Aluminum-titanium-tin-zirconium-molybdenum-silicon six-element intermediate alloy and preparation method and application thereof

Through the six-member intermediate alloy and self-propagation process of aluminum, titanium, tin, zirconium, molybdenum, silicon, and silicon, the difficulty and segregation problems of binary intermediate alloys in large-scale titanium alloy ingots are solved, and the performance stability and composition uniformity of titanium alloys are achieved, satisfying industrialization Production demand.

CN119082589APending Publication Date: 2024-12-06BAOJI ZHONGSE SPECIAL METAL CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411235121.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

When preparing large-scale titanium alloy ingots, the composition control is difficult and easy to cause segregation and inclusion, resulting in unstable performance of titanium alloys and unable to meet the needs of industrial production.

Method used

The six-membered intermediate alloy of aluminum, titanium, tin, zirconium, molybdenum, silicon is used to control the impurity content through specific ratios and self-propagation processes, ensure the stable performance of the aluminum, titanium, tin, zirconium, molybdenum intermediate alloy, improve the degree of titanium alloy, and reduce component segregation.

Benefits of technology

It effectively improves the performance of Ti-180 and TA19 titanium alloys, ensures the uniformity and stability of components, and meets the industrial production requirements of large-scale ingots.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082589A_ABST
    Figure CN119082589A_ABST
Patent Text Reader

Abstract

The invention discloses an aluminum-titanium-tin-zirconium-molybdenum-silicon six-element intermediate alloy as well as a preparation method and application thereof. The aluminum-titanium-tin-zirconium-molybdenum-silicon six-element intermediate alloy comprises the following components in percentage by weight: 11%-15% of titanium, 13%-16% of tin, 27%-30% of zirconium, 13%-16% of molybdenum and 0.04%-0.06% of silicon. And the balance of aluminum and inevitable impurity elements. The aluminum-titanium-tin-zirconium-molybdenum-silicon hexabasic intermediate alloy is designed and is suitable for preparation of titanium alloys such as Ti-180 and TiA19, the performance stability of the aluminum-titanium-tin-zirconium-molybdenum-silicon intermediate alloy is ensured by strictly controlling the impurity content and adopting a self-propagating process, the alloying degree of the Ti-180 and TiA19 is effectively improved, and composition segregation and inclusion are prevented, so that the performance of the Ti-180 and TiA19 titanium alloys is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of master alloy preparation, and in particular relates to an aluminum-titanium-tin-zirconium-molybdenum-silicon hexametal master alloy, a preparation method and application thereof. Background Art

[0002] Adding a master alloy with uniform composition is the key to improving the metallurgical quality of titanium alloys. This method has been widely used in the industrial production of titanium alloys. The elements Al, Mo, Sn, Si, Zr and other elements in titanium alloys such as Ti-180 and TA19 are added in the form of Al-60Mo master alloy, Al-37Sn master alloy, Al-11Si master alloy and sponge zirconium respectively; among which sponge zirconium has a high melting point and high density; Al-37Sn master alloy is easy to absorb moisture and increase oxygen; Al-60Mo master alloy has a large reaction heat effect and poor quality stability; these unfavorable factors brought by single and binary master alloys increase the difficulty of controlling the chemical composition of titanium alloy ingots such as Ti-180 and TA19. At the same time, it is easy to produce serious metallurgical defects such as segregation and inclusions, which seriously restricts the preparation of Ti-180 and TA19 titanium alloy ingots, especially large-size ingots, which cannot meet the subsequent titanium material performance. At present, the extreme values ​​of Al, Sn, Mo, Zr, Si and other elements of Φ720mm Ti-180 titanium alloy ingots produced by binary master alloys are controlled at 0.4%, 0.3%, 0.4%, 0.3% and 0.03% respectively. The extreme values ​​of Al, Sn, Mo, Zr, Si and other elements of Φ820mm TA19 titanium alloy ingots produced by binary master alloys are controlled at 0.4%, 0.3%, 0.4%, 0.4% and 0.04% respectively. The subsequent processed Ti-180 and TA19 bars also have relatively more β-spot problems due to local segregation of components. The alloying method of high-melting-point elements, the control of impurity elements in large-sized industrial-grade ingots, and the expansion of specifications (≥Φ820mm) that aggravates segregation elements all restrict the production of large-sized ingots. At present, it is only in the trial production stage and cannot be industrialized.

