Filter element material, preparation method and application thereof, filter element and application thereof
By using materials such as nylon 6 and polystyrene, combined with graphene oxide and reactive compatibilizer, filter element materials with porous structure were prepared, which solved the problems of small water-touch area and insufficient durability of existing filter element materials, and achieved the Improved efficient humidification and filtration capabilities.
Patent Information
- Application Number
- CN202411369859.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-12-06
AI Technical Summary
The existing humidifier filter element material has a small water-touch area, which leads to low humidification efficiency, and is difficult to filter fine particles. The material is not tough enough, making it difficult to meet the durability requirements for long-term use.
Using nylon 6 and polystyrene as the main raw materials, combined with graphene oxide and reactive compatibilizer, filter element materials with porous structure and high specific surface area are prepared through extrusion drawing, injection molding, thinning and etching processes. Increase the water-touch area and improve antibacterial properties.
It significantly improves the humidification efficiency and moisture evaporation efficiency of the filter element, has antibacterial properties and the ability to filter fine particles, and at the same time enhances the mechanical properties of the material, meeting the durability requirements for long-term use.
Smart Images

Figure BDA0005067290880000121 
Figure BDA0005067290880000131 
Figure BDA0005067290880000141
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of filter element materials, and in particular relates to a filter element material and a preparation method and application thereof, a filter element and application thereof. Background Art
[0002] Air humidifiers are common household appliances in people's daily lives, used to increase the humidity in the room. Compared with traditional humidifiers, fogless humidifiers are popular because of their safe, effective, energy-saving, environmentally friendly, and high humidification capacity, and the market demand is growing. The working principle of the cold evaporative fogless humidifier is to use a water pump to pump water out of the water tank and pour it onto the filter element, and then use a fan to blow air to evaporate the water molecules on the filter element into the air. The surface area and water absorption of the evaporation filter element are important indicators that affect the humidification capacity. At present, the materials of the humidifier filter element are mainly fiber cotton, sponge, activated carbon and hollow fiber membrane. The common characteristics of these materials are good water absorption, strong toughness, corrosion resistance, etc., but the filter element has a small water-wetting area. Summary of the invention
[0003] In view of this, the object of the present invention is to provide a filter element material and a preparation method and application thereof, a filter element and application thereof. The filter element material provided by the present invention has the advantage of a large water-wetting area.
[0004] The present invention provides a filter element material, the preparation raw materials include main raw materials and auxiliary raw materials;
[0005] The main raw materials include nylon 625-75 parts, polystyrene 25-75 parts and reactive compatibilizer 0.5-5 parts;
[0006] The auxiliary raw material is graphene oxide;
[0007] The amount of the auxiliary raw material is 0.5-2% of the mass of the main raw material;
[0008] The reactive compatibilizer is a graft copolymer of polystyrene and glycidyl methacrylate.
[0009] Preferably, the weight average molecular weight of the nylon 6 is 20000-30000 g / mol; the weight average molecular weight of the polystyrene is 250000-350000 g / mol; the particle size of the graphene oxide is 300-500 nm;
[0010] The reactive compatibilizer is PS-PGMA-G or PS-PGMA-P.
[0011] The present invention also provides a method for preparing the filter element material described in the above technical solution, comprising the following steps:
[0012] Nylon 6, polystyrene, a reactive compatibilizer and graphene oxide are mixed, and then extruded, drawn and granulated to obtain a premix;
[0013] Injection molding the premix to obtain an injection molded part;
[0014] Thinning the injection molded part to obtain a prefabricated sheet;
[0015] The prefabricated sheet is etched to obtain the filter element material.
[0016] Preferably, the temperature program of the extrusion wire drawing is 150-170°C, 190-210°C, 230-250°C, 230-250°C, 230-250°C, 230-250°C, 230-250°C, 230-250°C, 230-250°C, 230-250°C, 220-240°C;
[0017] The screw speed of the extrusion wire drawing is 110-130rpm;
[0018] The feeding rate of the extrusion wire drawing is 1 to 3%;
[0019] The screw torque of the extrusion wire drawing is ≤50Nm.
[0020] Preferably, the temperature program of the injection molding is: the heating temperature of the first injection molding stage is 230-250°C, the heating temperature of the second injection molding stage is 230-250°C, and the heating temperature of the injection molding head is 220-240°C;
[0021] The pressure procedure of the injection molding is as follows: the injection holding pressure is 4-8 MPa, and the injection extrusion pressure is 4-9 MPa.
[0022] Preferably, the thinning temperature is 200-210°C;
[0023] The thinning includes pre-pressing thinning and pressurizing thinning;
[0024] The pre-pressing and thinning pressure is 3-7 MPa and the time is 1-5 min;
[0025] The pressure of the pressurized thinning is 12-18 MPa, and the time is 5-10 minutes.
[0026] Preferably, the etching reagent used is tetrahydrofuran;
[0027] The etching time is 24 to 48 hours.
[0028] The present invention also provides a filter element, comprising fan blades, wherein the fan blades are assembled from the filter element material described in the above technical solution or the filter element material prepared by the preparation method.
[0029] Preferably, the number of the fan blades is 140 to 160;
[0030] The size of the fan blade is 50-300 mm*10-60 mm*0.4-1 mm.
[0031] The present invention also provides the use of the filter element material described in the above technical solution or the filter element material prepared by the preparation method or the filter element in the preparation of a humidifier.
