Screening method for spline strengthening and repairing nickel-plated composite coating of electric brush

Through density functional theory and sol-gel method combined with orthogonal test method, the brush plating process is optimized, and the problem of nanoparticle composite nickel-based coating is easily cracked under dynamic loads, achieving higher mechanical and wear resistance , provides scientific selection basis and design method.

CN119082811AInactive Publication Date: 2024-12-06GUANGDONG UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411210050.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Under dynamic loads and complex operating conditions, nanoparticle composite nickel-based coatings are prone to cracking and falling off due to interface incompatibility and low connection strength, resulting in spline connection failure, and lack of systematic and scientific selection and design methods.

Method used

The first-principle calculation method based on density functional theory is used to screen appropriate interface properties, combine sol-gel method and orthogonal test method to optimize the brush plating process, and optimize nickel-based composite through hardness, roughness and tribology tests. Coating properties.

Benefits of technology

It provides a systematic and scientific basis for selection, improves the mechanical and wear resistance of nickel-based composite coating, enhances the strength and stability of splines, and reduces the wear rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082811A_ABST
    Figure CN119082811A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of surface engineering, and particularly discloses a screening method of a spline strengthening and repairing electric brush nickel-plated composite coating, which comprises the following steps of: calculating and researching interface properties and separation work between coating composition phases by adopting a first principle calculation method based on a density functional theory; the composite reinforced coating meeting the requirements is selected out; a nano Al2O3 material is used, a sol-gel method is adopted, a stability analyzer is combined to screen out an active agent, and the nickel-based composite plating solution is prepared; according to the method, an orthogonal test method and an electric brush plating process are adopted, performance detection including hardness testing, roughness testing, tribology testing and data analysis and optimization is performed on a plating layer sample, the orthogonal test method is adopted, a proper variable parameter level is systematically screened out, and the mechanical and wear-resisting performance of the electric brush nickel-plated base coating is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of surface engineering, and in particular relates to a screening method for spline strengthening and repairing brush-plated nickel-based composite coatings. Background Art

[0002] Brush plating is a branch of electrodeposition technology. It is a technology that uses electrochemical methods to deposit metal or metallize a certain part of the surface of the plated part.

[0003] During plating, a pad or brush that is in contact with the anode and provides the electrolyte required for brush plating moves along a certain trajectory on the cathode to be plated. That is, in an electrolyte solution containing certain metal ions, the workpiece to be plated is used as the cathode, and a certain low-voltage direct current is passed through, so that the metal ions obtain electrons on the workpiece and are continuously deposited as a metal coating.

[0004] Brush plating uses electrolytic methods to obtain a coating on the surface of a workpiece. The purpose is to strengthen and improve the surface performance of the workpiece, obtain the decorative appearance, corrosion resistance, wear resistance and special optical, electrical, magnetic and thermal properties of the workpiece; it can also change the size of the workpiece, improve mechanical fit, and repair workpieces that are scrapped due to out-of-tolerance or wear, etc., so it has a wide range of applications in industry.

[0005] In order to further improve the performance of nickel plating, other alloy elements or particles are added to nickel plating to form alloy plating or composite plating. For example, particles such as diamond, graphite, SiC, Al2O3, SiO2, WC, MoS2, SiN, TiN, P, carbon nanotubes (CNTs) and graphene oxide (GO) are added to nickel-based plating as second-phase particles to improve the hardness, strength, high-temperature inertness, wear resistance and corrosion resistance of the plating. In composite electroplating, due to the unique surface / interface effect, small size effect and quantum size effect of nanoparticles, different nanoparticles themselves show special excellent properties such as high hardness and self-lubricity. Nanoparticle composite brush plating has higher microhardness and better corrosion resistance, which is mainly affected by the characteristics of the second-phase reinforcement particles themselves.

[0006] Researchers at home and abroad have conducted research on different types of nanoparticle composite reinforced nickel-based alloy coatings. The test results all show that they have good mechanical, chemical and friction and wear properties, but the mechanical and friction and wear properties are mostly measured under static conditions.

