Lubricating anticorrosive paint as well as preparation method and application thereof

By using GO/MXene@MOFs composite materials, combined with corrosion inhibitors, a nano container and physical barrier network is formed, which solves the corrosion and wear of water-based epoxy coatings in extreme environments, and achieves efficient lubrication, corrosion resistance and self-healing Performance significantly improves the protection capability of the coating.

CN119081510APending Publication Date: 2024-12-06QUFU NORMAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411408637.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-10
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing water-based epoxy coatings are easily damaged in extreme environments, resulting in insufficient corrosion and wear performance of the coating and cannot effectively resist the corrosion of corrosive media.

Method used

Using composite material GO/MXene@MOFs, a nano container and physical barrier network are formed through the combination of two-dimensional heterojunction materials and metal organic framework compounds, and a corrosion inhibitor is combined to achieve a self-healing protection mechanism.

Benefits of technology

It significantly improves the lubrication, corrosion and wear resistance of the coating, extends the service life, maintains high corrosion resistance, especially reduces friction and wear during friction, providing excellent lubrication and self-repair capabilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081510A_ABST
    Figure CN119081510A_ABST
Patent Text Reader

Abstract

The embodiment of the invention relates to a lubricating anti-corrosion coating and a preparation method and application thereof.The lubricating anti-corrosion coating comprises a composite material, the composite material comprises a two-dimensional heterojunction material and a metal organic framework compound loaded on the two-dimensional heterojunction material, the two-dimensional heterojunction material is of a two-dimensional nanosheet layer structure, and the metal organic framework compound is loaded on the two-dimensional heterojunction material. The metal organic framework compound is loaded on the two-dimensional heterojunction material, the two-dimensional heterojunction material comprises graphene oxide and MXene, the graphene oxide and the MXene are in grafting connection, and the graphene oxide has a wrinkle structure, so that the corrosion resistance and the wear resistance of the lubricating anticorrosive paint can be improved, and the lubricating anticorrosive paint has the advantages that the service life of the lubricating anticorrosive paint is prolonged, and the service life of the lubricating anticorrosive paint is prolonged. Therefore, adverse effects caused by the external environment can be resisted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of functional materials and lubricating anti-corrosion coatings, and more specifically, to a lubricating anti-corrosion coating and a preparation method and application thereof. Background Art

[0002] With the rapid development of key fields such as marine industry, aerospace, transportation, construction and energy, the demand for long-term protection of metal materials is becoming increasingly urgent. However, the two major problems of corrosion and wear continue to plague metal materials, not only causing huge economic losses and resource consumption, but also posing a major obstacle to technological progress. Among the many protection strategies, water-based epoxy coatings have become the focus of attention due to their easy operation, high cost-effectiveness, significant protection effect and environmental friendliness. Unfortunately, when this coating is exposed to corrosive media (such as chloride ions, Cl - When exposed to extreme environments such as oxygen (O2), water (H2O), its protective barrier is easily destroyed, which in turn induces electrochemical corrosion on the substrate. This corrosion mechanism not only causes the degradation of the base material performance, but is also accompanied by the formation of coating cracks, providing a direct channel for the corrosive medium to invade. These crack areas are very likely to form local corrosion micro-batteries, causing the corrosion rate to accelerate sharply and grow exponentially. In addition, external forces in the environment may also directly damage the coating surface, causing cracks and aggravating the corrosion process. Summary of the invention

[0003] The present application is provided to solve the above defects existing in the prior art. A lubricating anti-corrosion coating and its preparation method and application are needed to solve the problem that the anti-corrosion and anti-wear properties of the coating are not sufficient to resist the adverse effects caused by the external environment.

[0004] In a first aspect of the present application, a lubricating anti-corrosion coating is provided, which includes a composite material (GO / MXene@MOFs), the composite material includes a two-dimensional heterojunction material and MOFs (Metal Organic Frameworks), the MOFs are loaded on the two-dimensional heterojunction material, the two-dimensional heterojunction material has a two-dimensional nanosheet structure, the two-dimensional heterojunction material includes graphene oxide (GO) and MXene, GO and MXene are grafted and connected, and the GO has a wrinkled structure.

[0005] In a second aspect of the present application, a method for preparing the lubricating anti-corrosion coating according to any embodiment of the present application is provided, the method comprising: mixing a composite material, an epoxy resin curing agent, a defoaming agent, an epoxy resin and water to obtain the lubricating anti-corrosion coating. The preparation process is carried out at room temperature. Ultrasound may be used as an auxiliary in the reaction process.

[0006] In a third aspect, the present application provides a method for preparing the lubricating and anti-corrosion coating described in any embodiment of the present application or an application of the lubricating and anti-corrosion coating described in any embodiment of the present application in the coating field.

