylene is a polyethylene with a relative molecular weight of more than 1.5 million, and has excellent properties that other plastics do not have, such as high impact strength, excellent wear resistance, low friction coefficient, good low temperature resistance and good biocompatibility. It is easy to cooperate with linear low density polyethylene, compatibilizer, lubricant, processing base oil, antioxidant and anti-ultraviolet absorber, so as to improve the comprehensive performance of the prepared modified polypropylene.
[0023] in,
[0024] The addition of ultra-high molecular weight polyethylene (UHMWPE) is mainly to utilize the advantages of the lowest surface friction coefficient and the most lubricating surface of ultra-high molecular weight polyethylene to compound and modify polypropylene, thereby obtaining a smooth surface, anti-friction and wear-resistant polypropylene.
[0025] Linear low-density polyethylene (LLDPE) plays a transitional role in polypropylene modification. Since ultra-high molecular weight polyethylene has a large molecular weight and high melt viscosity and is difficult to process, adding some LLDPE can improve the melt strength and reduce the melt viscosity, making it easier for the mixed material to be extruded and granulated.
[0026] The addition of compatibilizer facilitates the melt compatibility of UHMWPE, LLDPE and PP after melting, so that the melts of each component are melted and mixed evenly;
[0027] The addition of lubricant promotes lubrication between UHMWPE, LLDPE and PP melt molecules, reduces extrusion resistance, and thus solves the problem of UHMWPE being difficult to extrude;
[0028] The addition of processing base oil is used to pre-fill and wet UHMWPE, so that UHMWPE can be mixed evenly with other components and extruded and granulated more easily;
[0029] The addition of antioxidants can prevent the raw materials from being oxidized during the modification and processing of PP, and can also play an anti-aging role in the modified polypropylene.
[0030] The addition of anti-ultraviolet absorbers makes it easier to use with antioxidants to prevent the surface of plastic products from prematurely aging and yellowing due to exposure to natural light, visible light, and outdoor sunlight.
[0031] In some embodiments of the present invention, the polypropylene modified with ultra-high molecular weight polyethylene comprises the following raw materials in parts by weight: 40-80 parts of polypropylene, 5-20 parts of ultra-high molecular weight polyethylene, 1-10 parts of linear low density polyethylene, 1-5 parts of compatibilizer, 1-5 parts of lubricant, 1-5 parts of processing base oil, 1-2 parts of antioxidant, and 1-5 parts of anti-ultraviolet absorber.
[0032] In some specific embodiments of the present invention, the polypropylene modified with ultra-high molecular weight polyethylene comprises the following raw materials in parts by weight: 40-60 parts of polypropylene, 5-15 parts of ultra-high molecular weight polyethylene, 1-6 parts of linear low density polyethylene, 1-3 parts of compatibilizer, 1-3 parts of lubricant, 1-3 parts of processing base oil, 1-2 parts of antioxidant, and 1-3 parts of anti-ultraviolet absorber.
[0033] In some specific embodiments of the present invention, the polypropylene modified with ultra-high molecular weight polyethylene comprises the following raw materials in parts by weight: 60-80 parts of polypropylene, 15-20 parts of ultra-high molecular weight polyethylene, 6-10 parts of linear low density polyethylene, 3-5 parts of compatibilizer, 3-5 parts of lubricant, 3-5 parts of processing base oil, 1-2 parts of antioxidant, and 3-5 parts of anti-ultraviolet absorber.
[0034] In some specific embodiments of the present invention, the polypropylene modified with ultra-high molecular weight polyethylene includes the following raw materials in parts by weight: 40 parts of polypropylene, 5 parts of ultra-high molecular weight polyethylene, 1 part of linear low density polyethylene, 1 part of compatibilizer, 1 part of lubricant, 1 part of processing base oil, 1 part of antioxidant, and 1 part of anti-ultraviolet absorber.
