Method for preventing basement exterior wall concrete from generating cracks
By setting up concrete deformation coordination belts and special concrete at the bottom of the basement exterior wall panel, combining expansion agents and fibers, the crack problems caused by volume expansion and cooling of the basement exterior wall are solved, and the effect of reducing cracks and improving durability is achieved.
Patent Information
- Application Number
- CN202411365940.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-12-06
AI Technical Summary
The basement exterior wall concrete is caused by volume expansion and later cooling due to early hydration heat, resulting in cracks and water leakage problems. The existing preventive measures are costly and have limited results.
A concrete deformation coordination belt is installed at the bottom of the basement exterior wall panel, and special concrete is used to reduce the constraints on the upper ordinary concrete in the plastic stage before initial setting, and combine expansion agents and reinforcement fibers to prevent the concrete from shrinking volume and restricting cracking during cooling.
It effectively reduces the cracks in basement wall panel concrete, eliminates water leakage and seepage, improves the durability of reinforced concrete, and reduces construction costs.
Smart Images

Figure CN119083490A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of concrete, and in particular relates to a method for preventing cracks from occurring in concrete of a basement exterior wall. Background Art
[0002] In the past 20 years, under the adjustment and support of national economic policies, my country's construction industry has achieved vigorous development, the number of construction projects has increased significantly, and the scale of basements has become larger and larger. Among them, due to its own characteristics and the environment in which it is located, the basements of construction projects often experience cracking, leakage, seepage and other phenomena on the exterior wall concrete, which seriously affects the use function of the building, and it is also difficult to deal with water seepage and leakage in the later stage. Under normal circumstances, the methods to prevent cracking of the exterior wall concrete of the basement include optimizing the design to change the number and density of horizontal reinforcements on the exterior wall, increasing the anti-cracking steel wire mesh, adding vertical post-casting strips, optimizing the concrete mix ratio, extending the demoulding time, doing a good job of thermal insulation and moisture maintenance, reducing the temperature and humidity difference between the inside and outside of the concrete, etc. Taking the above anti-cracking measures can greatly reduce the probability of concrete cracks, but it will also greatly increase the material and construction costs.
[0003] Among the above methods for preventing cracking of basement exterior wall concrete, two measures, “resistance” and “release”, are mainly adopted to reduce cracks. However, the main reason for cracking of basement exterior wall concrete is the early hydration heat of newly poured exterior wall concrete, which causes the concrete temperature to rise and the volume to expand (generally reaching the highest temperature within 3 days). When the concrete cools down in the later period, the volume shrinks. Under the constraint of the rigid bottom plate concrete, the exterior wall concrete is subjected to tensile stress greater than its tensile strength, thus causing concrete cracking. When vertical post-cast strips are adopted to prevent cracking of basement exterior wall concrete, the constraint of part of the basement bottom plate on the wall plate concrete can be reduced, but the reduction is limited. Therefore, in current construction projects, cracks in exterior wall concrete still have a high probability of occurring. Summary of the invention
[0004] The purpose of the present invention is to solve the above-mentioned technical problems and provide a method for preventing cracks in the concrete of the basement exterior wall. By setting a concrete deformation coordination zone at the bottom of the basement exterior wall panel, the constraint of the basement floor on the wall panel concrete is reduced, thereby preventing cracks in the basement wall panel concrete.
[0005] The method for preventing cracks from forming in the concrete of the basement exterior wall in the technical solution of the present invention comprises the following steps: after the basement floor slab concrete is poured and hardened, the exterior wall slab reinforcement is tied and the reinforcement formwork is installed, and then a layer of special concrete is poured along the bottom of the exterior wall formwork and the upper part of the horizontal construction joint between the basement floor slab and the exterior wall to form a deformation coordination zone, and then ordinary concrete is immediately poured on the upper part of the deformation coordination zone and maintained with the formwork.
[0006] The present invention arranges a concrete deformation coordination zone at the bottom of the basement exterior wall panel. When the ordinary concrete on the upper part of the exterior wall panel is in the concrete cooling and shrinking stage, the special concrete used in the deformation coordination zone is still in the plastic stage before initial setting, and has no restraining effect on the shrinkage of the upper ordinary concrete, so that the upper wall concrete can shrink freely without generating tensile stress, thereby reducing the restraint of the basement floor on the wall panel concrete, preventing the basement wall panel concrete from cracking, eliminating water leakage and water seepage, and improving the durability of reinforced concrete.
