Method for controlling nitrogen content of molten steel of RH furnace
By calculating the theoretical solubility and actual nitrogen content, and using the circulation gas operation mode to increase and decrease nitrogen in the RH furnace, the problem of abnormal nitrogen content in the water of RH furnace is solved, and the accurate control of nitrogen content and improvement of production efficiency is achieved.
Patent Information
- Application Number
- CN202411196288.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
AI Technical Summary
The existing RH furnace water nitrogen content control method is difficult to accurately adjust when the nitrogen content is higher or lower than the steel grade boundary after repressure, resulting in passive production and low remedial measures, with element mismatch and poor line feeding effect. The problem.
By obtaining the temperature, composition and nitrogen content information of RH furnace molten steel, calculating the theoretical solubility and actual nitrogen content, using different circulation gas operating modes to increase or reduce nitrogen, and using the molten steel in the rising impregnation tube to greatly increase and decrease nitrogen, ensuring that The nitrogen content of the whole furnace steel meets the requirements.
Accurate control of nitrogen content, improve efficiency, reduce costs, and ensure that the molten steel meets the requirements of steel grades.
Smart Images

Figure BDA0005016500300000041 
Figure BDA0005016500300000042 
Figure BDA0005016500300000061
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metallurgy, and in particular to a method for controlling nitrogen content in molten steel of an RH furnace. Background Art
[0002] During molten steel refining, increasing the nitrogen content in molten steel by methods such as LF bottom blowing N and RH circulating blowing N is more cost-effective than increasing N by using alloys such as chromium nitride, manganese nitride, or wire, and is therefore widely used.
[0003] At present, the nitrogen content or nitrogen increase in each furnace of molten steel can only be controlled more accurately by adopting the technology of blowing nitrogen to control nitrogen. For example, the nitrogen content in most furnaces can be controlled within the target value of ±20ppm. However, due to the influence of certain accidental factors, there will be furnaces with nitrogen content higher or lower than the boundary of steel grade occasionally. Because after RH is re-pressurized to atmospheric pressure, if the subsequent protective measures are well done, the soft blowing and continuous casting pouring processes basically do not increase or increase nitrogen very little. Therefore, if the RH furnace of a certain furnace has been re-pressurized to atmospheric pressure (re-pressurization means that the RH furnace is gradually re-pressurized from a certain vacuum state to the atmospheric state, and the molten steel in the RH furnace will gradually flow back to the ladle below the RH furnace through two immersion tubes) at this time, but it is suddenly known that the nitrogen content of the molten steel in this furnace may be higher or lower than the boundary of steel grade, production will be very passive. Although it is currently Previously, the abnormal low nitrogen content can be remedied by re-pressurizing the RH furnace to atmospheric pressure and then feeding chromium nitride wire and manganese nitride wire. However, there are problems such as "other elements except N (such as Cr and Mn) may not meet the steel grade requirements after wire feeding, slag mixing during wire feeding, large-scale exposure of molten steel surface is prone to macroscopic inclusions, and steel mills that use RH circulating N blowing method to increase N in large quantities may not necessarily have spare wires such as chromium nitride wire, or even if they have spare wires, they are prone to deterioration due to moisture and rust if not used for a long time, resulting in poor effect of wire feeding to increase N". Therefore, how to more reasonably deal with the above-mentioned nitrogen content abnormalities, that is, the situation where the nitrogen content after re-pressing is higher or lower than the boundary nitrogen content of the steel grade, especially the situation where N is lower than the boundary nitrogen content of the steel grade, is an urgent problem to be solved. Summary of the invention
[0004] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and provide a method for controlling the nitrogen content of molten steel in a RH furnace.
[0005] The present invention solves the technical problem by adopting the following technical solutions.
[0006] The present invention provides a method for controlling the nitrogen content of RH furnace molten steel, comprising the following steps: obtaining the temperature, composition and nitrogen content information of the RH furnace molten steel after re-pressurization, judging the nitrogen increase or decrease demand of the RH furnace molten steel, comparing and calculating the theoretical solubility X of nitrogen in the molten steel, and determining the nitrogen content of the molten steel after re-pressurization. 溶解度According to the final nitrogen content X' of the cylindrical molten steel in the actual immersion tube in the RH furnace, different circulating gas operation modes are used to increase or reduce nitrogen in the molten steel.
[0007] The present invention has the following beneficial effects:
[0008] The present invention provides a method for controlling the nitrogen content of molten steel in an RH furnace, which provides relatively accurate nitrogen increase or nitrogen reduction parameters through calculation, realizes accurate nitrogen control, and can not only improve efficiency but also reduce costs. DETAILED DESCRIPTION
[0009] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out under normal conditions. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.