[0035] In some specific embodiments of the present invention, the polypropylene modified with ultra-high molecular weight polyethylene includes the following raw materials in parts by weight: 80 parts of polypropylene, 20 parts of ultra-high molecular weight polyethylene, 10 parts of linear low density polyethylene, 5 parts of compatibilizer, 5 parts of lubricant, 5 parts of processing base oil, 2 parts of antioxidant, and 5 parts of anti-ultraviolet absorber.
[0036] In some embodiments of the present invention, the weight average molecular weight of the polypropylene is 2500-3500 g / mol, specifically 2500-2800 g / mol, 2800-3000 g / mol, 3000-3200 g / mol, 3200-3500 g / mol, typically but not limitingly, for example, 2500 g / mol, 2800 g / mol, 3000 g / mol, 3200 g / mol, 3500 g / mol.
[0037] In some embodiments of the present invention, the weight average molecular weight of the ultra-high molecular weight polyethylene is 1.7 million to 4.4 million g / mol, specifically 1.7 million to 2.5 million g / mol, 2.5 million to 3 million g / mol, 3 million to 3.8 million g / mol, 3.8 million to 4.4 million g / mol; typically but not limitingly, for example, 1.7 million g / mol, 2.5 million g / mol, 3 million g / mol, 3.8 million g / mol, 4.4 million g / mol.
[0038] In some embodiments of the present invention, the density of the linear low-density polyethylene is 0.92-0.93 g / cm 3 , weight average molecular weight is 10,000-25,000 g / mol, MI = 10g / 10min-60g / 10min.
[0039] In some embodiments of the present invention, the compatibilizer is selected from one or more of polypropylene grafted maleic anhydride and polyethylene grafted maleic anhydride.
[0040] In some embodiments of the present invention, the lubricant is an organic lubricant, preferably, the organic lubricant is selected from one or more of polypropylene wax, polyethylene wax, silicone masterbatch, polytetrafluoroethylene, and paraffin powder. The organic lubricant has better compatibility with other components and is not easy to change the color of the material.
[0041] In some embodiments of the present invention, the antioxidant is selected from one or more of antioxidant 1010, antioxidant 1076, and antioxidant BHT246.
[0042] In some embodiments of the present invention, the processing base oil is selected from one or more of 150N, 500N, KN4006 and KN4010.
[0043] In some embodiments of the present invention, the anti-ultraviolet absorber is selected from one or more of salicylates, benzophenones, benzotriazoles, substituted acrylonitriles and triazines. The anti-ultraviolet absorber is an anti-ultraviolet absorbing masterbatch.
[0044] The second aspect of the present invention is to provide a method for preparing polypropylene modified with ultra-high molecular weight polyethylene, comprising the following steps: (1) mixing ultra-high molecular weight polyethylene and processing base oil to obtain pretreated ultra-high molecular weight polyethylene;
[0045] (2) mixing polypropylene, linear low-density polyethylene, a compatibilizer, a lubricant, an antioxidant and an anti-ultraviolet absorber to obtain a mixture, adding the pretreated ultra-high molecular weight polyethylene obtained in step (1) to the mixture, stirring to obtain a mixture;
[0046] (3) melt-extruding the mixture obtained in step (2) to obtain a plastic strip;
[0047] (4) Cooling and pelletizing the plastic strips obtained in step (3) to obtain modified polypropylene particles.
[0048] The invention firstly uses processing base oil to process ultra-high molecular weight polyethylene, so that ultra-high molecular weight polyethylene powder is pre-filled with oil, which is convenient for the surface of ultra-high molecular weight polyethylene powder to be wetted and lubricated in advance, so that the melt processing resistance of ultra-high molecular weight polyethylene is small during processing, and then the ultra-high molecular weight polyethylene after oil filling is mixed with other components, so that the modified polypropylene particles prepared have better performance; in addition, if the ultra-high molecular weight polyethylene powder is not filled with oil, the mixing uniformity of the ultra-high molecular weight polyethylene not filled with oil and other components is not good, so that the modified polypropylene prepared has poor performance, and then the pre-treated ultra-high molecular weight polyethylene is matched with linear low-density polyethylene, a compatibilizer, a lubricant and an anti-ultraviolet absorber to modify the polypropylene, so that the modified polypropylene prepared has better performance.
