Method for preparing platinum group metal by recovering waste

The low recovery rate and energy consumption in the prior art are solved by the calcination pretreatment of activated carbon and black phosphorus/red phosphorus heterophase junction, zinc melting method and redox potential control, and the synergistic effect of modified CMK-3 and hydrazine hydrate. The major problem has achieved efficient recycling of high-purity iridium and rhodium, reducing environmental pollution and energy consumption.

CN119082474AActive Publication Date: 2024-12-06JIANGXI XILONG ENVIRONMENTAL PROTECTION TECHNOLOGY CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411256254.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-12-06
Estimated Expiration
2044-09-09

AI Technical Summary

Technical Problem

The prior art has low recovery rates, high environmental pollution, large energy consumption and serious technical bottlenecks when recycling platinum group metals from waste, making it difficult to achieve efficient, low energy consumption and high purity platinum group metal recycling.

Method used

The calcination pretreatment is performed using activated carbon and black phosphorus/red phosphorus heterophase junction as combustion aids, combined with zinc melting method and redox potential control, and modified CMK-3 as catalyst and hydrazine hydrate reaction aids, through multi-step acidity adjustment and adsorbent resin to remove impurities, and gradually purify iridium and rhodium metals.

Benefits of technology

The recycling of high-purity iridium and rhodium is achieved, which improves recycling efficiency, reduces energy consumption and environmental pollution, and ensures efficient and rapid recycling of platinum group metals.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a method for preparing platinum group metal through waste recovery. According to the method, the waste is subjected to high-temperature roasting through activated carbon and a combustion improver to efficiently remove organic matters, the waste and zinc powder are subjected to high-temperature roasting activation, part of impurities are removed through oxidation leaching subsequently, and a platinum group metal compound corresponding solution and crystals are obtained through an oxidation-reduction process; the preparation method comprises the following steps: carrying out reduction dissolution under the assistance of a reaction aid, purifying by ammonium sulfide to obtain a pure iridium compound, purifying by adsorbent resin to obtain pure rhodium compound crystals, and finally, carrying out calcination reduction to obtain corresponding high-purity platinum group metal powder.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of precious metal recovery, and more specifically to a method for recovering platinum group metals from waste materials. Background Art

[0002] With the continuous development of science and technology and the continuous consumption of resources, platinum group metals have become increasingly important in modern industry. However, platinum group metal resources are scarce and expensive, so the recovery of platinum group metals from waste has important economic and environmental significance.

[0003] At present, the main technical methods for recovering platinum group metals from waste materials include pyrometallurgy, hydrometallurgy and biometallurgy. Pyrometallurgy recovers platinum group metals through redox reactions at high temperatures, with a high recovery rate, but it will produce a large amount of waste gas and waste slag. Hydrometallurgy extracts platinum group metals through acid and alkali solutions, and then separates and enriches them by ion exchange, adsorption or precipitation. It is simple to operate and low in cost, but the recovery rate is relatively low. As an emerging technology, biometallurgy uses microorganisms or their metabolites to leach platinum group metals. It has the advantages of low cost and environmental friendliness, but it has not yet been industrialized.

[0004] Recovering platinum group metals from waste materials has the advantages of saving resources, protecting the environment and creating economic benefits. However, the existing technical methods still face difficulties such as low recovery rate, environmental pollution, high energy consumption and technical bottlenecks. Therefore, providing a method for preparing platinum group metals from waste materials with high recovery efficiency, low energy consumption and high product purity is the research focus of the present invention. Summary of the invention

[0005] 1. To solve the above technical problems, the technical solution provided by the present invention includes the following contents:

[0006] (1) The waste material, activated carbon and combustion aid are mixed evenly in a mass ratio of 10:6~8:2~3, roasted at 600℃ in a Marsh furnace for 2h, cooled to room temperature, and powder is collected;

[0007] (2) Take 100 parts of powder and mix them evenly with 600-700 parts of zinc powder, roast them in a Marsh furnace at 850°C for 8 hours, cool to room temperature, ball-mill them, pass them through a 60-mesh sieve, immerse them in 10% hydrochloric acid and add 10% hydrochloric acid while stirring until the suspended solids no longer decrease, filter and retain the solids, and dry them to obtain active ash;

[0008] (3) Add active ash into a titanium reactor, add 10% hydrochloric acid and stir, heat to 60-65°C, slowly add 25% sodium chlorate solution into the reactor, keep the 25% sodium chlorate solution added and stirred for 4 hours when the redox potential is greater than 970mV, then heat to 85°C and keep until no gas overflows, then cool to room temperature, filter, and collect the filtrate;

[0009] (4) The filtrate is transferred to an evaporator and heated to a boil. H2O2 and HNO3 are continuously added to maintain the acidity at 1.5-2.5 mol / L. Ammonium chloride is then added until the precipitation stops increasing. The acid is removed and filtered. Filtrate A is retained. The filter residue is washed with a 15% NH4Cl solution until it is light in color. H2O2 and HNO3 are added to the filtrate until the precipitation stops increasing. The filter residue is filtered and washed with a 15% NH4Cl solution until it is colorless. The washing solutions from the two washings are combined to obtain a crude rhodium-containing solution. The washed filter residues are combined to obtain a crude (NH4)2IrCl6.

[0010] (5) Add water to the crude (NH4)2IrCl6 to make a slurry, adjust the pH to 1-1.5, heat to boil, gently stir and add 300-500 parts of hydrazine hydrate solution and 0.2-0.5 parts of auxiliary agent. When the solid content stops decreasing, adjust the pH to 2-2.5 with ammonia water, boil for 1-2 hours, cool, filter, and retain the filtrate to obtain an iridium-containing solution;

[0011] (6) Add hydrochloric acid to the iridium solution to adjust the pH to 1.0-1.5, heat to 80°C, add 320-360 parts of ammonium sulfide, adjust the pH to 2.5-3.0 and boil for 2 hours, cool and store for 36 hours, then filter, add H2O2 and HNO3 to the filtrate until the precipitation no longer increases, wash the filter residue with 15% NH4Cl solution until it is light in color, and dry to obtain (NH4)2IrCl6 crystals;

[0012] (7) Taking the crude rhodium-containing solution, removing impurities with an adsorption resin pretreated with hydrochloric acid at pH = 2 to 3, continuously adding H2O2 and HNO3, and adding ammonium chloride until the precipitation no longer increases. After filtering, the filter residue is washed with 15% NH4Cl, and the washing liquid is combined with the filtrate, concentrated and dried to obtain (NH4)3RhCl6 crystals;

[0013] (8) (NH4)2IrCl6 crystals and (NH4)3RhCl6 crystals are calcined and hydrogen reduced to obtain high-purity iridium and rhodium metal powders.