[0007] During dynamic load service, due to the high brittleness and poor toughness of ceramic reinforcement particles, and the great differences in physical and chemical properties between them and the coating alloy or substrate material, problems such as excessive generation of interface compounds, chemical incompatibility, and low connection strength are prone to occur. Under complex working conditions such as alternating loads and large stress concentration, the composite coating is prone to cracking and falling off due to abnormal loads, thus causing the spline connection to fail. It cannot effectively protect the substrate itself, and has not formed a systematic, scientific and comprehensive selection basis and design method. Summary of the invention

[0008] The object of the present invention is to provide a screening method for spline strengthening and repairing brush-plated nickel-based composite coatings to solve the problems raised in the above-mentioned background technology.

[0009] To achieve the above object, the present invention provides the following technical solutions:

[0010] A screening method for spline strengthening and repairing brush-plated nickel-based composite coatings, S1, using a first-principle calculation method based on density functional theory to calculate and study the interface properties and separation work between the coating components, and select the composite strengthening coating that meets the requirements;

[0011] S2, using nano-Al2O3 material to adopt sol-gel method, and combining with stability analyzer to screen out active agent and prepare nickel-based composite plating solution;

[0012] S3. Use orthogonal test method and brush plating process to perform performance tests on coating samples, including hardness test, roughness test and tribology test, and analyze and optimize the data.

[0013] Preferably, the first principles calculation method based on density functional theory used in S1 is specifically to determine the material under study, use Vasp software, describe the electron-ion interaction of the system based on projected augmented wave (PAW), and approximate the electron exchange-correlation energy based on generalized gradient approximation (GGA).

[0014] Preferably, the activator includes but is not limited to benzalkonium chloride, dodecaned, tetradecyl and hexadecyl trimethyl ammonium bromide, and the spline strengthening and repairing brush plating screening method includes but is not limited to nickel-based composite coating and carburized 9310 steel, and also includes medium carbon steel, alloy steel, stainless steel and other steels used for splines, and chromium-based, cobalt-based, copper-based and other brush-plated metals.

[0015] Preferably, the brush plating process is specifically as follows: dissolving the prepared main salt, auxiliary salt and complexing agent in deionized water, adding them to a pure nickel plating solution after stirring and ultrasonic oscillation, preparing an activation solution, sandpapering the surface of the workpiece to remove surface oil and oxidized impurities, and then performing the brush plating process;

[0016] The main salt is nickel sulfate 300-350g / L, the auxiliary salt is nickel chloride 10-20g / L, the pure nickel plating solution is nickel sulfate 300-350g / L, nickel chloride 20-30g / L, boric acid 40g / L, sodium thiocyanate 10g / L, and sodium hydroxide and sulfuric acid are used to adjust the pH to 4.3-4.7; the activation solution is stirred with a magnetic stirrer for 5 minutes, the plating solution is stirred with a magnetic stirrer for 5 minutes, and then ultrasonically oscillated at 0°C for 30 minutes.

[0017] Preferably, the coating sample is subjected to performance testing in S3, including hardness testing, roughness testing and tribology testing respectively; coating performance testing:

[0018] ①Hardness test: Vickers hardness is used for testing. To prevent the indenter from pressing through the coating, the coating thickness and the indentation diagonal must meet a 0.4 times relationship;

[0019] ② Roughness test: The roughness of the sample needs to be measured and kept below Ra≤1.6;

[0020] ③Tribological performance test: The coating sample was placed on a friction and wear tester, and zirconia was used as a friction pair to rub against it. The load was 100N, the sliding friction speed was 200r / min, and the friction time was 15min. The wear resistance was tested by weight loss method and wear scar volume measurement method. The sample was cleaned and dried before and after friction, and the weight difference △W was weighed; the wear scar volume and sliding distance were obtained in a laser confocal microscope, and the wear rate was calculated using the formula.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] (1) The present invention adopts density functional theory to optimize the brush-plated nanocomposite coating on the surface of carburized 9310 steel by calculating the separation work between the coating constituent phases and the substrate. Compared with the past, it provides an effective systematic, scientific and comprehensive selection basis and design method.

