Production method of high-resilience polyurethane thermoplastic elastomer

By using the addition reaction of unsaturated polyether polyol and DOPO in the production of thermoplastic polyurethane elastomers, combined on the polymer chain and introducing chemical crosslinking points, the poor mechanical properties of thermoplastic polyurethane elastomers and the influence of flame retardants is solved. The problem is that high break strength, elongation of break and resilience are achieved.

CN119081388APending Publication Date: 2024-12-06KELCOMY (GUANGZHOU) HIGH-TECH MATERIALS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410985968.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing thermoplastic polyurethane elastomers have poor mechanical properties, flame retardants have a greater impact on temperature and mechanical properties, and the application units are narrower.

Method used

Unsaturated polyether polyols are used to replace traditional saturated polyether polyols, and DOPO is added to the process for addition reaction, bound to the polymer macromolecular chain, and chemical crosslinking points are introduced, through esterification or amidation reaction Prepare highly resilient polyurethane thermoplastic elastomers.

Benefits of technology

The break strength, elongation and resilience of thermoplastic polyurethane elastomers are improved, the negative impact of flame retardants on mechanical properties is avoided, and the mechanical properties and repetitive processability of the material are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081388A_ABST
    Figure CN119081388A_ABST
Patent Text Reader

Abstract

The invention discloses a production method of a high-resilience polyurethane thermoplastic elastomer, and relates to the technical field of high polymer materials, and the method comprises the following steps: S1, preparing a prepolymer through esterification or amidation reaction, S2, adding a chain extender, a catalyst and 0-50wt% of DOPO into the prepolymer, and carrying out a reaction for 2-3h to obtain the high-resilience polyurethane thermoplastic elastomer. S3, sequentially adding PVC resin, the mixture A, a heat stabilizer, a lubricant and a processing aid into a high-speed kneading machine, S4, heating a double-roller open mill to 80-110 DEG C, adding nitrile rubber and a vulcanizing agent, and uniformly mixing, and S5, feeding the mixture into a screw of a double-screw extruder through a feeding and filling system; according to the invention, unsaturated polyether polyol is adopted to replace saturated polyether polyol used in a traditional process, so that DOPO can be subjected to an addition reaction with unsaturated bonds after being added, and the influence of flame retardant particles on the mechanical properties of the thermoplastic polyurethane elastomer is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, in particular to a method for producing a high-elasticity polyurethane thermoplastic elastomer. Background Art

[0002] Thermoplastic polyester elastomer (TPEE), also known as polyester rubber, has both the excellent elasticity of rubber and the easy processing of thermoplastic plastics. After searching, the Chinese patent authorization number CN102816427A discloses a highly flame-retardant, highly heat-resistant, halogen-free flame-retardant thermoplastic polyurethane elastomer cable material and a preparation method thereof. The invention improves the problem of too narrow processing temperature range of thermoplastic polyurethane elastomer cable material, and at the same time improves the heat resistance of the cable material. Thermoplastic polyurethane elastomer is used as the matrix, and high-temperature resistant materials are melt-blended with it. A new type of intumescent flame retardant that does not migrate when exposed to water is used as the flame retardant of the matrix. Although this method uses an intumescent flame retardant to improve the flame retardant properties of the flame retardant, the mechanical properties of the TPU material are general, the application unit is narrow, and the use of an external flame retardant to improve the flame retardant properties of the material inevitably affects the temperature mechanical properties of the material. Summary of the invention

[0003] In view of the deficiencies of the prior art, the present invention provides a method for producing a high-resilience polyurethane thermoplastic elastomer, which solves the problems raised in the background technology.