[0014] 2. Furthermore, the combustion aid is a black phosphorus / red phosphorus heterogeneous junction.

[0015] 3. Further, the reaction aid is modified CMK-3, and the modification steps are as follows:

[0016] (1) Take CMK-3, 2-methylimidazole and ethanol in a mass ratio of 3-6:2-4:30-40;

[0017] (2) Add CMK-3 and 2-methylimidazole to ethanol, mix well, and treat with ultrasound for 30-40 minutes;

[0018] (3) The mixture was heated in a water bath at 40°C and evaporated to dryness. The solid was placed in a nitrogen atmosphere and heated to 800°C at 5°C / min for 3 h to obtain N-CMK-3.

[0019] (4) Place N-CMK-3 in 8-10 times the mass of deionized water and add 0.5w% 0.05mol / l H2PtCl6 aqueous solution, and ultrasonicate for 10-20min;

[0020] (5) The mixture was heated in a water bath at 40 °C and evaporated to dryness. The solid was placed in a nitrogen / hydrogen mixed atmosphere of 4:1 and heated to 200 °C at 5 °C / min and calcined for 3 h to obtain Pt / N-CMK-3, i.e., modified CMK-3.

[0021] 4. Furthermore, the adsorption resin is a polyethyleneimine-tannin based adsorption resin.

[0022] The beneficial effects of the present invention are:

[0023] (1) The present invention relies on activated carbon and combustion aids to more fully remove organic impurities, and uses a catalyst to improve the reduction efficiency in redox purification to separate most metal element impurities. The adsorption resin separates the base metals in the rhodium-containing solution, and efficiently and quickly recovers high-purity iridium powder and rhodium powder from the waste.

[0024] (2) In the pretreatment of waste materials, organic matter in the waste materials needs to be incinerated under high temperature conditions to remove most of the organic impurities. The organic matter is adsorbed by activated carbon to separate it from the waste materials as much as possible. However, even with the assistance of activated carbon, organic matter residues cannot be avoided. Therefore, an additional combustion aid is required to provide a heat source for the mixture to assist the combustion of organic matter during the pretreatment process. The present invention selects black phosphorus / red phosphorus heterogeneous junction as a combustion aid. The black phosphorus / red phosphorus heterogeneous junction has the characteristic of a low ignition point and can provide a heat source for the mixture to more fully burn the organic matter in the waste. The black phosphorus / red phosphorus heterogeneous junction is composed of an amorphous phase and a crystalline phase and has an overlapping structure. It has excellent electron supply ability and can reduce the metal elements in the waste materials during the pretreatment process. During roasting, it can prevent the metal elements from being over-oxidized, thereby affecting the subsequent zinc melting efficiency and reducing the recovery efficiency of platinum group metals.

[0025] (3) The crude (NH4)2IrCl6 contains a certain amount of base metals and other precious metal impurities, which need to be further removed to obtain iridium metal with higher purity. Therefore, it is necessary to carry out reduction dissolution and precipitation removal in another step. In this process, the reduction efficiency of hydrazine hydrate is poor, so it is necessary to assist with an auxiliary agent to better dissolve (NH4)2IrCl6. The present invention selects Pt / N-CMK-3 as the reaction auxiliary agent of the reaction. The main body of the reaction is mesoporous carbon material CMK-3, which has excellent adsorption effect to make hydrazine hydrate and suspended particles fully contact, thereby improving the reaction efficiency.

[0026] (4) Pt / -CMK-3 is a common catalyst but is prone to agglomeration of Pt nanoparticles, which reduces the promoting effect on the reaction to a certain extent. In the N-doped CMK-3, the presence of N element promotes the dispersion of Pt nanoparticles and reduces the particle size of Pt, which has a higher reaction catalytic activity. In addition, the synergistic effect of Pt and N in Pt / N-CMK-3 can promote the heterogeneous cleavage of hydrazine hydrate, and can form positive and negative H electron pairs in the system, promoting the reduction efficiency of hydrazine hydrate to (NH4)2IrCl6 in the system, greatly improving the impurity removal effect, and significantly improving the purity of the recovered iridium powder.

[0027] (5) There are various base metals remaining in the crude rhodium-containing solution, which need to be further purified and removed using an adsorption resin. The present invention selects polyethyleneimine-tannin-based adsorption resin as the cationic adsorption resin. The polyethyleneimine-tannin-based adsorption resin has a variety of adaptive orbital binding energies that can adsorb various base metals in the solution. The polyethyleneimine-tannin-based adsorption resin has a rough and irregular surface structure and many spatial gaps. It has an excellent adsorption effect on metal ions free in the solution and is selective during adsorption. It has a targeted adsorption effect on the base metals present in the solution, which can avoid affecting the rhodium component during the adsorption and impurity removal process and reducing the rhodium recovery efficiency. DETAILED DESCRIPTION

[0028] The present invention is further described in detail below with reference to the embodiments.

[0029] In the black phosphorus / red phosphorus heterojunction used in the present invention, black phosphorus accounts for 40% to 60% of the mass, and the overall particle size of the black phosphorus / red phosphorus heterojunction is 1 to 3 microns, of which the black phosphorus particle size is 20 to 25 nanometers. It is purchased from Guangdong Xiaoda Chemical Co., Ltd., and other raw materials are obtained through conventional commercial channels unless otherwise specified.

[0030] Example 1

[0031] 1. Take CMK-3, 2-methylimidazole and ethanol in a mass ratio of 4.5:3:35;

[0032] 2. Add CMK-3 and 2-methylimidazole to ethanol, mix well, and treat with ultrasound for 30-40 minutes;

[0033] 3. The mixture was heated in a water bath at 40°C and evaporated to dryness, and the solid was calcined at 800°C for 3h under a nitrogen atmosphere to obtain N-CMK-3;

[0034] 4. Place N-CMK-3 in 8-10 times the mass of deionized water and add 0.5w% 0.05mol / l H2PtCl6 aqueous solution, and ultrasonicate for 10-20min;

[0035] 5. The mixture was heated in a water bath at 40°C and evaporated to dryness, and the solid was calcined at 200°C for 3h in a nitrogen / hydrogen mixed atmosphere of 4:1 to obtain modified CMK-3;

[0036] 6. The waste material was mixed with activated carbon and black phosphorus / red phosphorus in a mass ratio of 10:7:2.5, and calcined at 600°C for 2h in a Marsh furnace, cooled to room temperature, and the powder was collected;

[0037] 7. Take 100 parts of powder and 650 parts of zinc powder and mix them evenly, roast them in a Marsh furnace at 850°C for 8 hours, cool to room temperature, ball-mill and pass through a 60-mesh sieve, immerse in 10% hydrochloric acid and add 10% hydrochloric acid while stirring until the suspended solids no longer decrease, filter and retain the solids, and dry them to obtain active ash;