[0049] In some embodiments of the present invention, the mixing temperature in step (1) is 10-40°C and the mixing time is 10-30min. The mixing temperature can be 10-20°C, 20-30°C, 30-40°C, typically but not limited to 10°C, 20°C, 30°C, 40°C; the mixing time can be 10-20min, 20-30min, typically but not limited to 10min, 20min, 30min.
[0050] In some embodiments of the present invention, the stirring temperature in step (2) is 30-70°C; the stirring time is 10-30 min. The stirring temperature can be 30-40°C, 40-50°C, 50-70°C, typically but not limiting, for example, 30°C, 40°C, 50°C, 70°C; the stirring time can be 10-20 min, 20-30 min, typically but not limiting, for example, 10 min, 20 min, 30 min.
[0051] In some embodiments of the present invention, the temperature of the melt extrusion section in the step (3) is divided into the following zones: zone 1 150°C, zone 2 160-180°C, zone 3 170-200°C, zone 4 170-200°C, zone 5 170-2100°C, zone 6 180-210°C, zone 7 180-210°C, zone 8 180-210°C, zone 9 180-210°C, zone 10 180-210°C, die head zone 170-200°C, the residence time in each zone is 1-5 min; the screw speed during the extrusion process is 200-450 rpm.
[0052] In some embodiments of the present invention, the extrusion equipment in step (3) is a conical twin-screw extruder.
[0053] Because ultra-high molecular weight polyethylene has a large molecular weight and a long molecular chain, the molecular weights are easily entangled with each other during processing to form a large number of entanglements. Pure ultra-high molecular weight polyethylene is extremely difficult to process and shape. For example, during melt processing, the melt annuality is extremely high, and the melt presents a rubber-like high elastic state with no fluidity; ultra-high molecular weight polyethylene has a small friction coefficient, and it is easy to process in an ordinary screw, but difficult to feed with high heat. Therefore, using ultra-high molecular weight polyethylene to modify polypropylene requires a special processing technology to extrude and granulate the modified material.
[0054] Conventional polymer material processing and modification usually uses twin-screw extruders for extrusion granulation. The twin-screw extruder is an ordinary parallel twin-screw extruder. The twin-screw extruder has the advantages of excellent mixed plasticization effect and high efficiency for the modification and granulation of ordinary general-purpose plastics or engineering plastics; however, some special polymers with low melt index will have feeding difficulties and cannot be squeezed. For example, powdery and low melt index polymer materials such as PVC and ultra-high molecular weight polyethylene are difficult to process and modify with twin-screw extruders. The depth of the twin-screw groove is uniform; while the conical twin-screw extruder is made of The feeding section to the discharging section has a taper angle, and the depth of the screw groove changes from deep to shallow, which makes feeding very easy and the ability to push materials to the extruder head is stronger than that of a twin screw. The conical twin screw has the following advantages: 1. Good feeding characteristics. The feeding section has a deeper screw groove depth and a larger diameter to ensure that larger volumes of materials can be added more easily; 2. The diameter of the screw gradually decreases along the extrusion direction, and the circumferential speed of the screw also decreases accordingly, so that the material does not have to withstand excessive shear; 3. Since the diameter of the conical twin screw extruder gradually decreases along the extrusion direction, the diameter of the screw at the discharging end is smaller, and the back pressure on the screw is also reduced. The extrusion modification of polypropylene by a conical twin screw extruder has a better modification effect.
[0055] The present invention is further described below by way of examples, but the scope of the present invention is not limited thereto.
[0056] When the embodiment gives a numerical range, it should be understood that, unless otherwise specified in the present invention, the two endpoints of each numerical range and any numerical value between the two endpoints can be selected. Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those generally understood by those skilled in the art. If specific conditions are not specified in the embodiment, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for all reagents or instruments, they are conventional products that can be purchased commercially. In addition to the specific methods, equipment, and materials used in the embodiments, according to the grasp of the prior art by those skilled in the art and the record of the present invention, any method, equipment, and material of the prior art similar or equivalent to the method, equipment, and material in the embodiments of the present invention can also be used to realize the present invention.