[0004] To achieve the above object, the present invention is implemented by the following technical scheme: a method for producing a high resilience polyurethane thermoplastic elastomer, the steps of which are as follows:

[0005] S1: Prepare a prepolymer by esterification or amidation reaction, add 100 parts of dibasic acid, 35-300 parts of diol and 0.4-33 parts of cross-linking agent into a reaction container, continuously discharge small molecules generated in the reaction system during the reaction, stop the reaction when the water output reaches 75%-85% of the theoretical water output, place it at 50-60°C and evacuate, the vacuum degree is -0.4--0.2kPa, and the prepolymer is obtained; S2: Add a chain extender, a catalyst and 0-50wt% of DOPO to the prepolymer, continue to react at 70-80°C for 2-4h, and add a polyether diol after the reaction to carry out ester exchange or amide exchange reaction: after the first step of the reaction is completed, reduce the pressure to normal pressure, add 15-2000 parts of polyether diol, 0.5-20 parts of catalyst and 0.5-20 parts of heat stabilizer to the prepolymer, dry it Then mixture A is obtained; S3: PVC resin, mixture A, heat stabilizer, lubricant and processing aid are added in sequence to a high-speed kneading machine, and the materials are completely plasticized and discharged, and the discharge temperature is controlled at 80-100°C to obtain mixture B; S4: The double-roll mill is heated to 80°C-110°C, nitrile rubber and vulcanizing agent are added, mixed evenly, and sheets are discharged. On a normal temperature roll, vulcanizing aid and plasticizer are added to the above materials in sequence, and mixed for 2-5 minutes to obtain mixture C; S5: First, mixture B is plasticized on a double roll for 2-5 minutes, and after plasticization, mixture C is added to a double-roll mill and mixed for 8-14 minutes at a temperature of 150-170°C, and then fed into the screw of a twin-screw extruder through a feeding and perfusion system; then a melt extrusion reaction is carried out, and underwater pelletizing and drying are carried out to obtain the thermoplastic polyurethane elastomer, that is, the product.

[0006] Preferably, the nitrile rubber formula in S4 includes the following components and contents in parts by weight: 80-100 parts of nitrile rubber, 4-12 parts of vulcanizing agent, 1-3 parts of vulcanizing aid, and 5-20 parts of plasticizer.

[0007] Preferably, the extrusion temperature of the twin-screw extruder described in S5 is 120-240° C., and the actual screw speed of the twin-screw extruder is 100-300 rpm.

[0008] Preferably, the mixture A in S2 contains hard segments and soft segments, the hard segments are polyesters, accounting for 10-90wt% of the total elastomer; the soft segments are unsaturated polyether polyols, accounting for 10-90wt% of the total elastomer.

[0009] Preferably, the unsaturation degree of the unsaturated polyether polyol in S2 is 0.020-0.050 mol / kg, and the number average molecular weight of the unsaturated polyether polyol is 2000-3000.

[0010] Preferably, the chain extender in S2 includes any one of 1,4-butenediol, 4-cyclopentene-1,3-diol or 4-benzodiquinone, or a combination of at least two thereof.

[0011] Preferably, the catalyst in S2 is any one of stannous octoate, dibutyltin dioctoate or dibutyltin dilaurate, or a combination of at least two thereof.

[0012] Preferably, the intrinsic viscosity of the prepared elastomer is 0.771 dL / g, the elastic recovery rate is 95%, the breaking strength is 33 MPa, the breaking elongation is 550%, and the Shore hardness is 41D.

[0013] Preferably, the reaction process in S1 includes introducing nitrogen to replace the air in the reactor, pressurizing to 2-4 bar, and heating to 230-260° C. at a stirring speed of 50-500 r / min.

[0014] Preferably, S2 also includes reacting at 200-220° C. and a stirring speed of 50-500 r / min for 0.5-1 h, then gradually reducing the pressure to 0-200 Pa, raising the temperature to 220-280° C., and continuing the reaction for 1-4 h.