[0010] The following is a detailed description of a method for controlling nitrogen content in molten steel in an RH furnace provided by an embodiment of the present invention.
[0011] The present invention is mainly aimed at the situation that the nitrogen content of molten steel still does not meet the steel grade control requirements after the RH furnace molten steel is subjected to the N increasing / controlling operation.
[0012] The molten steel in this part of the cylinder (and the molten steel below and nearby) is greatly increased / decreased in N2 gas or Ar gas circulation in a short period of time through the rising immersion pipe with a cylindrical inner cavity of RH. After the increase / decrease of N is completed or during the increase / decrease of N, it is mixed into the remaining molten steel to achieve the effect of increasing / decreasing N of the whole furnace molten steel as a whole, and finally meet the nitrogen content requirements of the steel grade. It is easy to know that without considering the subsequent impact on the soft blowing time of the molten steel, the nitrogen content in the molten steel can be further increased / decreased by multiple operations.
[0013] The following is an introduction taking the above-mentioned one-time increase N operation as an example.
[0014] First, lift or pull down the ladle so that the RH rising dip tube is almost filled with molten steel. The weight of the cylindrical molten steel in the rising dip tube is m, m = ρ*1 / 4π*D 2 *H=3.55t, where:
[0015] ρ is the density of molten steel, generally 7.4t / m 3 :
[0016] D is the inner diameter of the ascending immersion pipe, generally 0.6m;
[0017] H is the height inside the rising immersion pipe, which is generally 1.7m.
[0018] According to the equation: the total increase in N of the entire furnace molten steel = the total increase in N of the cylindrical molten steel in the rising immersion tube, that is, M*(N 后 -N 前 )=m*(XN 前 ),in:
[0019] M is the total weight of molten steel in a furnace, such as 130t.
[0020] m is the weight of the cylindrical molten steel in the rising immersion tube, such as 3.55t.
[0021] N 前 It is the initial value of nitrogen content in the whole furnace of molten steel after or during re-pressing, in % or ppm, such as 0.012% = 120ppm.
[0022] N 后 It is the target value of nitrogen content in the whole furnace of molten steel, in % or ppm, such as 0.013% = 130ppm.
[0023] X is the final nitrogen content of the theoretical cylindrical molten steel in the rising immersion tube, in % or ppm, such as 0.04% = 400 ppm.
[0024] It is easy to obtain that X=M*(N 后 -N 前 ) / m+N 前
[0025] The total weight of the molten steel is 130t, N 前 =80~160ppm, N 后 =90~190ppm as an example,
[0026] The theoretical values of X can be calculated separately and are shown in Table 1 below.
[0027] Table 1
[0028]
[0029] In addition, in the actual process of N increase by circulating blowing, due to the existence of diffusion, mass transfer and other effects, the molten steel that increases N is not only the cylindrical molten steel in the rising immersion tube, but also the molten steel near its bottom. If the circulation promotion effect of bottom blowing is taken into account, the actual amount of molten steel that increases N is greater. Therefore, the actual equivalent amount of molten steel that increases N is m'≈n*m, where:
[0030] n is: equivalent influence multiple of molten steel quantity, taking n=6 as an example.
[0031] m'≈n*m=6*3.55t=21.3t,
[0032] Then X'≈M*(N 后 -N 前 ) / m'+N 前≈M*(N 后 -N 前 ) / 6m+N 前
[0033] After conversion, X'≈(X+5N 前 ) / 6
[0034] X'≈[X+(n-1)N 前 ] / n
[0035] Similarly, the total weight of the molten steel in the furnace is 130t, N 前 =80~160ppm, N 后 =90~190ppm as an example,
[0036] The final nitrogen content requirement X' of the cylindrical molten steel in the actual ascending immersion tube (and the molten steel near its lower part) can be calculated and is shown in Table 2 below.
[0037] Table 2
[0038]
[0039] From the above, it can be seen that different n values have different requirements for the required X'. Generally, the larger the n value, the smaller the required X' is at the same increase in N.
[0040] However, under certain conditions, the amount of N added to molten steel is not infinite, and there is a certain theoretical upper limit:
[0041] The theoretical solubility of N can be calculated according to the following formula (1):
[0042] lg[N]=0.5lg(P N2 / P0)+lgX N- Y N (1)
[0043] Wherein, [N] is the mass fraction of nitrogen in molten steel, unit: %.
[0044] P N2 It is the partial pressure of N, in Pa.
[0045] P0 is the standard atmospheric pressure, unit is Pa; generally 101325Pa.
