Aluminum-magnesium-silicon alloy target material as well as preparation method and application thereof
Through the multi-step process of preheating, forging, rolling, hot isostatic pressure treatment and thermal insulation treatment of aluminum-magnesium silicon alloy, the problem of insufficient purity and grain fineness of aluminum-magnesium silicon alloy target materials in the prior art is solved. The preparation of high purity and fine uniform grains is achieved, meeting the high-quality requirements of the semiconductor industry.
Patent Information
- Application Number
- CN202411191407.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
AI Technical Summary
The prior art is difficult to prepare aluminum-magnesium silicon alloy targets with high purity, fine grains and defect-free internal defects, which cannot meet the high-quality requirements of the semiconductor industry for metal interconnection lines.
Preheating and forging by aluminum-magnesium silicon alloy ingots, preheating and rolling, followed by hot isostatic pressure treatment, followed by preheating and insulation treatment, and finally leveling and machine adding, controlling hot isostatic pressure Conditional parameters for treatment and insulation treatment to obtain high purity and fine uniform grains.
The high purity and fine uniform grains of aluminum-magnesium silicon alloy targets are achieved, and the internal defect-free preparation is met, which meets the high-quality requirements of the semiconductor industry for targets, and improves the operability and material yield of the preparation method.
Smart Images

Figure BDA0005015213220000121 
Figure BDA0005015213220000131
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of material processing, and in particular relates to an aluminum-magnesium-silicon alloy target material and a preparation method and application thereof. Background Art
[0002] The rapid development and increasing integration of semiconductor integrated circuits (ICs) have further increased the quality requirements for metal interconnects. As the primary supporting material for metal interconnects in IC manufacturing, the market for ultra-high-purity aluminum alloy targets is expanding. The quality of sputtering targets plays a crucial role in the performance of metal thin film materials. Pure aluminum interconnects have poor resistance to electromigration, stress migration, and chemical corrosion. Adding a certain amount of silicon to high-purity aluminum can improve the interconnect's resistance to electromigration and stress migration, increase the recrystallization temperature, and enhance the interconnect's hardness.
[0003] Al-Mg-Si alloys are pure aluminum alloys with small amounts of magnesium and silicon added. They offer advantages such as high strength, low density, and excellent heat dissipation, making them widely used in electronics, automotive, aerospace, and other fields. Therefore, developing an Al-Mg-Si alloy target that meets the semiconductor industry's sputtering target requirements has become a research hotspot. Summary of the Invention
[0004] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide an aluminum-magnesium-silicon alloy target material with a simple preparation process, high purity, small and uniform grain size and no internal defects, as well as a preparation method and application thereof.
[0005] To achieve the above objectives, in a first aspect of the present invention, the present invention provides a method for preparing an aluminum-magnesium-silicon alloy target, the preparation method comprising the following steps:
[0006] (1) Preheating the aluminum-magnesium-silicon alloy ingot to 450-600°C and then forging it, and then water cooling it after forging;
[0007] (2) preheating the workpiece after water cooling in step (1) for a second time, rolling it once after the second preheating, and air cooling it after the first rolling;
[0008] (3) performing hot isostatic pressing on the workpiece after air cooling in step (2); the hot isostatic pressing is performed at a temperature of 450-550° C., a time of 3-5 hours, and a pressure of 130-150 MPa;
[0009] (4) preheating the workpiece after hot isostatic pressing in step (3) three times, rolling it twice after the three preheatings, and air cooling it after the second rolling;
[0010] (5) keeping the workpiece after air cooling in step (4) at 300-400° C. for 60-120 min, and then air cooling;
[0011] (6) The workpiece after air cooling in step (5) is leveled and machined, and then bound with a backing plate to obtain an aluminum-magnesium-silicon alloy target.
[0012] The present invention provides a method for preparing an aluminum-magnesium-silicon alloy target material, which comprises the following steps: preheating an aluminum-magnesium-silicon alloy ingot and then forging it, preheating and rolling it after forging, then performing hot isostatic pressing, and then sequentially performing preheating and rolling and heat preservation treatment, and finally leveling and machining; at the same time, the present invention also controls the condition parameters of the hot isostatic pressing treatment and the heat preservation treatment, thereby effectively obtaining an aluminum-magnesium-silicon alloy target material with fine and uniform grains, high purity and few defects; and the preparation method of the aluminum-magnesium-silicon alloy target material provided by the present invention has strong operability and repeatability and a high yield rate.
