Thermal visbreaking PET (Polyethylene Terephthalate) protective film
By adding liquid crystal material and adhesion modifier to the acrylic resin layer of the PET protective film, combined with multi-stage curing treatment, the problem of difficult removal and aging of the traditional PET protective film at high temperature is solved, and the adhesive reduction at high temperature is achieved Adhesion and enhance mechanical properties significantly improve the convenience and reliability of use.
Patent Information
- Application Number
- CN202411231893.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-12-06
AI Technical Summary
Traditional PET protective films are difficult to remove in high temperature environments, easily damage the protected surface, leaving residual glue, and are prone to aging and brittle cracking at high temperatures, resulting in reduced mechanical properties and service life.
Using a heat-relieving PET protective film, by adding liquid crystal material to the acrylic resin layer, combining silane coupling agent or fluorine compound, the thermal responsiveness of the liquid crystal material reduces adhesion at high temperatures, ensuring good adhesion at room temperature. Attached performance, and improve mechanical properties and weather resistance through multi-stage curing treatment.
It realizes a protective film that is easy to remove at high temperature, prevents damage to the protected surface and residual glue problems, while improving mechanical performance and service life, providing a more balanced and efficient solution, and solving traditional PET protective film Problem of unstable adhesion performance under temperature changes.
Smart Images

Figure CN119081564A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials and surface treatment, in particular to a thermally viscous PET protective film. Background Art
[0002] In modern industrial and consumer electronics, PET protective films are widely used to protect display screens, touch screens and other sensitive surfaces. However, with the diversification of usage environments and application scenarios, especially in high temperature environments, traditional PET protective films have exposed many problems, affecting their use effect and user experience.
[0003] Traditional PET protective films usually use acrylic resin as an adhesive layer during the preparation process to ensure that they have good adhesion and transparency at room temperature. However, under high temperature conditions, this adhesive layer often exhibits too high adhesion, making the protective film difficult to remove, which not only easily damages the protected surface, but also may leave residual adhesive that is difficult to remove. In addition, traditional PET protective films are prone to aging and brittle cracking at high temperatures, which greatly reduces their mechanical properties and service life.
[0004] Therefore, the present invention provides a thermally de-viscous PET protective film to solve the deficiencies of the prior art. Summary of the invention
[0005] In view of the problems in the prior art that traditional PET protective films are difficult to remove under high temperature conditions, easily damage the protected surface, leave residual glue, and are prone to aging and cracking under high temperature, the present invention provides a thermally-reduced PET protective film, which enables the protective film to exhibit different adhesion strengths at room temperature and high temperature, optimizes the adhesion performance, and significantly improves the use effect and reliability of the protective film.
[0006] To achieve the above objectives, the present invention is implemented by the following technical scheme: a thermally de-viscous PET protective film, comprising:
[0007] PET substrate;
[0008] An acrylic resin layer coated on the surface of the PET substrate;
[0009] a liquid crystal material added to the acrylic resin layer;
[0010] The weight of the liquid crystal material accounts for 5% to 15% of the total weight of the acrylic resin layer.
[0011] Preferably, the acrylic resin layer has a thickness of 5 to 20 microns.
[0012] Preferably, the weight percentage composition of the acrylic resin layer includes:
[0013] Acrylic resin: 65% to 80%;
[0014] Liquid crystal material: 5% to 15%;
[0015] Plasticizer: 5% to 10%;
[0016] Stabilizer: 0.5% to 5%;
[0017] Adhesion modifiers: 1% to 5%.
[0018] Furthermore, the weight percentage of the liquid crystal material is 10 to 15%.
[0019] Preferably, the plasticizer is one or more of phthalates, adipates or citrates.
[0020] Preferably, the stabilizer is one or more of an antioxidant, a light stabilizer or a UV absorber.
[0021] Preferably, the adhesion modifier is one or more of a silane coupling agent or a fluorine compound.