[0023] (2) The present invention combines the sol-gel method with the cation-driven method to select 0.4 g / L of a cationic surfactant of hexadecyltrimethylammonium bromide as a complexing agent, thereby greatly improving the dispersibility and stability of the nanoparticles in the composite plating solution, and there is no obvious precipitation within 3 hours.

[0024] (3) The present invention adopts the orthogonal test method to systematically screen out appropriate variable parameter levels, thereby greatly improving the mechanical and wear resistance of the brush-plated nickel-based coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 Schematic diagram of the calculation model of Ni(111) / Fe3C(001) in the embodiment of the present invention;

[0026] Figure 2 This is a schematic diagram of separation work data in an embodiment of the present invention;

[0027] Figure 3 Schematic diagram of lattice mismatch rate data in an embodiment of the present invention;

[0028] Figure 4 Schematic diagram of the relationship between strain, energy and bond length as a function of strain in the flow embodiment of the present invention;

[0029] Figure 5 It is a schematic diagram of the volume wear rate of the sample in the embodiment of the present invention;

[0030] Figure 6 Schematic diagram of the friction coefficient curve of each sample in the orthogonal test in the embodiment of the present invention;

[0031] Figure 7 The cross-sectional SEM morphology and component distribution diagram of the sample with optimized parameters in the embodiment of the present invention;

[0032] Figure 8 It is a schematic diagram of the process of the present invention. DETAILED DESCRIPTION

[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] Embodiment 1:

[0035] The Vasp software was used to describe the electron-ion interaction of the system based on the projected augmented wave (PAW) and to approximate the electron exchange-correlation energy based on the generalized gradient approximation (GGA).

[0036] Models such as Figure 1 As shown in the figure, the interface binding energy between nickel-based metal, carburized 9310 steel and nanoparticles such as nano-Al2O3, nano-WC, nano-Y2O3, carbon nanotubes and graphene is calculated, and the stable interface model is obtained by analysis. The calculation results are shown in Figure 2 shown.

[0037] The experimental substrate is carburized and quenched 9310 steel, and the nano-ceramic particles as the second phase are nano-Al 2O3 with particle sizes of 20nm, 30nm and 50nm. The sol-gel method is used with appropriate cationic surfactants to solve the problems of dispersion, temperature and suspension of nanoparticles in the basic plating solution.

[0038] Benzalkonium chloride, dodecaned, tetradecyl and hexadecyl trimethyl ammonium bromide were selected, and finally 0.4 g / L of hexadecyl trimethyl ammonium bromide was selected through stability analyzer analysis.

[0039] Dissolve the prepared main salt, auxiliary salt and complexing agent in deionized water, stir thoroughly and add them to the pure nickel plating solution after ultrasonic oscillation. At the same time, prepare the activation solution, and polish the surface of the workpiece with sandpaper to remove surface oil and oxidized impurities. Then carry out the electro-brush plating process.

[0040] The main salt is nickel sulfate 300-350g / L, the auxiliary salt is nickel chloride 10-20g / L, the pure nickel plating solution is nickel sulfate 300-350g / L, nickel chloride 20-30g / L, boric acid 40g / L, sodium thiocyanate 10g / L, and sodium hydroxide and sulfuric acid are used to adjust the pH to 4.3-4.7; the activation solution is stirred with a magnetic stirrer for 5 minutes, the plating solution is stirred with a magnetic stirrer for 5 minutes, and then ultrasonically oscillated at 0°C for 30 minutes.

[0041] The coating samples were subjected to performance tests, including hardness test, roughness test and tribology test. The friction coefficient curve was obtained during the tribology test. It was found that as the friction and wear progressed, the friction coefficient was low and remained stable, indicating that the coating was evenly distributed and was not worn through during the friction process. The comprehensive test results are shown in Table 1.