[0013] Exemplarily, the temperature of the hot isostatic pressing treatment may be any point value or any two point range values between 450-550°C, for example, 450°C, 460°C, 470°C, 480°C, 490°C, 500°C, 510°C, 520°C, 530°C, 540°C, 550°C, etc.; the time may be any point value or any two point range values between 3-5h, for example, 3h, 3.5h, 4h, 4.5h, 5h, etc.; the pressure may be any point value or any two point range values between 130-150MPa, for example, 130MPa, 132MPa, 134MPa, 136MPa, 138MPa, 140MPa, 142MPa, 144MPa, 146MPa, 148MPa, 150MPa, etc.
[0014] Exemplarily, the temperature of the primary preheating may be any point value or any two point range values between 450-600°C, such as 450°C, 460°C, 470°C, 480°C, 490°C, 500°C, 510°C, 520°C, 530°C, 540°C, 550°C, 560°C, 570°C, 580°C, 590°C, 600°C, etc.
[0015] As a preferred embodiment of the preparation method of the present invention, the preparation method of the aluminum-magnesium-silicon alloy ingot is as follows: after mixing the raw materials, the mixture is heated under a vacuum degree of less than 10 -3 The aluminum-magnesium-silicon alloy ingot is obtained by vacuum melting for 30-60 minutes at a temperature of 700-850°C and then casting. The ingot is taken out from the mold after cooling.
[0016] The proportion of raw materials used in the preparation of the aluminum-silicon-magnesium alloy ingot of the present invention can be adjusted according to actual requirements.
[0017] Preferably, after cooling and taking out from the mold, the workpiece is further subjected to operations of cutting the head and tail, removing shrinkage holes and peeling, and finally obtaining an aluminum-magnesium-silicon alloy ingot.
[0018] As a preferred embodiment of the preparation method of the present invention, in the step (1), the preheating time is 60-120 minutes.
[0019] Exemplarily, the preheating time may be any point value or any two point range values between 60-120 minutes, such as 60 minutes, 70 minutes, 80 minutes, 90 minutes, 100 minutes, 110 minutes, 120 minutes, etc.
[0020] The present invention has found that subsequent forging can be more effectively performed within the preheating temperature and time range given by the present invention, which is conducive to achieving the corresponding deformation rate in a shorter time and avoiding cracking caused by long-term forging and causing internal defects.
[0021] As a preferred embodiment of the preparation method of the present invention, in the step (1), the forging adopts a roughing and drawing method, which is repeated 2-4 times, and the deformation rate each time is 60-80%.
[0022] The present invention has found that adopting the method of upsetting and drawing for forging and controlling the deformation rate at 60-80% each time can effectively refine the grains, thereby obtaining products with fine and uniform grains, and at the same time can help reduce internal defects of the products.
[0023] As a preferred embodiment of the preparation method of the present invention, in the step (2), the secondary preheating temperature is 450-550° C. and the time is 60-120 min.
[0024] Exemplarily, the temperature of the secondary preheating may be any point value or any two point range values between 450-550°C, such as 450°C, 460°C, 470°C, 480°C, 490°C, 500°C, 510°C, 520°C, 530°C, 540°C, 550°C, etc.; the time of the secondary preheating may be any point value or any two point range values between 60-120min, such as 60min, 70min, 80min, 90min, 100min, 110min, 120min, etc.
[0025] The present invention has found that preheating within the above-mentioned temperature and time range before a rolling operation can further help to refine the grains during the rolling process and improve the uniformity of the grain distribution.
[0026] As a preferred embodiment of the preparation method of the present invention, in the step (2), the deformation rate of one rolling is 45-55%, and the deformation rate of a single rolling is 0.5-1.5 mm.
[0027] The present invention has found that by controlling the deformation rate of each rolling pass to 45-55% and the thickness of each rolling pass to 0.5-1.5 mm, defects can be avoided while achieving grain refinement, thereby helping to achieve products with fine and uniform grains, no internal defects and high purity.
[0028] Preferably, the steel is melted down between each rolling pass at a temperature of 450-550°C for 30-40 minutes. The melt-down treatment can better achieve grain refinement during the rolling process and avoid the generation of internal defects.
[0029] As a preferred embodiment of the preparation method of the present invention, in the step (4), the temperature of the three preheatings is 450-550° C. and the time is 60-120 min.
[0030] As a preferred embodiment of the preparation method of the present invention, in the step (4), the deformation rate of the secondary rolling is 60-80%, and the deformation rate of a single pass is 0.5-1.0 mm.