[0022] Silane coupling agent or fluorine compound: These adhesion modifiers significantly improve the initial adhesion performance of the protective film through chemical bonding or strong interaction with acrylic resin and the protected surface at room temperature. Silane coupling agent forms a strong chemical bond with the surface of the substrate by forming a silicon-oxygen bond; fluorine compounds improve the weather resistance and adhesion strength of the protective film through their unique surface activity.
[0023] Preferably, the thickness of the PET substrate is 30 to 150 microns.
[0024] Preferably, the liquid crystal material is a liquid crystal compound having thermal responsiveness, including one or more of cholesteric liquid crystal, nematic liquid crystal or blue phase liquid crystal.
[0025] Liquid crystal materials have unique thermal responsiveness, that is, within a specific temperature range, the molecular arrangement state of liquid crystal materials will change, thereby changing their physical and chemical properties.
[0026] The liquid crystal material itself has good transparency and optical properties, which can ensure that the protective film does not affect the display effect during application. At room temperature, the silane coupling agent or fluorine compound ensures good adhesion between the protective film and the protected surface, and the liquid crystal material is in a stable state and does not interfere with the adhesion.
[0027] When the temperature changes, it can respond quickly and change the molecular arrangement state, which affects the microstructure of the liquid crystal material on the one hand, and at the macroscopic performance level, affects the interaction between adjacent materials in a short time, thereby reducing the adhesion. Therefore, under heating conditions, these liquid crystal materials can effectively reduce the adhesion of the acrylic resin layer, making the protective film easy to remove in a high temperature environment.
[0028] in:
[0029] Cholesteric liquid crystal has unique optical properties and good thermal responsiveness. When heated, its helical structure changes, resulting in a significant reduction in the adhesion of the acrylic resin layer coated on the PET substrate. When heated, the molecular arrangement of nematic liquid crystal changes from ordered to disordered, thereby reducing adhesion. Blue phase liquid crystal exhibits stable thermal responsiveness over a wide temperature range, and its molecular structure rearranges when heated, significantly reducing adhesion.
[0030] When the temperature rises to the phase transition temperature of the liquid crystal material, the molecular structure of the liquid crystal material changes (such as the nematic phase liquid crystal changes from ordered to disordered, the helical structure of the cholesteric phase liquid crystal becomes loose, etc.), resulting in the weakening of the interaction force between the liquid crystal molecules, which is then transmitted to the acrylic resin layer, significantly reducing the adhesion of the entire adhesion layer.
[0031] Although silane coupling agents or fluorine compounds improve adhesion, the phase change characteristics of liquid crystal materials at high temperatures dominate the change in overall adhesion. The thermal responsiveness of liquid crystal materials makes the effect of reducing adhesion at high temperatures more significant, thus achieving high-temperature viscosity reduction.
[0032] In an environment with little temperature fluctuation, silane coupling agents or fluorine compounds ensure the stability of the adhesion of the protective film, solving the problem of unstable adhesion caused by ambient temperature changes. The addition of liquid crystal materials provides a unique viscosity reduction function under high temperature conditions.
[0033] Preferably, a method for preparing a thermally detackified PET protective film comprises the following steps:
[0034] Provide PET substrate;
[0035] The acrylic resin, liquid crystal material, plasticizer, stabilizer and adhesion modifier are uniformly mixed according to the following weight percentages to prepare a coating liquid:
[0036] Acrylic resin: 65% to 80%;
[0037] Liquid crystal material: 5% to 15%;
[0038] Plasticizer: 5% to 10%;
[0039] Stabilizer: 0.5% to 5%;
[0040] Adhesion modifiers: 1% to 5%;
[0041] The coating liquid is evenly coated on the surface of the PET substrate;
[0042] The coating liquid coated on the surface of the PET substrate is subjected to a multi-stage curing treatment, first pre-curing at a low temperature and then completing curing at a high temperature to obtain a thermally viscous PET protective film.
[0043] Preferably, the multi-stage curing process comprises the following steps:
[0044] Pre-cure at 60 to 80°C for 10 to 20 minutes;
[0045] Complete curing at 120 to 150°C for 5 to 15 minutes;
[0046] or by UV curing, wherein the UV curing power is 100 to 200 mW / cm 2 , time is 10 to 30 seconds.