[0032] The invention provides a filter element material. The raw materials for preparing the filter element material include a main raw material and an auxiliary raw material. The main raw material includes 25-75 parts of nylon 6, 25-75 parts of polystyrene and 0.5-5 parts of a reactive compatibilizer. The auxiliary raw material is graphene oxide. The amount of the auxiliary raw material is 0.5-2% of the mass of the main raw material. The reactive compatibilizer is a graft copolymer of polystyrene and glycidyl methacrylate.
[0033] The present invention uses nylon 6 (PA6) and polystyrene (PS) as the main raw materials of the filter element material, because PA6 has excellent mechanical strength and corrosion resistance, and high toughness, and the PA6 molecular chain contains high-density amide groups, which are very easy to absorb water, so that the filter element material can quickly absorb water; PA6 and PS are blended, and the obtained mixed material forms a porous material after etching away part of PS, which can increase the specific surface area of the filter element material, thereby increasing the water-wetting area of the filter element material, and finally improving the humidification efficiency of the humidifier. Polystyrene is hydrophobic, which is conducive to water evaporation. At the same time, there is a certain polarity difference between PA6 and PS, which will reduce the mechanical properties of the blend of the two. The present invention uses a graft copolymer of polystyrene and glycidyl methacrylate as a reactive compatibilizer. The molecular structure of the reactive compatibilizer contains a polystyrene chain, and the end carries an epoxy group. The polystyrene chain can be well compatible with PS, and the epoxy group can also react and bond with the carboxyl and amino groups in the PA6 molecule to improve the compatibility of PA6 and PS, thereby obtaining a PA6 and PS blend with better compatibility and mechanical properties; and the reactive compatibilizer can make the PA6 and PS mix more uniform and delicate, laying the foundation for improving the water absorption and water evaporation capacity of the filter material, and being used in a humidifier, the humidification efficiency of the humidifier can be significantly improved. The raw materials for preparing the filter material provided by the present invention include graphene oxide (GO), GO has good antibacterial and antifungal capabilities, while improving the strength of the filter material, improving the antibacterial property of the filter material, making the filter material more durable in actual use. The present invention prepares the filter material by mixing PA6, PS, GO and a reactive compatibilizer in a specific ratio, which has an antibacterial effect and can also regulate the water absorption and evaporation balance of the filter material. In addition, PS is cheap and can effectively reduce the cost of the filter material.
[0034] The present invention also provides a method for preparing the filter element material described in the above technical solution, comprising the following steps: mixing nylon 6, polystyrene, a reactive expander and graphene oxide, and sequentially performing extrusion, drawing and granulation to obtain a premix; injection molding the premix to obtain an injection molded part; thinning the injection molded part to obtain a prefabricated sheet; etching the prefabricated sheet to obtain the filter element material.
[0035] The present invention makes PA6 have a certain melt orientation and forms an ordered fiber layer by extruding PA6, PS, a reactive compatibilizer and graphite oxide, and then performing injection molding and thinning. After the PS on the surface of the prefabricated sheet is etched away, grooves and porous structures appear on the surface of the obtained filter material, which increases the specific surface area of the filter material and enhances the water absorption performance; at the same time, the grooves and porous structures on the surface of the filter material are conducive to strengthening the capillary action of the filter material, accelerating the evaporation of water, and improving the humidification efficiency of the humidifier. The existing filter material sponge, fiber cotton and other materials are relatively soft and cannot be directly made into filter blades. The filter material of the present invention can be directly made into humidifier filter blades. After etching, a large number of fiber gaps, grooves and porous structures are generated on the surface of the filter material, which greatly increases the specific surface area of the filter material, can effectively increase the water-wetting area of the filter material, and help to improve the water evaporation efficiency. In addition, the filter material used in the present invention has sufficient mechanical strength and can meet the strength requirements of the filter blades. In addition, the filter element material with a large number of fiber gaps, grooves and porous structures can also filter out fine particles. In addition, the filter element material prepared by the present invention has an antibacterial effect. The preparation method provided by the present invention has abundant raw material sources, a simple preparation method, low cost, and has market application prospects.
[0036] The present invention also provides a filter element, whose fan blades are assembled from the filter element material described in the above technical solution, and the filter element is used to prepare a humidifier. Compared with the traditional humidifier filter element, the filter element provided by the present invention has the functions of both filter element water absorption and fan blades to increase the evaporation and flow of water. The humidifier uses a water pump to pump water out of the water tank and pour it onto the filter element, and then the fan blows air to evaporate the water on the filter element into the air. The filter element assembled with the filter element material of the present invention has a higher specific surface area and water absorption capacity, a large water-wetting area, and a higher water evaporation efficiency. It also has the advantages of antibacterial, filtering fine particles and durability. It does not need to be cleaned and replaced frequently, which greatly improves the convenience of using the humidifier. The filter element prepared from this new material is expected to replace the existing filter element on the market and become the filter element material of a high-efficiency cold evaporation humidifier, promoting technological progress and product upgrades in the home appliance industry. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 This is a schematic diagram of the filter element prepared in Example 1;
[0038] Figure 2 This is a SEM image of the filter element material prepared in Example 1;
[0039] Figure 3 This is a SEM image of the filter element material prepared in Comparative Example 1;
[0040] Figure 4 Schematic diagram of two common water evaporation methods in humidifiers;
[0041] Figure 5 This is a test diagram of water evaporation performance;
[0042] Figure 6 This is a photo of the filter element of a commercially available humidifier after being soaked in tap water for 14 days. DETAILED DESCRIPTION
[0043] The present invention provides a filter element material, the preparation raw materials include main raw materials and auxiliary raw materials;
[0044] The main raw materials include nylon 625-75 parts, polystyrene 25-75 parts and reactive compatibilizer 0.5-5 parts;
[0045] The auxiliary raw material is graphene oxide;
[0046] The amount of the auxiliary raw material is 0.5-2% of the mass of the main raw material;
[0047] The reactive compatibilizer is a graft copolymer of polystyrene and glycidyl methacrylate.