[0031] The present invention has found that further preheating three times within the above parameter range after hot isostatic pressing and secondary rolling after the three preheatings can further refine the grains and reduce internal defects of the product.
[0032] As a preferred embodiment of the preparation method of the present invention, in the step (6), the flatness after leveling is less than 0.5 mm.
[0033] As a preferred embodiment of the preparation method of the present invention, in step (6), the backplane includes any one of an aluminum backplane and a copper backplane.
[0034] In a second aspect of the present invention, the present invention provides an aluminum-magnesium-silicon alloy target material, which is prepared by the preparation method of the present invention.
[0035] As a preferred embodiment of the aluminum-magnesium-silicon alloy target material of the present invention, the aluminum-magnesium-silicon alloy target material has a grain size of ≤100 μm and a purity of ≥99.995%. The aluminum-magnesium-silicon alloy target material comprises 0.45-0.55% silicon by atomic weight, 0.09-0.11% magnesium by atomic weight, and the remainder being aluminum and trace unavoidable impurities.
[0036] The aluminum-magnesium-silicon alloy target provided by the present invention has excellent grain distribution uniformity and small grain size, and is high in purity and free of internal defects, thus meeting the requirements for target sputtering in the semiconductor industry.
[0037] In a third aspect of the present invention, the present invention provides a use of the aluminum-magnesium-silicon alloy target in preparing thin film deposition materials.
[0038] Compared with the prior art, the present invention has the following beneficial effects:
[0039] The present invention provides a method for preparing an aluminum-magnesium-silicon alloy target material, which comprises the following steps: preheating an aluminum-magnesium-silicon alloy ingot and then forging it, preheating and rolling it after forging, then performing hot isostatic pressing, and then sequentially performing preheating and rolling and heat preservation treatment, and finally leveling and machining; at the same time, the present invention also controls the condition parameters of the hot isostatic pressing treatment and the heat preservation treatment, thereby effectively obtaining an aluminum-magnesium-silicon alloy target material with fine and uniform grains, high purity and no internal defects; and the preparation method of the aluminum-magnesium-silicon alloy target material provided by the present invention has strong operability and repeatability and a high yield rate. DETAILED DESCRIPTION
[0040] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.
[0041] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0042] Example 1
[0043] An embodiment of the present invention provides an aluminum-magnesium-silicon alloy target material. A method for preparing the aluminum-magnesium-silicon alloy target material comprises the following steps:
[0044] (1) Mix silicon, magnesium and aluminum and place them in a vacuum of 10 -4 Pa, vacuum melting for 45 minutes under the conditions of melting temperature of 800℃, then selecting a suitable mold for casting, taking it out from the mold after cooling, cutting the head and tail, removing shrinkage holes and peeling, then reversely calculating the blanking size according to the finished product size, and cutting it using a horizontal sawing machine to obtain an aluminum-magnesium-silicon alloy ingot;
[0045] (2) preheating the aluminum-magnesium-silicon alloy ingot in step (1) in a box-type annealing furnace at a temperature of 500° C. for 90 min; then taking it out and performing free forging by using an air hammer, and performing free forging by upsetting and drawing, repeating the process three times, with a deformation rate of 70% each time, and water cooling after forging;
[0046] (3) The workpiece after water cooling in step (2) is preheated for a second time in a box-type annealing furnace at a temperature of 500°C for 90 minutes; then, a rolling process is started with a single pass of 1 mm, during which the workpiece is repeatedly returned to the furnace at a temperature of 500°C for 30 minutes, with the deformation rate of the first rolling controlled at 50%, and air-cooled after the rolling process is completed;
[0047] (4) subjecting the workpiece after air cooling in step (3) to hot isostatic pressing, wherein the conditions for hot isostatic pressing are: temperature of 500° C., time of 4 h, and pressure of 140 MPa;
[0048] (5) preheating the workpiece after hot isostatic pressing in step (4) three times at a temperature of 500°C and a time of 90 minutes; then starting secondary rolling with a single pass of 0.8 mm, repeatedly returning to the furnace during the process at a temperature of 500°C and a time of 30 minutes, controlling the secondary rolling deformation rate to 70%, and air cooling after rolling;
[0049] (6) The workpiece after air cooling in step (5) was kept at 350° C. for 90 min, and then air cooled;
[0050] (7) The workpiece after air cooling in step (6) is leveled to a flatness of 0.3 mm, then machined, and then bound with an aluminum backing plate to obtain a finished product to obtain an aluminum-magnesium-silicon alloy target;
[0051] The obtained aluminum-silicon-magnesium alloy target material has a silicon atomic mass percentage of 0.5%, a magnesium atomic mass percentage of 0.1%, and the rest being aluminum and inevitable trace impurity elements.