[0038] 8. Put the active ash into the titanium reactor, add 10% hydrochloric acid and stir, heat to 60-65°C, slowly add 25% sodium chlorate solution into the reactor, keep the 25% sodium chlorate solution added and stirred for 4 hours when the redox potential is greater than 970mV, then heat to 85°C and keep until no gas overflows, then cool to room temperature, filter, and collect the filtrate;

[0039] 9. The filtrate is transferred to an evaporator, heated and boiled, and H2O2 and HNO3 are continuously added to keep the acidity at 1.5-2.5 mol / L, and then ammonium chloride is added until the precipitation no longer increases, and the acid is removed and filtered, and the filtrate A is retained. The filter residue is washed with 15% NH4Cl solution until it is light in color. The filtrate is added with H2O2 and HNO3, and the precipitation no longer increases. Filter, and the filter residue is washed with 15% NH4Cl solution until it is colorless. The washing solutions from the two washings are combined to obtain a crude rhodium-containing solution, and the washed filter residues are combined to obtain a crude (NH4)2IrCl6;

[0040] 10. Add water to the crude (NH4)2IrCl6 to make a slurry, adjust the pH to 1-1.5, heat to boil, gently stir and add 400 parts of hydrazine hydrate solution and 0.35 parts of modified CMK-3. When the solid content stops decreasing, adjust the pH to 2-2.5 with ammonia water, boil for 1.5 hours, cool, filter, and retain the filtrate to obtain an iridium-containing solution;

[0041] 11. Add hydrochloric acid to the iridium solution to adjust the pH to 1.0-1.5, heat to 80°C, add 340 parts of ammonium sulfide, adjust the pH to 2.5-3.0 and boil for 2 hours, cool and store for 36 hours, filter, add H2O2 and HNO3 to the filtrate until the precipitation no longer increases, wash the filter residue with 15% NH4Cl solution until it is light in color, and dry to obtain (NH4)2IrCl6 crystals;

[0042] 12. (NH4)2IrCl6 crystals are calcined and hydrogen reduced to obtain high-purity iridium powder.

[0043] Example 2

[0044] 1. Take CMK-3, 2-methylimidazole and ethanol in a mass ratio of 4.5:3:35;

[0045] 2. Add CMK-3 and 2-methylimidazole to ethanol, mix well, and treat with ultrasound for 30-40 minutes;

[0046] 3. The mixture was heated in a water bath at 40°C and evaporated to dryness, and the solid was calcined at 800°C for 3h under a nitrogen atmosphere to obtain N-CMK-3;

[0047] 4. Place N-CMK-3 in 8-10 times the mass of deionized water and add 0.5w% 0.05mol / l H2PtCl6 aqueous solution, and ultrasonicate for 10-20min;

[0048] 5. The mixture was heated in a water bath at 40°C and evaporated to dryness, and the solid was calcined at 200°C for 3h in a nitrogen / hydrogen mixed atmosphere of 4:1 to obtain modified CMK-3;

[0049] 6. The waste material, activated carbon, and black phosphorus / red phosphorus heterogeneous phase were mixed evenly in a mass ratio of 10:7:2, and calcined at 600°C for 2h in a Marsh furnace, cooled to room temperature, and the powder was collected;

[0050] 7. Take 100 parts of powder and 650 parts of zinc powder and mix them evenly, roast them in a Marsh furnace at 850°C for 8 hours, cool to room temperature, ball-mill and pass through a 60-mesh sieve, immerse in 10% hydrochloric acid and add 10% hydrochloric acid while stirring until the suspended solids no longer decrease, filter and retain the solids, and dry them to obtain active ash;

[0051] 8. Put the active ash into the titanium reactor, add 10% hydrochloric acid and stir, heat to 60-65°C, slowly add 25% sodium chlorate solution into the reactor, keep the 25% sodium chlorate solution added and stirred for 4 hours when the redox potential is greater than 970mV, then heat to 85°C and keep until no gas overflows, then cool to room temperature, filter, and collect the filtrate;

[0052] 9. The filtrate is transferred to an evaporator, heated and boiled, and H2O2 and HNO3 are continuously added to keep the acidity at 1.5-2.5 mol / L, and then ammonium chloride is added until the precipitation no longer increases, and the acid is removed and filtered, and the filtrate A is retained. The filter residue is washed with 15% NH4Cl solution until it is light in color. The filtrate is added with H2O2 and HNO3, and the precipitation no longer increases. Filter, and the filter residue is washed with 15% NH4Cl solution until it is colorless. The washing solutions from the two washings are combined to obtain a crude rhodium-containing solution, and the washed filter residues are combined to obtain a crude (NH4)2IrCl6;

[0053] 10. Add water to the crude (NH4)2IrCl6 to make a slurry, adjust the pH to 1-1.5, heat to boil, gently stir and add 400 parts of hydrazine hydrate solution and 0.5 parts of modified CMK-3. When the solid content stops decreasing, adjust the pH to 2-2.5 with ammonia water, boil for 1.5 hours, cool, filter, and retain the filtrate to obtain an iridium-containing solution;

[0054] 11. Add hydrochloric acid to the iridium solution to adjust the pH to 1.0-1.5, heat to 80°C, add 340 parts of ammonium sulfide, adjust the pH to 2.5-3.0 and boil for 2 hours, cool and store for 36 hours, filter, add H2O2 and HNO3 to the filtrate until the precipitation no longer increases, wash the filter residue with 15% NH4Cl solution until it is light in color, and dry to obtain (NH4)2IrCl6 crystals;

[0055] 12. (NH4)2IrCl6 crystals are calcined and hydrogen reduced to obtain high-purity iridium powder.