[0048] In the present invention, unless otherwise specified, the raw materials used in the present invention are preferably commercially available products.
[0049] The raw materials for preparing the filter element material provided by the present invention include main raw materials and auxiliary raw materials. In the present invention, the main raw material includes 25 to 75 parts by mass of nylon 6, more preferably 40 to 70 parts by mass, and further preferably 40 to 60 parts by mass, and specifically can be 25 parts by mass, 30 parts by mass, 35 parts by mass, 40 parts by mass, 45 parts by mass, 50 parts by mass, 55 parts by mass, 60 parts by mass, 65 parts by mass, 70 parts by mass or 75 parts by mass. In the present invention, the weight average molecular weight of the nylon 6 is preferably 20,000 to 30,000 g / mol. In the present invention, the density of the nylon 6 is preferably 1.0 to 1.4 g / cm 3 , more preferably 1.05 to 1.3 g / cm 3 , more preferably 1.1 to 1.2 g / cm 3In the present invention, the main raw material includes 25 to 75 parts by mass of polystyrene, more preferably 25 to 70 parts by mass, and further preferably 40 to 60 parts by mass, and specifically 27 parts by mass, 37 parts by mass, 40 parts by mass, 47 parts by mass, 50 parts by mass, 51 parts by mass, 52 parts by mass, 57 parts by mass or 60 parts by mass. In the present invention, the weight average molecular weight of the polystyrene is 250,000 to 350,000 g / mol.
[0050] The present invention uses nylon 6 and polystyrene as the main raw materials for preparing the filter element material, because nylon 6 has excellent mechanical strength and corrosion resistance, and has high toughness, and the PA6 molecular chain contains high-density amide groups, which are very easy to absorb water, so that the filter element material can quickly absorb water; polystyrene is hydrophobic, which is conducive to water evaporation. The present invention blends PA6 and PS in a specific ratio, and modifies the blending of the two materials, and after etching and removing the PS on the surface of the prefabricated sheet, grooves and porous structures are formed on the surface of the filter element material, which can increase the specific surface area of the filter element material, and then increase the water-wetting area of the filter element material, and make a filter element for a humidifier, which can regulate the water absorption and evaporation balance of the filter element, improve the water evaporation efficiency, and then improve the humidification effect and mechanical properties of the humidifier, and PS is cheap, which can effectively reduce the cost of the filter element material.
[0051] In the present invention, the main raw material also includes 0.5 to 5 parts by mass of a reactive compatibilizer, more preferably 2 to 4 parts by mass, specifically 2.9 parts by mass, 3.0 parts by mass or 3.1 parts by mass. In the present invention, the reactive compatibilizer is a graft copolymer of polystyrene and glycidyl methacrylate, and the molecular structure of the reactive compatibilizer contains a polystyrene chain with an epoxy group at the end. In the present invention, the weight average molecular weight of the reactive compatibilizer is preferably 4000 to 6000 g / mol. In the present invention, the reactive compatibilizer is preferably PS-PGMA-G or PS-PGMA-P. In the present invention, the reactive compatibilizer is preferably derived from polystyrene (PS) and glycidyl methacrylate (GMA) by polycondensation reaction.
[0052] In the present invention, the preparation method of the reactive compatibilizer preferably comprises the following steps:
[0053] The polystyrene, the complexing agent, the catalyst and the solvent are mixed, and glycidyl methacrylate is added to carry out polycondensation reaction to obtain the reactive compatibilizer.
[0054] In the present invention, the complexing agent is preferably pentamethyldiethylenetriamine, the catalyst is preferably cuprous chloride, and the solvent is preferably tetrahydrofuran. In the present invention, the amount of the complexing agent is preferably 0.3-0.7% of the mass of polystyrene. In the present invention, the amount of the catalyst is preferably 0.2-0.6% of the mass of polystyrene. In the present invention, the amount of the solvent is preferably 140-170% of the mass of polystyrene.
[0055] In the present invention, when the mass ratio of the polystyrene to glycidyl methacrylate is 1:0.12-0.16, the obtained reactive compatibilizer has a short chain structure, which is PS-PGMA-G. In the present invention, when the mass ratio of the polystyrene to glycidyl methacrylate is 1:0.40-0.45, the obtained reactive compatibilizer has a long chain structure, which is PS-PGMA-P.
[0056] In the present invention, the mixing is preferably carried out under the condition of an ice bath, and the temperature of the ice bath is ≤0°C. In the present invention, the mixing is preferably carried out in a closed nitrogen atmosphere. In the present invention, the polycondensation reaction is preferably carried out in a closed nitrogen atmosphere. In the present invention, the temperature of the polycondensation reaction is preferably 45 to 60°C, more preferably 50°C, and the time is preferably 16 to 18h.
[0057] After the polycondensation reaction, the present invention preferably further comprises sequentially subjecting the reaction liquid to column filtration, vacuum rotary evaporation, suction filtration and drying. In the present invention, the solvent for the column filtration is preferably tetrahydrofuran, the solvent for the suction filtration is preferably ethanol, and the drying time is preferably 2 to 4 hours.