[0007] The lubricating and anti-corrosion coatings and their preparation methods and applications provided in various embodiments of the present application include composite materials, and the composite materials include two-dimensional heterojunction materials and MOFs. The effective compounding of GO, MXene and MOFs combines the excellent properties of two-dimensional heterojunctions and MOFs, so that the lubricating and anti-corrosion coatings of the present application have multiple properties of excellent lubrication, corrosion resistance and wear resistance, and have a long service life and stability. During the friction process, the two-dimensional material layers can peel off and roll each other, giving full play to the synergistic mechanism of zero-dimensional and two-dimensional lubrication, further reducing friction and wear. At the same time, BTA can be loaded in large quantities and released effectively under certain conditions, providing strong protection for corrosion active sites. In addition, the physical barrier network constructed by the two-dimensional filler plays a passive protective role at the initial stage of exposure. When the corrosive medium penetrates or defects appear in the coating, the nanocontainer and the corrosion inhibitor work together to form a self-healing and active protection mechanism. Lubricating and anti-corrosion coatings show broad application prospects in the field of tribology, providing a new and efficient solution for reducing friction, reducing wear and protecting corrosion active sites. The friction coefficient of the bionic lubricating and anti-corrosion coating is as low as about 0.03, showing excellent lubrication performance. After immersion in 3.5 wt% NaCl solution for 30 days, the impedance simulation value of the coating can still be maintained at 2.5×10 6 The high level of Ω·cm² fully proves its excellent anti-corrosion performance; it has good application prospects in the fields of lubrication and anti-corrosion. BRIEF DESCRIPTION OF THE DRAWINGS

[0008] In the drawings, which are not necessarily drawn to scale, the same reference numerals may describe similar parts in different views. The same reference numerals with letter suffixes or different letter suffixes may represent different instances of similar parts. The accompanying drawings generally illustrate various embodiments by way of example and not limitation, and together with the specification and claims, are used to illustrate the embodiments applied for. When appropriate, the same reference numerals are used throughout the drawings to refer to the same or similar parts. Such embodiments are illustrative and are not intended to be exhaustive or exclusive embodiments of the present apparatus or method.

[0009] Figure 1 The transmission electron microscope image of MXene of Example 1 of the present application is shown; Figure 2 A transmission electron microscope image of the GO / MXene heterojunction of Example 1 of the present application is shown; Figure 3 The transmission electron microscope image of GO / MXene@ZIF-8 of Example 1 of the present application is shown; Figure 4 The XRD patterns of GO / MXene@ZIF-8, GO / MXene, MXene and ZIF-8@BTA of Example 1 of the present application are shown; Figure 5 A comparison of the friction coefficients of different coatings after 30 min of friction is shown; Figure 6 A friction coefficient diagram of the GO / MXene@ZIF-8 coating of Example 1 of the present application during 120 min of friction is shown; Figure 7 The Nyquist plot of the GO / MXene@ZIF-8 coating of Example 1 of the present application is shown. DETAILED DESCRIPTION

[0010] In order to enable those skilled in the art to better understand the technical solution of the present application, the present application is described in detail below in conjunction with the accompanying drawings and specific implementation examples. The embodiments of the present application are further described in detail below in conjunction with the accompanying drawings and specific implementation examples, but are not intended to limit the present application.

[0011] The words "first", "second" and similar words used in this application do not indicate any order, quantity or importance, but are only used to distinguish. The words "include" or "comprise" and similar words mean that the elements before the word include the elements listed after the word, and do not exclude the possibility of including other elements.

[0012] According to an embodiment of the present application, a lubricating anti-corrosion coating is provided, which includes a composite material (GO / MXene@MOFs), the composite material includes a two-dimensional heterojunction material and MOFs (Metal Organic Frameworks), the two-dimensional heterojunction material has a two-dimensional nanosheet structure, the two-dimensional heterojunction material includes graphene oxide (GO) and MXene, GO and MXene are grafted and connected, and the GO has a wrinkled structure; the MOFs are loaded on the two-dimensional nanosheet.

[0013] Graphene oxide (GO) and MXene not only act as anti-corrosion barriers, but also as efficient friction lubricants. The resulting heterojunction layers are bound to each other by weak van der Waals forces, which endow them with the property of easy interlayer sliding when subjected to shear forces, thus achieving a significant lubrication effect. When two contacting surfaces rub against each other under the action of normal force, the two-dimensional nanosheets in the contact area are subjected not only to normal pressure but also to shear stress due to relative motion. This interlayer sliding mechanism in multilayer two-dimensional materials constitutes an efficient sliding system that can significantly reduce friction and achieve superior lubrication performance compared to hard contact. In addition, the special arrangement of two-dimensional nanosheets in the fluid environment can guide the fluid flow, affect the mass and heat transfer in the local area, and then regulate the viscosity and fluid dynamics of the lubricant. However, despite their excellent performance in the initial stage, these two-dimensional materials face increasing challenges when the coating is exposed to corrosive environments for a long time. The corrosive medium can quickly penetrate along the tiny channels in the coating and reach the interface between the coating and the metal substrate, initiating the corrosion process. Once corrosion occurs, traditional two-dimensional material fillers often cannot provide effective subsequent repair mechanisms, thus limiting their long-term protective capabilities under extreme corrosion conditions.