[0052] Example 2
[0053] An embodiment of the present invention provides an aluminum-magnesium-silicon alloy target material. A method for preparing the aluminum-magnesium-silicon alloy target material comprises the following steps:
[0054] (1) Mix silicon, magnesium and aluminum and place them in a vacuum of 10 -4 Pa, vacuum melting for 30 minutes under the conditions of melting temperature of 800℃, then selecting a suitable mold for casting, taking it out from the mold after cooling, cutting the head and tail, removing shrinkage holes and peeling, then reversely calculating the blanking size according to the finished product size, and cutting it using a horizontal sawing machine to obtain an aluminum-magnesium-silicon alloy ingot;
[0055] (2) preheating the aluminum-magnesium-silicon alloy ingot in step (1) in a box-type annealing furnace at a temperature of 450° C. for 120 min; then taking it out and performing free forging by using an air hammer, performing free forging by upsetting and drawing, repeating the process 4 times, with a deformation rate of 60% each time, and water cooling after forging;
[0056] (3) The workpiece after water cooling in step (2) is preheated for a second time in a box-type annealing furnace at a temperature of 450°C for 120 min; then, a rolling process is started with a single pass of 0.5 mm, and the workpiece is repeatedly returned to the furnace at a temperature of 450°C for 30 min. The deformation rate of the first rolling is controlled to be 50%, and air cooling is performed after the rolling process is completed;
[0057] (4) subjecting the workpiece after air cooling in step (3) to hot isostatic pressing, wherein the conditions for hot isostatic pressing are: temperature 450° C., time 5 h, and pressure 150 MPa;
[0058] (5) preheating the workpiece after hot isostatic pressing in step (4) three times at a temperature of 450°C and a time of 120 min; then starting secondary rolling with a single pass of 0.5 mm, repeatedly returning to the furnace during the process at a temperature of 450°C and a time of 30 min, controlling the secondary rolling deformation rate to 60%, and air cooling after rolling;
[0059] (6) The workpiece after air cooling in step (5) was placed at 300°C for 120 minutes and then air cooled;
[0060] (7) The workpiece after air cooling in step (6) is leveled to a flatness of 0.3 mm, then machined, and then bound with an aluminum backing plate to obtain a finished product to obtain an aluminum-magnesium-silicon alloy target;
[0061] The obtained aluminum-silicon-magnesium alloy target material has a silicon atomic mass percentage of 0.45%, a magnesium atomic mass percentage of 0.11%, and the rest being aluminum and inevitable trace impurity elements.
[0062] Example 3
[0063] An embodiment of the present invention provides an aluminum-magnesium-silicon alloy target material. A method for preparing the aluminum-magnesium-silicon alloy target material comprises the following steps:
[0064] (1) Mix silicon, magnesium and aluminum and place them in a vacuum of 10 -4 Pa, vacuum melting for 60 minutes under the conditions of melting temperature of 800℃, then selecting a suitable mold for casting, taking it out from the mold after cooling, cutting the head and tail, removing shrinkage holes and peeling, then reversely calculating the blanking size according to the finished product size, and cutting it using a horizontal sawing machine to obtain an aluminum-magnesium-silicon alloy ingot;
[0065] (2) preheating the aluminum-magnesium-silicon alloy ingot in step (1) in a box-type annealing furnace at a temperature of 550° C. for 60 min; then taking it out and performing free forging by using an air hammer, performing free forging by upsetting and drawing, repeating the process twice, with a deformation rate of 80% each time, and water cooling after forging;
[0066] (3) The workpiece after water cooling in step (2) is preheated for a second time in a box-type annealing furnace at a temperature of 550° C. for 60 min; then, a rolling process is started with a single pass of 1.5 mm, and the workpiece is repeatedly returned to the furnace at a temperature of 550° C. for 30 min. The deformation rate of the first rolling is controlled to be 50%, and air cooling is performed after the rolling process is completed;
[0067] (4) subjecting the workpiece after air cooling in step (3) to hot isostatic pressing, wherein the conditions for hot isostatic pressing are: temperature of 550° C., time of 3 h, and pressure of 130 MPa;
[0068] (5) preheating the workpiece after hot isostatic pressing in step (4) three times at a temperature of 550° C. and a time of 60 min; then starting secondary rolling with a single pass of 1.0 mm, repeatedly returning to the furnace during the process at a temperature of 550° C. and a time of 30 min, controlling the secondary rolling deformation rate to 80%, and air cooling after rolling;
[0069] (6) The workpiece after air cooling in step (5) was placed at 400° C. for 60 min, and then air cooled;
[0070] (7) The workpiece after air cooling in step (6) is leveled to a flatness of 0.3 mm, then machined, and then bound with an aluminum backing plate to obtain a finished product to obtain an aluminum-magnesium-silicon alloy target;
[0071] The obtained aluminum-silicon-magnesium alloy target material has a silicon atomic mass percentage of 0.55%, a magnesium atomic mass percentage of 0.09%, and the rest being aluminum and inevitable trace impurity elements.