[0046] X N is the equilibrium constant, unit 1; and lgX N =-276 / T-1.185
[0047] Y N is the activity coefficient, unit 1; and lgY N=(3150 / T-0.69)*Z, where Z=0.12[C]+0.045[Si]-0.022[Mn]+0.044[P]+0.007[S]-0.026[Al]-0.095[V]-0.047[Cr]-0.012[Mo]+0.009[Ni]-0.51[Ti]-0.05[Nb]+0.09[B]+0.048T.[O], [C], [Si], etc. are the mass fractions of the elements in the molten steel, that is, Z is related to the content of the main elements / components in the molten steel.
[0048] Transforming formula (1) we can get
[0049] lg[N]=0.5lg(P N2 / P0)-276 / T-1.185-(3150 / T-0.69)*Z
[0050] That is, lg[N] = 0.5lg(P N2 / P0)-(276+3150Z) / T-(1.185-0.69Z)
[0051] That is, [N] = (P N2 / P0) 0.5 *10 -(276+3150Z) / T-(1.185-0.69Z)
[0052] It is also easy to know that the final nitrogen content of the cylindrical molten steel in the ascending immersion tube and the molten steel near the bottom after the nitrogen addition operation is as follows:
[0053]
[0054] Because N is increased at normal pressure after RH recompression, P N2 =P0=101325Pa.
[0055] T 后 : It is the Kelvin temperature of the cylindrical molten steel in the ascending immersion tube after the nitrogen addition operation, in K.
[0056] Where T 前 =T 后 +t*△
[0057] T 前 :It is the normal temperature of the molten steel after re-pressing / before preparing to increase N during re-pressing, in K; considering that N-containing steels generally contain S and Al, a higher superheat is required for pouring (30-40°C), the temperature drop during the pouring process is generally 25-35°C, and the temperature drop from RH leaving the station to continuous casting and hoisting is generally 5°C, the RH soft blowing time is 20-30min / 130-140t molten steel (the process temperature drop is about 0.3-1°C / min), and the temperature drop of the Ca feeding line is about 3-8°C. Therefore, T 前=Liquidus temperature + pouring superheat + pouring temperature drop + lifting temperature drop + soft blowing temperature drop + Ca feeding line temperature drop = (1470~1510)℃+(30~40)℃+(25~35)℃+5℃+(6~30)℃+(3~8)℃=(1539~1628)℃, generally take the median value of 1584℃, i.e. 1857K.
[0058] △ is the temperature drop during the N increase process, which is generally 3-5℃ / min, with a median value of 4℃ / min.
[0059] t is the N increase time, which is generally 0 to 6 minutes (in order to avoid affecting the subsequent soft blowing time as much as possible, the upper limit is set to 6 minutes), and 5 minutes is taken.
[0060] Therefore, T 后 =T 前 -△*t=(1584-4*5)℃=1564℃=1837K.
[0061] If T 前 Upper limit, then T 后 =T 前 -△*t=(1628-4*5)℃=1608℃=1881K.
[0062] Considering that the composition does not change much before and after the increase of N, 前 ≈Z 后 Perform calculations.
[0063] Therefore, formula (2) can be transformed into formula (3)
[0064]
[0065] It is easy to see from formula (3) that for a certain type of steel, Z 前 Basically the same, but the Z value of different steel grades is generally different, and there are positive and negative values.
[0066] Therefore, if -(276+3150Z 前 ) / T 后 -(1.185-0.69Z 前 ) is larger, the larger X 溶解度 The bigger.
[0067] The following is an explanation using three typical steel grades as examples.
[0068] Take steel grade 46MnVNbS5 as an example1
[0069] Steel grade 46MnVNbS5 (actual liquidus temperature 1479°C), the composition before N addition is C: 0.45%, Si: 0.63%, Mn: 1.15%, P: 0.018%, S: 0.058%, Al: 0.01%, V: 0.17%, Cr: 0.25%, Mo: 0.02%, Ni: 0.18%, Ti: 0.002%, Nb: 0.035%, B: 0.0002%, T.[O]: 0.0012%.
[0070] Z=0.12[C]+0.045[Si]-0.022[Mn]+0.044[P]+0.007[S]-0.026[Al]-0.095[V]-0.047[C r]-0.012[Mo]+0.009[Ni]-0.51[Ti]-0.05[Nb]+0.09[B]+0.048T.[O]=0.12*0.45+0.045 *0.63-0.022*1.15+0.044*0.018+0.007*0.058-0.026*0.01-0.095*0.17-0.047*0.25-0.012*0.02+0.009*0.18-0.51*0.002-0.05*0.035+0.09*0.0002+0.048*0.0012≈0.0288.