[0014] The heterojunction nanosheets formed by GO and MXene provide a nanocontainer for loading MOFs and corrosion inhibitors. MXene is a metal carbide with a two-dimensional layered structure.

[0015] MOFs are a unique crystalline porous material that forms compounds with periodic network structures through the self-assembly process of inorganic metal centers (such as metal ions or metal clusters) and organic ligands. This material cleverly combines the rigidity of inorganic materials and the flexibility of organic materials, showing high porosity and excellent chemical stability. These characteristics enable MOFs to significantly affect the tribological and anti-corrosion properties of coatings. Specifically, when spherical or nearly spherical nanoparticles are added between the friction surfaces, the friction state will change from sliding friction to rolling friction, thereby effectively reducing friction resistance, surface wear and energy consumption.

[0016] MOFs can be controlled to deposit on the two-dimensional nanosheet layer, achieving effective wrapping and protection of the GO / MXene heterojunction. This unique design not only avoids the layered stacking of the GO / MXene two-dimensional heterojunction, but also inhibits the agglomeration of nanoparticles, significantly enhancing its stability and durability.

[0017] The lubricating anti-corrosion coating of the present application contains two-dimensional heterojunction nanosheets and MOFs. The two-dimensional filler builds a physical barrier network in the coating, which plays a passive protective role at the initial exposure and builds the first line of defense. At the same time, the zero-dimensional nanoparticles cleverly fill the gaps and uneven places on the surface of the friction pair, effectively reducing the aggregation and precipitation of the nanosheets, and further improving the stability and durability of the coating.

[0018] Therefore, the lubricating anti-corrosion coating of the present application has multiple properties of excellent lubrication, corrosion resistance and wear resistance.

[0019] In some embodiments, the composite material also includes a corrosion inhibitor, which is loaded on the MOFs. The MOFs loaded with corrosion inhibitors are controllably deposited on the two-dimensional nanosheet layer. The two-dimensional heterogeneous structure not only acts as a physical barrier network to effectively reduce the friction coefficient of the coating, but also provides a solid passive protective barrier for the metal substrate in the early stage. When the coating surface is damaged or the corrosive medium penetrates into the coating / metal interface or defects appear in the coating, the corrosion inhibitor in the nanocontainer can be intelligently released to quickly fill the defective area, realize the self-repair and active anti-corrosion function of the coating, form a self-healing mechanism, ensure the long-term effectiveness of the coating, and further enhance the protective ability of the coating.

[0020] The high porosity, regular pore structure and adjustable pore size of MOFs not only provide a high specific surface area for nanoparticles, thereby achieving a high loading amount of corrosion inhibitors, but also prolong the duration of corrosion inhibition through the slow release process. These characteristics not only meet the requirements of lubrication performance and high load-bearing capacity, but also improve the dispersibility by anchoring nanoparticles on the surface of nanosheets, effectively preventing the re-accumulation of exfoliated nanosheets.

[0021] The two-dimensional nanosheets with high specific surface area not only serve as excellent carriers for carrying the sustained-release agent, but also add additional performance advantages to the coating through their unique structural characteristics. Therefore, the lubricating anti-corrosion coating of the present application has multiple properties of excellent lubrication, corrosion resistance, wear resistance and self-repair.

[0022] In some embodiments, the MXene includes titanium carbide (Ti3C2T x , where T represents the surface functional group ends and x represents the number of these functional groups per unit). MXene can be prepared by acid etching of MAX phase.

[0023] In some embodiments, MOFs include ZIF-8 (zeolite imidazolate framework material), UiO-66 (zirconium 1,4-carboxybenzene), UiO-66-NH2, HKUST-1 (copper-based metal organic framework material, chemical formula C 18 H 12 Cu3O 15), one or more of MOF-5, MOF-74, NU-110, MIL-101 and MIL-53.

[0024] In some embodiments, the lubricating anti-corrosion coating further comprises epoxy resin. The epoxy resin is used as a base material in the lubricating anti-corrosion coating, so that the coating can have better water-based epoxy coating performance.