[0072] Example 4
[0073] An embodiment of the present invention provides an aluminum-magnesium-silicon alloy target material. The only difference between the preparation method of the aluminum-magnesium-silicon alloy target material and that of Example 1 is that the preheating temperature in step (2) is 600°C.
[0074] Example 5
[0075] An embodiment of the present invention provides an aluminum-magnesium-silicon alloy target material. The only difference between the preparation method of the aluminum-magnesium-silicon alloy target material and that of Example 1 is that the one-time rolling deformation rate in step (3) is 40%.
[0076] Example 6
[0077] An embodiment of the present invention provides an aluminum-magnesium-silicon alloy target material. The only difference between the preparation method of the aluminum-magnesium-silicon alloy target material and that of Example 1 is that the one-time rolling deformation rate in step (3) is 60%.
[0078] Comparative Example 1
[0079] The comparative example of the present invention provides an aluminum-magnesium-silicon alloy target. The preparation method of the aluminum-magnesium-silicon alloy target differs from that of Example 1 in that there is no preheating and no forging after preheating. Specifically, the method is as follows:
[0080] (1) Mix silicon, magnesium and aluminum and place them in a vacuum of 10 -4Pa, vacuum melting for 45 minutes under the conditions of melting temperature of 800℃, then selecting a suitable mold for casting, taking it out from the mold after cooling, cutting the head and tail, removing shrinkage holes and peeling, then reversely calculating the blanking size according to the finished product size, and cutting it using a horizontal sawing machine to obtain an aluminum-magnesium-silicon alloy ingot;
[0081] (2) The aluminum-magnesium-silicon alloy ingot prepared in step (1) is subjected to a secondary preheating process in a box-type annealing furnace at a temperature of 500° C. and a time of 90 min; then, a primary rolling process is started with a single pass of 1 mm, during which the ingot is repeatedly returned to the furnace at a temperature of 500° C. and a time of 30 min, with the primary rolling deformation rate controlled at 50%, and air-cooled after the rolling process is completed;
[0082] (3) subjecting the workpiece after air cooling in step (2) to hot isostatic pressing, wherein the conditions for hot isostatic pressing are: temperature of 500° C., time of 4 h, and pressure of 140 MPa;
[0083] (4) preheating the workpiece after hot isostatic pressing in step (3) three times at a temperature of 500° C. and a time of 90 min; then starting secondary rolling with a single pass of 0.8 mm, repeatedly returning to the furnace during the process at a temperature of 500° C. and a time of 30 min, controlling the secondary rolling deformation rate to 70%, and air cooling after rolling;
[0084] (5) The workpiece after air cooling in step (4) was placed at 350° C. for 90 minutes and then air cooled;
[0085] (6) The workpiece after air cooling in step (5) is leveled to a flatness of 0.3 mm, then machined, and then bound with an aluminum back plate to obtain a finished product to obtain an aluminum-magnesium-silicon alloy target.