[0056] Example 3

[0057] 1. Take CMK-3, 2-methylimidazole and ethanol in a mass ratio of 4.5:3:35;

[0058] 2. Add CMK-3 and 2-methylimidazole to ethanol, mix well, and treat with ultrasound for 30-40 minutes;

[0059] 3. The mixture was heated in a water bath at 40°C and evaporated to dryness, and the solid was calcined at 800°C for 3h under a nitrogen atmosphere to obtain N-CMK-3;

[0060] 4. Place N-CMK-3 in 8-10 times the mass of deionized water and add 0.5w% 0.05mol / l H2PtCl6 aqueous solution, and ultrasonicate for 10-20min;

[0061] 5. The mixture was heated in a water bath at 40°C and evaporated to dryness, and the solid was calcined at 200°C for 3h in a nitrogen / hydrogen mixed atmosphere of 4:1 to obtain modified CMK-3;

[0062] 6. The waste material, activated carbon, and black phosphorus / red phosphorus heterogeneous phase were mixed evenly in a mass ratio of 10:7:3, and calcined in a Marsh furnace at 600°C for 2h, cooled to room temperature, and the powder was collected;

[0063] 7. Take 100 parts of powder and 650 parts of zinc powder and mix them evenly, roast them in a Marsh furnace at 850°C for 8 hours, cool to room temperature, ball-mill and pass through a 60-mesh sieve, immerse in 10% hydrochloric acid and add 10% hydrochloric acid while stirring until the suspended solids no longer decrease, filter and retain the solids, and dry them to obtain active ash;

[0064] 8. Put the active ash into the titanium reactor, add 10% hydrochloric acid and stir, heat to 60-65°C, slowly add 25% sodium chlorate solution into the reactor, keep the 25% sodium chlorate solution added and stirred for 4 hours when the redox potential is greater than 970mV, then heat to 85°C and keep until no gas overflows, then cool to room temperature, filter, and collect the filtrate;

[0065] 9. The filtrate is transferred to an evaporator, heated and boiled, and H2O2 and HNO3 are continuously added to keep the acidity at 1.5-2.5 mol / L, and then ammonium chloride is added until the precipitation no longer increases, and the acid is removed and filtered, and the filtrate A is retained. The filter residue is washed with 15% NH4Cl solution until it is light in color. The filtrate is added with H2O2 and HNO3, and the precipitation no longer increases. Filter, and the filter residue is washed with 15% NH4Cl solution until it is colorless. The washing solutions from the two washings are combined to obtain a crude rhodium-containing solution, and the washed filter residues are combined to obtain a crude (NH4)2IrCl6;

[0066] 10. Add water to the crude (NH4)2IrCl6 to make a slurry, adjust the pH to 1-1.5, heat to boil, gently stir and add 400 parts of hydrazine hydrate solution and 0.2 parts of modified CMK-3. When the solid content stops decreasing, adjust the pH to 2-2.5 with ammonia water, boil for 1.5 hours, cool, filter, and retain the filtrate to obtain an iridium-containing solution;

[0067] 11. Add hydrochloric acid to the iridium solution to adjust the pH to 1.0-1.5, heat to 80°C, add 340 parts of ammonium sulfide, adjust the pH to 2.5-3.0 and boil for 2 hours, cool and store for 36 hours, filter, add H2O2 and HNO3 to the filtrate until the precipitation no longer increases, wash the filter residue with 15% NH4Cl solution until it is light in color, and dry to obtain (NH4)2IrCl 66 Crystals;

[0068] 12. (NH4)2IrCl6 crystals are calcined and hydrogen reduced to obtain high-purity iridium powder.

[0069] Comparative Example 1

[0070] The difference between this comparative example and Example 1 is that the black phosphorus / red phosphorus in step 1 is heterogeneously bonded to form red phosphorus, and the rest of the implementation is the same as Example 1.

[0071] Comparative Example 2

[0072] 1. Take CMK-3, 2-methylimidazole and ethanol in a mass ratio of 4.5:3:35;

[0073] 2. Add CMK-3 and 2-methylimidazole to ethanol, mix well, and treat with ultrasound for 30-40 minutes;

[0074] 3. The mixture was heated in a water bath at 40°C and evaporated to dryness, and the solid was calcined at 800°C for 3h under a nitrogen atmosphere to obtain N-CMK-3;

[0075] 4. Place N-CMK-3 in 8-10 times the mass of deionized water and add 0.5w% 0.05mol / l H2PtCl6 aqueous solution, and ultrasonicate for 10-20min;

[0076] 5. The mixture was heated in a water bath at 40°C and evaporated to dryness, and the solid was calcined at 200°C for 3h in a nitrogen / hydrogen mixed atmosphere of 4:1 to obtain modified CMK-3;

[0077] 6. The waste material, activated carbon, and black phosphorus / red phosphorus heterogeneous phase were mixed evenly in a mass ratio of 10:7:1, and calcined at 600°C for 2h in a Marsh furnace, cooled to room temperature, and the powder was collected;

[0078] 7. Take 100 parts of powder and 650 parts of zinc powder and mix them evenly, roast them in a Marsh furnace at 850°C for 8 hours, cool to room temperature, ball-mill and pass through a 60-mesh sieve, immerse in 10% hydrochloric acid and add 10% hydrochloric acid while stirring until the suspended solids no longer decrease, filter and retain the solids, and dry them to obtain active ash;

[0079] 8. Put the active ash into the titanium reactor, add 10% hydrochloric acid and stir, heat to 60-65°C, slowly add 25% sodium chlorate solution into the reactor, keep the 25% sodium chlorate solution added and stirred for 4 hours when the redox potential is greater than 970mV, then heat to 85°C and keep until no gas overflows, then cool to room temperature, filter, and collect the filtrate;

[0080] 9. The filtrate is transferred to an evaporator, heated and boiled, and H2O2 and HNO3 are continuously added to keep the acidity at 1.5-2.5 mol / L, and then ammonium chloride is added until the precipitation no longer increases, and the acid is removed and filtered, and the filtrate A is retained. The filter residue is washed with 15% NH4Cl solution until it is light in color. The filtrate is added with H2O2 and HNO3, and the precipitation no longer increases. Filter, and the filter residue is washed with 15% NH4Cl solution until it is colorless. The washing solutions from the two washings are combined to obtain a crude rhodium-containing solution, and the washed filter residues are combined to obtain a crude (NH4)2IrCl6;

[0081] 10. Add water to the crude (NH4)2IrCl6 to make a slurry, adjust the pH to 1-1.5, heat to boil, gently stir and add 400 parts of hydrazine hydrate solution and 0.35 parts of modified CMK-3. When the solids no longer decrease, adjust the pH to 2-2.5 with ammonia water, boil for 1.5 hours, cool, filter, and retain the filtrate to obtain an iridium-containing solution;

[0082] 11. Add hydrochloric acid to the iridium solution to adjust the pH to 1.0-1.5, heat to 80°C, add 340 parts of ammonium sulfide, adjust the pH to 2.5-3.0 and boil for 2 hours, cool and store for 36 hours, filter, add H2O2 and HNO3 to the filtrate until the precipitation no longer increases, wash the filter residue with 15% NH4Cl solution until it is light in color, and dry to obtain (NH4)2IrCl6 crystals;

[0083] 12. (NH4)2IrCl6 crystals are calcined and hydrogen reduced to obtain high-purity iridium powder.