[0025] In some embodiments, the lubricating anti-corrosion coating further comprises an additive. In some embodiments, the additive comprises one or more of a solvent, a defoamer, an epoxy resin curing agent, etc. In some embodiments, the corrosion inhibitor comprises one or more of benzotriazole, methylbenzotriazole, or mercaptobenzothiazole, etc. In some embodiments, the solvent comprises water, etc. In some embodiments, the epoxy resin curing agent comprises one or more of ethylenediamine, diethylenediamine, triethylenediamine, etc.

[0026] In some embodiments, the mass fraction of the composite material in the lubricating anti-corrosion coating is 0.1-2%; preferably, the mass fraction of the composite material in the lubricating anti-corrosion coating is 0.5-1%. In some embodiments, the mass ratio of the two-dimensional heterojunction material to MOFs in the composite material is 1:1-2; preferably, 1:1-1.5. In some embodiments, the mass ratio of GO to MXene in the two-dimensional heterojunction material is 0.8-5:1-3; preferably, the mass ratio of GO to MXene is 1-2:1-2.

[0027] In some embodiments, the mass fraction of the solvent water in the lubricating anti-corrosion coating is 10-30%; preferably, the mass fraction of the solvent water in the lubricating anti-corrosion coating is 10-20%.

[0028] In some embodiments, the mass ratio of the epoxy resin to the epoxy resin curing agent is 5-15:1; preferably, the mass ratio of the epoxy resin to the epoxy resin curing agent is 8-12:1. In some embodiments, the mass ratio of the epoxy resin to the defoamer is 80-120:1. In some embodiments, the mass ratio of the MOFs to the corrosion inhibitor is 1-5:1; preferably, the mass ratio of the MOFs to the corrosion inhibitor is 3-4:1. So that the MOFs are loaded with an appropriate amount of corrosion inhibitor to improve the corrosion inhibition ability of the lubricating anti-corrosion coating.

[0029] According to an embodiment of the present application, a method for preparing the lubricating anti-corrosion coating according to any embodiment is also provided, the method comprising: mixing a composite material, an epoxy resin curing agent, a defoaming agent, an epoxy resin and a solvent to obtain the lubricating anti-corrosion coating. The preparation process is carried out at room temperature. Ultrasound can be used as an auxiliary in the reaction process.

[0030] In some embodiments, the preparation method of the composite material includes: mixing an aqueous solution of a MOFs composite with a GO / MXene heterojunction aqueous solution to obtain a composite material aqueous solution, wherein the MOFs composite includes MOFs and a corrosion inhibitor. The obtained composite material aqueous solution is separated to obtain a composite material, or directly mixed with an epoxy resin curing agent, a defoaming agent and an epoxy resin to obtain a lubricating anti-corrosion coating. The preparation process is carried out at room temperature. Ultrasound can be assisted during the reaction process.

[0031] In some embodiments, the preparation method of GO / MXene heterojunction includes mixing GO and MXene in water, wherein MXene is added in batches, and reacting at room temperature to obtain a GO and MXene heterojunction. MXene and GO are gradually mixed and contacted to make the load more uniform. After the reaction, a heterojunction aqueous solution is obtained, which can be separated to obtain a heterojunction or the heterojunction aqueous solution can be directly used to prepare a composite material. Ultrasound can be assisted during the reaction, and the frequency of ultrasonic mixing is 40~60 Hz.

[0032] In some embodiments, the preparation method of the MOFs composite formed by the MOFs and the corrosion inhibitor is as follows: MOFs and the corrosion inhibitor are mixed and reacted at room temperature to obtain the MOFs composite. The reaction time is 3-8 h. The MOFs composite forms a composite material after reacting with the GO / MXene heterojunction, and the loaded corrosion inhibitor is released in the later stage of use, which is beneficial to improve the corrosion inhibition.

[0033] In some embodiments, the preparation method of MXene includes: pre-soaking MaX with acid; then etching MaX (Ti3AlC2) with acid to obtain MXene. Pre-soaking effectively improves the acid etching degree of titanium carbide. This step ensures that MaX-Ti3AlC2 is in full contact with the acid, further enhances the acid etching effect, is conducive to the deep stripping of MAX in the reactor, makes the temperature and distribution in the reactor more uniform and stable, and enhances the pressure in the reactor, thereby improving the etching ability of the solution. This improvement makes the reaction more thorough, not only improves the dispersibility and stability of titanium carbide materials, but also significantly reduces the thickness of titanium carbide monolayer, and obtains a higher specific surface area.

[0034] In some embodiments, the MaX is a transition metal carbide, including Ti3AlC2, Ti3SnC2, etc. In some embodiments, the acid includes HF or HCl. In some embodiments, the etching reaction temperature is 90-100°C, and the reaction time is 120-168 h.