[0086] Comparative Example 2
[0087] The comparative example of the present invention provides an aluminum-magnesium-silicon alloy target. The preparation method of the aluminum-magnesium-silicon alloy target differs from that of Example 1 in that no hot isostatic pressing treatment is performed. Specifically, the method is as follows:
[0088] (1) Mix silicon, magnesium and aluminum and place them in a vacuum of 10 -4 Pa, vacuum melting for 45 minutes under the conditions of melting temperature of 800℃, then selecting a suitable mold for casting, taking it out from the mold after cooling, cutting the head and tail, removing shrinkage holes and peeling, then reversely calculating the blanking size according to the finished product size, and cutting it using a horizontal sawing machine to obtain an aluminum-magnesium-silicon alloy ingot;
[0089] (2) preheating the aluminum-magnesium-silicon alloy ingot in step (1) in a box-type annealing furnace at a temperature of 500° C. for 90 min; then taking it out and performing free forging by using an air hammer, and performing free forging by upsetting and drawing, repeating the process three times, with a deformation rate of 70% each time, and water cooling after forging;
[0090] (3) The workpiece after water cooling in step (2) is preheated for a second time in a box-type annealing furnace at a temperature of 500°C for 90 minutes; then, a rolling process is started with a single pass of 1 mm, during which the workpiece is repeatedly returned to the furnace at a temperature of 500°C for 30 minutes, with the deformation rate of the first rolling controlled at 50%, and air-cooled after the rolling process is completed;
[0091] (4) preheating the workpiece after air cooling in step (3) three times at a temperature of 500°C for 90 minutes; then starting secondary rolling with a single pass of 0.8 mm, repeatedly returning to the furnace during the process at a temperature of 500°C for 30 minutes, controlling the secondary rolling deformation rate to 70%, and air cooling after rolling;
[0092] (5) The workpiece after air cooling in step (4) was placed at 350° C. for 90 minutes and then air cooled;
[0093] (6) The workpiece after air cooling in step (5) is leveled to a flatness of 0.3 mm, then machined, and then bound with an aluminum back plate to obtain a finished product to obtain an aluminum-magnesium-silicon alloy target.
[0094] Comparative Example 3
[0095] The comparative example of the present invention provides an aluminum-magnesium-silicon alloy target material. The preparation method of the aluminum-magnesium-silicon alloy target material differs from that of Example 1 in that there is no secondary preheating and primary rolling. Specifically, the method is as follows:
[0096] (1) Mix silicon, magnesium and aluminum and place them in a vacuum of 10 -4 Pa, vacuum melting for 45 minutes under the conditions of melting temperature of 800℃, then selecting a suitable mold for casting, taking it out from the mold after cooling, cutting the head and tail, removing shrinkage holes and peeling, then reversely calculating the blanking size according to the finished product size, and cutting it using a horizontal sawing machine to obtain an aluminum-magnesium-silicon alloy ingot;
[0097] (2) preheating the aluminum-magnesium-silicon alloy ingot in step (1) in a box-type annealing furnace at a temperature of 500° C. for 90 min; then taking it out and performing free forging by using an air hammer, and performing free forging by upsetting and drawing, repeating the process three times, with a deformation rate of 70% each time, and water cooling after forging;
[0098] (3) subjecting the workpiece after water cooling in step (2) to hot isostatic pressing, wherein the conditions for hot isostatic pressing are: temperature of 500° C., time of 4 h, and pressure of 140 MPa;
[0099] (4) preheating the workpiece after hot isostatic pressing in step (3) three times at a temperature of 500° C. and a time of 90 min; then starting secondary rolling with a single pass of 0.8 mm, repeatedly returning to the furnace during the process at a temperature of 500° C. and a time of 30 min, controlling the secondary rolling deformation rate to 70%, and air cooling after rolling;
[0100] (5) The workpiece after air cooling in step (4) was placed at 350° C. for 90 minutes and then air cooled;
[0101] (6) The workpiece after air cooling in step (5) is leveled to a flatness of 0.3 mm, then machined, and then bound with an aluminum back plate to obtain a finished product to obtain an aluminum-magnesium-silicon alloy target.