[0007] Further, the thickness of the deformation coordination zone is the same as the thickness of the exterior wall.
[0008] Furthermore, the layer height of the deformation coordination zone is greater than or equal to 400 mm, and greater than or equal to the thickness of the exterior wall panel.
[0009] As a preference, steel waterstops should be installed at horizontal construction joints of exterior walls.
[0010] Furthermore, ordinary concrete includes the following components in parts by weight: 260-400 parts of cement, 50-150 parts of fly ash, 50-150 parts of mineral powder, 1000-1300 parts of crushed stone, 550-780 parts of sand, 150-200 parts of water, and 3-15 parts of water reducing agent.
[0011] Furthermore, the water reducing agent in ordinary concrete is a polycarboxylate water reducing agent.
[0012] Furthermore, ordinary concrete is obtained by mixing cement, fly ash, mineral powder, crushed stone, sand, water and a water reducing agent.
[0013] Furthermore, the special concrete is obtained by mixing cement, fly ash, mineral powder and expansion agent to obtain a cementitious material, and then adding crushed stone, sand, water reducing agent, reinforcing fiber and water to mix.
[0014] Furthermore, the water reducing agent in the special concrete is composed of the following components in percentage by weight: 0.5-1.0% water reducing mother solution, 0.1-0.5% collapse retaining mother solution, 0.1-12.0% sodium gluconate and 0.1-3.0% soft white sugar, and the balance is water.
[0015] Preferably, the amount of cement, fly ash, mineral powder, crushed stone, sand, water and water reducing agent in the special concrete is 0.9 to 1.1 times the amount of the corresponding substances in ordinary concrete.
[0016] Furthermore, the mass of the expansion agent accounts for 2.5-5.5% of the mass of the gelling material.
[0017] Furthermore, the volume of the reinforcing fiber accounts for 0.06-1.0% of the volume of the special concrete.
[0018] The expansive agent in special concrete can compensate for the volume shrinkage of special concrete during the cooling stage. At the same time, the addition of reinforcing fibers can effectively inhibit the shrinkage and cracking of special concrete under the constraints of the upper and lower walls. The two work synergistically to prevent cracks in the concrete.
[0019] Further, the reinforcing fiber is any one of aromatic polyamide fiber and polyolefin fiber; the aromatic polyamide fiber can be one or more of poly(p-phenylene terephthalamide) fiber, poly(p-aminobenzamide) terephthalamide fiber and poly(p-phenylene terephthalamide) fiber, and the polyolefin fiber can be one or two of polyethylene fiber and polypropylene fiber. Further, the expansion agent is one or more of calcium oxide, magnesium oxide, calcium sulfoaluminate and silicate, preferably magnesium oxide.
[0020] Furthermore, after pouring ordinary concrete on the upper part of the deformation coordination zone, the time for curing with formwork is 14 to 20 days.
[0021] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:
[0022] (1) By setting a concrete deformation coordination zone at the bottom of the basement exterior wall slab, the constraint of the basement bottom slab on the wall slab concrete is reduced, thereby preventing cracks in the basement wall slab concrete;
[0023] (2) When the ordinary concrete on the upper part of the exterior wall panel is in the stage of concrete cooling and shrinkage, the special concrete used in the deformation coordination zone is still in the plastic stage before initial setting, which does not restrain the shrinkage of the ordinary concrete on the upper part, so that the upper wall concrete can shrink freely without generating tensile stress, thereby reducing the constraint of the basement floor on the wall panel concrete, preventing cracks in the basement wall panel concrete, eliminating water leakage and seepage, and improving the durability of reinforced concrete;
[0024] (3) The expansion agent in the special concrete can compensate for the volume shrinkage of the special concrete during the cooling stage. At the same time, the addition of reinforcing fibers can effectively inhibit the shrinkage and cracking of the special concrete under the constraints of the upper and lower walls. The two work synergistically to prevent cracks in the wall panel concrete.