[0057] The anti-ultraviolet absorber of the present invention is an anti-ultraviolet absorber masterbatch, which is selected from one or more of salicylates, benzophenones, benzotriazoles, substituted acrylonitriles and triazines. Specifically, the anti-ultraviolet absorber is an anti-UV light auxiliary agent masterbatch.
[0058] The present invention has no particular limitation on the source of raw materials, and commercially available products known to those skilled in the art may be used. Specifically, the sources of raw materials of the present invention are shown in Table 1.
[0059] Table 1
[0060]
[0061]
[0062] Table 2 Ratio of raw material components of modified polypropylene toughened, friction-reducing and wear-resistant materials of Examples 1-4 and Comparative Examples 1-2
[0063]
[0064] Example
[0065] Example 1
[0066] The modified polypropylene toughened, friction-reducing and wear-resistant material of this embodiment has a raw material composition ratio as shown in Table 2. The weight average molecular weight of the polypropylene is 3000 g / mol; the weight average molecular weight of the ultra-high molecular weight polyethylene is 4.2 million g / mol; the density of the linear low-density polyethylene is 0.92 g / cm 3 , weight average molecular weight is 15,000 g / mol, MI=50 g / 10min; the compatibilizer is polypropylene grafted maleic anhydride; the lubricant is silicone masterbatch; the antioxidant is antioxidant 1010; the anti-ultraviolet absorber is anti-UV light additive masterbatch.
[0067] The preparation method of the modified polypropylene toughened, friction-reducing and wear-resistant material of this embodiment comprises the following steps:
[0068] (1) mixing ultra-high molecular weight polyethylene and processing base oil to obtain pretreated ultra-high molecular weight polyethylene; wherein the mixing temperature is 25° C. and the mixing time is 30 minutes;
[0069] (2) mixing polypropylene, linear low-density polyethylene, a compatibilizer, a lubricant, an antioxidant and an anti-ultraviolet absorber to obtain a mixture, adding the pretreated ultra-high molecular weight polyethylene obtained in step (1) to the mixture, stirring to obtain a mixture; the stirring temperature is 50° C. and the stirring time is 20 min;
[0070] (3) melt-extrude the mixed material obtained in step (2) through a conical twin-screw extruder to obtain a plastic strip; the temperature of the melt extrusion section is divided into the following zones: zone 1 150° C., zone 2 160-180° C., zone 3 170-200° C., zone 4 170-200° C., zone 5 170-2100° C., zone 6 180-210° C., zone 7 180-210° C., zone 8 180-210° C., zone 9 180-210° C., zone 10 180-210° C., and die head zone 170-200° C., and the residence time in each zone is 1-5 min; the screw speed during the extrusion process is 200-450 rpm;
[0071] (4) Cooling and pelletizing the plastic strips obtained in step (3) to obtain modified polypropylene particles.
[0072] Example 2
[0073] The modified polypropylene toughened, friction-reducing, and wear-resistant material of this embodiment has a raw material composition ratio as shown in Table 2. The difference from Embodiment 1 is that the raw material composition ratio is different.
[0074] Example 3
[0075] The modified polypropylene toughened, friction-reducing, and wear-resistant material of this embodiment has a raw material composition ratio as shown in Table 2. The difference from Embodiment 1 is that the raw material composition ratio is different.
[0076] Example 4
[0077] The modified polypropylene toughened, friction-reducing, and wear-resistant material of this embodiment has a raw material composition ratio as shown in Table 2. The difference from Embodiment 1 is that the raw material composition ratio is different.
[0078] Comparative Example
[0079] Comparative Example 1
[0080] The modified polypropylene toughened, friction-reducing and wear-resistant material of this comparative example has a raw material composition ratio as shown in Table 2, which is different from Example 1 in that the raw material composition ratio is different, and no ultra-high molecular weight polyethylene, compatibilizer, or processing base oil is added.