[0058] In a specific embodiment of the present invention, the preparation method of the reactive compatibilizer preferably comprises: putting polystyrene into a reaction bottle, adding tetrahydrofuran, sealing and stirring to dissolve. After cooling in an ice bath, pentamethyldiethylenetriamine is added, nitrogen is charged and discharged 3 times, cuprous bromide powder is added, and after stirring for 5 minutes, glycidyl methacrylate monomer is added, and nitrogen is charged and discharged again 3 times. After sealing, it is transferred to an oil bath pot at 50°C for polycondensation reaction. After the reaction is completed, tetrahydrofuran is added for dilution, the reaction liquid is transferred to a filter column, and the filtrate is collected at the bottom. After the reaction is completed, the reaction bottle is rinsed with tetrahydrofuran, poured into the filter column and the combined filtrate is collected. The obtained filtrate is subjected to vacuum rotary evaporation to obtain a concentrated filtrate, ethanol is dripped into the concentrated filtrate, and suction filtration is performed to collect the precipitate on the filter paper, the precipitate is collected in a plastic box and sealed with gauze, and the whole is placed in a vacuum oven (room temperature and reduced pressure) for 2 to 4 hours to obtain the reactive compatibilizer.
[0059] In the present invention, there is a certain polarity difference between PA6 and PS, so the compatibility of PA6 and PS is poor, which will reduce the mechanical properties of the blend of the two. The present invention adopts a graft copolymer of polystyrene and glycidyl methacrylate as a reactive compatibilizer. The reactive compatibilizer contains a polystyrene chain in its molecular structure, and carries an epoxy group at the end. The styrene group can be well compatible with PS, and the epoxy group can also react and bond with the carboxyl and amino groups in the PA6 molecule to improve the compatibility of PA6 and PS, thereby obtaining a PA6 and PS blend with better compatibility and mechanical properties; and the reactive compatibilizer can make the mixing of PA6 and PS more uniform and delicate, so that uniform fiber gaps, grooves and porous structures appear on the surface of the filter element material after etching, and lay the foundation for obtaining a filter element material with capillary action, which can be used in a humidifier filter element to significantly improve the humidification efficiency.
[0060] The raw materials for preparing the filter element material provided by the present invention also include auxiliary raw materials. In the present invention, the auxiliary raw material is graphene oxide. In the present invention, the amount of the auxiliary raw material is 0.5-2% of the mass of the main raw material, preferably 0.5-1%, specifically 0.5%, 0.6% or 1%. In the present invention, the particle size of the graphene oxide is preferably 300-500nm. The graphene oxide used in the present invention has good antibacterial and antifungal capabilities. The present invention blends GO with PA6 and PS to make a filter element material, which improves the strength of the filter element material while improving the antibacterial properties of the filter element material, making the filter element material more durable during actual use.
[0061] The present invention also provides a method for preparing the filter element material described in the above technical solution, comprising the following steps:
[0062] Nylon 6, polystyrene, a reactive compatibilizer and graphene oxide are mixed, and then extruded, drawn and granulated to obtain a premix;
[0063] Injection molding the premix to obtain an injection molded part;
[0064] Thinning the injection molded part to obtain a prefabricated sheet;
[0065] The prefabricated sheet is etched to obtain the filter element material.
[0066] In the present invention, before preparing the filter element material, the PA6 is preferably dried. In the present invention, the drying equipment is preferably a vacuum oven, the drying temperature is preferably 90 to 110° C., and the drying time is preferably 22 to 26 hours. In the present invention, the PA6 is preferably sealed and stored after drying.
[0067] The present invention mixes nylon 6, polystyrene, a reactive compatibilizer and graphene oxide, and sequentially performs extrusion, wire drawing and granulation to obtain a premix.
[0068] In the present invention, the extrusion wire drawing is preferably carried out in a twin-screw extruder. In the present invention, the temperature program of the extrusion wire drawing (the temperature program is segmented heating) is preferably 150-170°C, 190-210°C, 230-250°C, 230-250°C, 230-250°C, 230-250°C, 230-250°C, 230-250°C, 230-250°C, 220-240°C. In the present invention, the temperatures of each segment of segmented heating in the temperature program of the extrusion wire drawing may be the same or different. In the present invention, the screw speed of the extrusion wire drawing is preferably 110-130rpm. In the present invention, the feed rate of the extrusion wire drawing is preferably 1-3%. In the present invention, the screw torque of the extrusion wire drawing is preferably ≤50Nm, more preferably 30-40Nm. In the present invention, the wire material obtained by extrusion wire drawing is preferably air-cooled and wound.
[0069] In the present invention, the granulation is preferably carried out in a cold-cut granulator. In the present invention, the model of the cold-cut granulator is preferably AKPL-100, and the manufacturer is preferably Nanjing Keya Chemical Complete Equipment Co., Ltd.
[0070] After obtaining the premix, the present invention performs injection molding on the premix to obtain an injection molded part.