[0071] Case 1: With T 后 =1837K(the aforementioned T 后 Medium limit 1564℃); Z 前 =0.0288 as an example, we can get:
[0072] X 溶解度 ≈10 -(276+3150*0.0288) / 1837-(1.185-0.69*0.0288) ≈0.04318%≈432ppm.
[0073] Case 2: With T 后 =1842K (the liquidus temperature of this steel is 1479℃+90℃=1569℃, 90℃ is the common temperature difference relative to the liquidus); Z 前 =0.0288 as an example, we can get:
[0074] X 溶解度 ≈10 -(276+3150*0.0288) / 1842-(1.185-0.69*0.0288) ≈0.04323%≈432ppm.
[0075] Case 3: With T 后 =1881K(the aforementioned T 后 Upper limit 1608℃); Z 前 =0.0288 as an example, we can get:
[0076] X溶解度 ≈10 -(276+3150*0.0288) / 1881-(1.185-0.69*0.0288) ≈0.04364%≈436ppm.
[0077] Comparing the above three cases, it can be seen that the temperature has little effect on the increase of N in 46MnVNbS5 steel. 溶解度 The difference is about 4ppm. Refer to Table 2. 后 The actual impact is less than 1ppm.
[0078] Take H13 steel with high alloy content as an example
[0079] Steel grade H13 (actual liquidus temperature 1471°C), the composition before N addition is C: 0.38%, Si: 1.00%, Mn: 0.40%, P: 0.015%, S: 0.004%, Al: 0.015%, V: 0.90%, Cr: 5.20%, Mo: 1.25%, Ni: 0.04%, Ti: 0.005%, Nb: 0.009%, B: 0.0006%, T.[O]: 0.0012%.
[0080] Z=0.12[C]+0.045[Si]-0.022[Mn]+0.044[P]+0.007[S]-0.026[Al]-0.095[V]-0.047[ Cr]-0.012[Mo]+0.009[Ni]-0.51[Ti]-0.05[Nb]+0.09[B]+0.048T.[O]=0.12*0.38+0.0 45*1-0.022*0.4+0.044*0.015+0.007*0.004-0.026*0.015-0.095*0.9-0.047*5.2-0.012*1.25+0.009*0.04-0.51*0.005-0.05*0.009+0.09*0.0006+0.048*0.0012≈-0.265.
[0081] Case 1: With T 后 =1837K (the above-mentioned T limit is 1564℃); Z 前 =-0.265 as an example, we can get:
[0082] X 溶解度 ≈10 -(276-3150*0.265) / 1837-(1.185+0.69*0.265) ≈0.08636%≈864ppm.
[0083] Case 2: With T 后 =1834K (the liquidus temperature of this steel is 1471℃+90℃=1561℃, 90℃ is the common temperature difference relative to the liquidus); Z 前 =-0.265 as an example, we can get:
[0084] X 溶解度 ≈10 -(276-3150*0.265) / 1834-(1.185+0.69*0.265) ≈0.08646%≈865ppm.
[0085] Case 3: With T 后 =1881K(the aforementioned T 后 Upper limit 1608℃); Z 前 =-0.265 as an example, we can get:
[0086] X 溶解度 ≈10 -(276-3150*0.265) / 1881-(1.185+0.69*0.265) ≈0.08496%≈850ppm.
[0087] Comparing the above three cases, it can be seen that temperature has a slightly greater effect on the increase of N in H13 steel. 溶解度 The difference is about 15ppm. Refer to Table 2. 后 The actual impact is only about 1 to 2 ppm.
[0088] Comparative Example 1 and Example 2, i.e. 46MnVNbS5 and H13 steel, show that the Z value is 溶解度 The impact is greater, that is, the impact of steel type is greater, especially high-alloy steel types containing V, Cr, etc.
[0089] Take a high alloy steel grade as an example3
[0090] Case 1: With T 后 =1837K(the aforementioned T 后 Medium limit 1564℃); Z 前 =-0.8 as an example, we can get:
[0091] X 溶解度 ≈10 -(276-3150*0.8) / 1837-(1.185+0.69*0.8) ≈0.30518%≈3052ppm.
[0092] Case 2: With T 后 =1881K(the aforementioned T 后 Upper limit 1608℃); Z 前 =-0.8 as an example, we can get:
[0093] X 溶解度 ≈10 -(276-3150*0.8) / 1881-(1.185+0.69*0.8) ≈0.28575%≈2858ppm.
