Construction forming method suitable for aluminum alloy deformation part
By combining the conventional homogenization annealing and hot press diffusion connection process of aluminum alloy, the interface oxide film of aluminum alloy material is transformed into nano-scale particle phase, solving the problem of low performance caused by the oxide film of aluminum alloy material during the construction and forming process, achieving high Massive aluminum alloy forgings forming.
Patent Information
- Application Number
- CN202411205290.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-30
AI Technical Summary
During the construction and forming process, aluminum alloy materials have low performance due to the large size of the interface oxide film, which cannot meet the needs of high strength and corrosion resistance, especially in large-sized key structural parts, the quality is difficult to guarantee.
The conventional homogenization annealing process of aluminum alloy is combined with the hot pressing and diffusion connection process. The oxide film is crushed by high temperature and short-term hot pressing and undergoes secondary homogenization annealing, and the oxide film is transformed into a nano-scale particle phase to achieve high-quality connection. Specific steps include the first stage homogenization annealing, the hot press diffusion connection, the second stage homogenization annealing and plastic forming.
Effectively control the number and size of the interface oxide film, significantly improve the performance of aluminum alloy materials, and ensure the quality and performance stability of subsequent deformation processing.
Smart Images

Figure CN119082628A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of metal material preparation, and relates to a construction forming method suitable for aluminum alloy deformed parts, and specifically, to a processing method for realizing deformation forming of aluminum alloy materials by construction. Background Art
[0002] Aluminum alloy has become one of the most outstanding metals in industrial development due to its advantages of low density, high strength, good comprehensive performance and excellent plasticity. It is also widely used in the automotive, aviation and electronic communications industries. The advancement of science and technology and the continuous development of industry have put forward higher requirements for the aluminum alloy materials used, such as high strength, corrosion resistance and low qualified rate. Especially for large-sized aluminum alloy key structural parts, the quality is difficult to guarantee and the uniformity of organizational performance is difficult to control.
[0003] The metal construction forming technology uses the idea of "using small to make big" to process multiple homogenized slabs through surface processing, cleaning, stacking and vacuum packaging, and then applies a deformation connection process characterized by pressure-maintaining forging and multi-directional forging at high temperature. This not only achieves a "seamless" connection with a completely consistent interface and substrate, but also improves the productivity and yield of the product.
[0004] Compared with the construction and forming technology of stainless steel and alloy steel, aluminum alloy has a low melting point and it is difficult to effectively decompose the aluminum oxide film with high thermal stability and high density. It is necessary to develop construction and forming technology suitable for aluminum alloy products to solve the problem of oxide film on the surface of aluminum alloy. Summary of the invention
[0005] The purpose of the present invention is to provide a construction and forming method suitable for aluminum alloy deformed parts to solve the problems existing in the above-mentioned prior art, and to effectively solve the problem of low performance of the constructed and formed products and inability to be applied due to the excessive size of the interface oxide film.
[0006] To achieve the above object, the present invention provides the following solutions:
[0007] A method for forming and constructing aluminum alloy deformed parts, which uses the time of the conventional homogenization annealing process of aluminum alloy to match the hot pressing diffusion bonding process, effectively controls the number and size of the interface oxide film, achieves high-quality connection, and meets the subsequent deformation requirements. Specifically, it includes the following steps:
[0008] In the first step, a plurality of small-volume homogeneous aluminum alloy elements are prepared using the aluminum alloy in the cast state, and a first-stage homogenization annealing treatment is performed, wherein the annealing treatment time is t1.
[0009] In the second step, multiple homogeneous aluminum alloy elements after annealing are stacked into a predetermined shape to make a preform.
[0010] The third step is to place the preform in a hot press and heat it at high temperature (T 热压 ), short-time (t2), low deformation (δ) hot pressing and heat preservation diffusion bonding, through heat preservation and pressure holding, the surface oxide film of the aluminum alloy element is quickly broken, and the interface is initially healed to form a whole, so as to obtain a pre-deformed billet.
[0011] In the fourth step, the pre-deformed blank after heat preservation is placed in a heat treatment furnace for a long time (t3) of secondary homogenization annealing to decompose the broken oxide film into a finer nano-scale particle phase.
[0012] The fifth step is to plastically form the annealed pre-deformed billet to complete the final construction and obtain high-quality aluminum alloy forgings.