[0071] In the present invention, the injection molding is preferably carried out in an injection molding machine. In the present invention, the specification of the injection molding machine is preferably BP-8180-A, and the manufacturer is preferably Baopin Precision Instrument Co., Ltd. In the present invention, the temperature program of the injection molding is preferably: the heating temperature of the first injection molding stage is 230-250°C, the heating temperature of the second injection molding stage is 230-250°C, and the heating temperature of the injection molding head is 220-240°C. In the present invention, the heating temperatures of each section in the temperature program of the injection molding may be the same or different. In the present invention, the pressure program of the injection molding is preferably: the injection holding pressure is 4-8MPa, and the injection extrusion pressure is 4-9MPa. In the present invention, when the amount of polystyrene (PS) exceeds 50 parts by mass, a release agent is preferably used, and the release agent is preferably TAIHOKOHZAI plant oil release agent JIP1240124.
[0072] After the injection molded part is obtained, the present invention thins the injection molded part to obtain a prefabricated thin sheet.
[0073] In the present invention, the thinning is preferably carried out in a flat-plate vulcanizer. In the present invention, the specification of the flat-plate vulcanizer is preferably BP8170-A, and the manufacturer is preferably Baopin Precision Instrument Co., Ltd. In the present invention, the temperature of the thinning is preferably 200-210°C. In the present invention, the thinning preferably includes pre-pressing thinning and pressurizing thinning performed in sequence. In the present invention, the pressure of the pre-pressing thinning is preferably 3-7MPa, and the time is preferably 1-5min. In the present invention, the pressure of the pressurizing thinning is preferably 12-18MPa, and the time is preferably 5-10min. In the present invention, the thickness of the prefabricated sheet is preferably 0.4-1mm, more preferably 0.5mm.
[0074] The present invention mixes PA6, PS, a reactive compatibilizer and a graphite oxide composite material and then sequentially extrude, draw and granulate, so that the raw materials can be mixed more evenly and the functions of each component can be fully exerted. The present invention injects and thins the premix so that the PA6 in the prefabricated sheet has a certain melt orientation to form ordered layered fibers.
[0075] After obtaining the prefabricated thin sheet, the present invention etches the prefabricated thin sheet to obtain the filter element material.
[0076] In the present invention, the reagent used for the etching is preferably tetrahydrofuran (THF). In the present invention, the etching time is preferably 24 to 48 hours, more preferably 24 hours. The present invention places the filter element material in tetrahydrofuran for etching. Within a specific time, tetrahydrofuran will etch away part of the PS on the surface of the filter element material, but will not completely etch the filter element material, which can not only ensure the mechanical strength of the fan blade used as the filter element, but also increase the water-wetting area, thereby better balancing the water absorption and water evaporation effects.
[0077] After the etching, the present invention preferably soaks the etched wafer in deionized water to remove THF.
[0078] After the present invention uses tetrahydrofuran to etch away part of the PS on the surface of the prefabricated sheet, a large number of fiber gaps, grooves and porous structures appear on the surface of the obtained filter element material, making the water absorption performance of the filter element material stronger, which is conducive to strengthening the capillary action of the filter element material, accelerating water evaporation, and improving the humidification efficiency of the humidifier. In addition, after the filter element material is etched, the specific surface area of the filter element material is greatly increased. When used in a humidifier filter element, it can effectively increase the water-wetting area of the humidifier filter element, which helps to improve the water evaporation efficiency. In addition, the filter element material with a large number of fiber gaps, grooves and porous structures can also filter out fine particles.
[0079] The present invention also provides a filter element (such as Figure 1 shown), including fan blades, from Figure 1It can be seen that the filter element contains multiple fan blades, which are evenly arranged radially with the rotating axis as the center, which can effectively increase the air intake and humidification amount of the filter element, thereby improving the overall use effect of the humidifier. Figure 1 There are other structural discs in the filter that have the function of fixing the filter element material and helping the operation of the equipment.
[0080] The filter element provided by the present invention includes fan blades. In the present invention, the fan blades are assembled from the filter element material described in the above technical solution or the filter element material prepared by the preparation method described in the above technical solution. In the present invention, the number of the fan blades is preferably 140 to 160 pieces, and more preferably 150 pieces. In the present invention, the size of the fan blades is preferably 50 to 300 mm*10 to 60 mm*0.4 to 1 mm, more preferably 60 to 200 mm*20 to 50 mm*0.4 to 1 mm, and further preferably 100 mm*35 mm*0.5 mm.
[0081] The filter element assembled by the filter element material of the present invention has higher specific surface area and water absorption capacity, higher water evaporation efficiency, and also has the advantages of antibacterial, fine particle filtering and durability.
[0082] The present invention also provides the use of the filter element material described in the above technical solution or the filter element material prepared by the preparation method described in the above technical solution or the filter element described in the above technical solution in preparing a humidifier. In the present invention, the humidifier includes the filter element described in the above technical solution.
[0083] The filter element assembled by the filter element material described in the above technical solution is used to prepare a humidifier, which has the advantages of being safe, effective, energy-saving, environmentally friendly, and a humidification method with high humidification capacity. The humidifier uses a water pump to pump water out of the water tank and pour it onto the filter element, and then the fan blows air to evaporate the water molecules on the filter element into the air. The filter element in the humidifier provided by the present invention has a higher specific surface area and water absorption capacity, a higher water evaporation efficiency, and also has antibacterial properties and is durable.