[0042] Table 1. Orthogonal test and results

[0043]

[0044]

[0045] Other conditions remain the same, PH = 4.4, dispersant concentration 2g / L, brush plating speed 0.2m / s

[0046]

[0047]

[0048] Table 3 Optimized process parameters of Ni-Al2O3 nanoparticle composite coating on 9310 steel surface

[0049]

[0050] Combination Figure 1 It was found that the wear rate of sample No. 3 was lower than that of the commonly used brush nickel plating on the market, and even lower than that of the carburized surface without plating;

[0051] Combined with the range analysis in Table 2, the optimized brush plating process can be obtained, that is, the order of primary and secondary relationships is voltage, nanoparticle concentration, nanoparticle size, and dispersant type.

[0052] They are marked as A, B, C, and D respectively. The larger the R value, the more significant the influence of the factor. The lower the wear rate, the better. The optimal combination is A1 B3C2D2. After comprehensive analysis, the optimal experimental scheme selected is the A1 B3C2D2 combination.

[0053] The results of brush plating with optimized parameters are shown in Table 3. The wear rate is further reduced. The cross-sectional morphology and composition distribution of the coating are shown in Table 3. Figure 7 As shown in the figure, the coating thickness is 21.94 μm. The sample prepared with optimized parameters has a smooth boundary between the coating and the substrate, and has good bonding strength.

[0054] The orthogonal test method of the present invention is a statistical method used to study the influence of multiple variables on target performance, and can effectively estimate the influence of each factor and its interaction within a limited number of experiments. In this study, the particle size of nanoparticles, nanoparticle concentration, voltage intensity and brush plating time are selected as variables, and several levels are set for each variable.

[0055] Variable and level settings

[0056] Nanoparticle size: For example, set three levels (20nm, 30nm, 50nm)

[0057] Nanoparticle concentration: For example, set three levels (2g / L, 10g / L, 20g / L)

[0058] Voltage intensity: For example, set three levels (2V, 4V, 6V)

[0059] Brush plating time: For example, set three levels (1h, 2h, 3h)

[0060] Orthogonal array design

[0061] According to the number of variables and levels, select a suitable orthogonal array, such as L9 (3^4) orthogonal array, which means that each variable has three levels and a total of 9 experiments are conducted.

[0062] 2. Implementation of brush plating process

[0063] Based on the orthogonal experimental design, the brush plating experiment was carried out. The specific steps are as follows:

[0064] Plating solution configuration:

[0065] The nanoparticles are dispersed in a plating solution using a sol-gel method, and a suitable surfactant (such as hexadecyltrimethylammonium bromide) is added to ensure the dispersibility and stability of the nanoparticles.

[0066] Substrate pretreatment:

[0067] Grind and clean the workpiece surface to remove oil and oxide layer to ensure good bonding between the coating and the substrate.

[0068] Brush plating process:

[0069] Install the configured plating solution and workpiece onto the brush plating equipment, and set the voltage intensity, brush plating time, etc. according to the parameters of the orthogonal experimental design.

[0070] During the brush plating process, the parameters such as the pH value of the plating solution, the dispersant concentration and the brush plating speed were kept constant to eliminate the influence of these parameters on the experimental results.

[0071] Coating performance test:

[0072] The coating is subjected to microhardness test, roughness test and tribology test. The specific test methods include using a microhardness tester to measure hardness, using a surface roughness tester to measure roughness, and performing friction and wear tests to obtain wear rate and friction coefficient.

[0073] 3. Data analysis and optimization

[0074] Data Collection

[0075] Record the performance data such as microhardness, roughness, wear rate, etc. of each experiment.

[0076] Range Analysis

[0077] Perform range analysis on the collected data, calculate the K value and R value of each factor, and determine the influence of each factor on the performance index.

[0078] The K value represents the sum of the performance indicators of a certain factor at a certain level.

[0079] The R value represents the difference between the maximum and minimum values ​​of the performance indicators at each level of the same factor, reflecting the degree of influence of the factor on the performance indicator.

[0080] Optimize results

[0081] According to the results of the range analysis, the optimal level combination of each factor is determined. In this example, the optimal combination obtained by calculation may be a nanoparticle size of 20nm, a nanoparticle concentration of 10g / L, a voltage intensity of 4V, and a brush plating time of 2h.