[0047] Finally, a release film is attached to the coating layer to protect the acrylic resin coating layer and facilitate subsequent use.
[0048] Pre-curing at 60 to 80°C can gradually volatilize the solvent in the coating liquid, and at the same time, the acrylic resin begins to cross-link to form a preliminary network structure, which helps to improve the adhesion and stability of the coating and prepare for subsequent full curing. At 120 to 150°C, the acrylic resin can be further cross-linked to form a tighter network structure, thereby improving the hardness, wear resistance and chemical resistance of the coating.
[0049] The present invention provides a thermally viscous PET protective film, which has the following beneficial effects:
[0050] 1. The present invention achieves the technical effect of reducing adhesion under heating conditions by adding a liquid crystal material (including cholesteric liquid crystal, nematic liquid crystal and blue phase liquid crystal) with thermal responsiveness to the acrylic resin layer. The problem of the traditional PET protective film being difficult to remove under high temperature environment is solved, and damage to the protected surface and residual adhesive problems are prevented. By optimizing and regulating the type and proportion of liquid crystal materials, as well as the compounding and synergistic effect between the components of the acrylic resin system, the practical convenience and reliability of the protective film are significantly improved.
[0051] 2. The acrylic resin layer of the present invention includes acrylic resin, liquid crystal material, plasticizer, stabilizer and adhesion modifier, so that the protective film has excellent mechanical properties, weather resistance and stability while realizing the heat-reducing viscosity function, solving the problem that a single component in the prior art is difficult to take into account multiple properties, and providing a more balanced and efficient solution.
[0052] 3. The use of additives such as plasticizers and stabilizers can effectively prevent the protective film from aging and cracking under high temperature conditions, extend its service life, and improve the reliability of overall performance.
[0053] 4. By compounding silane coupling agent or fluorine compound with liquid crystal material in the acrylic resin layer, the present invention achieves optimized adhesion performance under different temperature conditions. Silane coupling agent or fluorine compound ensures stable adhesion at room temperature, while liquid crystal material significantly reduces adhesion through phase change under high temperature conditions, thereby achieving a viscosity reduction effect. This combination enables the protective film to have a wide range of applicability and excellent thermal viscosity reduction performance, solving the problem of unstable adhesion performance of traditional PET protective film under temperature changes.
[0054] 5. The present invention adopts a multi-stage curing process, which not only improves the mechanical strength and adhesion of the coating, but also effectively prevents stress concentration and defect generation inside the coating, ensuring the high performance of the protective film in practical applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] Figure 1 The present invention is a flow chart of the preparation method of the thermally detackified PET protective film. DETAILED DESCRIPTION
[0056] The following will be combined with the drawings in the specification of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0057] Example: Please refer to the attached Figure 1 .
[0058] The raw materials used in the embodiments of the present invention can all be purchased directly from the market.
[0059] Example 1
[0060] Recipe composition:
[0061] Acrylic resin: 70%
[0062] Liquid crystal material: 5% (cholesteric liquid crystal)
[0063] Plasticizer: 8% (dioctyl phthalate)
[0064] Stabilizer: 2% (antioxidant)
[0065] Adhesion modifier: 5% (silane coupling agent)
[0066] Preparation steps:
[0067] PET substrate preparation: Select a PET substrate with a thickness of 50 microns.
[0068] Preparation of coating liquid: 70% acrylic resin, 5% liquid crystal material, 8% dioctyl phthalate, 2% antioxidant and 5% silane coupling agent are mixed evenly to prepare coating liquid.
[0069] Coating: Use a knife coater to evenly coat the coating liquid on the surface of the PET substrate, with a coating thickness of 15 microns.
[0070] Curing treatment:
[0071] Pre-cure at 70°C for 15 minutes;
[0072] Curing was completed at 130°C for 10 minutes.
[0073] Finally, a release film is attached to the coating layer to protect the acrylic resin coating layer and facilitate subsequent use.