[0003] In view of this, it is necessary to provide a new master alloy to solve the technical problem of large-size ingot production. Summary of the invention

[0004] In order to solve the above problems existing in the prior art, the present invention provides an aluminum-titanium-tin-zirconium-molybdenum-silicon hexavalent master alloy, a preparation method and its application. The technical problem to be solved by the present invention is achieved by the following technical solutions:

[0005] The invention discloses an aluminum-titanium-tin-zirconium-molybdenum-silicon hexa-element master alloy, which comprises the following components in weight percentage: titanium: 11%-15%, tin: 13%-16%, zirconium: 27%-30%, molybdenum: 13%-16%, silicon: 0.04%-0.06%; the balance is aluminum and unavoidable impurity elements.

[0006] Another embodiment of the present invention provides a method for preparing the above-mentioned aluminum-titanium-tin-zirconium-molybdenum-silicon hexavalent master alloy, comprising:

[0007] Step 1: Mix the heating agent, aluminum powder, titanium dioxide, tin dioxide, zirconium dioxide, molybdenum trioxide, industrial silicon and slag-forming agent according to the following weight percentages: titanium dioxide: 6.23%-8.56%, tin dioxide: 5.49%-7.09%, zirconium dioxide: 14.42-16.46%, molybdenum trioxide: 6.54%-8.15%, industrial silicon: 0.01%-0.02%, heating agent: 16.49%-17.61%, slag-forming agent: 16.49%-17.61%, and the balance is aluminum powder;

[0008] Step 2: putting the uniformly mixed materials into a reaction container, compacting them and then igniting them, controlling the reaction calorific value to be between 605 and 630 kcal / kg, and after the reaction is completed, cooling the alloy liquid to obtain an aluminum-titanium-tin-zirconium-molybdenum-silicon ingot;

[0009] Step 3: crushing and finishing the aluminum-titanium-tin-zirconium-molybdenum-silicon ingot to obtain the aluminum-titanium-tin-zirconium-molybdenum-silicon hexavalent master alloy.

[0010] Furthermore, the exothermic agent is potassium chlorate; and the slag-forming agent is calcium fluoride.

[0011] Furthermore, before step 1, the titanium dioxide, tin dioxide, zirconium dioxide, molybdenum trioxide, industrial silicon and slag-forming agent are first dried at a temperature of 80 to 120° C. for a drying time of 10 to 20 hours.

[0012] Furthermore, before step 1, the titanium dioxide, the heating agent, the tin dioxide and the zirconium dioxide are first passed through a 2.0×2.0 sieve.

[0013] Furthermore, in step 2, the slag temperature is controlled to be 1630-1710°C.

[0014] Another embodiment of the present invention provides a use of the above-mentioned aluminum-titanium-tin-zirconium-molybdenum-silicon hexavalent master alloy in the preparation of TA19 material.

[0015] Beneficial effects of the present invention:

[0016] 1. The present invention designs an aluminum-titanium-tin-zirconium-molybdenum-silicon hexavalent master alloy, which is suitable for the preparation of titanium alloys such as Ti-180 and TA19. By strictly controlling the impurity content and adopting a self-propagating process, the performance of the aluminum-titanium-tin-zirconium-molybdenum-silicon master alloy is ensured to be stable, the alloying degree of Ti-180 and TA19 is effectively improved, and component segregation and inclusion are prevented, thereby improving the performance of Ti-180 and TA19 titanium alloys.

