Method for recovering molybdenum-titanium alloy

Through multiple hydrogenation-crusting-dehydrogenation technology processes and airtight protection measures, the problems of high cost and long processing cycle of molybdenum titanium alloy recycling equipment have been solved, high-quality molybdenum titanium alloy remanufacturing has been realized, and the utilization of molybdenum titanium alloy has been improved. Rate.

CN119082499APending Publication Date: 2024-12-06宁波创润新材料有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410803521.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing molybdenum titanium alloy recycling methods have high equipment costs and long processing cycles, which are difficult to meet the economic affordability of small and medium-sized enterprises, and have failed to effectively improve the utilization rate of molybdenum titanium alloy.

Method used

Multiple hydrogenation-crumbing-dehydrogenation technology processes are adopted, including pickling, drying, multiple hydrogenation, crushing, grinding and dehydrogenation. Combined with strict airtight protection measures, the gas impurity content in the powder is controlled to be below 100ppm.

Benefits of technology

High-quality remanufacturing of high-density, microporous structure, and high-strength molybdenum titanium alloy materials has been achieved, reducing equipment costs and processing cycles, and improving the utilization rate of molybdenum titanium alloys.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the field of metal recovery, in particular to a molybdenum-titanium alloy recovery method which comprises the following steps: step 1, sequentially carrying out acid pickling treatment and drying treatment on a molybdenum-titanium alloy; secondly, the dried molybdenum-titanium alloy is subjected to first hydrogenation treatment, and first hydrogenated molybdenum-titanium alloy is obtained; thirdly, the first hydrogenated molybdenum-titanium alloy is crushed, and the first hydrogenated molybdenum-titanium alloy with the first size is obtained; fourthly, the hydrogenated molybdenum-titanium alloy with the first size is subjected to second hydrogenation treatment, and second hydrogenated molybdenum-titanium alloy with the first size is obtained; fifthly, the second hydrogenated molybdenum-titanium alloy with the first size is subjected to first grinding treatment, and the second hydrogenated molybdenum-titanium alloy with the second size is obtained; 6, the second hydrogenated molybdenum-titanium alloy with the second size is subjected to dehydrogenation treatment, and the molybdenum-titanium alloy with the second size is obtained; seventhly, the molybdenum-titanium alloy with the second size is subjected to second grinding treatment, and the molybdenum-titanium alloy with the third size is obtained; and the molybdenum-titanium alloy material with high density, micropore structure and high strength can be effectively recycled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of metal recovery, and in particular to a method for recovering a molybdenum-titanium alloy. Background Art

[0002] As an important structural material, molybdenum-titanium alloy has high strength and hardness. Molybdenum-titanium alloy is generally sintered and recycled by hot isostatic pressing. In the field of molybdenum-titanium alloy, hot isostatic pressing is usually used for sintering and recycling. However, the cost of sintering and recycling equipment using hot isostatic pressing is high. In order to achieve stable processing under high temperature and high pressure, special equipment and process flow are required. The cost of these equipment is relatively high, which is economically unaffordable for some small and medium-sized enterprises. Hot isostatic pressing sintering usually requires the use of molds for molding. Therefore, there are molding difficulties or restrictions for products with complex shapes and special structures. The entire processing cycle of hot isostatic pressing sintering and recycling is relatively long, which will affect the production cycle and delivery time of the product. At present, there is no molybdenum-titanium alloy recycling method in the market that can reduce the processing cost of enterprises and effectively improve the utilization rate of molybdenum-titanium alloy. Therefore, the market is in urgent need of a more advanced molybdenum-titanium alloy recycling method. Summary of the invention

[0003] The purpose of the present invention is to provide a method for recovering molybdenum-titanium alloy in view of the deficiencies in the prior art.