[0081] Comparative Example 2
[0082] The modified polypropylene toughened, friction-reducing and wear-resistant material of this comparative example has a raw material composition ratio as shown in Table 2, which is different from Example 1 in that the raw material composition ratio is different, and no ultra-high molecular weight polyethylene, compatibilizer, processing base oil, organic lubricant, and anti-UV light additive masterbatch are added.
[0083] Comparative Example 3
[0084] The modified polypropylene toughened, friction-reducing and wear-resistant material of this comparative example has a raw material composition ratio as shown in Table 2, which is different from Example 1 in that no linear low-density polyethylene, processing oil and lubricant are added, and the raw material composition ratio is different.
[0085] Comparative Example 4
[0086] The modified polypropylene toughened, friction-reducing and wear-resistant material of this comparative example has a raw material composition ratio as shown in Table 2. The difference from Example 1 is that the raw material composition ratio is different, and no processing base oil, lubricant and anti-ultraviolet absorber are added.
[0087] Performance Testing
[0088] The modified polypropylenes obtained in Examples 1-4 and Comparative Examples 1-4 were tested for melt index, tensile yield strength, elongation at break, impact strength and friction coefficient. The test results are shown in Table 3.
[0089] Take the modified polypropylene obtained in Examples 1-4 and Comparative Examples 1-4, and according to the detection method in GB / T14522-2008, add about 2% white masterbatch to the modified polypropylene raw material particles for injection molding to make a 95x30x3mm standard color block, and then put each group of color block samples into an ultraviolet UV aging box for 168h, and then take out the samples and cool them to room temperature and measure the color difference on a colorimeter to see the color difference value change between the sample and the white standard color plate after UV aging. The smaller the color difference value change, the better the UV resistance, wherein the white masterbatch is commercially available, and the commercially available white masterbatch well known to those skilled in the art can be used.
[0090] Table 3 Performance test results of modified polypropylene of Examples 1-4 and Comparative Examples 1-4
[0091]
[0092] Combining Example 1 and Comparative Example 1, and combining the data in Table 3, it can be seen that the difference between Example 1 and Comparative Example 1 is that ultra-high molecular weight polyethylene, a compatibilizer and a processing base oil are added to Example 1, and the modified polypropylene obtained thereby has a higher tensile yield strength, a higher elongation at break, a greater impact strength, a lower friction coefficient, and a stronger UV resistance. By using the processing base oil to fill the ultra-high molecular weight polyethylene and then modifying the polypropylene, the polypropylene obtained thereby has better performance in all aspects.
[0093] Combining Example 1 and Comparative Example 2, and combining the data in Table 3, it can be seen that the modified polypropylene obtained in Example 1 has better performance in all aspects. The difference between Example 1 and Comparative Example 2 is that no ultra-high molecular weight polyethylene, compatibilizer, processing base oil, lubricant and anti-ultraviolet absorber are added to Comparative Example 2, and the toughness, friction resistance and anti-ultraviolet performance of the modified polypropylene obtained thereby are not as good as those of the modified polypropylene obtained in Example 1. By matching polypropylene with raw materials such as ultra-high molecular weight polyethylene and anti-ultraviolet absorber, the modified polypropylene obtained thereby has better performance.
[0094] Combining Example 1 and Comparative Example 3, and combining the data in Table 3, it can be seen that the modified polypropylene prepared in Example 1 has a higher tensile yield strength, a lower friction coefficient, and better overall performance. The difference between Example 1 and Comparative Example 3 is that: Comparative Example 3 does not add linear low-density polyethylene, processing base oil, and lubricant, and the performance of the modified polypropylene prepared thereby is not as good as that of the modified polypropylene prepared in Example 1. By adding three components of linear low-density polyethylene, processing base oil and lubricant, the addition of these three components facilitates improving the modification effect of ultra-high molecular weight polyethylene on polypropylene, and the modified polypropylene prepared thereby has better performance.