[0017] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is a schematic diagram of longitudinal sampling of TA19 titanium alloy ingot;

[0019] Figure 2 This is a schematic diagram of transverse sampling of TA19 titanium alloy ingot;

[0020] Figure 3 This is the main element composition distribution diagram of the TA19 titanium alloy ingot in the longitudinal direction;

[0021] Figure 4 Schematic diagram of the lateral main element distribution of TA19 titanium alloy ingot. DETAILED DESCRIPTION

[0022] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments, but the embodiments of the present invention are not limited thereto.

[0023] Example 1: This example provides an aluminum-titanium-tin-zirconium-molybdenum-silicon hexa-element master alloy, which includes the following components in weight percentage: titanium: 11%-15%, tin: 13%-16%, zirconium: 27%-30%, molybdenum: 13%-16%, silicon: 0.04%-0.06%; the remainder is aluminum and unavoidable impurity elements.

[0024] Since ZrO 2 Can be used with Al 2 O 3 , MgO and other oxides with similar properties to form solid solutions or compounds. 2 With Al 2 O 3 As can be seen from the phase diagram, the two can easily form ZrO 2 With Al 2 O 3 Compound or solid solution. This makes ZrO 2 Not all of the ZrO was reduced by Al, and some of the ZrO did not participate in the reaction. 2 Will be with Al 2 O 3The solid solution or compound is formed, resulting in a low Zr element in the alloy. Therefore, the aluminum-titanium-tin-zirconium-molybdenum-silicon hexavalent master alloy provided by the present invention is increased by ZrO 2 By adding an amount of zirconium, an aluminum-titanium-tin-zirconium-molybdenum-silicon master alloy with stable zirconium element and meeting the requirements is obtained.

[0025] Embodiment 2: The embodiment of the present invention provides a method for preparing a hexameric master alloy of aluminum, titanium, tin, zirconium, molybdenum and silicon, which specifically comprises:

[0026] Step 1: Select raw materials of potassium chlorate, aluminum powder, titanium dioxide, tin dioxide, zirconium dioxide, molybdenum trioxide, industrial silicon and calcium fluoride, first dry the titanium dioxide, tin dioxide, zirconium dioxide, molybdenum trioxide, industrial silicon and calcium fluoride, the drying temperature is 80°C, the drying time is 20h, and the titanium dioxide, potassium chlorate, tin dioxide and zirconium dioxide are passed through a 2.0×2.0 sieve to facilitate full reaction.

[0027] Step 2: Weigh 16.64 kg potassium chlorate, 26.94 kg aluminum powder, 8.33 kg titanium dioxide, 5.49 kg tin dioxide, 15.73 kg zirconium dioxide, 7.99 kg molybdenum trioxide, 0.02 kg industrial silicon and 18.87 kg calcium fluoride and mix well.

[0028] Step 3: Then put the mixed materials into the reaction crucible and press them tightly before igniting, so that the materials in the crucible undergo a self-propagating reaction. At the same time, the reaction calorific value is controlled at 605-630 kcal / kg, and the slag temperature is controlled at 1650°C, so that the molten slag formed during the reaction continuously transfers heat to the alloy liquid, prolongs the solidification time of the alloy liquid, increases the self-diffusion time of chromium and aluminum elements in the alloy liquid, and makes the alloy composition more uniform. When casting titanium alloy, it can effectively improve the alloying degree of Ti-180 and TA19, and effectively reduce Less alloy component segregation, improve the performance of titanium alloys such as Ti-180 and TA19; after the reaction is completed, the alloy liquid is cooled to obtain a titanium, tin, zirconium, molybdenum and silicon ingot, the weight of the obtained ingot is 30.28kg, of which the aluminum content accounts for 27.84% of the ingot weight, the titanium content accounts for 14.36% of the ingot weight, the tin content accounts for 13.68% of the ingot weight, the zirconium content accounts for 29.48% of the ingot weight, the molybdenum content accounts for 15.39% of the ingot weight, and the silicon content accounts for 0.05% of the ingot weight.

[0029] Step 4: crushing and finishing the aluminum-titanium-tin-zirconium-molybdenum-silicon ingot to obtain the aluminum-titanium-tin-zirconium-molybdenum-silicon hexavalent master alloy.

