Method for reducing oxidation of intermediate alloy produced by aluminothermic method

By using argon protection technology in aluminum thermal production, the oxidation of intermediate alloys is reduced, and the problem of oxide film formation during the cooling process of intermediate alloys by aluminum thermal production is solved, the production efficiency and yield rate are improved, and the production cost and impurities are reduced. content.

CN119082519APending Publication Date: 2024-12-06BAOJI ZHONGSE SPECIAL METAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411235124.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The large-area oxide film formed by the aluminum-thermal production process during the cooling process leads to product quality defects. The existing treatment methods are cumbersome and low efficiency, resulting in high production costs and low yield.

Method used

In the aluminum thermal production process, the formation of the oxide film is reduced by allowing the crucible to stand and continuously pass through the inert gas argon to prevent oxidation, and then gradually cooled under the protection of argon. Specific steps include adjusting the standstill time and argon gas inlet time, setting reasonable intervals and times according to the feed volume, ensuring that the alloy ingot minimizes oxidation before cooling to the oxidation temperature.

Benefits of technology

It significantly reduces the oxidation area of ​​the intermediate alloy, reduces the workload of subsequent processing, shortens the production cycle, improves production efficiency and yield, reduces workers' labor intensity and production costs, and at the same time reduces the content of impurities and improves product quality. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082519A_ABST
    Figure CN119082519A_ABST
Patent Text Reader

Abstract

The invention discloses a method for reducing oxidation of an intermediate alloy produced by an aluminothermic method, which comprises the following steps: after the reaction for producing the intermediate alloy by the aluminothermic method is finished, keeping a crucible filled with an intermediate alloy liquid in a standing state, and fully separating slag from the intermediate alloy liquid; inert gas is continuously introduced into the crucible in the standing state, and after the inert gas is introduced, a crucible cover is adopted to seal a crucible opening, so that the alloy ingot in the crucible is gradually cooled under the protection of the inert gas; and then the crucible is continuously kept in the standing state, inert gas is continuously introduced into the crucible for multiple times according to the proper interval time, the alloy ingot in the crucible is cooled to the temperature below the oxidation temperature under the protection of the inert gas, and then the alloy ingot is naturally cooled and discharged out of the furnace. And before the intermediate alloy ingot is cooled to the oxidation temperature, argon is introduced for multiple times, so that the oxidation area of the alloy ingot is greatly reduced after the alloy ingot is discharged from the furnace, the production cycle of the product is shortened, the later processing loss is reduced, and the yield is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of intermediate alloy preparation, and in particular relates to a method for reducing oxidation of intermediate alloy produced by aluminothermic process. Background Art

[0002] The quality of the master alloy is related to many factors, among which the oxide film is a major quality defect of most master alloys produced by the aluminothermic method. When the aluminothermic reaction is over, the alloy liquid in the crucible is cooled in the atmosphere. The thermal crack section generated during the cooling process contacts the air at high temperature, forming a large area of ​​oxide film. If it is not handled thoroughly, once it enters the product, it will cause the oxygen, nitrogen and other elements in the product to exceed the standard, thus causing product defects. Therefore, the master alloy produced by the aluminothermic method often requires a lot of time and manpower for sandblasting and grinding after the ingot is out of the furnace to ensure that the oxide film on the surface of the master alloy is cleaned. In addition, in the final process of product production, the color sorter and manual method are required to perform multiple color sorting and manual picking of the alloy particles of the finished product specifications to completely remove the oxide particles in the master alloy products and meet the product quality requirements.

[0003] The method of removing oxide film through processes such as sandblasting, grinding, color sorting, and manual picking is a common treatment method after the production of intermediate alloys by the thermite method. The process is cumbersome and difficult to automate, so the operation efficiency is low. At the same time, it requires a lot of manpower and equipment support, and the processing process has large losses, low product yield, high production costs, and poor economic benefits. Summary of the invention

[0004] In order to solve the above problems existing in the prior art, the present invention provides a method for reducing oxidation of master alloy produced by aluminothermic process. The technical problem to be solved by the present invention is achieved by the following technical solution:

[0005] A method for reducing oxidation of a master alloy produced by an aluminothermic process, comprising:

[0006] Step 1: After the reaction of producing the master alloy by the aluminothermic method is completed, the crucible containing the master alloy liquid is kept in a static state to allow the slag and the master alloy liquid to be fully separated;

[0007] Step 2: continuously introducing an inert gas into the static crucible, and after the introduction of the inert gas is completed, the crucible mouth is covered with a graphite crucible cover, so that the alloy ingot in the crucible is gradually cooled under the protection of the inert gas to prevent oxidation;

[0008] Step 3: After the argon gas is introduced in step 2, the crucible is kept in a static state, and then the inert gas is continuously introduced into the crucible for multiple times at appropriate intervals to allow the alloy ingot in the crucible to be cooled to below the oxidation temperature under the protection of the inert gas, and then naturally cooled and taken out of the furnace.

[0009] Furthermore, the standing time of the crucible in step 1 is determined as follows: the standing time of a feed amount of (1-40) kg is (1-(feed amount kg / 20+2)) min; the standing time of a feed amount of (41-80) kg is (3-(feed amount kg / 20+3)) min, the standing time of a feed amount of (81-200) kg is (5-(feed amount kg / 40+4min)), the standing time of a feed amount of (201-400) kg is (7-(feed amount kg / 40+5)) min, and the standing time of a feed amount of >400 kg is (10-(feed amount kg / 40+6)) min, wherein the integer part of the calculation result is taken each time.

[0010] Furthermore, the time for continuously passing the inert gas in step 2 is determined according to the following method: the time for passing the inert gas for a feed amount of (1-40) kg is (1-(feed amount kg / 10)) min, the time for passing the inert gas for a feed amount of (41-80) kg is (2-(feed amount kg / 10)) min, the time for passing the inert gas for a feed amount of (81-200) kg is (5-(feed amount kg / 20)) min, the time for passing the inert gas for a feed amount of (201-400) kg is (8-(feed amount kg / 20)) min, and the time for passing the inert gas for a feed amount of >400 kg is (10-(feed amount kg / 30)) min, wherein the integer part of the calculation result is taken each time.

[0011] Furthermore, the interval time, the time of passing inert gas, and the number of times of continuous passing inert gas in step 3 are determined as follows: for a feed amount of (1-40) kg, after the first passing of inert gas, the inert gas is passed again for (1-2) min at an interval of ((0.3+(feed amount kg / 80)±0.1) h, and the lid is continuously sealed after each passing, for 2 times; for a feed amount of (41-80) kg, after the first passing of inert gas, the inert gas is passed again for (1-2) min at an interval of ((0.8+(feed amount kg / 120)±0.2) h, and the lid is continuously sealed after each passing, for 3 times; for a feed amount of (81-200) kg, after the first passing of inert gas, the inert gas is passed again for (1.0+(feed amount kg / 120)±0.2) h, and the lid is continuously sealed after each passing, for 3 times. For a feed amount of (201-400) kg, inert gas is introduced again for (5-7) min at intervals of (1.2 + (feed amount kg / 200) ± 0.4) h after the first inert gas introduction, and the lid is continuously sealed after each introduction, which is continued for 4 times. For a feed amount of more than 400 kg, inert gas is introduced again for (7-10) min at intervals of (1.4 + (feed amount kg / 240) ± 0.5) h after the first inert gas introduction, and the lid is continuously sealed after each introduction, which is continued for (5 + ((feed amount - 400) kg / 280)) times, wherein the integer part of the calculated result is taken each time.

[0012] Furthermore, the inert gases are all argon.

[0013] Beneficial effects of the present invention:

[0014] 1. Before the master alloy ingot is cooled to the oxidation temperature, argon gas is introduced into the crucible containing the master alloy ingot for multiple times, so that the oxidation area of ​​the alloy ingot is greatly reduced after it is taken out of the furnace, the workload of subsequent processing is reduced, the production cycle of the product is shortened, the production efficiency is improved, the labor intensity of workers is reduced, and the production cost is reduced. At the same time, the loss of later processing is reduced and the yield rate is improved;

[0015] 2. This method reduces the processing loss of ingot casting and improves the product yield. At the same time, the oxygen and nitrogen impurity content of alloy ingot casting can be reduced by about 50% on average, thereby reducing product quality risks and improving product quality;

[0016] 3. The present invention achieves the same effect as continuous introduction of argon by reasonably setting the time and frequency of introducing argon, while reducing the safety risk and production cost of continuous introduction of argon under high temperature conditions.

[0017] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is a schematic diagram of sampling of the master alloy ingot of the present invention;

[0019] Figures 2-3 is a cross-sectional photograph of the vanadium-aluminum alloy ingot in Example 1;

[0020] Figures 4-5 This is a cross-sectional photograph of the vanadium-aluminum alloy ingot in the control group 1. DETAILED DESCRIPTION

[0021] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments, but the embodiments of the present invention are not limited thereto.

[0022] Example 1

[0023] The embodiment of the present invention provides a method for reducing oxidation of a master alloy produced by an aluminothermic process, wherein the master alloy produced is a vanadium aluminum alloy, and the initial feed amount is 400 kg, and the method specifically comprises the following steps:

[0024] Step 1: After the reaction of producing vanadium-aluminum alloy by aluminothermic method is completed, the crucible containing vanadium-aluminum alloy liquid is kept at rest to separate the slag and vanadium-aluminum alloy liquid fully, wherein the resting time is 12 minutes.

[0025] Step 2: Continuously introduce argon gas into the static crucible for 14 minutes. After the introduction of argon gas, seal the crucible mouth with a graphite crucible cover to gradually cool the vanadium-aluminum alloy ingot in the crucible under the protection of argon gas to prevent oxidation.

[0026] Step 3: After the introduction of argon in step 2, the crucible is kept in a static state, and then argon is introduced once every 170 minutes, each time for 6 minutes, for a total of 4 times, and the cover is continued after each completion, so that the vanadium-aluminum alloy ingot in the crucible is cooled to below the oxidation temperature under the protection of argon, and finally the vanadium-aluminum alloy ingot is naturally cooled for 48 hours before being taken out of the furnace.

[0027] After the argon gas is introduced in step 2 and step 3, on the one hand, the contact between the vanadium-aluminum alloy ingot in the crucible and the air can be minimized when it is cooled to the oxidation temperature range; on the other hand, when the vanadium-aluminum alloy ingot is in the cooling process, the argon gas continuously introduced has a large specific gravity, which will enter the microcracks inside the ingot caused by stress concentration, isolating the contact between the air and the microcrack section of the ingot until the ingot is cooled to below the oxidation temperature, thereby minimizing the area of ​​the oxide film and the nitride film inside the ingot and reducing the content of impurity elements such as O and N in the alloy ingot.

[0028] The cooled vanadium-aluminum alloy ingot was sampled and analyzed. Figure 1As shown in the figure, with the center of the bottom of the ingot as the axis, three samples were taken at equal intervals from the top, middle and bottom thickness directions to the edge of the ingot, for a total of nine samples, and the chemical composition of oxygen and nitrogen elements in the nine samples was analyzed. The analysis results are shown in Table 1. The oxidation photo of the end surface of the vanadium aluminum alloy ingot is shown in Figures 2-3 As shown:

[0029] Table 1 Chemical composition of the vanadium aluminum alloy prepared in Example 1

[0030]

[0031]

[0032] In addition, the specific production data of Example 1 is shown in Table 2.

[0033] Table 2 Production data of vanadium aluminum alloy prepared in Example 1

[0034]

[0035] Control group 1

[0036] This control group provides a conventional processing method for the intermediate alloy after the intermediate alloy is produced by the aluminothermic method, wherein the intermediate alloy produced is a vanadium aluminum alloy, and the initial feed amount is 400 kg, which specifically includes the following steps:

[0037] Step 1: After the reaction of producing vanadium-aluminum alloy by the aluminothermic method is completed, the crucible containing the vanadium-aluminum alloy liquid is left to stand for 12 minutes to allow the slag and the vanadium-aluminum alloy liquid to be fully separated.

[0038] Step 2: After the standing time is over, transfer the crucible to the designated cooling area for cooling for 48 hours before taking it out of the furnace.

[0039] The cooled vanadium-aluminum alloy ingot was sampled and analyzed. With the center of the bottom of the ingot as the axis, three samples were taken at equal intervals from the top, middle and bottom thickness directions to the edge of the ingot. A total of nine samples were taken, and the chemical composition of oxygen and nitrogen in the nine samples was analyzed. The analysis results are shown in Table 3. The oxidation photos of the end surface of the vanadium-aluminum alloy ingot are shown in Table 3. Figures 4-5 As shown:

[0040] Table 3 Chemical composition of vanadium aluminum alloy prepared in control group 1

[0041]

[0042]

[0043] In addition, the specific production data of the control group 1 is shown in Table 4.

[0044] Table 4 Production data of vanadium aluminum alloy prepared in control group 1

[0045]

[0046] Example 2

[0047] The embodiment of the present invention provides a method for reducing oxidation of a master alloy produced by an aluminothermic process, wherein the master alloy produced is a molybdenum aluminum alloy, and the initial feed amount is 200 kg, and the method specifically comprises the following steps:

[0048] Step 1: After the reaction of producing molybdenum-aluminum alloy by the aluminothermic method is completed, the crucible containing the molybdenum-aluminum alloy liquid is kept static to allow the slag and the molybdenum-aluminum alloy liquid to be fully separated, wherein the static time is 7 minutes.

[0049] Step 2: Continuously introduce argon gas into the static crucible for 8 minutes. After the introduction of argon gas, cover the crucible mouth with a graphite crucible cover to gradually cool the molybdenum-aluminum alloy ingot in the crucible under the protection of argon gas to prevent oxidation.

[0050] Step 3: After the introduction of argon in step 2, the crucible continues to be kept in a static state, and then argon is introduced once every 153 minutes, each time for 4 minutes, for a total of 4 times, and the lid is continued to be sealed after each completion, so that the molybdenum-aluminum alloy ingot in the crucible is cooled to below the oxidation temperature under the protection of argon, and finally the molybdenum-aluminum alloy ingot is naturally cooled for 48 hours before being taken out of the furnace.

[0051] After the argon gas is introduced in step 2 and step 3, on the one hand, the contact with the air can be minimized when the molybdenum-aluminum alloy ingot in the crucible is cooled to the oxidation temperature range. On the other hand, when the molybdenum-aluminum alloy ingot is in the cooling process, the argon gas continuously introduced has a large specific gravity, which will enter the microcracks inside the ingot caused by stress concentration, isolating the contact between the air and the microcrack section of the ingot until the ingot is cooled to below the oxidation temperature, thereby minimizing the area of ​​the oxide film and nitride film inside the ingot and reducing the content of impurity elements such as O and N in the alloy ingot.

[0052] The cooled molybdenum-aluminum alloy ingot was sampled and analyzed. With the center of the bottom of the ingot as the axis, three samples were taken at equal intervals from the top, middle and bottom thickness directions to the edge of the ingot. A total of nine samples were taken, and the chemical composition of oxygen and nitrogen elements in the nine samples was analyzed. The analysis results are shown in Table 5.

[0053] Table 5 Chemical composition of the molybdenum aluminum alloy prepared in Example 2

[0054]

[0055] In addition, the specific production data of Example 2 is shown in Table 6.

[0056] Table 6 Production data of molybdenum aluminum alloy prepared in Example 2

[0057]

[0058]

[0059] Control group 2

[0060] This control group provides a conventional processing method for the intermediate alloy after the intermediate alloy is produced by the aluminothermic method, wherein the intermediate alloy produced is a molybdenum aluminum alloy, and the initial feed amount is 200 kg, which specifically includes the following steps:

[0061] Step 1: After the reaction of producing vanadium-aluminum alloy by aluminothermic method is completed, the crucible containing vanadium-aluminum alloy liquid is left to stand for 7 minutes to allow the slag and vanadium-aluminum alloy liquid to be fully separated.

[0062] Step 2: After the standing time is over, transfer the crucible to the designated cooling area for cooling for 48 hours before taking it out of the furnace.

[0063] The cooled vanadium-aluminum alloy ingot was sampled and analyzed. With the center of the bottom of the ingot as the axis, three samples were taken at equal intervals from the top, middle and bottom thickness directions to the edge of the ingot. A total of nine samples were taken, and the chemical composition of oxygen and nitrogen elements in the nine samples was analyzed. The analysis results are shown in Table 7.

[0064] Table 7 Chemical composition of molybdenum aluminum alloy prepared in control group 2

[0065]

[0066] In addition, the specific production data of the control group 2 is shown in Table 8.

[0067] Table 8 Production data of molybdenum aluminum alloy prepared in control group 2

[0068]

[0069] Example 3

[0070] The embodiment of the present invention provides a method for reducing oxidation of a master alloy produced by an aluminothermic process, wherein the master alloy produced is an aluminum-molybdenum-tungsten-titanium master alloy, and the initial feed amount is 40 kg, and the method specifically comprises the following steps:

[0071] Step 1: After the reaction of producing aluminum-molybdenum-tungsten-titanium master alloy by aluminothermic method is completed, the crucible containing the aluminum-molybdenum-tungsten-titanium master alloy liquid is kept static to allow the slag and the aluminum-molybdenum-tungsten-titanium master alloy liquid to be fully separated, wherein the static time is 3 minutes.

[0072] Step 2: Continuously introduce argon into the static crucible for 4 minutes. After the introduction of argon, seal the crucible mouth with a graphite crucible cover to gradually cool the aluminum-molybdenum-tungsten-titanium intermediate alloy ingot in the crucible under the protection of argon to prevent oxidation.

[0073] Step 3: After the argon is introduced in step 2, the crucible is kept in a static state, and then argon is introduced once every 54 minutes, each time for 2 minutes, for a total of 2 times, and the lid is sealed after each time, so that the aluminum-molybdenum-tungsten-titanium intermediate alloy ingot in the crucible is cooled to below the oxidation temperature under the protection of argon, and finally the aluminum-molybdenum-tungsten-titanium intermediate alloy ingot is naturally cooled for 48 hours before being taken out of the furnace.

[0074] After the argon gas is introduced in step 2 and step 3, on the one hand, the contact with the air can be minimized when the aluminum-molybdenum-tungsten-titanium master alloy ingot in the crucible is cooled to the oxidation temperature range; on the other hand, when the aluminum-molybdenum-tungsten-titanium master alloy ingot is in the cooling process, the argon gas continuously introduced has a large specific gravity, which will enter the microcracks inside the ingot caused by stress concentration, isolating the contact between the air and the microcrack section of the ingot until the ingot is cooled to below the oxidation temperature, thereby minimizing the area of ​​the oxide film and the nitride film inside the ingot, and reducing the content of impurity elements such as O and N in the alloy ingot.

[0075] The cooled aluminum-molybdenum-tungsten-titanium master alloy ingot was sampled and analyzed. With the center of the bottom of the ingot as the axis, three samples were taken at equal intervals from the top, middle and bottom thickness directions to the edge of the ingot, for a total of nine samples. The chemical composition of oxygen and nitrogen in the nine samples was analyzed. The analysis results are shown in Table 9.

[0076] Table 9 Chemical composition of the aluminum-molybdenum-tungsten-titanium master alloy prepared in Example 3

[0077]

[0078] In addition, the specific production data of Example 3 is shown in Table 10.

[0079] Table 10 Production data of aluminum-molybdenum-tungsten-titanium master alloy prepared in Example 3

[0080]

[0081] Control group 3

[0082] This control group provides a conventional processing method for the intermediate alloy after the intermediate alloy is produced by the aluminothermic method, wherein the intermediate alloy produced is an aluminum-molybdenum-tungsten-titanium intermediate alloy, and the initial feed amount is 40kg, which specifically includes the following steps:

[0083] Step 1: After the reaction of producing aluminum-molybdenum-tungsten-titanium master alloy by aluminothermic method is completed, the crucible containing the aluminum-molybdenum-tungsten-titanium master alloy liquid is allowed to stand for 3 minutes to allow the slag and the vanadium-aluminum alloy liquid to be fully separated.

[0084] Step 2: After the standing time is over, transfer the crucible to the designated cooling area for cooling for 48 hours before taking it out of the furnace.

[0085] The cooled aluminum-molybdenum-tungsten-titanium master alloy ingot was sampled and analyzed. Taking the center of the bottom of the ingot as the axis, three samples were taken at equal intervals from the top, middle and bottom thickness directions to the edge of the ingot. A total of nine samples were taken, and the chemical composition of oxygen and nitrogen elements in the nine samples was analyzed. The analysis results are shown in Table 11:

[0086] Table 11 Chemical composition of the aluminum-molybdenum-tungsten-titanium master alloy prepared in control group 3

[0087]

[0088] In addition, the specific production data of the control group 3 is shown in Table 12.

[0089] Table 12 Production data of aluminum-molybdenum-tungsten-titanium master alloy prepared in control group 3

[0090]

[0091] Example 4

[0092] The embodiment of the present invention provides a method for reducing oxidation of a master alloy produced by aluminothermic method, wherein the master alloy produced is a vanadium-aluminum-iron master alloy, and the initial feed amount is 80 kg, and the method specifically comprises the following steps:

[0093] Step 1: After the reaction of producing vanadium-aluminum-iron master alloy by aluminothermic method is completed, the crucible containing the vanadium-aluminum-iron master alloy liquid is kept at rest to fully separate the slag and the vanadium-aluminum-iron master alloy liquid, wherein the resting time is 6 minutes.

[0094] Step 2: Continuously introduce argon into the static crucible for 7 minutes. After the introduction of argon is completed, the crucible mouth is covered with a graphite crucible cover to gradually cool the vanadium-aluminum-iron intermediate alloy ingot in the crucible under the protection of argon to prevent oxidation.

[0095] Step 3: After the introduction of argon in step 2 is completed, the crucible is kept in a static state, and then argon is introduced once every 76 minutes, each time for 2 minutes, for a total of 3 times, and the cover is continued after each completion, so that the vanadium-aluminum-iron intermediate alloy ingot in the crucible is cooled to below the oxidation temperature under the protection of argon, and finally the vanadium-aluminum-iron intermediate alloy ingot is naturally cooled for 48 hours before being taken out of the furnace.

[0096] After the argon gas is introduced in step 2 and step 3, on the one hand, the contact with the air can be minimized when the vanadium-aluminum-iron master alloy ingot in the crucible is cooled to the oxidation temperature range; on the other hand, when the vanadium-aluminum-iron master alloy ingot is in the cooling process, the argon gas continuously introduced has a large specific gravity, which will enter the microcracks inside the ingot caused by stress concentration, isolating the contact between the air and the microcrack section of the ingot until the ingot is cooled to below the oxidation temperature, thereby minimizing the area of ​​the oxide film and the nitride film inside the ingot, and reducing the content of impurity elements such as O and N in the alloy ingot.

[0097] The cooled vanadium-aluminum-iron master alloy ingot was sampled and analyzed. With the center of the bottom of the ingot as the axis, three samples were taken at equal intervals from the top, middle and bottom thickness directions to the edge of the ingot. A total of nine samples were taken, and the chemical composition of oxygen and nitrogen elements in the nine samples was analyzed. The analysis results are shown in Table 13.

[0098] Table 13 Chemical composition of the vanadium-aluminum-iron master alloy prepared in Example 4

[0099]

[0100] In addition, the specific production data of Example 4 is shown in Table 14.

[0101] Table 14 Production data of vanadium-aluminum-iron master alloy prepared in Example 4

[0102]

[0103] Control group 4

[0104] This control group provides a conventional processing method for the intermediate alloy after the intermediate alloy is produced by the aluminothermic method, wherein the intermediate alloy produced is a vanadium aluminum iron intermediate alloy, and the initial feed amount is 80kg, which specifically includes the following steps:

[0105] Step 1: After the reaction of producing vanadium-aluminum-iron master alloy by aluminothermic method is completed, the crucible containing the vanadium-aluminum-iron master alloy liquid is left to stand for 6 minutes to allow the slag and the vanadium-aluminum alloy liquid to be fully separated.

[0106] Step 2: After the standing time is over, transfer the crucible to the designated cooling area for cooling for 48 hours before taking it out of the furnace.

[0107] The cooled vanadium-aluminum-iron master alloy ingot was sampled and analyzed. Taking the center of the bottom of the ingot as the axis, three samples were taken at equal intervals from the top, middle and bottom thickness directions to the edge of the ingot. A total of nine samples were taken, and the chemical composition of oxygen and nitrogen elements in the nine samples was analyzed. The analysis results are shown in Table 15:

[0108] Table 15 Chemical composition of the vanadium-aluminum-iron master alloy prepared in control group 4

[0109]

[0110] In addition, the specific production data of the control group 4 is shown in Table 16.

[0111] Table 16 Production data of vanadium-aluminum-iron master alloy prepared in control group 4

[0112]

[0113] Example 5

[0114] The embodiment of the present invention provides a method for reducing oxidation of a master alloy produced by an aluminothermic process, wherein the master alloy produced is an aluminum-molybdenum-vanadium-iron master alloy, and the initial feed amount is 500 kg, and the method specifically comprises the following steps:

[0115] Step 1: After the reaction of producing aluminum-molybdenum-vanadium-iron intermediate alloy by aluminothermic method is completed, the crucible containing the aluminum-molybdenum-vanadium-iron intermediate alloy liquid is kept static to fully separate the slag and the aluminum-molybdenum-vanadium-iron intermediate alloy liquid, wherein the static time is 17 minutes.

[0116] Step 2: Continuously introduce argon into the static crucible for 15 minutes. After the introduction of argon, seal the crucible mouth with a graphite crucible cover to gradually cool the aluminum-molybdenum-vanadium-iron intermediate alloy ingot in the crucible under the protection of argon to prevent oxidation.

[0117] Step 3: After the argon is introduced in step 2, the crucible is kept in a static state, and then argon is introduced once every 239 minutes, each time for 8 minutes, for a total of 5 times, and the lid is sealed after each time, so that the aluminum-molybdenum-vanadium-iron intermediate alloy ingot in the crucible is cooled to below the oxidation temperature under the protection of argon, and finally the aluminum-molybdenum-vanadium-iron intermediate alloy ingot is naturally cooled for 48 hours before being taken out of the furnace.

[0118] After the argon gas is introduced in step 2 and step 3, on the one hand, the contact with the air can be minimized when the aluminum-molybdenum-vanadium-iron master alloy ingot in the crucible is cooled to the oxidation temperature range; on the other hand, when the aluminum-molybdenum-vanadium-iron master alloy ingot is in the cooling process, the argon gas continuously introduced has a large specific gravity, which will enter the microcracks inside the ingot caused by stress concentration, isolating the contact between the air and the microcrack section of the ingot until the ingot is cooled to below the oxidation temperature, thereby minimizing the area of ​​the oxide film and the nitride film inside the ingot, and reducing the content of impurity elements such as O and N in the alloy ingot.

[0119] The cooled aluminum-molybdenum-vanadium-iron master alloy ingot was sampled and analyzed. With the center of the bottom of the ingot as the axis, three samples were taken at equal intervals from the top, middle and bottom thickness directions to the edge of the ingot, for a total of nine samples. The chemical composition of oxygen and nitrogen in the nine samples was analyzed. The analysis results are shown in Table 17.

[0120] Table 17 Chemical composition of the aluminum-molybdenum-vanadium-iron master alloy prepared in Example 5

[0121]

[0122]

[0123] In addition, the specific production data of Example 5 is shown in Table 18.

[0124] Table 18 Production data of aluminum-molybdenum-vanadium-iron master alloy prepared in Example 5

[0125]

[0126] Control group 5

[0127] This control group provides a conventional processing method for the intermediate alloy after the intermediate alloy is produced by the aluminothermic method, wherein the intermediate alloy produced is an aluminum-molybdenum-vanadium-iron intermediate alloy, and the initial feed amount is 500kg, which specifically includes the following steps:

[0128] Step 1: After the reaction of producing aluminum-molybdenum-vanadium-iron master alloy by aluminothermic method is completed, the crucible containing the aluminum-molybdenum-vanadium-iron master alloy liquid is left to stand for 17 minutes to allow the slag and the vanadium-aluminum alloy liquid to be fully separated.

[0129] Step 2: After the standing time is over, transfer the crucible to the designated cooling area for cooling for 48 hours before taking it out of the furnace.

[0130] The cooled aluminum-molybdenum-vanadium-iron master alloy ingot was sampled and analyzed. Taking the center of the bottom of the ingot as the axis, three samples were taken at equal intervals from the top, middle and bottom thickness directions to the edge of the ingot, for a total of nine samples. The chemical composition of oxygen and nitrogen elements in the nine samples was analyzed. The analysis results are shown in Table 19:

[0131] Table 19 Chemical composition of the aluminum-molybdenum-vanadium-iron master alloy prepared in control group 5

[0132]

[0133]

[0134] In addition, the specific production data of control group 5 is shown in Table 20.

[0135] Table 20 Production data of aluminum-molybdenum-vanadium-iron master alloy prepared in control group 5

[0136]

[0137] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.

Claims

1. A method for reducing oxidation of a master alloy produced by thermite process, It is characterized in that include: Step 1: After the reaction of producing the master alloy by the aluminothermic method is completed, the crucible containing the master alloy liquid is kept in a static state to allow the slag and the master alloy liquid to be fully separated; Step 2: continuously introducing an inert gas into the static crucible, and after the introduction of the inert gas is completed, the crucible mouth is covered with a graphite crucible cover, so that the alloy ingot in the crucible is gradually cooled under the protection of the inert gas to prevent oxidation; Step 3: After the argon gas is introduced in step 2, the crucible is kept in a static state, and then the inert gas is continuously introduced into the crucible for multiple times at appropriate intervals to allow the alloy ingot in the crucible to be cooled to below the oxidation temperature under the protection of the inert gas, and then naturally cooled and taken out of the furnace.

2. The method for reducing oxidation of a master alloy produced by thermite process according to claim 1, It is characterized in that The standing time of the crucible in step 1 is determined as follows: the standing time of a feed amount of (1-40) kg is (1-(feed amount kg / 20+2)) min; the standing time of a feed amount of (41-80) kg is (3-(feed amount kg / 20+3)) min, the standing time of a feed amount of (81-200) kg is (5-(feed amount kg / 40+4 min)), the standing time of a feed amount of (201-400) kg is (7-(feed amount kg / 40+5)) min, and the standing time of a feed amount of >400 kg is (10-(feed amount kg / 40+6)) min, wherein the integer part of the calculation result is taken each time.

3. The method for reducing oxidation of a master alloy produced by thermite process according to claim 1, It is characterized in that The time for continuously passing the inert gas in the step 2 is determined as follows: the time for passing the inert gas for a feed amount of (1-40) kg is (1-(feed amount kg / 10)) min, the time for passing the inert gas for a feed amount of (41-80) kg is (2-(feed amount kg / 10)) min, the time for passing the inert gas for a feed amount of (81-200) kg is (5-(feed amount kg / 20)) min, the time for passing the inert gas for a feed amount of (201-400) kg is (8-(feed amount kg / 20)) min, and the time for passing the inert gas for a feed amount of >400 kg is (10-(feed amount kg / 30)) min, wherein the integer part of the calculation result is taken each time.

4. The method for reducing oxidation of a master alloy produced by thermite process according to claim 1, It is characterized in that The interval time, the time of passing inert gas and the number of times of continuous passing inert gas in step 3 are determined as follows: for a feed amount of (1-40) kg, after the first passing of inert gas, the inert gas is passed again for (1-2) min at an interval of ((0.3+(feed amount kg / 80)±0.1) h, and the lid is continuously sealed after each passing, which is continued for 2 times; for a feed amount of (41-80) kg, after the first passing of inert gas, the inert gas is passed again for (1-2) min at an interval of ((0.8+(feed amount kg / 120)±0.2) h, and the lid is continuously sealed after each passing, which is continued for 3 times; for a feed amount of (81-200) kg, after the first passing of inert gas, the inert gas is passed again for (1.0+(feed amount kg / 120)±0.2) h, and the lid is continuously sealed after each passing, which is continued for 3 times. kg / 160)±0.3)h, then introduce inert gas again for (3-5) min, and continue to seal the lid after each time, for 4 times. For a feed amount of (201-400) kg, introduce inert gas again for (5-7) min every ((1.2+(feed amount kg / 200)±0.4)h after the first introduction of inert gas, and continue to seal the lid after each time, for 4 times. For a feed amount of >400 kg, introduce inert gas again for (7-10) min every ((1.4+(feed amount kg / 240)±0.5)h after the first introduction of inert gas, and continue to seal the lid after each time, for (5+((feed amount-400) kg / 280)) times, wherein the integer part of the calculation result is taken each time.

5. The method for reducing oxidation of the master alloy produced by thermite process according to claim 1, 2, 3 or 4, It is characterized in that The inert gas is argon.