[0035] According to the embodiments of the present application, a method for preparing the lubricating anti-corrosion coating of any embodiment of the present application or the application of the lubricating anti-corrosion coating of any embodiment of the present application in the field of coating is also provided. The application of the coating in the fields of marine industry, aerospace, transportation, construction and energy is included. In particular, the application in the coating of metal equipment can better protect the metal equipment.

[0036] Example 1 Step 1: Disperse 50 mg GO in 10 mL deionized water, then add 50 mg MXene to the prepared GO solution evenly and slowly in 10 times, mix by ultrasonication to obtain a GO / MXene heterojunction, and wash by centrifugation until neutral. Add deionized water to obtain a 10 mg / mL GO / MXene heterojunction aqueous solution.

[0037] Step 2: Take 0.06 g ZIF-8 and 0.015 g BTA (benzotriazole), crush them, dissolve them in 4 mL deionized water, stir for 8 h to ensure the reaction is complete, and form an aqueous solution of ZIF-8@BTA (ZIF-8 complex). Take 1 mL GO / MXene heterojunction aqueous solution and 1 mL ZIF-8@BTA aqueous solution, mix them after ultrasonic dispersion treatment and stir for 6 h to form an aqueous solution of GO / MXene@ZIF-8 complex.

[0038] Step 3: Add 1 mL of the aqueous solution of the GO / MXene@ZIF-8 complex prepared in step 2, 0.3 g of epoxy resin curing agent and 0.03 g of defoaming agent to 3 g of epoxy resin in sequence, and obtain the GO / MXene@ZIF-8 epoxy resin lubricating anti-corrosion coating after stirring and ultrasonic dispersion treatment.

[0039] Example 2 Step 1: Disperse 75 mg GO in 15 mL deionized water, then add 75 mg MXene to the prepared GO solution evenly and slowly in 15 times, mix by ultrasonication to obtain a GO / MXene heterojunction, and wash by centrifugation until neutral. Add deionized water to obtain a 10 mg / mL GO / MXene heterojunction aqueous solution.

[0040] Step 2: Take 0.09 g ZIF-8 and 0.025 g BTA, crush them, dissolve them in 6 mL deionized water, stir for 8 h to ensure the reaction is complete, and form a ZIF-8@BTA (ZIF-8 complex) aqueous solution. Take 1.5 mL GO / MXene heterojunction aqueous solution and 1.5 mL ZIF-8@BTA aqueous solution, mix them after ultrasonic dispersion treatment and stir for 6 h to form a GO / MXene@ZIF-8 complex aqueous solution.

[0041] Step 3: Add 1.5 mL of the aqueous solution of GO / MXene@ZIF-8 complex prepared in step 2, 0.45 g of epoxy resin curing agent and 0.045 g of defoaming agent to 4.5 g of epoxy resin in sequence, and obtain the GO / MXene@ZIF-8 epoxy resin lubricating anti-corrosion coating after stirring and ultrasonic dispersion treatment.

[0042] Example 3 Step 1: Disperse 75 mg GO in 15 mL deionized water, then add 75 mg MXene to the prepared GO solution evenly and slowly in 15 times, mix by ultrasonication to obtain a GO / MXene heterojunction, and wash by centrifugation until neutral. Add deionized water to obtain a 10 mg / mL GO / MXene heterojunction aqueous solution.

[0043] Step 2: Take 0.09 g UiO-66 and 0.025 g BTA, crush them, dissolve them in 6 mL deionized water, stir for 8 h to ensure the reaction is complete, and form an aqueous solution of UiO-66@BTA (UiO-66 complex). Take 1.5 mL GO / MXene heterojunction aqueous solution and 1.5 mL UiO-66@BTA aqueous solution, mix them after ultrasonic dispersion treatment and stir for 6 h to form an aqueous solution of GO / MXene@UiO-66 complex.

[0044] Step 3: Add 1.5 mL of the aqueous solution of GO / MXene@ZIF-8 complex prepared in step 2, 0.45 g of epoxy resin curing agent and 0.045 g of defoaming agent to 4.5 g of epoxy resin in sequence, and obtain the GO / MXene@ZIF-8 epoxy resin lubricating anti-corrosion coating after stirring and ultrasonic dispersion treatment.

[0045] Example 4 Step 1: Disperse 50 mg GO in 10 mL deionized water, then add 50 mg MXene to the prepared GO solution evenly and slowly in 10 times, mix by ultrasonication to obtain a GO / MXene heterojunction, and wash by centrifugation until neutral. Add deionized water to obtain a 10 mg / mL GO / MXene heterojunction aqueous solution.