[0013] Furthermore, the aluminum alloy element should be a casting billet that has not undergone any heat treatment, and the aluminum alloy is a deformable aluminum alloy such as 2 series, 5 series, 6 series and 7 series, and other aluminum alloy metal materials that can be used for building and forming. These materials are usually deformable alloys and are used to prepare various forgings, rolled parts or extruded parts. The shape of the aluminum alloy element is usually a cuboid or a cylinder.
[0014] Furthermore, the first stage homogenization time t1 ≥ 1h is used to ensure the stress relief annealing effect of the ingot during the homogenization process. This time should not be too long, and sufficient time should be left for the hot pressing process and the post-heat treatment process. Generally, it should not exceed 0.5t 均 , t 均 In order to select the conventional homogenization annealing time of aluminum alloy,.
[0015] Furthermore, the element stacking refers to arranging a plurality of aluminum alloy elements into multiple layers to form a preform, each layer including one element.
[0016] Furthermore, the shape of the preform is based on the deformation process requirements of the specific aluminum alloy product.
[0017] Furthermore, the hot pressing heating temperature T 热压 , is one of the key factors affecting the decomposition of the aluminum alloy oxide film. The temperature should be as high as possible, but not exceeding the solid solution temperature of the alloy. Therefore, the hot pressing temperature range must meet, T 固 >T 热压 ≥0.95T 固 , T 固 The solid solution temperature of the aluminum alloy material is selected in °C. Usually, this temperature can be directly selected as the homogenization annealing temperature.
[0018] Furthermore, the hot pressing time t2 is one of the keys to ensure the decomposition of the oxide film. Generally, a long time is required, usually t2 ≥ 1h. However, in order to leave enough time for the subsequent secondary homogenization annealing, t2 should not exceed 0.2t. 均 .
[0019] Furthermore, the deformation refers to the need to plastically deform the preform under a certain pressure during the hot pressing process in order to achieve the initial physical breaking of the oxide film. Usually, the holding pressure P≥1MPa. Because it is not within a reasonable aluminum alloy deformation temperature range, the deformation of the aluminum alloy needs to be controlled to δ≤20%.
[0020] Furthermore, the sealing welding means that under non-vacuum hot pressing conditions, the contact surfaces formed by stacking must be vacuum packaged and welded to ensure that no air remains between the contacts of each aluminum alloy element and there is no air leakage during subsequent hot pressing and heat treatment.
[0021] Furthermore, the secondary homogenization annealing refers to taking out the pre-deformed sample after the hot pressing is completed and placing it in a conventional heat treatment furnace for homogenization annealing. The homogenization annealing time t3≥t 均 -t1-t2, the total time of homogenization annealing cannot be less than t 均 .
[0022] The beneficial effects of the present invention are as follows:
[0023] The present invention utilizes a high-temperature, short-time hot-pressing diffusion process to quickly break up the oxide film and allow it to interact with the second phase on the interface, and then utilizes a secondary homogenization annealing treatment to further refine the oxide and transform it into a nano-scale particle phase, thereby significantly reducing the influence of the interface oxide film on the use, and can be directly used in subsequent deformation processing to produce the desired product. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 Schematic diagram of preparing preform for aluminum alloy element;
[0025] Figure 2 This is the oxide morphology and organization diagram of the interface of the aluminum alloy pre-deformed billet after hot pressing and diffusion bonding;
[0026] Figure 3 This is the interface oxide morphology and organization diagram of the aluminum alloy pre-deformed billet after the second homogenization annealing. DETAILED DESCRIPTION
[0027] The present invention is further described below in conjunction with specific implementation cases.
[0028] This embodiment selects 2219 aluminum alloy for forging. Four 2219 aluminum alloy cast primitives with a size of Φ100mm××30mm are selected. The conventional homogenization annealing temperature of the alloy is 540℃ / 24h. Therefore, the first homogenization annealing selects a heat treatment process of 540℃ / 6h to heat and keep warm in a heat treatment furnace. After completion, it is taken out and air-cooled and combined into two preforms with one interface.
[0029] The two preforms were subjected to hot pressing diffusion bonding experiments in a vacuum hot pressing device. Figure 1 The aluminum alloy element is pressed in the Z-axis direction as shown in the schematic diagram of the preform, and the pressure is 5 MPa. The hot pressing and holding temperature is the same as the homogenization annealing temperature, which is 540°C, and the total holding time is 2 hours. The deformation is controlled by the die to be 20%.