[0004] To achieve the above object, the technical solution adopted by the present invention is:

[0005] A method for recovering molybdenum-titanium alloy comprises the following steps:

[0006] Step 1, sequentially performing pickling treatment and drying treatment on the molybdenum-titanium alloy;

[0007] Step 2: performing a first hydrogenation treatment on the dried molybdenum-titanium alloy to obtain a first hydrogenated molybdenum-titanium alloy;

[0008] Step 3: crushing the first hydrogenated molybdenum-titanium alloy to obtain the first hydrogenated molybdenum-titanium alloy having a first size;

[0009] Step 4: performing a second hydrogenation treatment on the hydrogenated molybdenum-titanium alloy having the first size to obtain a second hydrogenated molybdenum-titanium alloy having the first size;

[0010] Step 5: performing a first grinding process on the second hydrogenated molybdenum-titanium alloy having the first size to obtain a second hydrogenated molybdenum-titanium alloy having the second size;

[0011] Step 6: Dehydrogenate the second hydrogenated molybdenum-titanium alloy having the second size to obtain the molybdenum-titanium alloy having the second size;

[0012] Step 7, performing a second grinding process on the molybdenum-titanium alloy having the second size to obtain the molybdenum-titanium alloy having the third size;

[0013] The first hydrogenation treatment and the second hydrogenation treatment both include: a heating stage, a heat preservation stage, a cooling stage, a hydrogenation stage, and a cooling stage;

[0014] The first size is larger than the second size, and the second size is larger than the third size.

[0015] Preferably, the zeroth dimension is a thickness no greater than 2 cm.

[0016] Preferably, the pickling treatment comprises: pickling the molybdenum-titanium alloy with nitric acid and hydrofluoric acid.

[0017] Preferably, the volume ratio of nitric acid to hydrofluoric acid is (1-3):(4-6).

[0018] Preferably, the temperature is raised to 800-1000°C during the heating stage, the temperature is kept at 800-1000°C for 8h-12h during the heat preservation stage, and the temperature is cooled to 600-800°C during the cooling stage.

[0019] Preferably, the first size is a particle size of 1 cm-5 cm.

[0020] Preferably, the first grinding process is a vacuum ball milling process, and the second grinding process is a jet milling process.

[0021] Preferably, the dehydrogenation treatment comprises: heating to 600°C-800°C for dehydrogenation treatment.

[0022] Preferably, it also includes:

[0023] Step 8: Screening and packaging the molybdenum-titanium alloy having the third size in sequence.

[0024] The present invention adopts the above technical solution, and has the following technical effects compared with the prior art:

[0025] The present invention adopts advanced multiple hydrogenation-crushing-dehydrogenation technical process, which can effectively recover high-density, microporous structure, and high-strength molybdenum-titanium alloy materials. During the entire conversion and processing stage, strict airtight protection measures are taken to ensure the sealing of the environment, thereby accurately controlling the gas impurity content in the powder to below 100ppm, achieving the application standard of high-quality remanufacturing of molybdenum-titanium alloy powder. DETAILED DESCRIPTION

[0026] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.

[0028] The following specific examples further illustrate the present invention but are not intended to limit the present invention.

[0029] Example 1

[0030] This embodiment provides a method for recovering molybdenum-titanium alloy, the steps comprising:

[0031] Step 1, pickling the molybdenum-titanium alloy with a thickness not greater than 2 cm with a mixed solution of nitric acid and hydrofluoric acid in a volume ratio of 2:5, and drying the alloy after the pickling;

[0032] Step 2: Loading the dried molybdenum-titanium alloy into a hydrogenation furnace for a first hydrogenation treatment, wherein the first hydrogenation treatment includes: a heating stage, a heat preservation stage, a cooling stage, and a hydrogenation stage;

[0033] The heating stage is to heat the material to 800°C, the heat preservation stage is to keep the material at 800°C for 8 hours, the cooling stage is to cool the material to 600°C, and the hydrogenation stage is to obtain the first hydrogenated molybdenum-titanium alloy after the pressure in the hydrogenation furnace is stabilized;

[0034] Step 3, cooling the first hydrogenated molybdenum-titanium alloy and then crushing it to obtain the first hydrogenated molybdenum-titanium alloy with a particle size of 1 cm;

[0035] Step 4: subjecting the first hydrogenated molybdenum-titanium alloy having a particle size of 1 cm to a second hydrogenation treatment, wherein the second hydrogenation treatment comprises: a heating stage, a heat preservation stage, a cooling stage, and a hydrogenation stage;