[0102] Comparative Example 4
[0103] The comparative example of the present invention provides an aluminum-magnesium-silicon alloy target material. The preparation method of the aluminum-magnesium-silicon alloy target material differs from that of Example 1 in that there is no three preheating and two rolling. Specifically, the method is as follows:
[0104] (1) Mix silicon, magnesium and aluminum and place them in a vacuum of 10 -4 Pa, vacuum melting for 45 minutes under the conditions of melting temperature of 800℃, then selecting a suitable mold for casting, taking it out from the mold after cooling, cutting the head and tail, removing shrinkage holes and peeling, then reversely calculating the blanking size according to the finished product size, and cutting it using a horizontal sawing machine to obtain an aluminum-magnesium-silicon alloy ingot;
[0105] (2) preheating the aluminum-magnesium-silicon alloy ingot in step (1) in a box-type annealing furnace at a temperature of 500° C. for 90 min; then taking it out and performing free forging by using an air hammer, and performing free forging by upsetting and drawing, repeating the process three times, with a deformation rate of 70% each time, and water cooling after forging;
[0106] (3) The workpiece after water cooling in step (2) is preheated for a second time in a box-type annealing furnace at a temperature of 500°C for 90 minutes; then, a rolling process is started with a single pass of 1 mm, during which the workpiece is repeatedly returned to the furnace at a temperature of 500°C for 30 minutes, with the deformation rate of the first rolling controlled at 50%, and air-cooled after the rolling process is completed;
[0107] (4) subjecting the workpiece after air cooling in step (3) to hot isostatic pressing, wherein the conditions for hot isostatic pressing are: temperature of 500° C., time of 4 h, and pressure of 140 MPa;
[0108] (5) placing the workpiece after hot isostatic pressing in step (4) at 350° C. for 90 minutes, followed by air cooling;
[0109] (6) The workpiece after air cooling in step (5) is leveled to a flatness of 0.3 mm, then machined, and then bound with an aluminum back plate to obtain a finished product to obtain an aluminum-magnesium-silicon alloy target.
[0110] Comparative Example 5
[0111] The comparative example of the present invention provides an aluminum-magnesium-silicon alloy target material. The preparation method of the aluminum-magnesium-silicon alloy target material differs from that of Example 1 in that there is no heat preservation process. Specifically, the method is as follows:
[0112] (1) Mix silicon, magnesium and aluminum and place them in a vacuum of 10 -4 Pa, vacuum melting for 45 minutes under the conditions of melting temperature of 800℃, then selecting a suitable mold for casting, taking it out from the mold after cooling, cutting the head and tail, removing shrinkage holes and peeling, then reversely calculating the blanking size according to the finished product size, and cutting it using a horizontal sawing machine to obtain an aluminum-magnesium-silicon alloy ingot;
[0113] (2) preheating the aluminum-magnesium-silicon alloy ingot in step (1) in a box-type annealing furnace at a temperature of 500° C. for 90 min; then taking it out and performing free forging by using an air hammer, and performing free forging by upsetting and drawing, repeating the process three times, with a deformation rate of 70% each time, and water cooling after forging;
[0114] (3) The workpiece after water cooling in step (2) is preheated for a second time in a box-type annealing furnace at a temperature of 500°C for 90 minutes; then, a rolling process is started with a single pass of 1 mm, during which the workpiece is repeatedly returned to the furnace at a temperature of 500°C for 30 minutes, with the deformation rate of the first rolling controlled at 50%, and air-cooled after the rolling process is completed;
[0115] (4) subjecting the workpiece after air cooling in step (3) to hot isostatic pressing, wherein the conditions for hot isostatic pressing are: temperature of 500° C., time of 4 h, and pressure of 140 MPa;
[0116] (5) preheating the workpiece after hot isostatic pressing in step (4) three times at a temperature of 500°C and a time of 90 minutes; then starting secondary rolling with a single pass of 0.8 mm, repeatedly returning to the furnace during the process at a temperature of 500°C and a time of 30 minutes, controlling the secondary rolling deformation rate to 70%, and air cooling after rolling;
[0117] (6) The workpiece after air cooling in step (5) is leveled to a flatness of 0.3 mm, then machined, and then bound with an aluminum back plate to obtain a finished product to obtain an aluminum-magnesium-silicon alloy target.
[0118] Comparative Example 6
[0119] The comparative example of the present invention provides an aluminum-magnesium-silicon alloy target material. The only difference between the preparation method of the aluminum-magnesium-silicon alloy target material and that of Example 1 is that the temperature of the first preheating in step (2) is 400°C.
[0120] Comparative Example 7
[0121] The comparative example of the present invention provides an aluminum-magnesium-silicon alloy target material. The only difference between the preparation method of the aluminum-magnesium-silicon alloy target material and that of Example 1 is that the pressure of the hot isostatic pressing treatment in step (4) is 100 MPa.
[0122] Comparative Example 8
[0123] The comparative example of the present invention provides an aluminum-magnesium-silicon alloy target material. The only difference between the preparation method of the aluminum-magnesium-silicon alloy target material and that of Example 1 is that the hot isostatic pressing treatment time in step (4) is 1 hour.
[0124] Comparative Example 9
[0125] The comparative example of the present invention provides an aluminum-magnesium-silicon alloy target material. The only difference between the preparation method of the aluminum-magnesium-silicon alloy target material and that of Example 1 is that in step (6), the target material is kept at 200° C. for 90 minutes.