[0030] Embodiment 3: This embodiment provides a method for preparing an aluminum-titanium-tin-zirconium-molybdenum-silicon hexavalent master alloy, which specifically includes:

[0031] Step 1: Select raw materials of potassium chlorate, aluminum powder, titanium dioxide, tin dioxide, zirconium dioxide, molybdenum trioxide, industrial silicon and calcium fluoride, first dry the titanium dioxide, tin dioxide, zirconium dioxide, molybdenum trioxide, industrial silicon and calcium fluoride, the drying temperature is 120°C, the drying time is 10 hours, and the titanium dioxide, potassium chlorate, tin dioxide and zirconium dioxide are passed through a 2.0×2.0 sieve to facilitate full reaction.

[0032] Step 2: Weigh 8.80 kg potassium chlorate, 14.98 kg aluminum powder, 3.23 kg titanium dioxide, 2.90 kg tin dioxide, 7.62 kg zirconium dioxide, 3.44 kg molybdenum trioxide, 0.02 kg industrial silicon and 9.01 kg calcium fluoride and mix well.

[0033] Step 3: Then put the mixed materials into the reaction crucible and press them tightly before igniting, so that the materials in the crucible undergo a self-propagating reaction. At the same time, the reaction calorific value is controlled at 605-630 kcal / kg, and the slag temperature is controlled at 1710°C, so that the molten slag formed during the reaction can continuously transfer heat to the alloy liquid, prolong the solidification time of the alloy liquid, increase the self-diffusion time of chromium and aluminum elements in the alloy liquid, and make the alloy composition more uniform. When casting titanium alloy, it can effectively improve the alloying degree of Ti-180 and TA19, and effectively reduce The alloy components are segregated to improve the performance of titanium alloys such as Ti-180 and TA19; after the reaction is completed, the alloy liquid is cooled to obtain a titanium-tin-zirconium-molybdenum-silicon hexa-alloy ingot, and the weight of the obtained ingot is 32.80 kg, of which the aluminum content accounts for 33.37% of the ingot weight, the titanium content accounts for 11.26% of the ingot weight, the tin content accounts for 13.22% of the ingot weight, the zirconium content accounts for 28.32% of the ingot weight, the molybdenum content accounts for 13.78% of the ingot weight, and the silicon content accounts for 0.05% of the ingot weight.

[0034] Step 4: crushing and finishing the aluminum-titanium-tin-zirconium-molybdenum-silicon hexa-element master alloy ingot to obtain the aluminum-titanium-tin-zirconium-molybdenum-silicon hexa-element master alloy.

[0035] Example 4: This example discloses a process of using the aluminum-titanium-tin-zirconium-molybdenum-silicon hexavalent master alloy prepared in the above examples 2 to 3 to prepare TA19 titanium alloy. Specifically,

[0036] Step 1: Calculate the weight of the aluminum-titanium-tin-zirconium-molybdenum-silicon master alloy to be added based on the weight of the TA19 alloy and the contents of Al, Mo, Sn, Zr and Si elements.

[0037] The weight percentage of each element in the TA19 alloy is Al: 5.5% to 6.5%, Mo: 1.8% to 2.2%, Sn: 1.8% to 2.2%, Zr: 3.6% to 4.4%, Si: 0.05% to 0.12%, O: 0.05% to 0.15%, and the balance is Ti and unavoidable impurities; the content of impurity elements does not exceed 0.3%, and the sum of the weight percentages of the above components is 100%; among them, the contents of Al, Mo, Sn, Zr, and Si are basically composed of aluminum, titanium, tin, zirconium, molybdenum, and silicon intermediates. Gold is added. If the content of a certain element is insufficient, it is supplemented by Al-60Mo, Al-37Sn, Al-11Si, sponge zirconium and aluminum beans. According to the amount of TA19 alloy to be prepared, the required amount of intermediate alloy is weighed, and a single electrode is mixed with a corresponding weight of small-particle sponge titanium with a particle size of 0.83mm to 12.7mm, and a large hydraulic press is used to press it into a large single-weight electrode block. The O element in the electrode block is brought by the raw material, such as sponge titanium. When the O element brought by the raw material cannot meet the ratio, TiO 2 Adjust the oxygen content.