[0084] Comparative Example 3

[0085] 1. Take CMK-3, 2-methylimidazole and ethanol in a mass ratio of 4.5:3:35;

[0086] 2. Add CMK-3 and 2-methylimidazole to ethanol, mix well, and treat with ultrasound for 30-40 minutes;

[0087] 3. The mixture was heated in a water bath at 40°C and evaporated to dryness, and the solid was calcined at 800°C for 3h under a nitrogen atmosphere to obtain N-CMK-3;

[0088] 4. Place N-CMK-3 in 8-10 times the mass of deionized water and add 0.5w% 0.05mol / l H2PtCl6 aqueous solution, and ultrasonicate for 10-20min;

[0089] 5. The mixture was heated in a water bath at 40°C and evaporated to dryness, and the solid was calcined at 200°C for 3h in a nitrogen / hydrogen mixed atmosphere of 4:1 to obtain modified CMK-3;

[0090] 6. The waste material, activated carbon, and black phosphorus / red phosphorus heterogeneous phase were mixed evenly in a mass ratio of 10:7:4, and calcined in a Marsh furnace at 600°C for 2h, cooled to room temperature, and the powder was collected;

[0091] 7. Take 100 parts of powder and 650 parts of zinc powder and mix them evenly, roast them in a Marsh furnace at 850°C for 8 hours, cool to room temperature, ball-mill and pass through a 60-mesh sieve, immerse in 10% hydrochloric acid and add 10% hydrochloric acid while stirring until the suspended solids no longer decrease, filter and retain the solids, and dry them to obtain active ash;

[0092] 8. Put the active ash into the titanium reactor, add 10% hydrochloric acid and stir, heat to 60-65°C, slowly add 25% sodium chlorate solution into the reactor, keep the 25% sodium chlorate solution added and stirred for 4 hours when the redox potential is greater than 970mV, then heat to 85°C and keep until no gas overflows, then cool to room temperature, filter, and collect the filtrate;

[0093] 9. The filtrate is transferred to an evaporator, heated and boiled, and H2O2 and HNO3 are continuously added to keep the acidity at 1.5-2.5 mol / L, and then ammonium chloride is added until the precipitation no longer increases, and the acid is removed and filtered, and the filtrate A is retained. The filter residue is washed with 15% NH4Cl solution until it is light in color. The filtrate is added with H2O2 and HNO3, and the precipitation no longer increases. Filter, and the filter residue is washed with 15% NH4Cl solution until it is colorless. The washing solutions from the two washings are combined to obtain a crude rhodium-containing solution, and the washed filter residues are combined to obtain a crude (NH4)2IrCl6;

[0094] 10. Add water to the crude (NH4)2IrCl6 to make a slurry, adjust the pH to 1-1.5, heat to boil, gently stir and add 400 parts of hydrazine hydrate solution and 0.2-0.5 parts of modified CMK-3. When the solid content stops decreasing, adjust the pH to 2-2.5 with ammonia water, boil for 1.5 hours, cool, filter, and retain the filtrate to obtain an iridium-containing solution;

[0095] 11. Add hydrochloric acid to the iridium solution to adjust the pH to 1.0-1.5, heat to 80°C, add 340 parts of ammonium sulfide, adjust the pH to 2.5-3.0 and boil for 2 hours, cool and store for 36 hours, filter, add H2O2 and HNO3 to the filtrate until the precipitation no longer increases, wash the filter residue with 15% NH4Cl solution until it is light in color, and dry to obtain (NH4)2IrCl6 crystals;

[0096] 12. (NH4)2IrCl6 crystals are calcined and hydrogen reduced to obtain high-purity iridium powder.

[0097] Comparative Example 4

[0098] The difference between this comparative example and Example 1 is that the Pt / N-CMK-3 in step 5 is Pt / CMK-3, and the rest of the implementation methods are the same as Example 1.

[0099] Comparative Example 5

[0100] 1. Take CMK-3, 2-methylimidazole and ethanol in a mass ratio of 4.5:3:35;

[0101] 2. Add CMK-3 and 2-methylimidazole to ethanol, mix well, and treat with ultrasound for 30-40 minutes;

[0102] 3. The mixture was heated in a water bath at 40°C and evaporated to dryness, and the solid was calcined at 800°C for 3h under a nitrogen atmosphere to obtain N-CMK-3;

[0103] 4. Place N-CMK-3 in 8-10 times the mass of deionized water and add 0.5w% 0.05mol / l H2PtCl6 aqueous solution, and ultrasonicate for 10-20min;

[0104] 5. The mixture was heated in a water bath at 40°C and evaporated to dryness, and the solid was calcined at 200°C for 3h in a nitrogen / hydrogen mixed atmosphere of 4:1 to obtain modified CMK-3;

[0105] 6. The waste material was mixed with activated carbon and black phosphorus / red phosphorus in a mass ratio of 10:7:2.5, and calcined at 600°C for 2h in a Marsh furnace, cooled to room temperature, and the powder was collected;

[0106] 7. Take 100 parts of powder and 650 parts of zinc powder and mix them evenly, roast them in a Marsh furnace at 850°C for 8 hours, cool to room temperature, ball-mill and pass through a 60-mesh sieve, immerse in 10% hydrochloric acid and add 10% hydrochloric acid while stirring until the suspended solids no longer decrease, filter and retain the solids, and dry them to obtain active ash;

[0107] 8. Put the active ash into the titanium reactor, add 10% hydrochloric acid and stir, heat to 60-65°C, slowly add 25% sodium chlorate solution into the reactor, keep the 25% sodium chlorate solution added and stirred for 4 hours when the redox potential is greater than 970mV, then heat to 85°C and keep until no gas overflows, then cool to room temperature, filter, and collect the filtrate;

[0108] 9. The filtrate is transferred to an evaporator, heated and boiled, and H2O2 and HNO3 are continuously added to keep the acidity at 1.5-2.5 mol / L, and then ammonium chloride is added until the precipitation no longer increases, and the acid is removed and filtered, and the filtrate A is retained. The filter residue is washed with 15% NH4Cl solution until it is light in color. The filtrate is added with H2O2 and HNO3, and the precipitation no longer increases. Filter, and the filter residue is washed with 15% NH4Cl solution until it is colorless. The washing solutions from the two washings are combined to obtain a crude rhodium-containing solution, and the washed filter residues are combined to obtain a crude (NH4)2IrCl6;

[0109] 10. Add water to the crude (NH4)2IrCl6 to make a slurry, adjust the pH to 1-1.5, heat to boil, gently stir and add 400 parts of hydrazine hydrate solution and 0.1 parts of modified CMK-3. When the solid content stops decreasing, adjust the pH to 2-2.5 with ammonia water, boil for 1.5 hours, cool, filter, and retain the filtrate to obtain an iridium-containing solution;

[0110] 11. Add hydrochloric acid to the iridium solution to adjust the pH to 1.0-1.5, heat to 80°C, add 340 parts of ammonium sulfide, adjust the pH to 2.5-3.0 and boil for 2 hours, cool and store for 36 hours, filter, add H2O2 and HNO3 to the filtrate until the precipitation no longer increases, wash the filter residue with 15% NH4Cl solution until it is light in color, and dry to obtain (NH4)2IrCl6 crystals;

[0111] 12. (NH4)2IrCl6 crystals are calcined and hydrogen reduced to obtain high-purity iridium powder.