[0126] Comparative Example 10
[0127] The comparative example of the present invention provides an aluminum-magnesium-silicon alloy target material. The only difference between the preparation method of the aluminum-magnesium-silicon alloy target material and that of Example 1 is that in step (6), the target material is kept at 500° C. for 90 minutes.
[0128] Effect Examples
[0129] The effects of the present invention are as follows:
[0130] 1) Grain size: measured by crystallographic microscope using the straight line intercept method;
[0131] 2) Macro grain uniformity: After the surface is machined to remove the oxide scale, the entire surface is macro-etched with CuCl2 solution, and the grain uniformity is checked visually;
[0132] 3) Internal defect rate: detected by C-type ultrasonic scanning;
[0133] 4) Purity: tested by GDMS;
[0134] The results are shown in Table 1;
[0135] Table 1
[0136]
[0137]
[0138] As can be seen from Table 1, the aluminum-magnesium-silicon alloy target material prepared by the preparation method provided by the present invention has fine grains within 90 μm, and the grain uniformity is excellent when observed macroscopically. At the same time, the purity of the obtained product is high, above 99.995%, and the internal defect rate is below 1%.
[0139] It can be seen from Example 1 and Comparative Examples 1-5 that when any one of the steps of forging, hot isostatic pressing, primary rolling, secondary rolling or post-rolling insulation treatment is missing, the comprehensive performance of the obtained aluminum-silicon-magnesium alloy target material is significantly reduced; it can be seen from Example 1 and Comparative Examples 6-10 that the parameters of the preparation process also have a certain influence on the results. When the parameters of the preparation process are not within the range given in the present invention, the comprehensive performance of the obtained product also shows a clear downward trend.
[0140] Finally, it should be noted that the above embodiments are intended to illustrate the technical solutions of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the essence and scope of the technical solutions of the present invention.
Claims
1. A method for preparing an aluminum-magnesium-silicon alloy target, characterized in that: The preparation method comprises the following steps: (1) Preheating the aluminum-magnesium-silicon alloy ingot to 450-600°C and then forging it, and water cooling it after forging; (2) preheating the workpiece after water cooling in step (1) for a second time, rolling it once after the second preheating, and air cooling it after the first rolling; (3) performing hot isostatic pressing on the workpiece after air cooling in step (2); the hot isostatic pressing is performed at a temperature of 450-550° C., a time of 3-5 h, and a pressure of 130-150 MPa; (4) preheating the workpiece after hot isostatic pressing in step (3) three times, rolling it twice after the three preheating, and air cooling it after the second rolling; (5) placing the workpiece after air cooling in step (4) at 300-400° C. for 60-120 min, and then air cooling; (6) The workpiece after air cooling in step (5) is leveled and machined, and then bound with a back plate to obtain an aluminum-magnesium-silicon alloy target.
2. The preparation method according to claim 1, characterized in that: The preparation method of the aluminum-magnesium-silicon alloy ingot is as follows: mixing the raw materials and placing them under vacuum degree less than 10 -3 The alloy is vacuum melted for 30-60 minutes at a temperature of 700-850°C and then cast. After cooling, the alloy is taken out from the mold to obtain an aluminum-magnesium-silicon alloy ingot.
3. The preparation method according to claim 1, characterized in that: In the step (1), the preheating time is 60-120 minutes.
4. The preparation method according to claim 1, characterized in that: In the step (1), the forging is performed by roughing and drawing, which is repeated 2-4 times, and the deformation rate is 60-80% each time.
5. The preparation method according to claim 1, characterized in that: In the step (2), the secondary preheating temperature is 450-550° C. and the time is 60-120 min.
6. The preparation method according to claim 1, characterized in that: In the step (2), the deformation rate of one rolling is 45-55%, and the deformation of a single pass is 0.5-1.5 mm.
7. The preparation method according to claim 1, characterized in that: In the step (4), the temperature of the three preheating steps is 450-550° C. and the time is 60-120 min.
8. The preparation method according to claim 1, characterized in that: In the step (4), the deformation rate of the secondary rolling is 60-80%, and the deformation of a single pass is 0.5-1.0 mm.
9. An aluminum-magnesium-silicon alloy target, characterized in that: The aluminum-magnesium-silicon alloy target is prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the aluminum-magnesium-silicon alloy target material as claimed in claim 9 in preparing thin film deposition materials.
Citation Information
Cited By
Aluminum magnesium alloy target as well as preparation method and application thereof
CN121183174A