[0084] The technical solution of the present invention is further described below through specific implementation methods. Those skilled in the art should understand that the embodiments are only used to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0085] Example 1
[0086] Preparation of reactive compatibilizer PS-PGMA-P: Put 10 parts by mass of polystyrene into a reaction bottle, add 15 parts by mass of tetrahydrofuran, seal and stir to dissolve. After cooling in an ice bath, add 0.05 parts by mass of pentamethyldiethylenetriamine, charge and discharge nitrogen 3 times, add 0.04 parts by mass of cuprous bromide powder, stir for 5 minutes, then add 4.5 parts by mass of glycidyl methacrylate monomer, charge and discharge nitrogen 3 times again. After sealing, transfer to an oil bath pot at 50°C for polycondensation reaction for 18 hours. After the reaction is completed, add tetrahydrofuran to dilute, transfer the reaction liquid to the filter column, and collect the filtrate at the bottom. After the reaction is completed, rinse the reaction bottle with tetrahydrofuran, pour into the filter column and collect the combined filtrate. The collected filtrate is subjected to reduced pressure rotary evaporation to obtain a concentrated filtrate, a large amount of ethanol is dropped into the concentrated filtrate, and suction filtration is performed to collect the precipitate on the filter paper, the precipitate is collected in a plastic box and sealed with gauze, and the whole is placed in a vacuum oven (room temperature and reduced pressure) for drying for 4 hours to obtain a reactive compatibilizer PS-PGMA-P, and the weight average molecular weight of the obtained reactive compatibilizer is 6000 g / mol.
[0087] Raw materials include: Nylon 6: model PA6-YH800, molecular weight 23000g / mol, density 1.157g / cm 3 , purchased from Yuyue Chemical Co., Ltd.; polystyrene: purchased from Formosa Chemical Corporation, model PS (GP-535N), molecular weight 300000 g / mol, general-purpose polystyrene particles; tetrahydrofuran: analytical grade, purchased from McLean Chemical Reagent Co., Ltd.; graphene oxide: purchased from Beike Nano szbknm2010, powder, particle size 400nm; vegetable oil-based release agent: model JIP1240124, purchased from TAIHOKOHZAI, Japan.
[0088] The preparation steps include:
[0089] Place the PA6 in a vacuum oven and dry it at 100°C for 24 hours. The dried PA6 is sealed and stored.
[0090] 50 parts by mass of dried PA6, 47 parts by mass of PS, 3 parts by mass of reactive compatibilizer PS-PGMA-P and 0.5 parts by mass of GO were added into a twin-screw extruder at a feeding rate of 3% for extrusion and drawing. The temperature program for extrusion and drawing was 160°C, 200°C, 240°C, 240°C, 240°C, 240°C, 240°C, 240°C, 230°C. The screw speed was 120 rpm, the screw torque was 35 Nm, and the wire material obtained by extrusion and drawing was air-cooled and wound into a coil.
[0091] The wire material obtained by extrusion and drawing is added into a cold cutting granulator for granulation to obtain a premix.
[0092] The obtained premix is added to the injection molding machine for injection molding. The program temperature of the injection molding is: the heating temperature of the first stage of the injection molding is 240°C, the heating temperature of the second stage of the injection molding is 240°C, the heating temperature of the injection molding head is 230°C, and the pressure program of the injection molding is: the injection holding pressure is 6MPa, and the injection extrusion pressure is 8MPa to obtain the injection molded parts. Before injection molding, a release agent is used for treatment.
[0093] The obtained injection molded part was placed in a flat vulcanizer for thinning at a temperature of 205°C. Pre-pressing and thinning were first performed at 5MPa for 5 minutes, and then the pressure was increased to 15MPa for pressurized thinning for 10 minutes to obtain a prefabricated sheet with a thickness of 0.5mm.
[0094] The obtained prefabricated thin sheet was etched in tetrahydrofuran for 24 hours to obtain a filter element material. Figure 2 This is the SEM image of the filter element material prepared in Example 1. Figure 2 The magnification of the two pictures on the left and right is different. The magnification of the picture on the right is larger. Figure 2 It can be seen that: it can be clearly seen that the PA6 in the filter material presents a relatively round fiber morphology, and there are spherical granular GO attached to the surface, indicating that the raw materials PA6, PS, reactive compatibilizer and GO are mixed evenly. Therefore, after part of the PS is etched away, the PA6 presents an obvious fibrous melt orientation. However, there is still a small amount of PS attached between the fibrous PA6. A large number of fiber gaps, grooves and porous structures appear on the surface of the filter material after etching, which increases the specific surface area of the filter material and the water-wetting area. The larger the water-wetting area, the better the water absorption and water evaporation capacity of the filter material; the rounded fibers present a certain orientation, forming ordered layered fibers, which can form microscopic capillary action, thereby improving the water absorption and water evaporation capacity of the filter material. The fiber diameter is between 2 and 20 μm, and they fuse with each other on the local surface to maintain a macroscopic continuous structure.
[0095] The obtained filter element material is cut into blades of 100mm*35mm*0.5mm, and 160 blades are assembled into a filter element.
[0096] The obtained filter element was installed into a humidifier and the performance was tested.
[0097] Example 2
[0098] The difference from Example 1 is that 1.6 parts by mass of glycidyl methacrylate is added, and the prepared reactive compatibilizer is PS-PGMA-G.
[0099] The prepared PS-PGMA-G is used instead of PS-PGMA-P to prepare filter element materials.
[0100] Example 3
[0101] The differences from Example 1 are as follows: PA6 is 60 parts by mass, PS is 37 parts by mass, PS-PGMA-G prepared in Example 2 is used instead of PS-PGMA-P, and GO is 1 part by mass.
[0102] Example 4
[0103] The difference from Example 1 is that PA6 is 40 parts by mass and PS is 57 parts by mass.