[0015] The present invention provides a method for producing a high-resilience polyurethane thermoplastic elastomer, which has the following beneficial effects:

[0016] The method for producing a high-resilience polyurethane thermoplastic elastomer adopts unsaturated polyether polyol to replace the saturated polyether polyol used in the traditional process, so that DOPO can undergo addition reaction with unsaturated bonds after being added, thereby combining with the polymer macromolecular chain, avoiding the influence of flame retardant particles on the mechanical properties of the thermoplastic polyurethane elastomer, and improving the mechanical properties of the elastomer by introducing a proper amount of chemical cross-linking points. The prepared elastomer has high breaking strength, breaking elongation, rebound resilience and repeatability, making up for the shortcomings of the prior art. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is a schematic diagram of the process of the present invention. DETAILED DESCRIPTION

[0018] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0019] Embodiment 1:

[0020] A method for producing a high resilience polyurethane thermoplastic elastomer, the steps of which are as follows:

[0021] S1: Preparing a prepolymer by esterification or amidation reaction, adding 100 parts of dibasic acid, 300 parts of diol and 33 parts of cross-linking agent into a reaction vessel, introducing nitrogen to replace the air in the reactor, pressurizing to 4 bar, and heating to 260° C. at a stirring speed of 500 r / min. During the reaction, small molecules generated in the reaction system are continuously discharged. When the water output reaches 85% of the theoretical water output, the reaction is stopped, and the reactor is placed at 60° C. and evacuated to a vacuum degree of -0.2 kPa to obtain a prepolymer;

[0022] S2: adding a chain extender, a catalyst and 50 wt% DOPO to the prepolymer, and continuing the reaction at 80°C for 4 hours, wherein the chain extender includes 1,4-butene diol, and the catalyst is stannous octoate. After the reaction, adding a polyether diol for ester exchange or amide exchange reaction: after the first step of the reaction is completed, reducing the pressure to normal pressure, adding 2000 parts of polyether diol, 20 parts of catalyst and 20 parts of heat stabilizer to the prepolymer, reacting at 220°C and a stirring speed of 500r / min for 1 hour, then gradually reducing the pressure to 200Pa, raising the temperature to 280°C, continuing the reaction for 4 hours, and drying to obtain a mixture A, which contains a hard segment and a soft segment, wherein the hard segment is polyester, accounting for 90 wt% of the total amount of the elastomer; the soft segment is an unsaturated polyether polyol, accounting for 90 wt% of the total amount of the elastomer; the unsaturation degree of the unsaturated polyether polyol is 0.050 mol / kg, and the number average molecular weight of the unsaturated polyether polyol is 3000;

[0023] S3: Add PVC resin, mixture A, heat stabilizer, lubricant and processing aid in a high-speed kneader in sequence, and discharge the materials after they are completely plasticized. The discharge temperature is controlled at 100° C. to obtain mixture B;

[0024] S4: The double-roll mill is heated to 110°C, and nitrile rubber and vulcanizing agent are added, mixed evenly, and sheets are produced. On a normal temperature roll, a vulcanizing agent and a plasticizer are added to the above materials in sequence, and mixed for 5 minutes to obtain a mixture C, wherein the nitrile rubber formula includes the following components and weight parts: 100 parts of nitrile rubber, 12 parts of vulcanizing agent, 3 parts of vulcanizing agent, and 20 parts of plasticizer;

[0025] S5: First, plasticize the mixture B on a twin-roller for 5 minutes. After the plasticization is completed, add the mixture C into a twin-roller mill and mix for 14 minutes at a temperature of 170°C. Then, feed it into the screw of a twin-screw extruder through a feeding and perfusion system; the extrusion temperature of the twin-screw extruder is 240°C, and the actual screw speed of the twin-screw extruder is 300rpm. Then, a melt extrusion reaction is carried out, and after underwater pelletizing and drying, the thermoplastic polyurethane elastomer is obtained, that is, the product.