[0038] Step 2: The pressed electrode block is welded into a consumable electrode by argon plasma arc welding in a vacuum welding box. The welding current is 250A~600A, the welding voltage is 30V~70V, and the weld point is required to be silvery white or light yellow to prevent metallurgical defects such as weld point oxidation and high-density inclusions.

[0039] Step 3: The consumable electrode obtained in step 2 is vacuum melted three times in a vacuum consumable arc furnace to obtain a Φ820 mm ingot. The specific melting parameters are as follows:

[0040] Primary smelting: crucible specification Φ650mm, vacuum degree before melting ≤3.0Pa, gas leakage rate ≤1.1Pa / min, smelting voltage 25V~38V, smelting current 15kA~20kA, arc stabilization current DC 10.0~15.0A, cooling time 7.0h;

[0041] Secondary smelting: crucible specification Φ750mm, vacuum degree before melting ≤2.0Pa, leakage rate ≤0.93Pa / min, smelting voltage 25V~40V, smelting current 25kA~30kA, arc stabilization current DC 10.0~15.0A, cooling time 8.0h;

[0042] Three smeltings: crucible specification Φ820mm, vacuum degree before melting ≤2.0Pa, leakage rate ≤0.93Pa / min, smelting voltage 25V~40V, smelting current 24kA~35kA, arc stabilization current AC 5.0~10.0A / 5~10S, cooling time 10.0h, and a TA19 titanium alloy ingot with a specification of Φ820mm is obtained.

[0043] like Figure 1 and Figure 2 As shown in the figure, the TA19 titanium alloy 6.5-ton industrial ingot with a specification of Φ820 mm was sampled at 5 points in the longitudinal direction, including the head, top, middle, bottom, and tail, and 13 points in the cross section, and the chemical composition was tested. The data are shown in Tables 1, 2, and Figures 1-2 , indicating that the element composition distribution uniformity of each part of the ingot is good. From the test results, it can be seen that the Ti-6242 titanium alloy industrial-grade large ingot produced by the smelting process technology of the present invention has uniform composition.

[0044] Table 1 Chemical composition analysis results of each element in the longitudinal direction of TA19 titanium alloy ingot with a size of Φ820mm

[0045]

[0046] Table 2 Chemical composition analysis results of each element in the transverse direction of TA19 titanium alloy ingot with a size of Φ820 mm

[0047]

[0048]

[0049] From Table 1, Table 2, Figure 1-2 It can be seen that the main composition and impurity element analysis results of the Φ820mm, 6.5t TA19 titanium alloy ingot prepared based on the aluminum-titanium-tin-zirconium-molybdenum-silicon hexavalent master alloy all meet the standard requirements, with a small overall deviation, good ingot composition uniformity, and a small range of main elements.

[0050] Comparative Example 1: This comparative example adopts the same production process route and smelting process as Example 4, but uses binary alloys such as Al-Mo, Al-Sn, Al-Si and pure alloy additives such as sponge zirconium and aluminum beans to produce TA19 titanium alloy with a specification of Φ820mm. The chemical composition of the TA19 titanium alloy is shown in Table 3 and Table 4:

[0051] Table 3 Chemical composition analysis results of each element in the longitudinal direction of TA19 titanium alloy ingot produced by binary alloy (in the table, T represents the head and B represents the tail)

[0052]

[0053]

[0054]

[0055] Table 4 Chemical composition analysis results of each element in the transverse direction of TA19 titanium alloy ingot produced by binary alloy

[0056]

[0057] It can be seen from Tables 3 and 4 that the chemical composition and impurity element analysis results of Φ820mm TA19 titanium alloy produced based on binary alloys such as Al-Mo, Al-Sn, Ti-Sn and pure alloy additives such as sponge zirconium and Al beans meet the standard requirements, but there are certain deviations in the composition, as shown in Tables 5 and 6:

[0058] Table 5 Comparison of longitudinal element deviations of TA19 titanium alloy ingots produced by hexa-alloy and binary alloy

[0059]

[0060] Table 6 Comparison of lateral element deviations of TA19 titanium alloy ingots produced by hexa-alloy and binary alloy

[0061]

[0062] It can be seen from this that the hexameric master alloy of TA19 titanium alloy prepared using the hexameric master alloy of aluminum, titanium, tin, zirconium, molybdenum and silicon has a uniform composition and a low content of impurity elements, which fully meets the composition control requirements of TA19 alloy.

[0063] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.

Claims

1. A hexavalent master alloy of aluminum, titanium, tin, zirconium, molybdenum and silicon, It is characterized in that The aluminum-titanium-tin-zirconium-molybdenum-silicon hexavalent master alloy includes the following components in weight percentage: titanium: 11%-15%, tin: 13%-16%, zirconium: 27%-30%, molybdenum: 13%-16%, silicon: 0.04%-0.06%; the remainder is aluminum and inevitable impurity elements.

2. A method for preparing the aluminum-titanium-tin-zirconium-molybdenum-silicon hexavalent master alloy as claimed in claim 1, It is characterized in that include: Step 1: Mix the heating agent, aluminum powder, titanium dioxide, tin dioxide, zirconium dioxide, molybdenum trioxide, industrial silicon and slag-forming agent according to the following weight percentages: titanium dioxide: 6.23%-8.56%, tin dioxide: 5.49%-7.09%, zirconium dioxide: 14.42-16.46%, molybdenum trioxide: 6.54%-8.15%, industrial silicon: 0.01%-0.02%, heating agent: 16.49%-17.61%, slag-forming agent: 16.49%-17.61%, and the balance is aluminum powder; Step 2: putting the uniformly mixed materials into a reaction container, compacting them and then igniting them, controlling the reaction calorific value to be between 605 and 630 kcal / kg, and after the reaction is completed, cooling the alloy liquid to obtain an aluminum-titanium-tin-zirconium-molybdenum-silicon ingot; Step 3: crushing and finishing the aluminum-titanium-tin-zirconium-molybdenum-silicon ingot to obtain the aluminum-titanium-tin-zirconium-molybdenum-silicon hexavalent master alloy.

3. The method for preparing the aluminum-titanium-tin-zirconium-molybdenum-silicon hexavalent master alloy according to claim 2, It is characterized in that The exothermic agent is potassium chlorate; the slag-forming agent is calcium fluoride.

4. The method for preparing the aluminum-titanium-tin-zirconium-molybdenum-silicon hexavalent master alloy according to claim 2, It is characterized in that Before step 1, the titanium dioxide, tin dioxide, zirconium dioxide, molybdenum trioxide, industrial silicon and slag-forming agent are first dried at a temperature of 80 to 120° C. for a drying time of 10 to 20 hours.

5. The method for preparing the titanium-tin-zirconium-molybdenum-silicon hexavalent master alloy according to claim 2, It is characterized in that Before step 1, the titanium dioxide, the heating agent, the tin dioxide and the zirconium dioxide are first passed through a 2.0×2.0 sieve.

6. The method for preparing the aluminum-titanium-tin-zirconium-molybdenum-silicon hexavalent master alloy according to claim 2, It is characterized in that In step 2, the slag temperature is controlled to be 1630-1710°C.

7. Use of the aluminum-titanium-tin-zirconium-molybdenum-silicon hexavalent master alloy according to claim 1 in the preparation of TA19 material.

Citation Information

Cited By

  • Aluminum-titanium-zirconium-molybdenum-tin quinary intermediate alloy and preparation method thereof as well as preparation method of titanium alloy cast ingot

    CN120464928A

  • Aluminum-titanium-zirconium-molybdenum-tin quinary intermediate alloy, preparation method thereof and preparation method of titanium alloy ingot