[0025] (4) Only a small amount of concrete used in the deformation coordination zone is special concrete, and most of the other exterior wall slab concrete is ordinary concrete, which can prevent cracks in the basement wall slab concrete at a relatively low cost;
[0026] (5) Special concrete is used for the deformation coordination zone. After the vibrating and pouring of the material is completed, ordinary concrete for the wall panel is poured on the upper part immediately. The construction is continuous and the construction period is not increased. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1It is a schematic diagram of setting a concrete deformation coordination zone at the bottom of the basement exterior wall slab according to the present invention;
[0028] In the figure: 1-basement top plate, 2-exterior wall plate, 3-basement floor plate, 4-rebar, 5-deformation coordination strip, 6-steel plate waterstop, 7-exterior wall horizontal construction joint. DETAILED DESCRIPTION
[0029] The technical scheme of the present invention is further described below by specific examples and accompanying drawings. It should be understood that the specific examples described herein are only used to help understand the present invention and are not intended for specific limitations of the present invention. The accompanying drawings used herein are only for better illustrating the disclosed content of the present invention and do not have a limiting effect on the scope of protection. If not otherwise specified, the raw materials used in the embodiments of the present invention are all commonly used raw materials in the art, and the methods used in the embodiments are all conventional methods in the art.
[0030] like Figure 1 As shown, after the concrete of the basement floor 3 is poured and hardened, the reinforcement steel bars 4 of the exterior wall panel 2 are tied and the reinforcement formwork is installed. Then, along the bottom of the exterior wall formwork and the upper part of the horizontal construction joint 7 between the basement floor 1 and the exterior wall, a layer of special concrete is poured to form a deformation coordination zone 5. A steel plate waterstop 6 should be set at the horizontal construction joint 7 of the exterior wall. Then, ordinary concrete is immediately poured on the upper part of the deformation coordination zone and maintained with formwork.
[0031] Example 1
[0032] The method for preventing cracks from forming in the concrete of the basement exterior wall in this embodiment comprises the following steps:
[0033] (1) 300 parts of cement, 120 parts of fly ash, 80 parts of mineral powder, 1050 parts of crushed stone, 700 parts of sand, 160 parts of water and 10 parts of polycarboxylate water reducer were stirred and mixed to obtain ordinary concrete;
[0034] (2) 300 parts of cement, 120 parts of fly ash, 80 parts of mineral powder and 15 parts of magnesium oxide expansion agent are mixed to obtain a cementitious material, and then 1050 parts of crushed stone, 700 parts of sand, 160 parts of water, 10 parts of water reducer and polypropylene fiber are added and stirred to obtain a special concrete; wherein the water reducer is obtained by mixing 0.7 parts of water reducing mother liquid, 0.3 parts of collapse retaining mother liquid, 5.0 parts of sodium gluconate, 1.0 parts of soft white sugar and 93 parts of water, and the volume of the polypropylene fiber accounts for 0.3% of the volume of the special concrete;
[0035] (3) After the basement slab concrete is poured and hardened, the external wall slab reinforcement is tied and the reinforcement formwork is installed. Then, along the bottom of the external wall formwork and above the horizontal construction joint between the basement slab and the external wall, a layer of special concrete is poured to form a deformation coordination zone with the same thickness as the external wall and a floor height of 500 mm. Immediately thereafter, ordinary concrete is poured on the upper part of the deformation coordination zone and maintained with formwork for 14 days.
[0036] Example 2
[0037] The method for preventing cracks from forming in the concrete of the basement exterior wall in this embodiment comprises the following steps:
[0038] (1) 320 parts of cement, 110 parts of fly ash, 100 parts of mineral powder, 1100 parts of crushed stone, 660 parts of sand, 160 parts of water and 8 parts of polycarboxylate water reducer were stirred and mixed to obtain ordinary concrete;
[0039] (2) 320 parts of cement, 110 parts of fly ash, 100 parts of mineral powder and 16 parts of magnesium oxide expansion agent are mixed to obtain a cementitious material, and then 1100 parts of crushed stone, 660 parts of sand, 160 parts of water, 8 parts of water reducer and polypropylene fiber are added and stirred to obtain a special concrete; wherein the water reducer is obtained by mixing 0.6 parts of water reducing mother liquid, 0.4 parts of collapse retaining mother liquid, 6.0 parts of sodium gluconate, 1.0 parts of soft white sugar and 92 parts of water, and the volume of the polyethylene fiber accounts for 0.3% of the volume of the special concrete;
[0040] (3) After the basement slab concrete is poured and hardened, the external wall slab reinforcement is tied and the reinforcement formwork is installed. Then, along the bottom of the external wall formwork and above the horizontal construction joint between the basement slab and the external wall, a layer of special concrete is poured to form a deformation coordination zone with a thickness of the same as that of the external wall and a floor height of 500 mm. Immediately thereafter, ordinary concrete is poured on the upper part of the deformation coordination zone and maintained with formwork for 15 days.