[0026] Embodiment 2:

[0027] A method for producing a high resilience polyurethane thermoplastic elastomer, the steps of which are as follows:

[0028] S1: Preparing a prepolymer by esterification or amidation reaction, adding 100 parts of dibasic acid, 35 parts of diol and 0.4 parts of cross-linking agent into a reaction vessel, introducing nitrogen to replace the air in the reactor, pressurizing to 2 bar, and heating to 230° C. at a stirring speed of 50 r / min. During the reaction, small molecules generated in the reaction system are continuously discharged. When the water output reaches 75% of the theoretical water output, the reaction is stopped, and the reactor is placed at 50° C. and evacuated to a vacuum degree of -0.4 kPa to obtain a prepolymer;

[0029] S2: Add chain extender, catalyst and 20wt% DOPO to the prepolymer, and continue to react at 70°C for 2h, wherein the chain extender includes 1,4-butene diol and 4-cyclopentene-1, and the catalyst is a combination of stannous octoate and dibutyltin dioctoate. After the reaction, add polyether diol to carry out ester exchange or amide exchange reaction: after the first step of the reaction is completed, reduce the pressure to normal pressure, add 15 parts of polyether diol, 0.5 parts of catalyst and 0.5 parts of heat stabilizer to the prepolymer, and heat at 200°C. , reacting at a stirring speed of 50r / min for 0.5h, then gradually reducing the pressure to 0Pa, raising the temperature to 220°C, continuing the reaction for 1h, and drying to obtain a mixture A, which contains a hard segment and a soft segment, wherein the hard segment is polyester, accounting for 10wt% of the total amount of the elastomer; the soft segment is an unsaturated polyether polyol, accounting for 10wt% of the total amount of the elastomer; the unsaturation degree of the unsaturated polyether polyol is 0.020mol / kg, and the number average molecular weight of the unsaturated polyether polyol is 2000;

[0030] S3: Add PVC resin, mixture A, heat stabilizer, lubricant and processing aid in a high-speed kneader in sequence, and discharge the materials after they are completely plasticized. The discharge temperature is controlled at 80° C. to obtain mixture B;

[0031] S4: The temperature of the double-roll mill is raised to 80°C, and nitrile rubber and vulcanizing agent are added, mixed evenly, and sheets are produced. On a normal temperature roll, a vulcanizing agent and a plasticizer are added to the above materials in sequence, and mixed for 2 minutes to obtain a mixture C, wherein the nitrile rubber formula includes the following components and weight contents: 80 parts of nitrile rubber, 4 parts of vulcanizing agent, 1 part of vulcanizing agent, and 5 parts of plasticizer;

[0032] S5: First, plasticize the mixture B on a twin-roller for 2 minutes. After the plasticization is completed, add the mixture C into a twin-roller mill and mix for 8 minutes at a temperature of 150°C. Then, feed it into the screw of a twin-screw extruder through a feeding and perfusion system; the extrusion temperature of the twin-screw extruder is 120°C, and the actual screw speed of the twin-screw extruder is 100rpm. Then, a melt extrusion reaction is carried out, and after underwater pelletizing and drying, the thermoplastic polyurethane elastomer is obtained, that is, the product.

[0033] Embodiment 3:

[0034] A method for producing a high resilience polyurethane thermoplastic elastomer, the steps of which are as follows:

[0035] S1: Preparing a prepolymer by esterification or amidation reaction, adding 100 parts of dibasic acid, 100 parts of diol and 20 parts of cross-linking agent into a reaction vessel, introducing nitrogen to replace the air in the reactor, pressurizing to 3 bar, and heating to 240° C. at a stirring speed of 100 r / min. During the reaction, small molecules generated in the reaction system are continuously discharged. When the water output reaches 80% of the theoretical water output, the reaction is stopped, and the reactor is placed at 55° C. and evacuated to a vacuum degree of -0.1 kPa to obtain a prepolymer;