[0094] From Examples 1, 2, and 3 combined with Table 2, it can be seen that for gear steel, non-adjustable steel, and high alloy steel, theoretically, if the N increase time is sufficient, for example, N 前 80ppm, N 后 It can be 190ppm or more.
[0095] However, considering that the increase / decrease of N quantity / efficiency is closely related to pressure, flow rate, etc., and the general RH circulation N 2 / The Ar pressure is between 0.8 and 1.3 MPa, and the flow rate is between 60 and 120 m 3 / h, therefore, in order not to affect the production / soft blowing time (i.e. each N increase time ≤ 6min), and at the same time reduce the erosion of bubbles on the rising immersion tube when blowing N2 / Ar (i.e. the blowing flow rate cannot be too large and the time cannot be too long), the theoretical maximum N increase / decrease efficiency is about 70ppm / min, that is, the stable increase / decrease amount X' of the cylindrical molten steel in the rising immersion tube (and the molten steel below it) within a certain period of time each time has a theoretical limit. Considering that the final nitrogen content of general steel grades such as non-adjustable steel, gear steel, etc. is generally required to be 60-190ppm, for the increase in N, this method generally has a maximum stable increase in N of ≤20ppm each time (i.e. N 后 -N 前 ≤20ppm). Of course, for high alloy steel, it is easy to infer that the stable increase in N by this method should be higher; and for N reduction, the maximum stable N reduction by this method is generally ≤10ppm (i.e. N 前 -N 后 ≤10ppm).
[0096] Now X' and the circulating gas pressure P: (0.8 ~ 1.3) Mpa, flow rate L: (60 ~ 120) m 3 / h, increase / decrease N time t: (0~6)min, molten steel equivalent influence multiple n: (1~6) The relationship is explained through experiments.
[0097] For circulating N2 blowing N increasing operation: X'=14.4*t 0.3 *n 0.2 *P 0.1 *L 0.5
[0098] For the circulating Ar-blowing minus N operation: X' = 3.5*t 0.3 *n 0.2 *P 0.1 *L 0.5
[0099] And where n = 0.0107*P 0.4068 *L 1.3 .
[0100] To achieve the above object, the present invention provides the following technical solutions:
[0101] In view of the low nitrogen content in molten steel, the method for controlling the nitrogen content in molten steel in an RH furnace includes the following steps:
[0102] S1: Get the temperature of molten steel before N increase T 前 , composition and nitrogen content N前 and other information, judge (steel nitrogen content requirement lower limit -20ppm) ≤ N 前 ≤The lower limit of nitrogen content in steel grade is established. If yes, proceed to the next step.
[0103] S2: The molten steel temperature T before N increase obtained from S1 前 , composition and nitrogen content N 前 And other information, using the formula Calculate the theoretical maximum dissolved nitrogen content X in molten steel under this condition 溶解度 .
[0104] Where Z 前 =0.12[C]+0.045[Si]-0.022[Mn]+0.044[P]+0.007[S]-0.026[Al]-0.095[V]-0.047[Cr]-0.012[Mo]+0.009[Ni]-0.51[Ti]-0.05[Nb]+0.09[B]+0.048T.[O], [C], [Si], etc. are the mass fractions of elements in molten steel.
[0105] T 后 is the temperature of the molten steel after N is increased, in K, and T 后 =T 前 -△*t.
[0106] T 前 It is the temperature of molten steel before increasing N, in K, and its range is generally 1539~1628℃, that is, 1812~1901K, and is generally taken as (liquidus temperature + 90℃).
[0107] △ is the temperature drop during the N increase process, which is generally 3-5℃ / min, with a median value of 4℃ / min.
[0108] t is the N increase time, generally 0 to 6 minutes, 5 minutes is taken.
[0109] S3: Calculate the value of X', and X'=[X+(n-1)N 前 ] / n; X = M*(N 后 -N 前 ) / m+N 前 ,
[0110] Wherein, X' is the final nitrogen content of the cylindrical molten steel in the actual ascending immersion tube, in % or ppm.
[0111] X is the final nitrogen content of the theoretical cylindrical molten steel in the rising immersion tube, in % or ppm.
[0112] N 前 It is the initial value of nitrogen content in the whole furnace of molten steel after or during re-pressing, in % or ppm.
[0113] N 后 It is the target value of nitrogen content in the whole furnace of molten steel, in % or ppm.
[0114] M is the total weight of the entire furnace of molten steel, in t.
[0115] n: is the equivalent influence multiple of the molten steel volume, generally between 1 and 6. In order to obtain the actual maximum final nitrogen content of the cylindrical molten steel in the rising immersion tube, it is generally pre-calculated to be 6.