[0046] Step 2: Take 0.06 g MIL-100 and 0.015 g BTA, crush them, dissolve them in 4 mL deionized water, stir for 8 h to ensure the reaction is complete, and form a MIL-100@BTA (MIL-100 complex) aqueous solution. Take 1 mL GO / MXene heterojunction aqueous solution and 1 mL MIL-100@BTA aqueous solution, mix them after ultrasonic dispersion treatment and stir for 6 h to form a GO / MXene@MIL-100 complex aqueous solution.

[0047] Step 3: Add 1 mL of the aqueous solution of the GO / MXene@MIL-100 composite prepared in step 2, 0.3 g of epoxy resin curing agent and 0.03 g of defoaming agent into 3 g of epoxy resin in sequence, and obtain the GO / MXene@MIL-100 epoxy resin lubricating anti-corrosion coating after stirring and ultrasonic dispersion treatment.

[0048] Example 5 Step 1: Disperse 50 mg GO in 10 mL deionized water, then add 50 mg MXene to the prepared GO solution evenly and slowly in 10 times, mix by ultrasonication to obtain a GO / MXene heterojunction, and wash by centrifugation until neutral. Add deionized water to obtain a 10 mg / mL GO / MXene heterojunction aqueous solution.

[0049] Step 2: Take 0.09 g MIL-100 and 0.025 g mercaptobenzothiazole, crush them, dissolve them in 4 mL deionized water, stir for 8 h to ensure the reaction is complete, and form MIL-100@mercaptobenzothiazole (MIL-100 composite). Take 1 mL GO / MXene heterojunction aqueous solution and 1 mL MIL-100@mercaptobenzothiazole aqueous solution, mix them after ultrasonic dispersion treatment, and stir for 6 h to form an aqueous solution of GO / MXene@MIL-100 composite.

[0050] Step 3: Add 1 mL of the aqueous solution of the GO / MXene@MIL-100 composite prepared in step 2, 0.3 g of epoxy resin curing agent and 0.03 g of defoaming agent into 3 g of epoxy resin in sequence, and obtain the GO / MXene@MIL-100 epoxy resin lubricating anti-corrosion coating after stirring and ultrasonic dispersion treatment.

[0051] Comparative Example 1 0.3 g of epoxy resin curing agent and 0.03 g of defoaming agent were added to 3 g of epoxy resin in sequence, and pure EP coating was obtained after stirring and ultrasonic dispersion treatment.

[0052] Comparative Example 2 Step 1: Disperse 50 mg GO in 10 mL deionized water, then add 50 mg MXene to the prepared GO solution evenly and slowly in 10 times, mix by ultrasonication to obtain a GO / MXene heterojunction, and wash by centrifugation until neutral. Add deionized water to obtain a 10 mg / mL GO / MXene heterojunction aqueous solution.

[0053] Step 2: Take 0.06 g ZIF-8 and 0.025 g BTA, crush them, dissolve them in 4 mL deionized water, stir for 8 h to ensure the reaction is complete, and form a ZIF-8@BTA aqueous solution. Take 1 mL GO / MXene heterojunction aqueous solution and 1 mL ZIF-8@BTA aqueous solution, mix them after ultrasonic dispersion treatment and stir for 6 h to form a GO / MXene@ZIF-8 mixture.

[0054] Step 3: 1 mL of the GO / MXene@ZIF-8 mixture prepared in step 2, 0.3 g of polyurethane curing agent and 0.03 g of defoaming agent were added to 3 g of polyurethane in sequence, and the GO / MXene@ZIF-8 polyurethane lubricating anti-corrosion coating was obtained after stirring and ultrasonic dispersion treatment. The friction coefficient of the prepared GO / MXene@ZIF-8 polyurethane lubricating anti-corrosion coating was higher than that of the epoxy resin lubricating anti-corrosion coating in Example 1 after the friction test.

[0055] Comparative Example 3 10 mg MoS2, 0.3 g epoxy resin curing agent and 0.03 g defoaming agent were added to 3 g epoxy resin in sequence, and MoS2 / EP (epoxy resin) coating was obtained after stirring and ultrasonic dispersion treatment.

[0056] Comparative Example 4 10 mg MXene, 0.3 g epoxy resin curing agent and 0.03 g defoaming agent were added to 3 g epoxy resin in sequence, and MXene / EP (epoxy resin) coating was obtained after stirring and ultrasonic dispersion treatment.

[0057] Comparative Example 5 5 mg ZIF-8, 0.3 g epoxy resin curing agent and 0.03 g defoaming agent were added to 3 g epoxy resin in sequence, and ZIF-8 / EP coating was obtained after stirring and ultrasonic dispersion treatment.

[0058] Performance Testing 1. Structural observation of MXene, GO / MXene and GO / MXene@ZIF-8 prepared in Example 1 Figure 1This is the transmission electron microscope (TEM) image of the MXene obtained in Example 1; the results show that the MXene presents a typical thin layer flake shape.