[0082] The brush plating experiment was carried out again using the optimized parameter combination to verify the effectiveness of the optimization results.

[0083] 4. Conclusion

[0084] By combining the above orthogonal test method with the brush plating process, we can systematically explore the effects of nanoparticle size, concentration, voltage intensity, brush plating time and other parameters on the workpiece microhardness, wear rate, thickness and other properties, and optimize the best composite strengthening coating process parameters. This not only improves the experimental efficiency, but also provides a scientific basis for process selection in actual production.

[0085] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A screening method for spline strengthening and repairing brush-plated nickel-based composite coatings, It is characterized in that The following steps are involved: S1. Use the first principle calculation method based on density functional theory to calculate and study the interface properties and separation work between the coating components, and select the composite strengthening coating that meets the requirements; S2. Use Nano Al 2 O 3 The material adopts the sol-gel method and combines with the stability analyzer to screen out the active agent and prepare the nickel-based composite plating solution; S3. Use orthogonal test method and brush plating process to perform performance tests on coating samples, including hardness test, roughness test and tribology test, and analyze and optimize the data.

2. A method for screening a spline strengthening and repairing brush-plated nickel-based composite coating according to claim 1, It is characterized in that The first-principles calculation method based on density functional theory used in S1 is specifically to determine the material under study, use Vasp software, describe the electron-ion interaction of the system based on projected augmented wave (PAW), and approximate the electron exchange-correlation energy based on generalized gradient approximation (GGA).

3. The screening method for spline strengthening and repairing brush-plated nickel-based composite coating according to claim 1, It is characterized in that The composite strengthening coating is carburized 9310 steel, and the activator is hexadecyltrimethylammonium bromide.

4. The screening method for spline strengthening and repairing brush-plated nickel-based composite coating according to claim 1, It is characterized in that The spline strengthening and repairing brush plating screening method includes but is not limited to nickel-based composite coating and carburized 9310 steel, and also includes medium carbon steel, alloy steel, stainless steel spline steel, chromium-based, cobalt-based, copper-based brush plating metals.

5. The screening method for spline strengthening and repairing brush-plated nickel-based composite coating according to claim 1, It is characterized in that The brush plating process is specifically as follows: dissolving the prepared main salt, auxiliary salt and complexing agent in deionized water, stirring and ultrasonically oscillating, and then adding them into a pure nickel plating solution; preparing an activation solution, sandpapering the surface of the workpiece to remove surface oil and oxidized impurities, and then performing the brush plating process; The main salt is nickel sulfate 300-350g / L, the auxiliary salt is nickel chloride 10-20g / L, the pure nickel plating solution is nickel sulfate 300-350g / L, nickel chloride 20-30g / L, boric acid 40g / L, sodium thiocyanate 10g / L, and sodium hydroxide and sulfuric acid are used to adjust the pH to 4.3-4.7; the activation solution is stirred with a magnetic stirrer for 5 minutes, the plating solution is stirred with a magnetic stirrer for 5 minutes, and then ultrasonically oscillated at 0°C for 30 minutes.

6. The screening method for spline strengthening and repairing brush-plated nickel-based composite coating according to claim 1, It is characterized in that In S3, the coating samples are subjected to performance tests, including hardness test, roughness test and tribology test; coating performance test: ①Hardness test: Vickers hardness is used for testing. To prevent the indenter from pressing through the coating, the coating thickness and the indentation diagonal must meet a 0.4 times relationship; ② Roughness test: The roughness of the sample needs to be measured and kept below Ra≤1.6; ③Tribological performance test: The coated sample was placed on a friction and wear testing machine, and zirconia was used as the friction pair to rub against it. The load was 100N, the sliding friction speed was 200r / min, and the friction time was 15min. The wear resistance was tested by weight loss method and wear scar volume measurement method. The sample was cleaned and dried before and after friction, and the weight difference △W was weighed. The wear scar volume and sliding distance were obtained in a laser confocal microscope, and the wear rate was calculated using the formula.