[0116] m: the weight of the cylindrical molten steel in the ascending immersion tube, in t, and m = ρ*1 / 4π*D 2 *H, where ρ is the density of molten steel, generally 7.4t / m 3 , D is the inner diameter of the rising immersion pipe, which is generally 0.6m, and H is the inner height of the rising immersion pipe, which is generally 1.7m.
[0117] S4: Judgement X 溶解度 ≥X' is true, if so, proceed to the next step.
[0118] S5: Based on the value of X' calculated from S3, use the empirical formula X' = 14.4*t 0.3 *n 0.2 *P 0.1 *L 0.5 , where n = 0.0107*P 0.4068 *L 1.3 , to determine the subsequent values of t, P, L, n and feasible operation modes.
[0119] S6: After performing the nitrogen increasing operation according to the aforementioned operation mode, the molten steel is subjected to possible operations such as soft blowing to achieve nitrogen increasing of the molten steel after the RH furnace molten steel is re-pressurized.
[0120] In view of the high nitrogen content in molten steel, the method for controlling the nitrogen content in molten steel in an RH furnace includes the following steps:
[0121] From the Excel file provided by the author, we can know that (of course, when X' is a negative number, it has no specific meaning, because the nitrogen content of molten steel cannot be a negative number and should be at least 0), in some special cases, such as n = 3, N 前 =140, N 后 =130, indicating that the nitrogen content of the molten steel has been reduced, which can be achieved by circulating air blowing (usually Ar) to make X'=18ppm.
[0122] S1: Get the molten steel temperature T before N reduction 前 , composition and nitrogen content N 前 and other information to determine the upper limit of nitrogen content in steel grade ≤N 前≤(upper limit of nitrogen content in steel grade + 10ppm), whether it is established, if so, proceed to the next step.
[0123] S2: Calculate the final nitrogen content X' of the cylindrical molten steel in the actual ascending immersion tube in the RH furnace;
[0124] S3: The value of X' calculated using S2, according to the empirical formula X' = 3.5*t 0.3 *n 0.2 *P 0.1 *L 0.5 , where n is the equivalent influence multiple of molten steel volume, n is usually 1 to 6, P is the circulating gas pressure, L is the circulating gas flow rate, t is the circulating gas circulation time, and the subsequent values of t, P, L, n and feasible operation modes are determined;
[0125] S4: After the nitrogen reduction operation is performed according to the operation mode determined in S3, the molten steel is soft-blown to achieve nitrogen reduction in the molten steel after the RH furnace molten steel is re-pressurized.
[0126] It is worth noting that for the final nitrogen content X' of the cylindrical steel liquid in the actual immersion tube in the RH furnace, if the total weight of the steel liquid in the whole furnace is 130t, N 前 =80~160ppm, N 后 =90~190ppm, when n≈6, the value of X' calculated by the formula can be seen in Table 2.
[0127] Example 1
[0128] Take the steel grade 46MnVNbS5 as an example (circulating N2 blowing is required to increase N).
[0129] After RH re-pressing of a furnace of molten steel, it was found that the temperature of the molten steel was 1569°C, and the composition was C: 0.45%, Si: 0.63%, Mn: 1.15%, P: 0.018%, S: 0.058%, Al: 0.01%, V: 0.17%, Cr: 0.25%, Mo: 0.02%, Ni: 0.18%, Ti: 0.002%, Nb: 0.035%, B: 0.0002%, T.[O]: 0.0012%, N: 100ppm (i.e. N 前 =100ppm), which is 20ppm less than the lower limit of 120ppm required for the N content of the steel grade.
[0130] Calculate X first 溶解度 ≈10 -(276+3150*0.0288) / 1842-(1.185-0.69*0.0288) ≈0.04323%≈432ppm, compared with Table 2, it can be seen that when n=6, N 前 100ppm, N 后 is 120ppm, X' can meet the requirement with only 222ppm, and because 222ppm<X 溶解度≈432ppm, so this method can be used to increase N.
[0131] First, lift the ladle to make the RH rising immersion tube almost full of molten steel; then continue to select possible parameters to increase N, for example, select the circulating N2 pressure P = 1.3Mpa, select the circulating N2 flow L = 120m 3 / h (n=0.0107*P 0.4068 *L 1.3 =0.0107*1.3 0.4068 *120 1.3 ≈6), at this time X'=14.4*t 0.3 *n 0.2 *P 0.1 *L 0.5 =14.4*t 0.3 *6 0.2 *1.3 0.1 *120 0.5 =231.73*t 0.3 =222, from which we can calculate t≈0.8668min≈52s.