[0112] Comparative Example 6

[0113] 1. Take CMK-3, 2-methylimidazole and ethanol in a mass ratio of 4.5:3:35;

[0114] 2. Add CMK-3 and 2-methylimidazole to ethanol, mix well, and treat with ultrasound for 30-40 minutes;

[0115] 3. The mixture was heated in a water bath at 40°C and evaporated to dryness, and the solid was calcined at 800°C for 3h under a nitrogen atmosphere to obtain N-CMK-3;

[0116] 4. Place N-CMK-3 in 8-10 times the mass of deionized water and add 0.5w% 0.05mol / l H2PtCl6 aqueous solution, and ultrasonicate for 10-20min;

[0117] 5. The mixture was heated in a water bath at 40°C and evaporated to dryness, and the solid was calcined at 200°C for 3h in a nitrogen / hydrogen mixed atmosphere of 4:1 to obtain modified CMK-3;

[0118] 6. The waste material was mixed with activated carbon and black phosphorus / red phosphorus in a mass ratio of 10:7:2.5, and calcined at 600°C for 2h in a Marsh furnace, cooled to room temperature, and the powder was collected;

[0119] 7. Take 100 parts of powder and 650 parts of zinc powder and mix them evenly, roast them in a Marsh furnace at 850°C for 8 hours, cool to room temperature, ball-mill and pass through a 60-mesh sieve, immerse in 10% hydrochloric acid and add 10% hydrochloric acid while stirring until the suspended solids no longer decrease, filter and retain the solids, and dry them to obtain active ash;

[0120] 8. Put the active ash into the titanium reactor, add 10% hydrochloric acid and stir, heat to 60-65°C, slowly add 25% sodium chlorate solution into the reactor, keep the 25% sodium chlorate solution added and stirred for 4 hours when the redox potential is greater than 970mV, then heat to 85°C and keep until no gas overflows, then cool to room temperature, filter, and collect the filtrate;

[0121] 9. The filtrate is transferred to an evaporator, heated and boiled, and H2O2 and HNO3 are continuously added to keep the acidity at 1.5-2.5 mol / L, and then ammonium chloride is added until the precipitation no longer increases, and the acid is removed and filtered, and the filtrate A is retained. The filter residue is washed with 15% NH4Cl solution until it is light in color. The filtrate is added with H2O2 and HNO3, and the precipitation no longer increases. Filter, and the filter residue is washed with 15% NH4Cl solution until it is colorless. The washing solutions from the two washings are combined to obtain a crude rhodium-containing solution, and the washed filter residues are combined to obtain a crude (NH4)2IrCl6;

[0122] 10. Add water to the crude (NH4)2IrCl6 to make a slurry, adjust the pH to 1-1.5, heat to boil, gently stir and add 400 parts of hydrazine hydrate solution and 0.6 parts of modified CMK-3. When the solid content stops decreasing, adjust the pH to 2-2.5 with ammonia water, boil for 1.5 hours, cool, filter, and retain the filtrate to obtain an iridium-containing solution;

[0123] 11. Add hydrochloric acid to the iridium solution to adjust the pH to 1.0-1.5, heat to 80°C, add 340 parts of ammonium sulfide, adjust the pH to 2.5-3.0 and boil for 2 hours, cool and store for 36 hours, filter, add H2O2 and HNO3 to the filtrate until the precipitation no longer increases, wash the filter residue with 15% NH4Cl solution until it is light in color, and dry to obtain (NH4)2IrCl6 crystals;

[0124] 12. (NH4)2IrCl6 crystals are calcined and hydrogen reduced to obtain high-purity iridium powder.

[0125] Product determination:

[0126] Iridium powder samples were prepared according to Examples 1-3 and Comparative Examples 1-6 respectively;

[0127] 1. Purity determination: Take three samples of nine iridium powders, each weighing 0.1 g, and measure the impurities using an inductively coupled plasma atomic emission spectrometer and ignition loss according to GB / T 1422-2018. The purity of the iridium powder is calculated by calculation. The results are the average values ​​of the three groups of experiments, as shown in Table 1.

[0128] 2. Recovery rate determination: Use waste materials to prepare the test solution, and prepare standard solution to obtain a standard curve by atomic emission spectrometer (ICP-AES), and detect the test solution to obtain the iridium content in the ingredients. The average value of three tests is taken as the Ir content in the waste. Three iridium powder samples are prepared in each case, and the iridium recovery rate (iridium powder mass / Ir content in the waste) is obtained by calculation. The results are averaged, as shown in Table 1.

[0129] Table 1 Iridium powder test results

[0130] purity(%) Recovery rate (%) Example 1 99.97±0.03 90.5±0.3 Example 2 99.96±0.04 90.2±0.6 Example 3 99.98±0.03 90.4±0.4 Comparative Example 1 98.41±0.04 86.7±0.5 Comparative Example 2 98.76±0.07 85.4±0.6 Comparative Example 3 99.94±0.06 88.6±0.4 Comparative Example 4 99.93±0.03 80.7±0.5 Comparative Example 5 99.94±0.07 84.3±0.3 Comparative Example 6 99.94±0.05 89.8±0.4

[0131] Example 4

[0132] 1. The waste material, activated carbon, and black phosphorus / red phosphorus were mixed evenly in a mass ratio of 10:7:2.5, and calcined at 600°C for 2h in a Marsh furnace, cooled to room temperature, and the powder was collected;

[0133] 2. Put the powder into the titanium reactor, add 10% hydrochloric acid and stir, heat to 60-65°C, slowly add 25% sodium chlorate solution into the reactor, keep the 25% sodium chlorate solution added and stirred for 4 hours when the redox potential is greater than 970mV, then heat to 85°C and keep until no gas overflows, then cool to room temperature, filter, and collect the filtrate;

[0134] 3. The filtrate is transferred to an evaporator, heated and boiled, H2O2 and HNO3 are continuously added to keep the acidity at 1.5-2.5 mol / L, and then ammonium chloride is added until the precipitation no longer increases, the acid is removed and filtered, and the filtrate A is retained. The filter residue is washed with 15% NH4Cl solution until it is light in color. H2O2 and HNO3 are added to the filtrate until the precipitation no longer increases, and the filter residue is washed with 15% NH4Cl solution until it is colorless. The washing solutions from the two washings are combined to obtain a crude rhodium-containing solution;

[0135] 4. Take the crude rhodium-containing solution, remove impurities with polyethyleneimine-tannin-based adsorption resin pretreated with hydrochloric acid at pH=2.5, continue to add H2O2 and HNO3, add ammonium chloride until the precipitation no longer increases, filter and wash the residue with 15% NH4Cl, combine the washing liquid with the filtrate, concentrate and dry, and finally obtain (NH4)3RhCl6 crystals;

[0136] 5. (NH4)3RhCl6 crystals are calcined and hydrogen reduced to obtain high-purity rhodium powder.