[0074] Example 1 uses a higher proportion of silane coupling agent (5%) to enhance the adhesion modification effect, and selects dioctyl phthalate as a plasticizer to ensure the flexibility of the film. This formula exhibits excellent thermal viscosity reduction performance under high temperature conditions while maintaining good mechanical strength and flexibility.
[0075] Embodiment 2:
[0076] Recipe composition:
[0077] Acrylic resin: 75%
[0078] Liquid crystal material: 8% (cholesteric liquid crystal)
[0079] Plasticizer: 7% (dioctyl adipate)
[0080] Stabilizer: 3% (light stabilizer)
[0081] Adhesion modifier: 3% (fluorine compound)
[0082] Preparation steps:
[0083] PET substrate preparation: Select a PET substrate with a thickness of 75 microns.
[0084] Preparation of coating liquid: 75% acrylic resin, 8% liquid crystal material, 7% dioctyl adipate, 3% light stabilizer and 7% fluorine compound are mixed evenly to prepare coating liquid.
[0085] Coating: Use spraying equipment to evenly coat the coating liquid on the surface of the PET substrate, with a coating thickness of 10 microns.
[0086] Curing treatment:
[0087] Pre-cure at 80°C for 20 minutes;
[0088] Curing was completed at 150°C for 5 minutes.
[0089] Finally, a release film is attached to the coating layer to protect the acrylic resin coating layer and facilitate subsequent use.
[0090] In Example 2, the mechanical strength of the film is improved by increasing the proportion of acrylic resin to 75%, and the weather resistance of the film is enhanced by using light stabilizers and fluorine compounds. The formula is optimized in the proportion of adhesion modifier and liquid crystal material, so that it maintains good viscosity reduction effect and mechanical properties under high temperature conditions.
[0091] Embodiment 3:
[0092] Recipe composition:
[0093] Acrylic resin: 65%
[0094] Liquid crystal material: 15% (cholesteric liquid crystal)
[0095] Plasticizer: 10% (tributyl citrate)
[0096] Stabilizer: 5% (UV absorber)
[0097] Adhesion modifier: 1% (silane coupling agent)
[0098] Preparation steps:
[0099] PET substrate preparation: Select a PET substrate with a thickness of 100 microns.
[0100] Preparation of coating liquid: 65% acrylic resin, 15% liquid crystal material, 10% tributyl citrate, 5% ultraviolet absorber and 8% silane coupling agent are mixed evenly to prepare coating liquid.
[0101] Coating: The coating liquid was evenly coated on the surface of the PET substrate using a dip coating process, with a coating thickness of 20 microns.
[0102] Curing treatment:
[0103] Pre-cure at 60°C for 10 minutes;
[0104] Complete curing at 120°C for 15 minutes;
[0105] UV curing: UV curing power is 150mW / cm 2 , time is 20 seconds.
[0106] Finally, a release film is attached to the coating layer to protect the acrylic resin coating layer and facilitate subsequent use.
[0107] Example 3 further enhances the thermal viscosity reduction performance by increasing the proportion of liquid crystal material to 15%, and uses ultraviolet absorbers to enhance the light resistance of the film. Tributyl citrate is used as a plasticizer to ensure the flexibility and elongation of the film. This formula shows a balanced effect in all aspects of performance, especially showing a significant viscosity reduction effect under high temperature conditions.
[0108] Example 4
[0109] The difference between this embodiment and embodiment 3 is that the liquid crystal material used in this embodiment is nematic liquid crystal.
[0110] Example 5
[0111] The difference between this embodiment and embodiment 3 is that the liquid crystal material used in this embodiment is blue phase liquid crystal.
[0112] Example 6
[0113] The difference between this embodiment and embodiment 3 is that the liquid crystal materials used in this embodiment are nematic liquid crystal and cholesteric liquid crystal, and the ratio thereof is 1:1.
[0114] Example 7
[0115] The difference between this embodiment and embodiment 3 is that the liquid crystal materials used in this embodiment are nematic liquid crystal, cholesteric liquid crystal and blue phase liquid crystal, and the ratio thereof is 1:1:0.5.
[0116] Example 8
[0117] The difference between this embodiment and Embodiment 6 is that the mass percentage of the liquid crystal material used in this embodiment is 10%.