[0104] Example 5
[0105] The difference from Example 4 is that PS-PGMA-G prepared in Example 2 is used instead of PS-PGMA-P.
[0106] Example 6
[0107] The difference from Example 3 is that PS-PGMA-P is used instead of PS-PGMA-G.
[0108] Example 7
[0109] The difference from Example 1 is: 70 parts by mass of PA6 and 27 parts by mass of PS.
[0110] Comparative Example 1
[0111] The difference from Example 1 is that: 50 parts by mass of PS, and no reactive compatibilizer and graphene oxide (GO) are added.
[0112] Figure 3 This is the SEM image of the filter element material prepared in Comparative Example 1. Figure 3 The magnification of the two pictures on the left and right is different. The magnification of the picture on the right is larger. Figure 3 It can be seen that: the filter element material presents a certain melt orientation, but no obvious rounded fibrous layer is formed, there are no GO particles on the surface, PS and PA6 cannot be distinguished after etching, the groove structure is not flat and regular, and there are irregular corrosion holes on the surface, which will hinder capillary action and affect the absorption and evaporation of water; the fibrous structure on the surface of the filter element material is broken, and there is no bonding and support between each other, so the tensile strength, Young's modulus and elongation at break of the obtained filter element material are all lower than the filter element material obtained in Example 1.
[0113] Comparative Example 2
[0114] The difference from Example 1 is that no etching is performed.
[0115] Comparative Example 3
[0116] The difference from Example 1 is: 80 parts by mass of PA6 and 17 parts by mass of PS.
[0117] Comparative Example 4
[0118] The difference from Example 1 is: 20 parts by mass of PA6 and 77 parts by mass of PS.
[0119] Comparative Example 5
[0120] The difference from Example 1 is that graphene oxide (GO) is not added.
[0121] Table 1 List of raw materials for filter element materials prepared in Examples 1 to 7 and Comparative Examples 1 to 5
[0122]
[0123] According to the standard GB / T 1040.3-2006, a universal tensile testing machine (Shenzhen Sansi Zongheng Technology Co., Ltd., model UTM5504) was used to test the tensile strength, Young's modulus and elongation at break of the filter element materials prepared in Examples 1 to 7 and Comparative Examples 1 to 5, and the tensile rate was 50 mm / min. The test specimen length was 120 mm, the width was 20 mm and the thickness was 1 mm, and the test fixture distance was 100 mm. The dry sample was placed in a 60°C blast oven for 24 hours before testing, and the wet sample was pre-soaked in deionized water for 24 hours. The surface water was wiped off during the test. The test results are shown in Table 2.
[0124] Table 2 Mechanical properties of filter element materials prepared in Examples 1 to 7 and Comparative Examples 1 to 5
[0125]
[0126] It can be seen from Table 2 that: 1. Whether in a dry state or in a water-saturated state, the tensile strength of the filter element material gradually increases with the increase of the PA6 content. Compared with Example 1, Example 4 and Examples 6 to 7, as the amount of PA6 increases, the Young's modulus of the filter element material increases significantly, whether in a dry state or a wet state. This is because as the PA6 / PS blending ratio increases, the volume proportion of the PA6 phase increases, that is, the amount of nylon phase that actually bears the force when the sample is subjected to force increases. Secondly, as the PA6 / PS blending ratio increases, more fusion is formed between the PA6 phases in the blend, and the effective connections between the nylon phases increase, so that the etched sample can transfer stress more effectively when subjected to force.
[0127] 2. The elongation at break of the filter element materials obtained in Examples 1 to 7 and Comparative Examples 1 to 5 in the wet state is higher than that in the dry state, but the test results of tensile strength and Young's modulus in the dry state are higher. The tensile strength of the sample decreases significantly after water absorption, but the elongation at break increases significantly. In the dry state, the elongation at break of the sample of the embodiment is basically distributed in the range of 2% to 6%, showing brittle fracture; and after water absorption, the elongation at break increases to 12% to 60%.
[0128] 3. By comparing Example 1 and Comparative Example 1, after adding the reactive compatibilizer, the tensile properties of the filter element material are significantly improved regardless of whether it is in a dry or wet state, and the elongation at break of Example 1 is greater than that of Comparative Example 1.
[0129] 4. The tensile strength, Young's modulus and elongation at break of the filter element material obtained in the dry and wet states of the unetched comparative example 2 are similar to the test results of the filter element material obtained in Example 1, indicating that etching has little effect on the mechanical properties of the filter element material.
[0130] 5. Compared with Example 1, the mass fraction of PA6 in Comparative Example 4 is 20 parts and that of PS is 77 parts. However, the tensile strength, Young's modulus and elongation at break of the filter element material obtained in Comparative Example 4 are lower than those in the example both in dry and wet states, and cannot meet the basic requirements of the filter element material.
[0131] Generally speaking, the humidifier filter element is required to have a certain stiffness to maintain its shape and stability to prevent the humidifier from deformation or damage during operation; it is also required to have a certain tensile breaking strength to ensure that the filter element is not easily broken when subjected to external forces, which helps the filter element maintain its integrity and effectiveness during long-term use; the filter element will produce friction with water or air during operation, so it needs to have a certain wear resistance to reduce wear and extend its service life.