[0036] S2: Add chain extender, catalyst and 20wt% DOPO to the prepolymer, and continue to react at 75°C for 3h, wherein the chain extender includes 1,4-butene diol, and the catalyst is a combination of stannous octoate and dibutyltin dioctoate. After the reaction, add polyether diol to carry out ester exchange or amide exchange reaction: After the first step of the reaction is completed, reduce the pressure to normal pressure, add 1000 parts of polyether diol, 15 parts of catalyst and 15 parts of heat stabilizer to the prepolymer, and heat at 210°C and 100r / min stirring speed for 0.7h, then gradually reduce the pressure to 50Pa, raise the temperature to 230°C, continue to react for 2h, and obtain mixture A after drying. Mixture A contains hard segments and soft segments. The hard segment is polyester, accounting for 80wt% of the total amount of the elastomer; the soft segment is unsaturated polyether polyol, accounting for 80wt% of the total amount of the elastomer; the unsaturation degree of the unsaturated polyether polyol is 0.025mol / kg, and the number average molecular weight of the unsaturated polyether polyol is 2500;

[0037] S3: Add PVC resin, mixture A, heat stabilizer, lubricant and processing aid in a high-speed kneader in sequence, and discharge the materials after they are completely plasticized. The discharge temperature is controlled at 85° C. to obtain mixture B;

[0038] S4: The double-roll mill is heated to 100°C, and nitrile rubber and vulcanizing agent are added, mixed evenly, and sheets are produced. On a normal temperature roll, a vulcanizing agent and a plasticizer are added to the above materials in sequence, and mixed for 3 minutes to obtain a mixture C, wherein the nitrile rubber formula includes the following components and weight contents: 85 parts of nitrile rubber, 8 parts of vulcanizing agent, 2 parts of vulcanizing agent, and 15 parts of plasticizer;

[0039] S5: First, plasticize the mixture B on a twin-roller for 4 minutes. After the plasticization is completed, add the mixture C into a twin-roller mill and mix for 12 minutes at a temperature of 155°C. Then, feed it into the screw of a twin-screw extruder through a feeding and perfusion system; the extrusion temperature of the twin-screw extruder is 200°C, and the actual screw speed of the twin-screw extruder is 200rpm. Then, a melt extrusion reaction is carried out, and after underwater pelletizing and drying, the thermoplastic polyurethane elastomer is obtained, that is, the product.

[0040] Embodiment 4:

[0041] A method for producing a high resilience polyurethane thermoplastic elastomer, the steps of which are as follows:

[0042] S1: Preparing a prepolymer by esterification or amidation reaction, adding 100 parts of dibasic acid, 100 parts of diol and 20 parts of cross-linking agent into a reaction container, introducing nitrogen to replace the air in the reactor, pressurizing to 3.5 bar, and heating to 240° C. at a stirring speed of 350 r / min. During the reaction, small molecules generated in the reaction system are continuously discharged. When the water output reaches 77% of the theoretical water output, the reaction is stopped, and the reactor is placed at 56° C. and evacuated to a vacuum degree of -0.4 kPa to obtain a prepolymer;

[0043] S2: Add chain extender, catalyst and 50wt% DOPO to the prepolymer, and continue to react at 75°C for 3.5h, wherein the chain extender includes 3-diol, and the catalyst is a combination of dibutyltin dioctoate and dibutyltin dilaurate. After the reaction, add polyether diol to carry out ester exchange or amide exchange reaction: After the first step of the reaction is completed, reduce the pressure to normal pressure, add 1500 parts of polyether diol, 15 parts of catalyst and 15 parts of heat stabilizer to the prepolymer, and heat at 215°C and 300 r / min stirring speed for 0.8h, then gradually reduce the pressure to 20Pa, raise the temperature to 255°C, continue to react for 3h, and obtain mixture A after drying. Mixture A contains hard segments and soft segments. The hard segment is polyester, accounting for 80wt% of the total amount of elastomer; the soft segment is unsaturated polyether polyol, accounting for 70wt% of the total amount of elastomer; the unsaturation degree of the unsaturated polyether polyol is 0.020mol / kg, and the number average molecular weight of the unsaturated polyether polyol is 2500;