[0041] Example 3
[0042] The method for preventing cracks from forming in the concrete of the basement exterior wall in this embodiment comprises the following steps:
[0043] (1) 350 parts of cement, 100 parts of fly ash, 120 parts of mineral powder, 1150 parts of crushed stone, 600 parts of sand, 160 parts of water and 6 parts of polycarboxylate water reducer were stirred and mixed to obtain ordinary concrete;
[0044] (2) 350 parts of cement, 100 parts of fly ash, 120 parts of mineral powder and 17 parts of magnesium oxide expansion agent are mixed to obtain a cementitious material, and then 1150 parts of crushed stone, 600 parts of sand, 160 parts of water, 6 parts of water reducer and polypropylene fiber are added and stirred to obtain a special concrete; wherein the water reducer is obtained by mixing 0.7 parts of water reducing mother liquid, 0.3 parts of collapse retaining mother liquid, 6.0 parts of sodium gluconate, 2.0 parts of soft white sugar and 91 parts of water, and the volume of poly(p-phenylene terephthalamide) fiber accounts for 0.3% of the volume of the special concrete;
[0045] (3) After the basement slab concrete is poured and hardened, the external wall slab reinforcement is tied and the reinforcement formwork is installed. Then, along the bottom of the external wall formwork and above the horizontal construction joint between the basement slab and the external wall, a layer of special concrete is poured to form a deformation coordination zone with a thickness of the same as that of the external wall and a floor height of 500 mm. Immediately thereafter, ordinary concrete is poured on the upper part of the deformation coordination zone and maintained with formwork for 16 days.
[0046] Example 4
[0047] The difference between this embodiment and embodiment 1 is that in step (2), 300 parts of cement, 120 parts of fly ash, 80 parts of mineral powder and 20 parts of magnesium oxide expansion agent are mixed to obtain a cementitious material, and then 1050 parts of crushed stone, 700 parts of sand, 160 parts of water, 10 parts of water reducer and polypropylene fiber are added and stirred to obtain special concrete; wherein the water reducer is composed of 0.7 parts of water reducing mother solution, 0.3 parts of collapse-preserving mother solution, 5.0 parts of sodium gluconate, 1.0 parts of soft white sugar and 93 parts of
[0048] The volume of polypropylene fiber accounts for 0.3% of the volume of special concrete.
[0049] Example 5
[0050] The difference between this embodiment and embodiment 1 is that in step (2), 300 parts of cement, 120 parts of fly ash, 80 parts of mineral powder and 23 parts of magnesium oxide expansion agent are mixed to obtain a cementitious material, and then 1050 parts of crushed stone, 700 parts of sand, 160 parts of water, 10 parts of water reducer and polypropylene fiber are added and stirred to obtain special concrete; wherein the water reducer is composed of 0.7 parts of water reducing mother solution, 0.3 parts of collapse-preserving mother solution, 5.0 parts of sodium gluconate, 1.0 parts of soft white sugar and 93 parts of
[0051] The volume of polypropylene fiber accounts for 0.3% of the volume of special concrete.
[0052] Example 6
[0053] The difference between this embodiment and embodiment 1 is that in step (2), 300 parts of cement, 120 parts of fly ash, 80 parts of mineral powder and 10 parts of magnesium oxide expansion agent are mixed to obtain a cementitious material, and then 1050 parts of crushed stone, 700 parts of sand, 160 parts of water, 10 parts of water reducer and polypropylene fiber are added and stirred to obtain special concrete; wherein the water reducer is composed of 0.7 parts of water reducing mother solution, 0.3 parts of collapse-preserving mother solution, 5.0 parts of sodium gluconate, 1.0 parts of soft white sugar and 93 parts of
[0054] The volume of polypropylene fiber accounts for 0.3% of the volume of special concrete.
[0055] Example 7
[0056] The difference between this embodiment and embodiment 1 is that in step (2), 300 parts of cement, 120 parts of fly ash, 80 parts of mineral powder and 32 parts of magnesium oxide expansion agent are mixed to obtain a cementitious material, and then 1050 parts of crushed stone, 700 parts of sand, 160 parts of water, 10 parts of water reducer and polypropylene fiber are added and stirred to obtain special concrete; wherein the water reducer is composed of 0.7 parts of water reducing mother solution, 0.3 parts of collapse-preserving mother solution, 5.0 parts of sodium gluconate, 1.0 parts of soft white sugar and 93 parts of
[0057] The volume of polypropylene fiber accounts for 0.3% of the volume of special concrete.