[0132] Figure 4 The present invention tests the water evaporation performance of the filter element material according to the standards GB / T 21655.1 and GB / T 21655.2. The filter element materials prepared in Examples 1 to 7 and Comparative Examples 1 to 5 are made into fan blades, the fan blades are assembled into a filter element, the filter element is installed in a humidifier, and the water evaporation performance test is performed (such as Figure 5 The specific test method includes: turning on the strong humidification mode under the conditions of indoor ambient temperature of 22.3℃ and relative humidity of 34%. After half an hour, the thermometer and hygrometer on the top of the humidifier shows that the air outlet temperature drops to 18.4℃ and the relative humidity increases to 53%. The calculation formula of evaporation rate is: evaporation rate = (the mass of pure water in the humidifier before the test - the mass of pure water in the humidifier after the test) / (test time × filter surface area), the unit is g / (h*m 2 ), the test results are shown in Table 3.
[0133] Table 3 Water evaporation performance test results of filter element materials prepared in Examples 1 to 7 and Comparative Examples 1 to 5
[0134]
[0135]
[0136] It can be seen from Table 3 that the filter element material obtained in Example 1 has excellent water evaporation performance and high mechanical strength. This is because a large amount of rounded fiber structure nylon 6 is produced inside the filter element material after etching, which greatly increases the specific surface area, which is equivalent to increasing the water-wetting area; at the same time, the addition of the compatibilizer refines the polymer phase, further strengthens the capillary action, and improves the ability to transport water, thereby making the porous nylon material show good water evaporation performance. Significantly better than commercially available filter element products. In Comparative Example 3, since the amount of PA6 is very high, the tensile strength, Young's modulus and elongation at break of the filter element material obtained in Comparative Example 3 are relatively high, but the amount of PS in Comparative Example 3 is very low, and the pores and grooves on the surface of the filter element material after etching are very small. Therefore, the water evaporation performance of the filter element material obtained in Comparative Example 3 is very poor and cannot meet the requirements for preparing humidifier filter elements.
[0137] After the filter element prepared in Example 1 of the present invention was soaked in tap water for 14 days, no odor was generated and no mold was grown. However, after the filter element of the commercially available humidifier was soaked in tap water for 14 days, a large number of mold spots (such as Figure 6 As shown in the figure, the filter element is a commonly used filter element material for humidifiers on the market. Graphene oxide is not added. After being soaked in tap water for 14 days, a large amount of visible mold appeared. The filter element could not be used any more and needed to be cleaned or replaced in time.
[0138] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.
Claims
1. A filter element material, characterized in that: The preparation raw materials include main raw materials and auxiliary raw materials; The main raw materials include nylon 625-75 mass parts, polystyrene 25-75 mass parts and reactive compatibilizer 0.5-5 mass parts; The auxiliary raw material is graphene oxide; The amount of the auxiliary raw material is 0.5-2% of the mass of the main raw material; The reactive compatibilizer is a graft copolymer of polystyrene and glycidyl methacrylate.
2. The filter element material according to claim 1, characterized in that: The weight average molecular weight of the nylon 6 is 20000-30000 g / mol; the weight average molecular weight of the polystyrene is 250000-350000 g / mol; the particle size of the graphene oxide is 300-500 nm; The reactive compatibilizer is PS-PGMA-G or PS-PGMA-P.
3. The method for preparing the filter element material according to any one of claims 1 to 2, characterized in that: The following steps are involved: Nylon 6, polystyrene, a reactive compatibilizer and graphene oxide are mixed, and extruded, drawn and granulated in sequence to obtain a premix; Injection molding the premix to obtain an injection molded part; Thinning the injection molded part to obtain a prefabricated sheet; The prefabricated sheet is etched to obtain the filter element material.
4. The preparation method according to claim 3, characterized in that: The temperature program of the extrusion wire drawing is 150-170°C, 190-210°C, 230-250°C, 230-250°C, 230-250°C, 230-250°C, 230-250°C, 230-250°C, 230-250°C, 230-250°C, 220-240°C; The screw speed of the extrusion wire drawing is 110-130rpm; The feeding rate of the extrusion wire drawing is 1 to 3%; The screw torque of the extrusion wire drawing is ≤50Nm.
5. The preparation method according to claim 3, characterized in that: The temperature program of the injection molding is as follows: the heating temperature of the first injection molding stage is 230-250°C, the heating temperature of the second injection molding stage is 230-250°C, and the heating temperature of the injection molding head is 220-240°C; The pressure procedure of the injection molding is as follows: the injection holding pressure is 4-8 MPa, and the injection extrusion pressure is 4-9 MPa.
6. The preparation method according to claim 3, characterized in that: The thinning temperature is 200-210°C; The thinning includes pre-pressing thinning and pressurizing thinning; The pre-pressing and thinning pressure is 3-7 MPa and the time is 1-5 min; The pressure of the pressurized thinning is 12-18 MPa, and the time is 5-10 minutes.
7. The preparation method according to claim 3, characterized in that: The etching reagent used is tetrahydrofuran; The etching time is 24 to 48 hours.
8. A filter element, comprising a fan blade, characterized in that: The fan blades are assembled from the filter element material described in any one of claims 1 to 2 or the filter element material prepared by the preparation method described in any one of claims 4 to 7.
9. The filter element according to claim 8, characterized in that: The number of the fan blades is 140 to 160; The size of the fan blade is 50-300 mm*10-60 mm*0.4-1 mm.
10. Use of the filter element material according to any one of claims 1 to 2, the filter element material prepared by the preparation method according to any one of claims 4 to 7, or the filter element according to any one of claims 8 to 9 in the preparation of a humidifier.