[0095] Combining Example 1 and Comparative Example 4, and combining the data in Table 3, it can be seen that the overall performance of the modified polypropylene obtained in Example 1 is better than the overall performance of the modified polypropylene obtained in Comparative Example 4. The difference between Example 1 and Comparative Example 4 is that no processing base oil, base oil and anti-ultraviolet absorber are added to Comparative Example 4. It can be inferred that the addition of processing base oil, base oil and anti-ultraviolet absorber helps to cooperate with ultra-high molecular weight polyethylene, thereby improving the modification effect on polypropylene.
[0096] In combination with Examples 1-4 and the data in Table 3, it can be seen that by adjusting the amount of ultra-high molecular weight polyethylene added in Examples 1-4, the amount of ultra-high molecular weight polyethylene added in Examples 1-4 gradually increases, and the tensile yield strength of the modified polypropylene thus obtained shows a trend of first increasing and then decreasing, the elongation at break shows a trend of first increasing and then decreasing, the impact strength shows a trend of first increasing and then decreasing, the friction coefficient shows a trend of continuously decreasing, the UV resistance is better, and the ultra-high molecular weight polyethylene has a greater influence on the performance of the modified polypropylene.
[0097] Combining Comparative Example 1 and Comparative Example 2, and combining the data in Table 3, it can be seen that the ΔE of Comparative Example 2 is greater than the ΔE of Comparative Example 1. The difference between Comparative Example 2 and Comparative Example 1 is that no anti-ultraviolet absorber is added in Comparative Example 2, and the addition of anti-ultraviolet absorber has a greater effect on improving the anti-ultraviolet performance of polypropylene.
[0098] Combining Comparative Example 1 and Comparative Example 3, and combining the data in Table 3, it can be seen that the melt index of Comparative Example 3 is less than the melt index of Comparative Example 1, and the tensile yield strength, elongation at break, and impact strength of Comparative Example 3 are all less than the tensile yield strength, elongation at break, and impact strength of Comparative Example 1. The friction coefficient of Comparative Example 3 is less than the friction coefficient of Comparative Example 1. The difference between Comparative Example 1 and Comparative Example 3 is that the amounts of polypropylene and ultra-high molecular weight polyethylene added in Comparative Example 3 are different, and no processing base oil, linear low density polyethylene, or lubricant is added in Comparative Example 3. It can be found that although the ultra-high molecular weight polyethylene itself has better tensile strength and toughness, if When mixed with polypropylene without adding processing base oil, linear low-density polyethylene and lubricant, the tensile properties and strength of polypropylene become worse. The inventors speculate that this may be because: ultra-high molecular weight polyethylene has a large molecular weight and a long molecular chain. During processing, the molecular weights are easily entangled with each other to form a large number of entanglements, making processing and molding difficult. When ultra-high molecular weight polyethylene is treated with linear low-density polyethylene, processing base oil and lubricant, the fluidity of ultra-high molecular weight polyethylene becomes better, which is convenient for being fully mixed with polypropylene, thereby improving the tensile yield strength, elongation at break and impact strength of polypropylene, and at the same time, reducing the friction coefficient of polypropylene.
[0099] Combining Comparative Example 1 and Comparative Example 4, and combining the data in Table 3, it can be seen that the melt index of Comparative Example 4 is less than the melt index of Comparative Example 1, and the tensile yield strength, elongation at break, and impact strength of Comparative Example 4 are all less than the tensile yield strength, elongation at break, and impact strength of Comparative Example 1, and the friction coefficient of Comparative Example 4 is greater than the friction coefficient of Comparative Example 1. The difference between Comparative Example 1 and Comparative Example 4 is that the amounts of polypropylene and ultra-high molecular weight polyethylene added in Comparative Example 4 are different, and an excessive amount of ultra-high molecular weight polyethylene is added to Comparative Example 4. At the same time, no processing base oil, lubricant, or anti-ultraviolet absorber is added to Comparative Example 4. It can be found that when an excessive amount of ultra-high molecular weight polyethylene is added, the mechanical properties of the blended polypropylene become worse. The inventors speculate that when no processing base oil and lubricant are added, the excessive ultra-high molecular weight polyethylene is difficult to process and mold, that is, after excessive addition of UHMWPE, it is difficult to fully melt, plasticize, and mix evenly, and the UHMWPE and PP melts are unevenly mixed, thereby resulting in poor tensile yield strength, elongation at break, and impact strength performance of the modified polypropylene.