[0118] Example 9
[0119] The difference between this embodiment and Embodiment 6 is that the mass percentage of the liquid crystal material used in this embodiment is 12%.
[0120] Example 10
[0121] The difference between this embodiment and embodiment 9 is that the mass percentage of the adhesion modifier used in this embodiment is 2%.
[0122] Embodiment 11
[0123] The difference between this embodiment and embodiment 9 is that the mass percentage of the adhesion modifier used in this embodiment is 3%.
[0124] The mechanical properties and weather resistance of the heat-reducing protective film prepared in the examples of the present application are the same as those of the traditional PET protective film, and are not the focus of experimental testing here.
[0125] Comparative Example:
[0126] Comparative Example 1
[0127] The difference between Comparative Example 1 and Example 1 is that an equal amount of acrylic resin is used in this comparative example to replace the liquid crystal material.
[0128] Comparative Example 1 does not add liquid crystal material, and its adhesion performance under high temperature conditions is tested to evaluate the key role of the liquid crystal material in achieving the thermal viscosity reduction effect.
[0129] Comparative Example 2
[0130] The difference between Comparative Example 2 and Example 1 is that this comparative example uses 20% of liquid crystal material.
[0131] The proportion of liquid crystal material in Comparative Example 2 is beyond the scope of this patent, and its adhesion performance under high temperature conditions is tested to evaluate the effect of the proportion of liquid crystal material on the thermal viscosity reduction effect.
[0132] Comparative Example 3
[0133] The difference between Comparative Example 3 and Example 1 is that the curing step of this comparative example does not undergo pre-curing, but adopts one-time curing molding, specifically, the curing is completed at 130° C. for 25 minutes.
[0134] Comparative Example 4
[0135] The difference between Comparative Example 4 and Example 1 is that the curing step of this comparative example does not undergo high-temperature curing, but instead adopts one-time curing molding. Specifically, the curing is carried out at 70°C. Since the pre-curing step fails to complete the curing process within 25 minutes, the time is postponed until complete curing, which is 75 minutes.
[0136] The curing steps of Comparative Examples 3 and 4 are different from the curing steps of the present invention, and their adhesion properties under high temperature conditions are tested to evaluate the effect of the curing steps used in the present invention on the thermal viscosity reduction effect.
[0137] Comparative Example 5
[0138] The difference between Comparative Example 5 and Example 1 is that in this comparative example, the coating liquid is uniformly coated on the surface of the PET substrate, and the coating thickness is 23 microns.
[0139] The coating thickness of Comparative Example 5 is different from that of the present invention, and its adhesion performance under high temperature conditions is tested to evaluate the effect of the coating thickness of the present invention on the thermal viscosity reduction effect.
[0140] Comparative Experimental Design and Analysis
[0141] Comparative experiment scheme: In order to comprehensively evaluate the adhesion of Examples 1-113, Comparative Examples 1-5 and traditional PET protective films at room temperature and high temperature environments, the following experiments were conducted.
[0142] Experimental steps:
[0143] Sample preparation: Several samples of Examples 1-11, Comparative Examples 1-5 and traditional PET protective film were placed in a room temperature (25° C.) environment for stabilization for 24 hours to ensure the accuracy of the test results, and then cut into sizes of 20 cm*15 cm for testing.
[0144] Peel strength test: The force required to peel each sample from the adhered object at room temperature (25°C), 40°C, 55°C and 70°C was measured to obtain the peel strength / adhesion force of each sample.
[0145] Residue test: Check whether there is residual glue on the surface of the object after the thermally debonded PET protective film sample is peeled off, to ensure that its residual glue performance meets the electronic industry standards.
[0146] The test data are shown in Table 1.
[0147] Table 1 Test data of Examples 1-11, Comparative Examples 1-5, and traditional PET protective film
[0148]
[0149] Result analysis:
[0150] It can be seen from the test data that the present invention utilizes the compounding and synergistic effect between the components to have good bonding performance at room temperature, while the bonding performance gradually decreases under the condition of rising temperature, and exhibits a significant viscosity reduction effect under high temperature conditions.