[0132] That is, when P = 1.3Mpa, L = 120m 3 / h, t=52s, circulating N2 blowing operation can make N 前 =100ppm 46MnVNbS5 steel increases N to 120ppm to meet the steel grade requirements.
[0133] Example 2
[0134] Take the steel grade 46MnVNbS5 as an example (circulating Ar blowing is required to reduce N).
[0135] After RH re-pressing of a furnace of molten steel, it was found that the temperature of the molten steel was 1569°C, and the composition was C: 0.45%, Si: 0.63%, Mn: 1.15%, P: 0.018%, S: 0.058%, Al: 0.01%, V: 0.17%, Cr: 0.25%, Mo: 0.02%, Ni: 0.18%, Ti: 0.002%, Nb: 0.035%, B: 0.0002%, T.[O]: 0.0012%, N: 140ppm (i.e. N 前 =140ppm), which is 10ppm less than the upper limit of 130ppm required for the steel grade N content.
[0136] Calculate X first 溶解度 ≈10 -(276+3150*0.0288) / 1842-(1.185-0.69*0.0288) ≈0.04323%≈432ppm (can also be ignored, because it is a N reduction operation, there is no solubility problem), and then compared with Table 2, it can be seen that when n=6, N 前 140ppm, N后 If the value is 130ppm, X' is only 79ppm to meet the requirement, so N can be reduced in this way.
[0137] First, lift the ladle up to make the RH rising immersion tube basically filled with molten steel; then continue to select possible parameters to reduce N, for example, select the circulation Ar pressure P = 1.3Mpa, the circulation Ar flow L = 120m 3 / h (n=0.0107*P 0.4068 *L 1.3 =0.0107*1.3 0.4068 *120 1.3 ≈6), at this time X'=3.5*t 0.3 *n 0.2 *P 0.1 *L 0.5 =3.5*t 0.3 *6 0.2 *1.3 0.1 *120 0.5 =56.323*t 0.3 =79, from which we can calculate t≈3.0889min≈185s.
[0138] That is, when P = 1.3Mpa, L = 120m 3 / h, t = 185s, the circulating Ar blowing operation can make N 前 =140ppm 46MnVNbS5 steel reduces N to 130ppm to meet the steel grade requirements.
[0139] S3: Carry out protective work such as Ar sealing of subsequent continuous casting long nozzle to minimize the increase of N.
[0140] It should be noted that the above only describes a single operation under the possible condition of "when the N of molten steel may occasionally be abnormal, in order not to affect the production / soft blowing time (that is, each N increase time ≤ 6min)". If you want to use it as a new N control process (increase or decrease N) without considering other unfavorable factors (such as indefinitely extending the N control time), it is theoretically feasible.
[0141] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for controlling nitrogen content in molten steel in an RH furnace, characterized in that: The following steps are involved: Obtain the temperature, composition and nitrogen content information of RH furnace molten steel after re-pressurization, determine the nitrogen increase or decrease demand of RH furnace molten steel, and compare the calculated theoretical solubility X of nitrogen in molten steel 溶解度 According to the final nitrogen content X' of the cylindrical molten steel in the actual immersion tube in the RH furnace, different circulating gas operation modes are used to increase or reduce nitrogen in the molten steel.
2. The control method according to claim 1, characterized in that: The nitrogen addition operation is performed on the RH furnace molten steel after re-pressurization, including the following steps: S1: Obtain the temperature, composition and nitrogen content information of the RH furnace molten steel after re-pressing, and judge whether (the lower limit of the nitrogen content requirement of the steel grade - 20ppm) ≤ the nitrogen content of the RH furnace molten steel after re-pressing ≤ the lower limit of the nitrogen content requirement of the steel grade is established. If so, proceed to the next step; S2: Based on the temperature, composition and nitrogen content information of the RH furnace molten steel after re-pressurization, calculate the theoretical solubility X of nitrogen in the molten steel under this condition. 溶解度 ; S3: Calculate the final nitrogen content X' of the cylindrical molten steel in the actual ascending immersion tube in the RH furnace; S4: Judgement X 溶解度 ≥X' is true, if true, proceed to the next step; S5: Based on the X' calculated from S3, use the empirical formula X' = 14.4*t 0.3 *n 0.2 *P 0.1 *L 0.5 , where n is the equivalent influence multiple of molten steel volume, n is usually 1 to 6, P is the circulating gas pressure, L is the circulating gas flow rate, t is the circulating gas circulation time, and the subsequent values of t, P, L, n and feasible operation modes are determined; S6: After the nitrogen addition operation is performed according to the operation mode determined in S5, the molten steel is soft-blown to achieve nitrogen addition to the molten steel after the RH furnace molten steel is re-pressurized.