[0100] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A polypropylene modified with ultra-high molecular weight polyethylene, characterized in that: The invention comprises the following raw materials in parts by weight: 40-80 parts of polypropylene, 5-20 parts of ultra-high molecular weight polyethylene, 1-10 parts of linear low-density polyethylene, 1-5 parts of compatibilizer, 1-5 parts of lubricant, 1-5 parts of processing base oil, 1-2 parts of antioxidant and 1-5 parts of anti-ultraviolet absorber.
2. The polypropylene modified with ultra-high molecular weight polyethylene according to claim 1, characterized in that: The weight average molecular weight of the polypropylene is 2500-3500 g / mol.
3. The polypropylene modified with ultra-high molecular weight polyethylene according to claim 1, characterized in that: The weight average molecular weight of the ultra-high molecular weight polyethylene is 1.7 million to 4.4 million g / mol.
4. The polypropylene modified with ultra-high molecular weight polyethylene according to claim 1, characterized in that: The density of the linear low-density polyethylene is 0.92-0.93 g / cm 3 , weight average molecular weight is 10,000-25,000 g / mol, MI = 10g / 10min-60g / 10min.
5. The polypropylene modified with ultra-high molecular weight polyethylene according to claim 1, characterized in that: Also includes one or more of the following characteristics: A1) the compatibilizer is selected from one or more of polypropylene grafted maleic anhydride and polyethylene grafted maleic anhydride; A2) the lubricant is an organic lubricant, preferably, the organic lubricant is selected from one or more of polypropylene wax, polyethylene wax, silicone masterbatch, polytetrafluoroethylene, and paraffin powder; A3) the antioxidant is selected from one or more of antioxidant 1010, antioxidant 1076, and antioxidant BHT246; A4) The processing base oil is selected from one or more of 150N, 500N, KN4006 and KN4010.
6. The polypropylene modified with ultra-high molecular weight polyethylene according to claim 1, characterized in that: The anti-ultraviolet absorber is selected from one or more of salicylates, benzophenones, benzotriazoles, substituted acrylonitriles and triazines.
7. A method for preparing polypropylene modified with ultra-high molecular weight polyethylene as claimed in any one of claims 1 to 6, characterized in that: The steps include: (1) mixing ultra-high molecular weight polyethylene and processing base oil to obtain pretreated ultra-high molecular weight polyethylene; (2) mixing polypropylene, linear low-density polyethylene, a compatibilizer, a lubricant, an antioxidant and an anti-ultraviolet absorber to obtain a mixture, adding the pretreated ultra-high molecular weight polyethylene obtained in step (1) to the mixture, stirring to obtain a mixture; (3) melt-extruding the mixture obtained in step (2) to obtain a plastic strip; (4) Cooling and pelletizing the plastic strips obtained in step (3) to obtain modified polypropylene particles.
8. The method for preparing polypropylene modified with ultra-high molecular weight polyethylene according to claim 7, characterized in that: The temperature of the melt extrusion section in the step (3) is divided into the following zones: zone 1 150°C, zone 2 160-180°C, zone 3 170-200°C, zone 4 170-200°C, zone 5 170-2100°C, zone 6 180-210°C, zone 7 180-210°C, zone 8 180-210°C, zone 9 180-210°C, zone 10 180-210°C, and die head zone 170-200°C, and the residence time in each zone is 1-5 min; the screw speed during the extrusion process is 200-450 rpm.
9. The method for preparing polypropylene modified with ultra-high molecular weight polyethylene according to claim 7, characterized in that: The extrusion equipment in step (3) is a conical twin-screw extruder.
10. The method for preparing polypropylene modified with ultra-high molecular weight polyethylene according to claim 7, characterized in that: Also includes one or more of the following features: 11) The mixing temperature in step (1) is 10-40°C and the mixing time is 10-30min; 21) The stirring temperature in step (2) is 30-70°C; the stirring time is 10-30 min.