[0151] Combining the data of Example 3, Example 9, Example 10, and Example 11, the dosage relationship between the liquid crystal material and the adhesion modifier has an impact on the thermal viscosity reduction of the PET protective film. When the weight percentage of the liquid crystal material is 12% and the weight percentage of the adhesion modifier is 2%, the overall performance of the PET protective film is excellent.
[0152] Combining the data of Example 1 with Comparative Examples 3 and 4, the staged curing in the re-preparation process of the present invention has a certain influence on the performance of the thermally debonded PET protective film. The staged curing can improve the adhesion ability of the system material at room temperature and the peeling property at high temperature.
[0153] It should be understood that the above embodiments are exemplary and are not intended to include all possible implementations included in the claims. Various modifications and changes may be made on the basis of the above embodiments without departing from the scope of the present disclosure. Similarly, the various technical features of the above embodiments may be arbitrarily combined to form other embodiments of the present invention that may not be explicitly described. Therefore, the above embodiments only express several implementations of the present invention and do not limit the scope of protection of the patent of the present invention.
Claims
1. A thermally de-viscous PET protective film, characterized in that: include: PET substrate; An acrylic resin layer coated on the surface of the PET substrate; a liquid crystal material added to the acrylic resin layer; The weight of the liquid crystal material accounts for 5% to 15% of the total weight of the acrylic resin layer.
2. A thermally de-viscous PET protective film according to claim 1, characterized in that: The thickness of the acrylic resin layer is 5 to 20 micrometers.
3. A thermally de-viscous PET protective film according to claim 1, characterized in that: The weight percentage composition of the acrylic resin layer includes: Acrylic resin: 65% to 80%; Liquid crystal material: 5% to 15%; Plasticizer: 5% to 10%; Stabilizer: 0.5% to 5%; Adhesion modifiers: 1% to 5%.
4. A thermally de-viscous PET protective film according to claim 3, characterized in that: The plasticizer is one or more of phthalates, adipates or citrates.
5. A thermally de-viscous PET protective film according to claim 3, characterized in that: The stabilizer is one or more of an antioxidant, a light stabilizer or a UV absorber.
6. A thermally de-viscous PET protective film according to claim 3, characterized in that: The adhesion modifier is one or more of a silane coupling agent or a fluorine compound.
7. A thermally de-viscous PET protective film according to claim 1, characterized in that: The thickness of the PET substrate is 30 to 150 microns.
8. A thermally de-viscous PET protective film according to claim 1, characterized in that: The liquid crystal material is a liquid crystal compound with thermal responsiveness, including one or more of cholesteric liquid crystal, nematic liquid crystal or blue phase liquid crystal.
9. A method for preparing a thermally de-viscous PET protective film according to any one of claims 1 to 8, characterized in that: The following steps are involved: Provide PET substrate; The acrylic resin, liquid crystal material, plasticizer, stabilizer and adhesion modifier are uniformly mixed according to the following weight percentages to prepare a coating liquid: Acrylic resin: 65% to 80%; Liquid crystal material: 5% to 15%; Plasticizer: 5% to 10%; Stabilizer: 0.5% to 5%; Adhesion modifiers: 1% to 5%; The coating liquid is evenly coated on the surface of the PET substrate; The coating liquid coated on the surface of the PET substrate is subjected to a multi-stage curing treatment, first pre-curing at a low temperature and then completing the curing at a high temperature; finally, a release film is attached to the coating layer to obtain a thermally de-viscous PET protective film.
10. The method for preparing a thermally de-viscous PET protective film according to claim 9, characterized in that: The multi-stage curing process comprises the following steps: Pre-cure at 60 to 80°C for 10 to 20 minutes; Complete curing at 120 to 150°C for 5 to 15 minutes; or by UV curing, wherein the UV curing power is 100 to 200 mW / cm 2 , time is 10 to 30 seconds.
Citation Information
Cited By
Electrified visbreaking easy-to-peel adhesive tape and preparation method thereof
CN121319806A