[0059] Figure 2 This is a transmission electron microscopy image of GO / MXene obtained in Example 1; the results show that GO / MXene are grafted together and the wrinkled structure of graphene oxide can be found.

[0060] Figure 3 This is a transmission electron microscopy image of GO / MXene@ZIF-8 obtained in Example 1; the results show that ZIF-8 nanoparticles are attached to the surface and lower layer of GO / MXene.

[0061] 2. XRD spectra of GO / MXene@ZIF-8, GO / MXene, MXene and ZIF-8@BTA obtained in Example 1.

[0062] Figure 4 XRD patterns of GO / MXene@ZIF-8, GO / MXene, MXene and ZIF-8@BTA obtained in Example 1; the results show that for MXene, the peaks at 5°, 16.2°, 36.8°, 53° and 60.9° correspond to the (002), (004), (104), (107) and (110) crystal planes of MXene; and the (002) peak of GO / MXene corresponds to the characteristic peak of graphene oxide, with a slight shift due to the formation of the heterojunction, and also shows the characteristic peaks of MXene at (004), (104), (107) and (110); GO / MXene@ZIF-8 shows the characteristic peaks of ZIF-8@BTA, which indicates that the crystal structure of ZIF-8 is anchored on the surface of the GO / MXene heterojunction.

[0063] 3. Determination of the friction properties of GO / MXene@ZIF-8 obtained in Example 1 Testing method: Using Q235 steel block (2×2 cm) and Si3N4 ball (6 mm in diameter) as friction pairs, tribological performance tests were performed on a material surface performance comprehensive tester. The Si3N4 ball remained relatively stationary, and the Q235 steel block slid back and forth with an amplitude of 2 mm. The test frequency was 1 Hz, the test load was 1 N, and the temperature was 25 °C. The friction coefficient was automatically recorded by a computer system connected to the test machine.

[0064] Figure 5 The friction coefficients of the GO / MXene@ZIF-8 coating, pure EP coating and MXene / EP coating of Comparative Example 4 prepared in Example 1 under specific test conditions are compared. Figure 5The EP curve represents the pure EP coating, the MXene curve represents the MXene / EP coating, and the GO / MXene@ZIF-8 curve represents the GO / MXene@ZIF-8 coating. The specific test conditions are: in a 3.5 wt% NaCl solution, a load of 100 g is applied, and the friction test is performed at a frequency of 1 Hz for 30 minutes. GO / MXene@ZIF-8 coating: Under the test conditions, the coating exhibits an extremely low friction coefficient, with an average value as low as 0.03. This value is significantly lower than the other two coatings, showing its significant advantage in lubrication performance. Pure EP coating: In contrast, the pure EP coating has a higher friction coefficient under the same test conditions, indicating that its lubrication performance is relatively weak. MXene / EP coating: Although the two-dimensional material MXene is added to improve the lubrication performance, its friction coefficient is still higher than that of the GO / MXene@ZIF-8 coating, indicating that the single component MXene is limited in improving the lubrication performance.

[0065] Figure 6 The friction coefficient statistics of the GO / MXene@ZIF-8 coating prepared in Example 1 after 120 minutes of continuous friction test are presented. The figure clearly shows the performance stability of the coating under long-term friction conditions. The test results show that the friction coefficient of the GO / MXene@ZIF-8 epoxy resin coating can still be stably maintained at around 0.03 after 120 minutes of continuous friction. This value is much lower than the friction coefficient of many traditional coatings, which fully demonstrates that the GO / MXene@ZIF-8 coating has excellent low friction characteristics and can significantly reduce energy loss and wear during friction.

[0066] Figure 7 The Nyquist plot of the GO / MXene@ZIF-8 composite anti-corrosion coating prepared in Example 1 after being immersed in a 3.5 wt% NaCl aqueous solution for different times (0th day, 10th day, 21st day and 30th day) is shown. This figure intuitively reflects the change of the corrosion resistance of the coating over time.

[0067] The experimental data revealed that the GO / MXene@ZIF-8 coating exhibited amazing impedance performance in the initial immersion stage (first day), which was as high as 3.2×10 7 The impedance simulation value of Ω·cm² directly proves that the coating has excellent anti-corrosion barrier function in the initial stage, which can effectively isolate the corrosive medium and ensure that the base material is not damaged.

[0068] As the immersion time continued, until the 30th day, despite the long-term exposure of the coating to the corrosive environment, its impedance simulation value remained stable at about 2.5×10 6This data strongly demonstrates that the GO / MXene@ZIF-8 coating still maintains a strong anti-corrosion ability under long-term service conditions, can significantly slow down the corrosion process, and ensure the long-term integrity of the substrate material is not damaged.