[0036] The heating stage is to heat the material to 800°C, the heat preservation stage is to keep the material at 800°C for 8 hours, the cooling stage is to cool the material to 600°C, and the hydrogenation stage is to obtain a second hydrogenated molybdenum-titanium alloy after the pressure in the hydrogenation furnace is stabilized; the second hydrogenated molybdenum-titanium alloy is obtained;

[0037] Step 5, cooling the second hydrogenated molybdenum-titanium alloy and then putting it into a vacuum ball mill for grinding to obtain a second hydrogenated molybdenum-titanium alloy having a second size;

[0038] Step 6: The second hydrogenated molybdenum-titanium alloy with the second size is transferred to a dehydrogenation furnace through a transfer tank under the protection of argon gas. When the temperature in the dehydrogenation furnace rises to 600° C., the vacuum machine in the dehydrogenation furnace is turned on to perform dehydrogenation treatment. When the pressure in the dehydrogenation furnace is lower than 20 Pa, the dehydrogenation of the fully hydrogenated molybdenum-titanium alloy is completed, and the dehydrogenated molybdenum-titanium alloy with the second size is obtained.

[0039] Step 7, subjecting the dehydrogenated molybdenum-titanium alloy having the second size to a jet milling process to obtain a molybdenum-titanium alloy having a third size;

[0040] Step 8: Screening the molybdenum-titanium alloy having the third size using an airtight protective screen, and packaging the alloy after screening;

[0041] Wherein, the mesh number of the sieve used in the screening process is less than 200 mesh;

[0042] Wherein, the first size is larger than the second size, and the second size is larger than the third size;

[0043] Among them, the operations in the above step six are all carried out under protective gas, and the protective gas is argon.

[0044] Example 2

[0045] This embodiment provides a method for recovering molybdenum-titanium alloy, the steps comprising:

[0046] Step 1: pickling the molybdenum-titanium alloy with a thickness of no more than 2 cm with a mixed solution of nitric acid and hydrofluoric acid in a volume ratio of 3:6, and drying the alloy after the pickling;

[0047] Step 2: Loading the dried molybdenum-titanium alloy into a hydrogenation furnace for a first hydrogenation treatment, wherein the first hydrogenation treatment includes: a heating stage, a heat preservation stage, a cooling stage, and a hydrogenation stage;

[0048] The heating stage is to heat the material to 1000°C, the heat preservation stage is to keep the material at 1000°C for 12 hours, the cooling stage is to cool the material to 800°C, and the hydrogenation stage is to obtain the first hydrogenated molybdenum-titanium alloy after the pressure in the hydrogenation furnace is stabilized;

[0049] Step 3, cooling the first hydrogenated molybdenum-titanium alloy and crushing it to obtain the first hydrogenated molybdenum-titanium alloy with a particle size of 5 cm;

[0050] Step 4: subjecting the first hydrogenated molybdenum-titanium alloy having a particle size of 5 cm to a second hydrogenation treatment, wherein the second hydrogenation treatment comprises: a heating stage, a heat preservation stage, a cooling stage, and a hydrogenation stage;

[0051] The heating stage is to heat the material to 1000°C, the heat preservation stage is to keep the material at 1000°C for 12 hours, the cooling stage is to cool the material to 800°C, and the hydrogenation stage is to obtain a second hydrogenated molybdenum-titanium alloy after the pressure in the hydrogenation furnace is stabilized.

[0052] Step 5, placing the second hydrogenated molybdenum-titanium alloy into a vacuum ball mill for grinding to obtain a second hydrogenated molybdenum-titanium alloy having a second size;

[0053] Step 6: The second hydrogenated molybdenum-titanium alloy with the second size is transferred to a dehydrogenation furnace through a transfer tank under the protection of argon gas. When the temperature in the dehydrogenation furnace rises to 800° C., the vacuum machine in the dehydrogenation furnace is turned on to perform dehydrogenation treatment. When the pressure in the dehydrogenation furnace is lower than 20 Pa, the dehydrogenation of the fully hydrogenated molybdenum-titanium alloy is completed, and the dehydrogenated molybdenum-titanium alloy with the second size is obtained.