[0044] S3: Add PVC resin, mixture A, heat stabilizer, lubricant and processing aid in a high-speed kneader in sequence, and discharge the materials after they are completely plasticized. The discharge temperature is controlled at 100° C. to obtain mixture B;

[0045] S4: The double-roll mill is heated to 105°C, and nitrile rubber and vulcanizing agent are added, mixed evenly, and sheets are produced. On a normal temperature roll, a vulcanizing agent and a plasticizer are added to the above materials in sequence, and mixed for 4 minutes to obtain a mixture C, wherein the nitrile rubber formula includes the following components and weight contents: 95 parts of nitrile rubber, 10 parts of vulcanizing agent, 2 parts of vulcanizing agent, and 15 parts of plasticizer;

[0046] S5: First, plasticize the mixture B on a twin-roller for 3.5 minutes. After the plasticization is completed, add the mixture C into a twin-roller mill and mix for 12 minutes at a temperature of 160°C. Then, feed it into the screw of a twin-screw extruder through a feeding and perfusion system; the extrusion temperature of the twin-screw extruder is 220°C, and the actual screw speed of the twin-screw extruder is 150rpm. Then, a melt extrusion reaction is carried out, and underwater pelletizing and drying are carried out to obtain the thermoplastic polyurethane elastomer, that is, the product.

[0047] Comparative Example 1:

[0048] In this comparative example, except that the unsaturated polyether polyol was replaced by a saturated polyether polyol, other conditions were the same as those in Example 1.

[0049] Comparative Example 2:

[0050] In this comparative example, except that DOPO was not added, other conditions were the same as those in Example 2.

[0051] Table 1:

[0052]

[0053] According to the results in Table 1, it can be seen that the thermoplastic polyurethane elastomer prepared by the present invention has excellent mechanical properties, with a tensile strength of up to 69 MPa, an elongation at break of up to 320%, and a rebound rate of about 35%. However, in Comparative Example 1, saturated polyether polyols were added, resulting in DOPO being unable to be incorporated into the polymer macromolecule, thereby causing the mechanical properties and flame retardant properties of the prepared thermoplastic polyurethane elastomer to decrease; in Comparative Example 2, DOPO was not added, resulting in a flame retardant property of only V-2 level, and the mechanical properties and flame retardant properties of the prepared thermoplastic polyurethane elastomer were worse than those of Examples 1-4.

[0054] In summary, the present invention adopts unsaturated polyether polyols to replace the saturated polyether polyols used in the traditional process, so that DOPO can undergo addition reaction with the unsaturated bonds after being added, thereby combining with the polymer macromolecular chain, avoiding the influence of flame retardant particles on the mechanical properties of thermoplastic polyurethane elastomer, and improving the mechanical properties of the elastomer by introducing an appropriate amount of chemical cross-linking points. The prepared elastomer has high breaking strength, elongation at break, resilience and repeatability, which makes up for the shortcomings of the prior art.

[0055] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is defined by the attached claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention. Any figure mark in the claims should not be regarded as limiting the claims involved.