[0058] Example 8
[0059] The difference between this embodiment and embodiment 1 is that in step (2), 300 parts of cement, 120 parts of fly ash, 80 parts of mineral powder and 15 parts of magnesium oxide expansion agent are mixed to obtain a cementitious material, and then 1050 parts of crushed stone, 700 parts of sand, 160 parts of water, 10 parts of water reducer and polypropylene fiber are added and stirred to obtain special concrete; wherein the water reducer is composed of 0.7 parts of water reducing mother solution, 0.3 parts of collapse-preserving mother solution, 5.0 parts of sodium gluconate, 1.0 parts of soft white sugar and 93 parts of
[0060] The volume of polypropylene fiber accounts for 0.03% of the volume of special concrete.
[0061] Example 9
[0062] The difference between this embodiment and embodiment 1 is that in step (2), 300 parts of cement, 120 parts of fly ash, 80 parts of mineral powder and 15 parts of magnesium oxide expansion agent are mixed to obtain a cementitious material, and then 1050 parts of crushed stone, 700 parts of sand, 160 parts of water, 10 parts of water reducer and polypropylene fiber are added and stirred to obtain special concrete; wherein the water reducer is composed of 0.7 parts of water reducing mother solution, 0.3 parts of collapse-preserving mother solution, 5.0 parts of sodium gluconate, 1.0 parts of soft white sugar and 93 parts of
[0063] The volume of polypropylene fiber accounts for 1.3% of the volume of special concrete.
[0064] Example 10
[0065] The difference between this embodiment and embodiment 1 is that in step (2), 300 parts of cement, 120 parts of fly ash, 80 parts of mineral powder and 15 parts of magnesium oxide expansion agent are mixed to obtain a cementitious material, and then 1050 parts of crushed stone, 700 parts of sand, 160 parts of water and 10 parts of water reducer are added and stirred to obtain special concrete; wherein the water reducer is obtained by mixing 0.7 parts of water-reducing mother liquor, 0.3 parts of collapse-preserving mother liquor, 5.0 parts of sodium gluconate, 1.0 parts of soft white sugar and 93 parts of water.
[0066] Embodiment 11
[0067] The difference between this embodiment and embodiment 1 is that in step (2), 300 parts of cement, 120 parts of fly ash and 80 parts of mineral powder are mixed to obtain a cementitious material, and then 1050 parts of crushed stone, 700 parts of sand, 160 parts of water, 10 parts of water reducer and polypropylene fiber are added and stirred to obtain special concrete; wherein the water reducer is obtained by mixing 0.7 parts of water-reducing mother liquor, 0.3 parts of collapse-preserving mother liquor, 5.0 parts of sodium gluconate, 1.0 parts of soft white sugar and 93 parts of water, and the volume of the polypropylene fiber accounts for 0.3% of the volume of the special concrete.
[0068] Comparative Example 1
[0069] The method for pouring concrete for the basement exterior wall in this comparative example comprises the following steps:
[0070] (1) 300 parts of cement, 120 parts of fly ash, 80 parts of mineral powder, 1050 parts of crushed stone, 700 parts of sand, 160 parts of water and 10 parts of polycarboxylate water reducer were stirred and mixed to obtain ordinary concrete;
[0071] (2) After the basement slab concrete is poured and hardened, the external wall slab reinforcement is tied and the reinforcement formwork is installed. Then, along the bottom of the external wall formwork and above the horizontal construction joint between the basement slab and the external wall, ordinary concrete is poured and cured with the formwork for 14 days.