[0137] Example 5

[0138] 1. The waste material, activated carbon, and black phosphorus / red phosphorus were mixed evenly in a mass ratio of 10:7:2.5, and calcined at 600°C for 2h in a Marsh furnace, cooled to room temperature, and the powder was collected;

[0139] 2. Put the powder into the titanium reactor, add 10% hydrochloric acid and stir, heat to 60-65°C, slowly add 25% sodium chlorate solution into the reactor, keep the 25% sodium chlorate solution added and stirred for 4 hours when the redox potential is greater than 970mV, then heat to 85°C and keep until no gas overflows, then cool to room temperature, filter, and collect the filtrate;

[0140] 3. The filtrate is transferred to an evaporator, heated and boiled, H2O2 and HNO3 are continuously added to keep the acidity at 1.5-2.5 mol / L, and then ammonium chloride is added until the precipitation no longer increases, the acid is removed and filtered, and the filtrate A is retained. The filter residue is washed with 15% NH4Cl solution until it is light in color. H2O2 and HNO3 are added to the filtrate until the precipitation no longer increases, and the filter residue is washed with 15% NH4Cl solution until it is colorless. The washing solutions from the two washings are combined to obtain a crude rhodium-containing solution;

[0141] 4. Take the crude rhodium-containing solution, remove impurities with polyethyleneimine-tannin-based adsorption resin pretreated with hydrochloric acid at pH=2, continue to add H2O2 and HNO3, add ammonium chloride until the precipitation no longer increases, filter and wash the residue with 15% NH4Cl, combine the washing liquid with the filtrate, concentrate and dry, and finally obtain (NH4)3RhCl6 crystals;

[0142] 5. (NH4)3RhCl6 crystals are calcined and hydrogen reduced to obtain high-purity rhodium powder.

[0143] Example 6

[0144] 1. The waste material, activated carbon, and black phosphorus / red phosphorus were mixed evenly in a mass ratio of 10:7:2.5, and calcined at 600°C for 2h in a Marsh furnace, cooled to room temperature, and the powder was collected;

[0145] 2. Put the powder into the titanium reactor, add 10% hydrochloric acid and stir, heat to 60-65°C, slowly add 25% sodium chlorate solution into the reactor, keep the 25% sodium chlorate solution added and stirred for 4 hours when the redox potential is greater than 970mV, then heat to 85°C and keep until no gas overflows, then cool to room temperature, filter, and collect the filtrate;

[0146] 3. The filtrate is transferred to an evaporator, heated and boiled, H2O2 and HNO3 are continuously added to keep the acidity at 1.5-2.5 mol / L, and then ammonium chloride is added until the precipitation no longer increases, the acid is removed and filtered, and the filtrate A is retained. The filter residue is washed with 15% NH4Cl solution until it is light in color. H2O2 and HNO3 are added to the filtrate until the precipitation no longer increases, and the filter residue is washed with 15% NH4Cl solution until it is colorless. The washing solutions from the two washings are combined to obtain a crude rhodium-containing solution;

[0147] 4. Take the crude rhodium-containing solution, remove impurities with polyethyleneimine-tannin-based adsorption resin pretreated with hydrochloric acid at pH=3, continue to add H2O2 and HNO3, add ammonium chloride until the precipitation no longer increases, filter and wash the residue with 15% NH4Cl, combine the washing liquid with the filtrate, concentrate and dry, and finally obtain (NH4)3RhCl6 crystals;

[0148] 5. (NH4)3RhCl6 crystals are calcined and hydrogen reduced to obtain high-purity rhodium powder.

[0149] Comparative Example 7

[0150] The difference between this comparative example and Example 4 is that the polyethyleneimine-tannin-based adsorption resin in step 4 is a styrene-based cationic adsorption resin, and the rest of the implementation is the same as Example 1.

[0151] Comparative Example 8

[0152] 1. The waste material, activated carbon, and black phosphorus / red phosphorus were mixed evenly in a mass ratio of 10:7:2.5, and calcined at 600°C for 2h in a Marsh furnace, cooled to room temperature, and the powder was collected;

[0153] 2. Put the powder into the titanium reactor, add 10% hydrochloric acid and stir, heat to 60-65°C, slowly add 25% sodium chlorate solution into the reactor, keep the 25% sodium chlorate solution added and stirred for 4 hours when the redox potential is greater than 970mV, then heat to 85°C and keep until no gas overflows, then cool to room temperature, filter, and collect the filtrate;

[0154] 3. The filtrate is transferred to an evaporator, heated and boiled, H2O2 and HNO3 are continuously added to keep the acidity at 1.5-2.5 mol / L, and then ammonium chloride is added until the precipitation no longer increases, the acid is removed and filtered, and the filtrate A is retained. The filter residue is washed with 15% NH4Cl solution until it is light in color. H2O2 and HNO3 are added to the filtrate until the precipitation no longer increases, and the filter residue is washed with 15% NH4Cl solution until it is colorless. The washing solutions from the two washings are combined to obtain a crude rhodium-containing solution;

[0155] 4. Take the crude rhodium-containing solution, remove impurities with polyethyleneimine-tannin-based adsorption resin pretreated with hydrochloric acid at pH=1, continue to add H2O2 and HNO3, add ammonium chloride until the precipitation no longer increases, filter and wash the residue with 15% NH4Cl, combine the washing liquid with the filtrate, concentrate and dry, and finally obtain (NH4)3RhCl6 crystals;

[0156] 5. (NH4)3RhCl6 crystals are calcined and hydrogen reduced to obtain high-purity rhodium powder.