[0054] Step 7, subjecting the dehydrogenated molybdenum-titanium alloy having the second size to a jet milling process to obtain a molybdenum-titanium alloy having a third size;

[0055] Step 8: Screening the molybdenum-titanium alloy having the third size using an airtight protective screen, and packaging the alloy after screening;

[0056] Wherein, the mesh number of the sieve used in the screening process is less than 200 mesh;

[0057] The first size is larger than the second size, and the second size is larger than the third size.

[0058] Among them, the operations in the above step six are all carried out under protective gas, and the protective gas is argon.

[0059] The present invention adopts advanced multiple hydrogenation-crushing-dehydrogenation technical process, which can effectively recover high-density, microporous structure, and high-strength molybdenum-titanium alloy materials. During the entire conversion and processing stage, strict airtight protection measures are taken to ensure the sealing of the environment, thereby accurately controlling the gas impurity content in the powder to below 100ppm, achieving the application standard of high-quality remanufacturing of molybdenum-titanium alloy powder.

[0060] The above description is only a preferred embodiment of the present invention, and does not limit the implementation mode and protection scope of the present invention. For those skilled in the art, it should be aware that all solutions obtained by equivalent substitutions and obvious changes made using the contents of the specification of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for recovering molybdenum-titanium alloy, It is characterized in that the steps include: Step 1, sequentially performing pickling treatment and drying treatment on the molybdenum-titanium alloy; Step 2: performing a first hydrogenation treatment on the molybdenum-titanium alloy after the drying treatment to obtain a first hydrogenated molybdenum-titanium alloy; Step 3: crushing the first hydrogenated molybdenum-titanium alloy to obtain a first hydrogenated molybdenum-titanium alloy having a first size; Step 4: performing a second hydrogenation treatment on the hydrogenated molybdenum-titanium alloy having the first size to obtain a second hydrogenated molybdenum-titanium alloy having the first size; Step 5: performing a first grinding process on the second hydrogenated molybdenum-titanium alloy having the first size to obtain a second hydrogenated molybdenum-titanium alloy having the second size; Step 6: Dehydrogenate the second hydrogenated molybdenum-titanium alloy having the second size to obtain the molybdenum-titanium alloy having the second size; Step 7: performing a second grinding process on the molybdenum-titanium alloy having the second size to obtain a molybdenum-titanium alloy having a third size; Wherein, the first hydrogenation treatment and the second hydrogenation treatment both include: a temperature rising stage, a temperature keeping stage, a temperature falling stage, a hydrogenation stage, and a cooling stage; The first size is larger than the second size, and the second size is larger than the third size.

2. The recycling method according to claim 1, It is characterized in that The molybdenum-titanium alloy has a zeroth dimension, and the zeroth dimension is a thickness not greater than 2 cm.

3. The recycling method according to claim 1, It is characterized in that The pickling treatment includes: pickling the molybdenum-titanium alloy with nitric acid and hydrofluoric acid.

4. The recycling method according to claim 1, It is characterized in that The volume ratio of the nitric acid to the hydrofluoric acid is (1-3):(4-6).

5. The recycling method according to claim 1, It is characterized in that The temperature rising stage is to rise the temperature to 800°C-1000°C, the temperature keeping stage is to keep the temperature at 800°C-1000°C for 8h-12h, and the temperature falling stage is to fall the temperature to 600°C-800°C.

6. The recycling method according to claim 1, It is characterized in that The first size is a particle size of 1 cm-5 cm.

7. The recycling method according to claim 1, It is characterized in that The first grinding process is a vacuum ball milling process, and the second grinding process is a jet milling process.

8. The recycling method according to claim 1, It is characterized in that The dehydrogenation treatment includes: heating to 600° C.-800° C. for dehydrogenation treatment.

9. The recycling method according to claim 1, It is characterized in that Also includes: Step eight, screening and packaging the molybdenum-titanium alloy having the third size in sequence.