3. The control method according to claim 1, characterized in that: The nitrogen reduction operation is performed on the RH furnace molten steel after re-pressurization, including the following steps: S1: Obtain the temperature, composition and nitrogen content information of the RH furnace molten steel after re-pressing, and judge whether the upper limit of the nitrogen content requirement of the steel grade is ≤ the nitrogen content requirement of the RH furnace molten steel after re-pressing ≤ (the upper limit of the nitrogen content requirement of the steel grade + 10ppm). If so, proceed to the next step; S2: Calculate the final nitrogen content X' of the cylindrical molten steel in the actual ascending immersion tube in the RH furnace; S3: X' calculated from S2, using the empirical formula X' = 3.5*t 0.3 *n 0.2 *P 0.1 *L 0.5 , where n is the equivalent influence multiple of molten steel volume, n is usually 1 to 6, P is the circulating gas pressure, L is the circulating gas flow rate, t is the circulating gas circulation time, and the subsequent values of t, P, L, n and feasible operation modes are determined; S4: After the nitrogen reduction operation is performed according to the operation mode determined in S3, the molten steel is soft-blown to achieve nitrogen reduction in the molten steel after the RH furnace molten steel is re-pressurized.
4. The control method according to claim 2, characterized in that: When using circulating gas for nitrogen addition operation, X'=14.4*t 0.3 *n 0.2 *P 0.1 *L 0.5 , where n = 0.0107*P 0.4068 *L 1.3 .
5. The control method according to claim 4, characterized in that: When the circulating gas is used for nitrogen enrichment operation, the circulating gas is selected from nitrogen.
6. The control method according to claim 3, characterized in that: When using circulating gas for nitrogen reduction operation, X'=3.5*t 0.3 *n 0.2 *P 0.1 *L 0.5 , where n = 0.0107*P 0.4068 *L 1.3 .
7. The control method according to claim 6, characterized in that: When a circulating gas is used for nitrogen reduction operation, the circulating gas is selected from argon.
8. The control method according to claim 2 or 3, characterized in that: Theoretical solubility of nitrogen in molten steel 溶解度 It is calculated using the following formula: X 溶解度 =10 -(276+3150Z 前 ) / T 后 -(1.185-0.69Z 前 ) Among them, Z 前 =0.12[C]+0.045[Si]-0.022[Mn]+0.044[P]+0.007[S]-0.026[Al]-0.095[V]-0.047[Cr]-0.012[Mo]+0.009[Ni]-0.51[Ti]-0.05[Nb]+0.09[B]+0.048T.[O], [C], [Si], [Mn], [P], [S], [Al], [V], [Cr], [Mo], [Ni], [Ti], [Nb], [B], T.[O] are the mass fractions of the elements in the molten steel; T 后 is the temperature of the molten steel after N is increased, in K, and T 后 =T 前 -△*t; T 前 The temperature of molten steel before N addition, in K, is usually in the range of 1539-1628°C, i.e. liquidus temperature + 90°C; △ is the temperature drop during the N-increasing process, usually ranging from 3 to 5°C / min; t is the N increase time, usually ranging from 0 to 6 minutes.
9. The control method according to claim 2 or 3, characterized in that: The final nitrogen content X' of the cylindrical molten steel in the actual ascending immersion tube in the RH furnace is calculated using the following formula: X’=[X+(n-1)N 前 ] / n,X=M*(N 后 -N 前 ) / m+N 前 Wherein, X' is the final nitrogen content of the cylindrical molten steel in the actual ascending immersion tube, in % or ppm; X is the final nitrogen content of the theoretical cylindrical molten steel in the ascending immersion tube, in % or ppm; N 前 It is the initial value of nitrogen content in the whole furnace molten steel after or during re-pressing, in % or ppm; N 后 The target value of nitrogen content in the whole furnace molten steel, in % or ppm; M is the total weight of the whole furnace of molten steel, in t; n is the equivalent influence multiple of molten steel volume, and the value of n is usually 1 to 6; m is the weight of the cylindrical molten steel in the ascending immersion tube, in t, and m = ρ*1 / 4π*D 2 *H, where ρ is the density of molten steel, D is the inner diameter of the rising immersion tube, and H is the height inside the rising immersion tube.
10. The control method according to claim 9, characterized in that: If the total weight of the molten steel in the furnace is 130t, N 前 =80~160ppm, N 后 =90~190ppm, when n≈6, the value of X' calculated by the formula is shown in the following table: