High-temperature-resistant material applied to aerospace craft

By spraying a specially made corrosion inhibitor on the surface of the spacecraft material to form a protective film, the problem of corrosion in the long-term use of the spacecraft material is solved, and significant high temperature resistance and corrosion inhibition effects are achieved.

CN119082588AInactive Publication Date: 2024-12-06JIANGSU KELUWEI NEW MATERIAL TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411301208.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Spacecraft materials are susceptible to corrosion by water and inorganic salts in the air during long-term use, and the corrosion inhibition effect in the prior art has not been effectively improved.

Method used

A high temperature resistant material containing silicon, iron, copper, manganese, magnesium, zinc, titanium, cadmium, titanium dioxide and carbon steel is used, and a surface of which is sprayed is made of hexadecimal-1,15-dihydroxy octadecet The corrosion inhibitor made of compounds such as siloxane, p-toluenesulfonyl chloride, aminophenylboric acid and 1,3-propanesulfonolide forms a protective film to prevent corrosion.

Benefits of technology

The material has a complete surface after 1100℃ and 10 hours of thermal exposure, and showed a significant corrosion inhibition effect in the corrosion hanging sheet experiment at 200℃, significantly improving the high temperature and corrosion inhibition performance of the spacecraft materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of materials, and discloses a high-temperature-resistant material applied to aerospace crafts, silicon, iron, copper, manganese, magnesium, zinc, titanium, cadmium, titanium dioxide and carbon steel are added into a smelting furnace, smelting and ingot casting forming are carried out, then a corrosion inhibitor is sprayed on the surface, and the high-temperature-resistant material applied to the aerospace crafts is obtained. And a good high-temperature-resistant effect is achieved. The boron element in the corrosion inhibitor has a certain corrosion inhibition effect, siloxane and sulfonic acid groups in the boron element can be adsorbed on the surface of metal to form a protective film so as to prevent or slow down the corrosion process, and 4-aminophenylboronic acid reacts with the intermediate 2 to obtain a large amount of hydroxyl groups, so that the substitution degree of the boron element and the sulfonic acid groups is further improved, and the corrosion inhibition effect is improved. The corrosion inhibition effect is better.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of materials, and in particular to a high temperature resistant material used in aerospace vehicles. Background Art

[0002] Metal materials such as steel, iron, and aluminum alloys are widely used in aerospace, machinery manufacturing, and other fields. When cleaning the surface of metal materials, it is usually necessary to add corrosion inhibitors to the pickling solution to slow down and prevent acid corrosion on the surface of metal materials. During long-term use, aerospace materials will come into contact with water and inorganic salts in the air and cause corrosion on their surfaces. Therefore, how to avoid this phenomenon is the key to solving the problem. For example, CN111074123A discloses a method for producing 7055 alloy for aviation. The alloy has good tensile strength and electrical conductivity, but its corrosion inhibition effect is not improved. Summary of the invention

[0003] 1. Technical issues to be resolved In view of the deficiencies in the prior art, the present invention provides a high temperature resistant material for use in aerospace vehicles, which has good high temperature resistance and corrosion inhibition effects.

[0004] (II) Technical solution To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a high temperature resistant material used in aerospace vehicles, comprising the following components by weight: 3-5 parts by weight of silicon, 2-6 parts by weight of iron, 1-4 parts by weight of copper, 2-3 parts by weight of manganese, 2-4 parts by weight of magnesium, 1-2 parts by weight of zinc, 2-6 parts by weight of titanium, 1-2 parts by weight of cadmium, 1-3 parts by weight of titanium dioxide, 2-4 parts by weight of carbon steel, and 0.4-0.8 parts by weight of corrosion inhibitor.

[0005] Preferably, the preparation method of the corrosion inhibitor is: (1) Hexamethyl-1,15-dihydroxyoctasiloxane is added to N,N-dimethylformamide solvent, and then p-toluenesulfonyl chloride is added dropwise, stirred and mixed, and sodium hydroxide is added dropwise to adjust the pH of the reaction solution to 11-11.5. The reaction is carried out at 30-40°C for 3-6 hours. After the reaction, the solvent is removed by distillation under reduced pressure, and the product is washed with distilled water and acetone in sequence to obtain intermediate 1; (2) adding intermediate 1 and diethanolamine to a dichloromethane solvent, then adding a sodium carbonate catalyst, reacting at 55-70°C for 7-12 hours, and then distilling under reduced pressure to remove the solvent, and washing with distilled water and dichloromethane by centrifugation in turn to obtain intermediate 2; (3) Add 4-aminophenylboronic acid to N,N-dimethylformamide solvent, stir and disperse, continue to add intermediate 2, react at 100-120° C. for 9-14 hours, and then distill under reduced pressure, filter and dry to obtain aminophenylboronic acid modified siloxane; (4) Dissolve aminophenylboronic acid modified siloxane and 1,3-propane sultone in a 1,4-dioxane reaction solvent, then dropwise add a 4-6% by mass sodium hydroxide solution, raise the temperature to 75-90° C., react for 7-10 hours, and after the reaction, concentrate under reduced pressure to remove the solvent. The crude product is recrystallized in ethanol to obtain a corrosion inhibitor.

[0006] Preferably, the mass ratio of hexamethyl-1,15-dihydroxyoctasiloxane to p-toluenesulfonyl chloride in (1) is 1:1.6-2.2.

[0007] Preferably, the mass ratio of the intermediate 1, diethanolamine and sodium carbonate catalyst in (2) is 1.1-1.3:1:0.01-0.03.

[0008] Preferably, the mass ratio of 4-aminophenylboronic acid to intermediate 2 in (3) is 2.1-2.4:1.

[0009] Preferably, the mass ratio of aminophenylboronic acid modified siloxane to 1,3-propane sultone in (4) is 1:1.4-1.8.

[0010] Preferably, the preparation method of the high-temperature resistant material used in aerospace vehicles is: adding silicon, iron, copper, manganese, magnesium, zinc, titanium, cadmium, titanium dioxide, and carbon steel into a smelting furnace, smelting at a smelting temperature of 650-750°C, casting into ingots, and then spraying a corrosion inhibitor on the surface to obtain the high-temperature resistant material used in aerospace vehicles.

[0011] 3. Beneficial technical effects The invention adds silicon, iron, copper, manganese, magnesium, zinc, titanium, cadmium, titanium dioxide and carbon steel into a smelting furnace, smelts them, casts them into ingots, and then sprays corrosion inhibitors on the surfaces thereof to obtain high-temperature resistant materials used in aerospace vehicles, which have good high-temperature resistant effects.

[0012] Hexamethyl-1,15-dihydroxyoctasiloxane and p-toluenesulfonyl chloride are reacted to obtain intermediate 1, and intermediate 1 and diethanolamine are reacted under the action of sodium carbonate catalyst to obtain intermediate 2; 4-aminophenylboronic acid and intermediate 2 are reacted to obtain aminophenylboronic acid modified siloxane, which is further reacted with 1,3-propane sultone to obtain a corrosion inhibitor. The boron element in the corrosion inhibitor has a certain corrosion inhibition effect, and the siloxane and sulfonic acid groups therein can be adsorbed on the metal surface to form a protective film, thereby preventing or slowing down the corrosion process, and 4-aminophenylboronic acid and intermediate 2 react to obtain a large number of hydroxyl groups, which further increases the substitution degree of the boron element and the sulfonic acid group, making its corrosion inhibition effect better. DETAILED DESCRIPTION

[0013] Example 1 (1) Add hexamethyl-1,15-dihydroxyoctasiloxane to N,N-dimethylformamide solvent, then add p-toluenesulfonyl chloride dropwise, wherein the mass ratio of hexamethyl-1,15-dihydroxyoctasiloxane to p-toluenesulfonyl chloride is 1:1.6, stir and mix, continue to add sodium hydroxide dropwise, adjust the pH of the reaction solution to 11, react at 30°C for 3h, remove the solvent by distillation under reduced pressure after the reaction, wash the product with distilled water and acetone in turn, to obtain intermediate 1; (2) adding intermediate 1 and diethanolamine to a dichloromethane solvent, and then adding a sodium carbonate catalyst, wherein the mass ratio of intermediate 1, diethanolamine, and sodium carbonate catalyst is 1.1:1:0.01, reacting at 55°C for 7 hours, and after the reaction, removing the solvent by distillation under reduced pressure, and washing by centrifugation with distilled water and dichloromethane in sequence to obtain intermediate 2; (3) Add 4-aminophenylboronic acid to N,N-dimethylformamide solvent, stir and disperse, and continue to add intermediate 2, wherein the mass ratio of 4-aminophenylboronic acid to intermediate 2 is 2.1:1, react at 100° C. for 9 hours, and then perform reduced pressure distillation after the reaction, filter and dry to obtain aminophenylboronic acid modified siloxane; (4) dissolving aminophenylboronic acid modified siloxane and 1,3-propane sultone in a 1,4-dioxane reaction solvent, wherein the mass ratio of aminophenylboronic acid modified siloxane to 1,3-propane sultone is 1:1.4, then dropping a 4% sodium hydroxide solution, heating to 75°C and reacting for 7 hours, and after the reaction, concentrating under reduced pressure to remove the solvent, and recrystallizing the crude product in ethanol to obtain a corrosion inhibitor; (5) 3 parts by weight of silicon, 2 parts by weight of iron, 1 part by weight of copper, 2 parts by weight of manganese, 2 parts by weight of magnesium, 1 part by weight of zinc, 2 parts by weight of titanium, 1 part by weight of cadmium, 1 part by weight of titanium dioxide, and 2 parts by weight of carbon steel were added into a smelting furnace, smelted at a smelting temperature of 650°C, cast into an ingot, and then 0.4 parts by weight of a corrosion inhibitor was sprayed on its surface to obtain a high-temperature resistant material for aerospace vehicles. The test results show that the high-temperature resistant material prepared by this embodiment has an intact surface after being thermally exposed at 1100°C for 10 hours.

[0014] Example 2 (1) Add hexamethyl-1,15-dihydroxyoctasiloxane to N,N-dimethylformamide solvent, then add p-toluenesulfonyl chloride dropwise, wherein the mass ratio of hexamethyl-1,15-dihydroxyoctasiloxane to p-toluenesulfonyl chloride is 1:2.2, stir and mix, continue to add sodium hydroxide dropwise, adjust the pH of the reaction solution to 11.5, react at 40°C for 6h, and after the reaction, distill under reduced pressure to remove the solvent, wash the product with distilled water and acetone in turn, to obtain intermediate 1; (2) adding intermediate 1 and diethanolamine to a dichloromethane solvent, and then adding a sodium carbonate catalyst, wherein the mass ratio of intermediate 1, diethanolamine, and sodium carbonate catalyst is 1.1-1.3:1:0.03, reacting at 70°C for 12 hours, and after the reaction, removing the solvent by distillation under reduced pressure, and washing by centrifugation with distilled water and dichloromethane in sequence to obtain intermediate 2; (3) Add 4-aminophenylboronic acid to N,N-dimethylformamide solvent, stir and disperse, and continue to add intermediate 2, wherein the mass ratio of 4-aminophenylboronic acid to intermediate 2 is 2.4:1, react at 120° C. for 14 h, and then perform reduced pressure distillation after reaction, filter and dry to obtain aminophenylboronic acid modified siloxane; (4) dissolving aminophenylboronic acid modified siloxane and 1,3-propane sultone in a 1,4-dioxane reaction solvent, wherein the mass ratio of aminophenylboronic acid modified siloxane to 1,3-propane sultone is 1:1.8, then dropping a 6% sodium hydroxide solution, heating to 90°C for 10 hours, and then concentrating under reduced pressure to remove the solvent after the reaction, and the crude product is recrystallized in ethanol to obtain a corrosion inhibitor; (5) Add 5 parts by weight of silicon, 6 parts by weight of iron, 4 parts by weight of copper, 3 parts by weight of manganese, 4 parts by weight of magnesium, 2 parts by weight of zinc, 6 parts by weight of titanium, 2 parts by weight of cadmium, 3 parts by weight of titanium dioxide, and 4 parts by weight of carbon steel into a smelting furnace, smelt at a smelting temperature of 750°C, cast into an ingot, and then spray 0.8 parts by weight of a corrosion inhibitor on its surface to obtain a high-temperature resistant material for aerospace vehicles. The test results show that the high-temperature resistant material prepared by this embodiment has an intact surface after being thermally exposed at 1100°C for 10 hours.

[0015] Example 3 (1) Add hexamethyl-1,15-dihydroxyoctasiloxane to N,N-dimethylformamide solvent, then dropwise add p-toluenesulfonyl chloride, wherein the mass ratio of hexamethyl-1,15-dihydroxyoctasiloxane to p-toluenesulfonyl chloride is 1:1.9, stir and mix, continue to dropwise add sodium hydroxide, adjust the pH of the reaction solution to 11.25, react at 35°C for 4.5 hours, and after the reaction, distill under reduced pressure to remove the solvent, wash the product with distilled water and acetone in turn, to obtain intermediate 1; (2) adding intermediate 1 and diethanolamine to a dichloromethane solvent, and then adding a sodium carbonate catalyst, wherein the mass ratio of intermediate 1, diethanolamine, and sodium carbonate catalyst is 1.2:1:0.015, reacting at 60°C for 10 hours, and after the reaction, removing the solvent by distillation under reduced pressure, and washing by centrifugation with distilled water and dichloromethane in sequence to obtain intermediate 2; (3) Add 4-aminophenylboronic acid to N,N-dimethylformamide solvent, stir and disperse, and continue to add intermediate 2, wherein the mass ratio of 4-aminophenylboronic acid to intermediate 2 is 2.25:1, react at 110° C. for 11.5 hours, and then perform reduced pressure distillation after the reaction, filter and dry to obtain aminophenylboronic acid modified siloxane; (4) dissolving aminophenylboronic acid modified siloxane and 1,3-propane sultone in a 1,4-dioxane reaction solvent, wherein the mass ratio of aminophenylboronic acid modified siloxane to 1,3-propane sultone is 1:1.6, then dropping a 5% by mass sodium hydroxide solution, heating to 80° C. and reacting for 8.5 hours, and after the reaction, concentrating under reduced pressure to remove the solvent, and the crude product is recrystallized in ethanol to obtain a corrosion inhibitor; (5) 4 parts by weight of silicon, 4 parts by weight of iron, 2.5 parts by weight of copper, 2 parts by weight of manganese, 3 parts by weight of magnesium, 1.5 parts by weight of zinc, 5 parts by weight of titanium, 1.5 parts by weight of cadmium, 2 parts by weight of titanium dioxide, and 3 parts by weight of carbon steel are added to a smelting furnace, smelted at a smelting temperature of 700°C, cast into an ingot, and then 0.6 parts by weight of a corrosion inhibitor is sprayed on the surface thereof to obtain a high-temperature resistant material for aerospace vehicles. The test results show that the high-temperature resistant material prepared by this embodiment has an intact surface after being thermally exposed at 1100°C for 10 hours.

[0016] Example 4 (1) Add hexamethyl-1,15-dihydroxyoctasiloxane to N,N-dimethylformamide solvent, then add p-toluenesulfonyl chloride dropwise, wherein the mass ratio of hexamethyl-1,15-dihydroxyoctasiloxane to p-toluenesulfonyl chloride is 1:1.6, stir and mix, continue to add sodium hydroxide dropwise, adjust the pH of the reaction solution to 11, react at 30°C for 3h, remove the solvent by distillation under reduced pressure after the reaction, wash the product with distilled water and acetone in turn, to obtain intermediate 1; (2) adding intermediate 1 and diethanolamine to a dichloromethane solvent, and then adding a sodium carbonate catalyst, wherein the mass ratio of intermediate 1, diethanolamine, and sodium carbonate catalyst is 1.1:1:0.01, reacting at 55°C for 7 hours, and after the reaction, removing the solvent by distillation under reduced pressure, and washing by centrifugation with distilled water and dichloromethane in sequence to obtain intermediate 2; (3) Add 4-aminophenylboronic acid to N,N-dimethylformamide solvent, stir and disperse, and continue to add intermediate 2, wherein the mass ratio of 4-aminophenylboronic acid to intermediate 2 is 2.4:1, react at 120° C. for 14 h, and then perform reduced pressure distillation after reaction, filter and dry to obtain aminophenylboronic acid modified siloxane; (4) dissolving aminophenylboronic acid modified siloxane and 1,3-propane sultone in a 1,4-dioxane reaction solvent, wherein the mass ratio of aminophenylboronic acid modified siloxane to 1,3-propane sultone is 1:1.8, then dropping a 6% sodium hydroxide solution, heating to 90°C for 10 hours, and then concentrating under reduced pressure to remove the solvent after the reaction, and the crude product is recrystallized in ethanol to obtain a corrosion inhibitor; (5) 4 parts by weight of silicon, 4 parts by weight of iron, 2.5 parts by weight of copper, 2 parts by weight of manganese, 3 parts by weight of magnesium, 1.5 parts by weight of zinc, 5 parts by weight of titanium, 1.5 parts by weight of cadmium, 2 parts by weight of titanium dioxide, and 3 parts by weight of carbon steel are added to a smelting furnace, smelted at a smelting temperature of 700°C, cast into an ingot, and then 0.6 parts by weight of a corrosion inhibitor is sprayed on the surface thereof to obtain a high-temperature resistant material for aerospace vehicles. The test results show that the high-temperature resistant material prepared by this embodiment has an intact surface after being thermally exposed at 1100°C for 10 hours.

[0017] Comparative Example 1 4 parts by weight of silicon, 4 parts by weight of iron, 2.5 parts by weight of copper, 2 parts by weight of manganese, 3 parts by weight of magnesium, 1.5 parts by weight of zinc, 5 parts by weight of titanium, 1.5 parts by weight of cadmium, 2 parts by weight of titanium dioxide, and 3 parts by weight of carbon steel are added to a smelting furnace, smelted at a smelting temperature of 700°C, and ingots are formed to obtain a high-temperature resistant material for aerospace vehicles. The test results show that the high-temperature resistant material prepared by this embodiment has an intact surface after being thermally exposed at 1100°C for 10 hours.

[0018] Determination of the corrosion inhibition performance of the corrosion inhibitor: Using 20% ​​hydrochloric acid as the corrosive medium and the high temperature resistant material of the aerospace vehicle, the corrosion inhibition performance of Examples 1-4 and Comparative Example 1 was determined by a 4h corrosion coupon test at 200°C. The amount of corrosion inhibitor used was 1000ppm. The results are shown in Table 1.

[0019] It can be seen from Table 1 that Examples 1-4 of the present invention have better corrosion inhibition effects than Comparative Example 1.

[0020] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A high temperature resistant material used in aerospace vehicles, characterized in that: It includes the following components by weight: 3-5 parts by weight of silicon, 2-6 parts by weight of iron, 1-4 parts by weight of copper, 2-3 parts by weight of manganese, 2-4 parts by weight of magnesium, 1-2 parts by weight of zinc, 2-6 parts by weight of titanium, 1-2 parts by weight of cadmium, 1-3 parts by weight of titanium dioxide, 2-4 parts by weight of carbon steel, and 0.4-0.8 parts by weight of corrosion inhibitor.

2. The high temperature resistant material for aerospace vehicles according to claim 1, characterized in that: The preparation method of the corrosion inhibitor is: (1) Hexamethyl-1,15-dihydroxyoctasiloxane is added to N,N-dimethylformamide solvent, and then p-toluenesulfonyl chloride is added dropwise, stirred and mixed, and sodium hydroxide is added dropwise to adjust the pH of the reaction solution to 11-11.

5. The reaction is carried out at 30-40°C for 3-6 hours. After the reaction, the solvent is removed by distillation under reduced pressure, and the product is washed with distilled water and acetone in sequence to obtain intermediate 1; (2) adding intermediate 1 and diethanolamine to a dichloromethane solvent, then adding a sodium carbonate catalyst, reacting at 55-70°C for 7-12 hours, and then distilling under reduced pressure to remove the solvent, and washing with distilled water and dichloromethane by centrifugation in turn to obtain intermediate 2; (3) Add 4-aminophenylboronic acid to N,N-dimethylformamide solvent, stir and disperse, continue to add intermediate 2, react at 100-120° C. for 9-14 hours, and then distill under reduced pressure, filter and dry to obtain aminophenylboronic acid modified siloxane; (4) Dissolve aminophenylboronic acid modified siloxane and 1,3-propane sultone in a 1,4-dioxane reaction solvent, then dropwise add a 4-6% by mass sodium hydroxide solution, raise the temperature to 75-90° C., react for 7-10 hours, and after the reaction, concentrate under reduced pressure to remove the solvent. The crude product is recrystallized in ethanol to obtain a corrosion inhibitor.

3. The high temperature resistant material for aerospace vehicles according to claim 2, characterized in that: The mass ratio of hexadecyl-1,15-dihydroxyoctasiloxane to p-toluenesulfonyl chloride in (1) is 1:1.6-2.

2.

4. The high temperature resistant material for aerospace vehicles according to claim 2, characterized in that: The mass ratio of the intermediate 1, diethanolamine and sodium carbonate catalyst in (2) is 1.1-1.3:1:0.01-0.

03.

5. The high temperature resistant material for aerospace vehicles according to claim 2, characterized in that: The mass ratio of 4-aminophenylboronic acid to intermediate 2 in (3) is 2.1-2.4:

1.

6. The high temperature resistant material for aerospace vehicles according to claim 2, characterized in that: The mass ratio of aminophenylboronic acid modified siloxane to 1,3-propane sultone in (4) is 1:1.4-1.

8.

7. A high temperature resistant material for use in aerospace vehicles according to any one of claims 1 to 6, characterized in that: The preparation method of the high-temperature resistant material used in aerospace vehicles is as follows: silicon, iron, copper, manganese, magnesium, zinc, titanium, cadmium, titanium dioxide, and carbon steel are added into a smelting furnace, smelted at a smelting temperature of 650-750° C., ingot-shaped, and then a corrosion inhibitor is sprayed on the surface thereof to obtain the high-temperature resistant material used in aerospace vehicles.

Citation Information

Patent Citations

  • Sulfonate functional organopolysiloxanes

    CN101080435A

  • Comb-shaped modified polysiloxane anion water-base thick oil viscosity reducer and synthesizing method thereof

    CN102516972A

  • Fireproof flame-retardant coating for surface of plastic part

    CN113004781A

  • Acidifying corrosion inhibitor and preparation method thereof

    CN118421294A

  • Heat-resistant lithium ion battery diaphragm and preparation method thereof