[0069] In summary, in the corrosion test of 3.5 wt% NaCl aqueous solution, the GO / MXene@ZIF-8 composite anti-corrosion coating not only has excellent initial protection performance, but also can maintain a high level of impedance characteristics over a long period of time, showing great potential and application prospects as a high-performance anti-corrosion material.

[0070] In addition, although exemplary embodiments have been described herein, the scope includes any and all embodiments based on the present application with equivalent elements, modifications, omissions, combinations (e.g., various embodiments intersecting schemes), adaptations or changes. The elements in the claims are to be interpreted broadly based on the language adopted in the claims, and are not limited to the examples described in this specification or during the practice of this application, and the examples are to be interpreted as non-exclusive. Therefore, this specification and examples are intended to be considered as examples only, and the true scope and spirit are indicated by the following claims and the full scope of their equivalents.

[0071] The above description is intended to be illustrative rather than restrictive. For example, the above examples (or one or more schemes thereof) may be used in combination with each other. For example, a person of ordinary skill in the art may use other embodiments when reading the above description. In addition, in the above-mentioned specific embodiments, various features may be grouped together to simplify the present application. This should not be interpreted as an intention that a feature of an application that does not require protection is necessary for any claim. On the contrary, the subject matter of the present application may be less than all the features of an embodiment of a particular application. Thus, the following claims are incorporated herein in the specific embodiments as examples or embodiments, wherein each claim is independently a separate embodiment, and it is considered that these embodiments may be combined with each other in various combinations or arrangements. The scope of the present invention should be determined with reference to the appended claims and the full scope of equivalent forms granted by these claims.

[0072] The above embodiments are only exemplary embodiments of the present application and are not intended to limit the present invention. The protection scope of the present invention is defined by the claims. Those skilled in the art may make various modifications or equivalent substitutions to the present invention within the essence and protection scope of the present application, and such modifications or equivalent substitutions shall also be deemed to fall within the protection scope of the present invention.

Claims

1. A lubricating anti-corrosion coating, characterized in that: The lubricating anti-corrosion coating includes a composite material, which includes a two-dimensional heterojunction material and a metal organic framework compound loaded on the two-dimensional heterojunction material, the two-dimensional heterojunction material has a two-dimensional nanosheet structure, the metal organic framework compound is loaded on the two-dimensional heterojunction material, the two-dimensional heterojunction material includes graphene oxide and MXene, the graphene oxide and MXene are grafted and connected, and the graphene oxide has a wrinkled structure.

2. The lubricating anti-corrosion coating according to claim 1, characterized in that: The composite material also includes a corrosion inhibitor, which is loaded on the metal organic framework compound.

3. The lubricating anti-corrosion coating according to claim 1, characterized in that: The metal organic framework compound includes one or more of ZIF-8, UiO-66, UiO-66-NH2, HKUST-1, MOF-5, MOF-74, NU-110, MIL-101 and MIL-53; the MXene includes titanium carbide; and the lubricating anti-corrosion coating also includes epoxy resin.

4. The lubricating anti-corrosion coating according to claim 2, characterized in that: The lubricating anti-corrosion coating also includes additives; the additives include one or more of solvents, defoamers, epoxy resin curing agents, etc.

5. The lubricating anti-corrosion coating according to claim 2, characterized in that: The mass fraction of the composite material in the lubricating anti-corrosion coating is 0.1-2%; the mass ratio of the metal organic framework compound to the corrosion inhibitor is 1-5:

1.

6. The lubricating anti-corrosion coating according to claim 2, characterized in that: The mass ratio of the two-dimensional heterojunction material and the metal organic framework compound in the composite material is 1:1-2; the mass ratio of graphene oxide and MXene in the two-dimensional heterojunction material is 0.8-5:1-3.

7. The lubricating anti-corrosion coating according to claim 4, characterized in that: The corrosion inhibitor includes one or more of benzotriazole, methylbenzotriazole or mercaptobenzothiazole; the epoxy resin curing agent includes one or more of ethylenediamine, diethylenediamine, triethylenediamine, etc.; the solvent includes water.

8. The method for preparing the lubricating anticorrosive coating according to claim 4, characterized in that: The preparation method comprises: mixing composite material, epoxy resin curing agent, defoaming agent, epoxy resin and solvent to obtain lubricating anti-corrosion coating.

9. The preparation method according to claim 8, characterized in that: The preparation method of the two-dimensional heterojunction material in the composite material includes: mixing graphene oxide and MXene in water, wherein MXene is added in batches, and reacting at room temperature to obtain a heterojunction of graphene oxide and MXene.

10. Use of the lubricating anti-corrosion coating according to any one of claims 1 to 7 or the preparation method of the lubricating anti-corrosion coating according to any one of claims 8 to 9 in the field of coatings.