[0056] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A method for producing a high resilience polyurethane thermoplastic elastomer, characterized in that: The steps are as follows: S1: Preparing a prepolymer by esterification or amidation reaction, adding 100 parts of dibasic acid, 35-300 parts of diol and 0.4-33 parts of cross-linking agent into a reaction container, continuously discharging small molecules generated in the reaction system during the reaction, stopping the reaction when the water output reaches 75%-85% of the theoretical water output, placing it at 50-60°C and evacuating the vacuum to -0.4-0.2kPa, and thus obtaining the prepolymer; S2: adding a chain extender, a catalyst and 0-50wt% of DOPO to the prepolymer, continuing the reaction at 70-80°C for 2-4h, and adding a polyether diol to carry out an ester exchange or an amide exchange reaction after the reaction is completed: after the first step of the reaction is completed, reducing the pressure to normal pressure, adding 15-2000 parts of polyether diol, 0.5-20 parts of a catalyst and 0.5-20 parts of a heat stabilizer to the prepolymer, and obtaining a mixture A after drying; S3: Add PVC resin, mixture A, heat stabilizer, lubricant and processing aid in a high-speed kneader in sequence, and discharge the materials after they are completely plasticized. The discharge temperature is controlled at 80-100° C. to obtain mixture B; S4: The double-roll mill is heated to 80-110°C, and nitrile rubber and vulcanizing agent are added and mixed evenly to form a sheet. On a normal temperature roll, a vulcanizing agent and a plasticizer are added to the above materials in sequence, and mixed for 2-5 minutes to obtain a mixture C; S5: First, plasticize the mixture B on a twin-roller for 2-5 minutes. After the plasticization is completed, add the mixture C into a twin-roller mill and mix for 8-14 minutes at a temperature of 150-170° C., and then feed it into the screw of a twin-screw extruder through a feeding and injection system; then, perform a melt extrusion reaction, perform underwater pelletizing and drying, and obtain the thermoplastic polyurethane elastomer, that is, the product.

2. A method for producing a highly resilient polyurethane thermoplastic elastomer according to claim 1, characterized in that: The nitrile rubber formula in S4 includes the following components and contents in parts by weight: 80-100 parts of nitrile rubber, 4-12 parts of vulcanizing agent, 1-3 parts of vulcanizing aid, and 5-20 parts of plasticizer.

3. The method for producing a highly resilient polyurethane thermoplastic elastomer according to claim 1, characterized in that: The extrusion temperature of the twin-screw extruder described in S5 is 120-240° C., and the actual screw speed of the twin-screw extruder is 100-300 rpm.

4. The method for producing a highly resilient polyurethane thermoplastic elastomer according to claim 1, characterized in that: The mixture A in S2 contains hard segments and soft segments, wherein the hard segments are polyesters, accounting for 10-90 wt % of the total amount of the elastomer; and the soft segments are unsaturated polyether polyols, accounting for 10-90 wt % of the total amount of the elastomer.

5. The method for producing a highly resilient polyurethane thermoplastic elastomer according to claim 1, characterized in that: The unsaturation degree of the unsaturated polyether polyol in S2 is 0.020-0.050 mol / kg, and the number average molecular weight of the unsaturated polyether polyol is 2000-3000.

6. The method for producing a highly resilient polyurethane thermoplastic elastomer according to claim 1, characterized in that: The chain extender in S2 includes any one of 1,4-butenediol, 4-cyclopentene-1,3-diol or 4-benzodiquinone, or a combination of at least two thereof.

7. The method for producing a high resilience polyurethane thermoplastic elastomer according to claim 1, characterized in that: The catalyst in S2 is any one of stannous octoate, dibutyltin dioctoate or dibutyltin dilaurate, or a combination of at least two thereof.

8. The method for producing a high resilience polyurethane thermoplastic elastomer according to claim 1, characterized in that: The intrinsic viscosity of the prepared elastomer is 0.771 dL / g, the elastic recovery rate is 95%, the breaking strength is 33 MPa, the breaking elongation is 550%, and the Shore hardness is 41D.

9. The method for producing a highly resilient polyurethane thermoplastic elastomer according to claim 1, characterized in that: The reaction process in S1 includes introducing nitrogen to replace the air in the reactor, pressurizing to 2-4 bar, and heating to 230-260° C. at a stirring speed of 50-500 r / min.

10. The method for producing a high resilience polyurethane thermoplastic elastomer according to claim 1, characterized in that: The step S2 also includes reacting at 200-220° C. and a stirring speed of 50-500 r / min for 0.5-1 h, then gradually reducing the pressure to 0-200 Pa, raising the temperature to 220-280° C., and continuing the reaction for 1-4 h.