[0030] After the diffusion bonding is completed, two pre-deformed blanks are obtained. One of the pre-deformed blanks is put into the heat treatment furnace again, kept at 540℃ for 16h, and then the sample is taken out and air-cooled. For the sample after hot pressing diffusion and the sample after secondary homogenization annealing, the interface position is cut by double-beam focused ion beam (FIB) for transmission microscope (TEM) observation.
[0031] Figure 2 This is the interface structure feature of the aluminum alloy pre-deformed billet after hot pressing and diffusion bonding. It can be seen from the figure that there are long white oxide particles wrapped by the gray second phase at the interface, and the length of the oxide phase is about 1μm. Figure 3 This is the interface structure feature of the aluminum alloy pre-deformed billet after secondary homogenization annealing. It can be seen from the figure that the gray second phase at the interface disappears in large quantities, and no obvious white oxide particle phase is found in the residual phase. At the same time, a small amount of 100-200nm scale white particle phase is found at the grain boundary. Obviously, the oxide film of the sample after hot pressing diffusion bonding and secondary homogenization annealing has been greatly eliminated, which provides an important guarantee for the subsequent deformation process and performance stability.
[0032] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for forming a deformed aluminum alloy part, characterized in that: The construction forming method comprises the following steps: The first step is to prepare a plurality of small-volume homogeneous aluminum alloy primitives that have been subjected to the first stage homogenization annealing treatment, wherein the annealing treatment time is t1; The second step is to stack the annealed homogeneous aluminum alloy primitives into a predetermined shape to make a preform; The third step is to place the preform in a hot pressing device and perform hot pressing, heat preservation and diffusion bonding at high temperature, short time and low deformation to make the interface heal to form a whole and obtain a pre-deformed blank; wherein the high temperature is T 热压 , the short-term time is t2, and the deformation is δ; The fourth step is to place the pre-deformed blank after heat preservation in a heat treatment furnace for a long time of secondary homogenization annealing, wherein the secondary homogenization annealing time is t3; The fifth step is to plastically form the annealed pre-deformed billet to complete the final construction and obtain high-quality aluminum alloy forgings.
2. A method for forming aluminum alloy deformed parts according to claim 1, characterized in that: The aluminum alloy element is an uncast billet, and the aluminum alloy is a 2 series, 5 series, 6 series and 7 series deformed aluminum alloy and other aluminum alloy metal materials that can be used for construction and forming.
3. A method for forming aluminum alloy deformed parts according to claim 1, characterized in that: The first stage homogenization time t1 ≥ 1h and does not exceed 0.5t 均 , t 均 The conventional homogenization annealing time for aluminum alloy is selected.
4. A method for forming aluminum alloy deformed parts according to claim 1, characterized in that: The element stacking mentioned above refers to arranging a plurality of aluminum alloy elements into multiple layers to form a preform, each layer including one element.
5. The method for forming an aluminum alloy deformed part according to claim 1, characterized in that: The hot pressing heating temperature T 热压 Satisfied, T 固 >T 热压 ≥0.95T 固 , T 固 It is the solution temperature of the selected aluminum alloy material.
6. The method for forming an aluminum alloy deformed part according to claim 1, characterized in that: The hot pressing time t2 is ≥ 1h, and t2 does not exceed 0.2t 均 .
7. A method for forming aluminum alloy deformed parts according to claim 1, characterized in that: During the hot pressing process, it is necessary to maintain the pressure, the pressure P≥1MPa, and at the same time control the deformation amount δ of the aluminum alloy to be ≤20%.
8. The method for forming an aluminum alloy deformed part according to claim 1, characterized in that: The aluminum alloy can be hot pressed and diffusion bonded under non-vacuum or vacuum conditions.
9. A method for forming and constructing an aluminum alloy deformed part according to claim 8, characterized in that: When the aluminum alloy is subjected to hot pressing diffusion bonding under non-vacuum conditions, the preform needs to be subjected to vacuum sealing welding.
10. A method for forming aluminum alloy deformed parts according to claim 1, characterized in that: The secondary homogenization annealing time t3≥t 均 -t1-t2.
Citation Information
Patent Citations
Thermal coupling method for metal solid-solid composite additive blank manufacturing
CN112643300A
Multi-layer metal cold deformation building forming method
CN113695502A
Pre-connection method for constructing base material interface
CN115846843A
Method for preparing large-size high-entropy alloy by constructing small high-quality blank
CN116921835A
Manufacturing method of high-purity and high-homogeneity nuclear power pressure vessel
CN117340543A