[0157] Comparative Example 9

[0158] 1. The waste material, activated carbon, and black phosphorus / red phosphorus were mixed evenly in a mass ratio of 10:7:2.5, and calcined at 600°C for 2h in a Marsh furnace, cooled to room temperature, and the powder was collected;

[0159] 2. Put the powder into the titanium reactor, add 10% hydrochloric acid and stir, heat to 60-65°C, slowly add 25% sodium chlorate solution into the reactor, keep the 25% sodium chlorate solution added and stirred for 4 hours when the redox potential is greater than 970mV, then heat to 85°C and keep until no gas overflows, then cool to room temperature, filter, and collect the filtrate;

[0160] 3. The filtrate is transferred to an evaporator, heated and boiled, H2O2 and HNO3 are continuously added to keep the acidity at 1.5-2.5 mol / L, and then ammonium chloride is added until the precipitation no longer increases, the acid is removed and filtered, and the filtrate A is retained. The filter residue is washed with 15% NH4Cl solution until it is light in color. H2O2 and HNO3 are added to the filtrate until the precipitation no longer increases, and the filter residue is washed with 15% NH4Cl solution until it is colorless. The washing solutions from the two washings are combined to obtain a crude rhodium-containing solution;

[0161] 4. Take the crude rhodium-containing solution, remove impurities with polyethyleneimine-tannin-based adsorption resin pretreated with hydrochloric acid at pH = 4, continue to add H2O2 and HNO3, add ammonium chloride until the precipitation no longer increases, filter and wash the residue with 15% NH4Cl, combine the washing liquid with the filtrate, concentrate and dry, and finally obtain (NH4)3RhCl6 crystals;

[0162] 5. (NH4)3RhCl6 crystals are calcined and hydrogen reduced to obtain high-purity rhodium powder.

[0163] Product determination:

[0164] Rhodium powder samples were prepared according to Examples 4-6 and Comparative Examples 7-9 respectively;

[0165] 1. Take three samples of nine rhodium powders, each weighing 0.1 g, and measure the impurities using an inductively coupled plasma atomic emission spectrometer and ignition loss according to GB / T 1421-2018. The purity of the rhodium powder is calculated by calculation. The results are the average values ​​of the three groups of experiments, as shown in Table 1.

[0166] Table 2

[0167] purity(%) Example 4 99.95±0.02 Example 5 99.94±0.03 Example 6 99.95±0.03 Comparative Example 7 97.89±0.05 Comparative Example 8 95.71±0.04 Comparative Example 9 98.84±0.03

Claims

1. A method for recycling waste materials to prepare platinum group metals, characterized in that: The preparation steps are as follows: (1) The waste material, activated carbon and combustion aid are mixed evenly in a mass ratio of 10:6~8:2~3, roasted at 600℃ in a Marsh furnace for 2h, cooled to room temperature, and powder is collected; (2) Take 100 parts of powder and mix them evenly with 600-700 parts of zinc powder, roast them in a Marsh furnace at 850°C for 8 hours, cool to room temperature, ball-mill them, pass them through a 60-mesh sieve, immerse them in 10% hydrochloric acid and add 10% hydrochloric acid while stirring until the suspended solids no longer decrease, filter and retain the solids, and dry them to obtain active ash; (3) Add active ash into a titanium reactor, add 10% hydrochloric acid and stir, heat to 60-65°C, slowly add 25% sodium chlorate solution into the reactor, keep the 25% sodium chlorate solution added and stirred for 4 hours when the redox potential is greater than 970mV, then heat to 85°C and keep until no gas overflows, then cool to room temperature, filter, and collect the filtrate; (4) The filtrate is transferred to an evaporator and heated to a boil. H2O2 and HNO3 are continuously added to maintain the acidity at 1.5-2.5 mol / L. Ammonium chloride is then added until the precipitation stops increasing. The acid is removed and filtered. Filtrate A is retained. The filter residue is washed with a 15% NH4Cl solution until it is light in color. H2O2 and HNO3 are added to the filtrate until the precipitation stops increasing. The filter residue is filtered and washed with a 15% NH4Cl solution until it is colorless. The washing solutions from the two washings are combined to obtain a crude rhodium-containing solution. The washed filter residues are combined to obtain a crude (NH4)2IrCl6. (5) Add water to the crude (NH4)2IrCl6 to make a slurry, adjust the pH to 1-1.5, heat to boil, stir and add 300-500 parts of hydrazine hydrate solution and 0.2-0.5 parts of a reaction aid. When the solid content stops decreasing, adjust the pH to 2-2.5 with aqueous ammonia, boil for 1-2 hours, cool, filter, and retain the filtrate to obtain an iridium-containing solution; (6) Add hydrochloric acid to the iridium solution to adjust the pH to 1.0-1.5, heat to 80°C, add 320-360 parts of ammonium sulfide, adjust the pH to 2.5-3.0 and boil for 2 hours, cool and store for 36 hours, then filter, add H2O2 and HNO3 to the filtrate until the precipitation no longer increases, wash the filter residue with 15% NH4Cl solution until it is light in color, and dry to obtain (NH4)2IrCl6 crystals; (7) After the crude rhodium-containing solution is impurized by using an adsorption resin pretreated with hydrochloric acid at a pH of 2 to 3, H2O2 and HNO3 are continuously added, and ammonium chloride is added until the precipitation no longer increases. After filtering, the filter residue is washed with 15% NH4Cl, and the washing liquid is combined with the filtrate, concentrated and dried to obtain (NH4)3RhCl6 crystals; (8) (NH4)2IrCl6 crystals and (NH4)3RhCl6 crystals are calcined and hydrogen reduced to obtain high-purity iridium and rhodium metal powders.

2. The method for recovering platinum group metals from waste materials according to claim 1, characterized in that: The combustion aid is a black phosphorus / red phosphorus heterojunction.

3. The method for recovering platinum group metals from waste materials according to claim 1, characterized in that: The reaction aid is modified CMK-3, and the modification steps are as follows: (1) Take CMK-3, 2-methylimidazole and ethanol in a mass ratio of 3-6:2-4:30-40; (2) Add CMK-3 and 2-methylimidazole to ethanol, mix well, and treat with ultrasound for 30-40 minutes; (3) The mixture was heated in a water bath at 40°C and evaporated to dryness, and the solid was calcined at 800°C for 3 h in a nitrogen atmosphere to obtain N-CMK-3; (4) Place N-CMK-3 in 8-10 times the mass of deionized water and add 0.5w% 0.05mol / l H2PtCl6 aqueous solution, and ultrasonicate for 10-20min; (5) The mixture was heated in a water bath at 40°C and evaporated to dryness. The solid was calcined at 200°C for 3 h in a nitrogen / hydrogen mixed atmosphere of 4:1 to obtain Pt / N-CMK-3, i.e., modified CMK-3.

4. The method for recovering platinum group metals from waste materials according to claim 1, characterized in that: The adsorption resin is polyethyleneimine-tannin based adsorption resin.

Citation Information

Patent Citations

  • Method for recovering iridium from waste materials and residues

    CN111961865A

  • Method for recovering platinum from spent platinum-vanadium catalyst with carbon carrier

    CN117305617A

  • Process for separating metals from aqueous solutions

    US4392962A