[0072] In Examples 1-5, by setting a deformation coordination zone for pouring special concrete at the bottom of the basement exterior wall panel, the constraint of the basement floor on the wall panel concrete can be effectively reduced, thereby preventing cracks from occurring in the basement wall panel concrete. In Example 6, a small amount of magnesium oxide expansion agent is added to the special concrete, which weakens the compensation effect on the volume shrinkage of the special concrete during the cooling stage, thereby increasing the probability of cracks occurring in the concrete. In Example 7, an excessive amount of magnesium oxide expansion agent is added to the special concrete, which has a greater expansion and reinforcement effect, thereby generating greater stress inside the concrete, which in turn increases the risk of cracks occurring. In Example 8, a small amount of polypropylene fiber is added to the special concrete, which weakens the inhibitory effect on shrinkage cracking of the special concrete under the constraints of the upper and lower walls, thereby making the basement wall panel concrete more susceptible to cracks. In Example 9, a large amount of magnesium oxide expansion agent is added to the special concrete, thereby reducing the inhibitory effect on shrinkage cracking of the special concrete under the constraints of the upper and lower walls, thereby making the basement wall panel concrete more susceptible to cracks. Adding an excessive amount of polypropylene fiber increases the difficulty of dispersion and easily causes uneven components inside the concrete; in Example 10, only magnesium oxide expansion agent is added to the special concrete without adding polypropylene fiber, which can only compensate for the volume shrinkage of the special concrete in the cooling stage, has no supporting effect, and cannot inhibit the shrinkage and cracking of the special concrete under the constraints of the upper and lower walls, increasing the risk of cracks; in Example 11, only polypropylene fiber is added to the special concrete without adding magnesium oxide expansion agent, which can only inhibit the shrinkage of the special concrete under the constraints of the upper and lower walls, has no compensatory effect, and also increases the risk of cracks; in Comparative Example 1, no special concrete casting deformation coordination belt is used. When the concrete cools down and shrinks, cracks are more likely to occur, causing leakage and seepage, reducing the durability of the reinforced concrete.
[0073] Finally, it should be noted that the specific embodiments described herein are merely examples of the spirit of the present invention, and are not intended to limit the implementation methods of the present invention. Those skilled in the art of the present invention may make various modifications or supplements to the described embodiments or replace them in similar ways. It is not necessary and impossible to provide all examples of all implementation methods here. However, these obvious changes or modifications derived from the essential spirit of the present invention still fall within the scope of protection of the present invention, and interpreting them as any additional limitation is contrary to the spirit of the present invention.
Claims
1. A method for preventing cracks in basement exterior wall concrete, characterized in that: The method includes the following steps: after the basement slab concrete is poured and hardened, the external wall slab reinforcement is tied and the reinforcement formwork is installed; then a layer of special concrete is poured along the bottom of the external wall formwork and the upper part of the horizontal construction joint between the basement slab and the external wall to form a deformation coordination zone; then, ordinary concrete is immediately poured on the upper part of the deformation coordination zone and maintained with the formwork.
2. The method for preventing cracks in basement exterior wall concrete according to claim 1, characterized in that: The layer height of the deformation coordination zone is greater than or equal to 400mm and greater than or equal to the thickness of the exterior wall panel.
3. The method for preventing cracks in basement exterior wall concrete according to claim 1, characterized in that: Ordinary concrete includes the following components in parts by weight: 260-400 parts of cement, 50-150 parts of fly ash, 50-150 parts of mineral powder, 1000-1300 parts of crushed stone, 550-780 parts of sand, 150-200 parts of water, and 3-15 parts of water reducing agent.
4. The method for preventing cracks in basement exterior wall concrete according to claim 1, characterized in that: Special concrete is obtained by mixing cement, fly ash, mineral powder and expansion agent to obtain a cementitious material, and then adding crushed stone, sand, water reducing agent, reinforcing fiber and water to mix.
5. The method for preventing cracks in basement exterior wall concrete according to claim 4, characterized in that: The water reducing agent in the special concrete is composed of the following components in percentage by weight: 0.5-1.0% water reducing mother solution, 0.1-0.5% collapse retaining mother solution, 0.1-12.0% sodium gluconate and 0.1-3.0% soft white sugar, and the balance is water.
6. The method for preventing cracks in basement exterior wall concrete according to claim 4, characterized in that: The mass of the expansion agent accounts for 2.5 to 5.5% of the mass of the cementitious material.
7. The method for preventing cracks in basement exterior wall concrete according to claim 4, characterized in that: The volume of the reinforcing fiber accounts for 0.06 to 1.0% of the volume of the special concrete.
8. The method for preventing cracks in basement exterior wall concrete according to claim 7, characterized in that: The reinforcing fiber is either aromatic polyamide fiber or polyolefin fiber.
9. The method for preventing cracks in basement exterior wall concrete according to claim 4, characterized in that: The expansion agent is one or more of calcium oxide, magnesium oxide, calcium sulfoaluminate and silicate.
10. The method for preventing cracks in basement exterior wall concrete according to claim 1, characterized in that: After pouring ordinary concrete on the upper part of the deformation coordination zone, the time for formwork curing is 14 to 20 days.