Testing device and testing method for simulating reaction in hydrogen-based shaft furnace

By using electric heating furnaces, reactors and steam feeders in the hydrogen metallurgy test device to simulate the reaction in the hydrogen-based vertical furnace, the problem of low accuracy of the test results in the prior art is solved, and a more accurate hydrogen metallurgy reaction simulation is achieved. and sponge iron sample test.

CN119086343APending Publication Date: 2024-12-06CISDI ENGINEERING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411493444.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-24
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing hydrogen metallurgy testing device simulates the reaction in the hydrogen-based vertical furnace and the actual reaction, resulting in low accuracy of the test results.

Method used

A test device including an electric heating furnace, reactor, load mechanism, reducing gas generator and steam supply was designed. By simulating the reaction in the hydrogen-based vertical furnace, hydrogen, methane, carbon monoxide and carbon dioxide were introduced into the reaction chamber. The mixture of reducing gas with nitrogen and combined with steam supply simulates the reaction conditions in the hydrogen-based vertical furnace.

Benefits of technology

The accuracy of the test results is improved, and through the combination of reducing gas and steam, the reaction in the hydrogen-based vertical furnace is more accurately simulated, which enhances the accuracy of determining the bond index and metallization rate of the sponge iron sample.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119086343A_ABST
    Figure CN119086343A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of hydrogen metallurgy, in particular to a testing device and a testing method for simulating a reaction in a hydrogen-based shaft furnace. The testing device comprises an electric heating furnace; the reactor is arranged in the electric heating furnace, and the reactor is provided with a reaction cavity for accommodating an iron ore sample layer; at least part of the loading mechanism extends into the reaction cavity so as to apply load to the iron ore sample layer; the reducing gas generating mechanism is communicated with the reactor and is used for introducing reducing gas into the reaction cavity; the steam supplier is communicated with the reactor and is used for introducing steam into the reaction cavity. The hydrogen-based shaft furnace internal reaction simulation device at least has the following beneficial effects that the reducing gas generation mechanism and the steam supply device are matched for use to provide reducing gas and steam for the reaction cavity, so that the reducing gas generation mechanism, the steam supply device, the loading mechanism, the reactor and the electric heating furnace are matched to more accurately simulate the reaction in the hydrogen-based shaft furnace, and the accuracy of a test result is favorably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hydrogen metallurgy, and in particular to a testing device and a testing method for simulating the reaction in a hydrogen-based vertical furnace. Background Art

[0002] At present, in the field of hydrogen metallurgy, there are already some test devices and methods for simulating the reaction in the hydrogen-based vertical furnace. For example, ISO11256, ISO11257 and ISO11258 respectively give the determination methods of the agglomeration index, low-temperature reduction pulverization index and reduction index of the vertical furnace charge. However, these determination methods mainly use CO, CO2, H2 and N2 as reducing gases, and do not consider the existence of CH4 and steam. According to existing research, in the tuyere area of ​​the hydrogen-based vertical furnace, the external unconverted CH4 and steam will undergo in-situ reforming, which increases the proportion of CO and H2 in the reducing gas, but at the same time greatly reduces the temperature of the reducing gas, which has a certain negative impact on gas-solid reduction. It can be seen that the furnace reaction simulated by the existing test devices and test methods is quite different from the actual furnace reaction, and the test results are of low accuracy.

[0003] Therefore, there is an urgent need for a testing device and a testing method to improve the accuracy of the test results. Summary of the invention

[0004] In view of the above-mentioned shortcomings of the prior art, the purpose of the present invention is to provide a test device and a test method for simulating the reaction in a hydrogen-based vertical furnace, so as to solve the problem that the reaction in a hydrogen-based vertical furnace simulated by the test device in the prior art is greatly different from the actual reaction in the furnace and the accuracy of the test results is low.

[0005] To achieve the above-mentioned and other related purposes, the present invention provides a test device for simulating the reaction in a hydrogen-based vertical furnace, comprising:

[0006] Electric heating furnace;

[0007] A reactor, the reactor being placed in the electric heating furnace, the reactor having a reaction chamber for accommodating an iron ore sample layer;

[0008] A load mechanism, at least a portion of which extends into the reaction chamber to apply a load to the iron ore sample layer;

[0009] A reducing gas generating mechanism, connected to the reactor and used to introduce reducing gas into the reaction chamber;

[0010] A steam supplier is connected to the reactor and is used to introduce steam into the reaction chamber.

[0011] Optionally, the reactor includes an inner tube and an outer tube, the outer tube includes an outer tube bottom wall and an outer tube side wall, the inner tube is located inside the outer tube and supported on the outer tube bottom wall, the inner side wall of the inner tube and the outer tube bottom wall jointly define the reaction chamber, an air inlet channel is formed between the outer side wall of the inner tube and the outer tube side wall, a ventilation structure is provided at the lower part of the inner tube or between the inner tube and the outer tube bottom wall, and the air inlet channel is connected to the reaction chamber through the ventilation structure.

[0012] Optionally, the ventilation structure is a through hole arranged on the lower side wall of the inner tube, or the ventilation structure is formed by a gap between the lower end wall of the inner tube and the bottom wall of the outer tube.

[0013] Optionally, a support seat located in the reaction chamber is provided on the bottom wall of the outer tube, and the support seat includes a support plate and a plurality of support columns, and the top and bottom of the support columns are respectively welded and fixed to the support plate and the bottom wall of the outer tube, and the support plate is used to support the iron ore sample layer, and the support plate is provided with air holes for the reducing gas and the steam to pass through.

[0014] Optionally, the outer tube is a stainless steel tube, and the inner tube is a corundum tube.

[0015] Optionally, the inner wall of the inner tube is an inclined wall.

[0016] Optionally, the inner tube includes an upper tube section and a lower tube section that are connected, the upper tube section is a straight tube, and the inner side wall of the lower tube section is an inclined wall.

[0017] Optionally, the inner diameter of the pipe section whose inner side wall is an inclined wall gradually increases from top to bottom.

[0018] Optionally, the angle between the inclined wall and the axis of the inner tube is α, 2°≤α<10°.

[0019] Optionally, the reactor also includes a top cover, the lower end of the inner tube extends into the outer tube, the upper end of the inner tube is sealed with the upper end of the outer tube by a first seal, the top cover is sealed with the upper port of the inner tube by a second seal, and the top cover is provided with a reducing gas inlet connected to the air inlet channel and a top coal gas outlet connected to the reaction chamber.

[0020] Optionally, the load mechanism includes a driving member, a pressure head and a longitudinal thermocouple extending into the reaction chamber. The driving member is connected to the pressure head via a pressure rod, and drives the pressure head to move longitudinally in the reaction chamber to adjust the load on the iron ore sample layer. The longitudinal thermocouple extends into the iron ore sample layer after passing through the driving member, the pressure rod and the pressure head.

[0021] Optionally, the reducing gas generating mechanism includes a hydrogen supplier, a methane supplier, a carbon monoxide supplier, a carbon dioxide supplier, a nitrogen supplier and a flow control box, the flow control box is respectively connected to the hydrogen supplier, the methane supplier, the carbon monoxide supplier, the carbon dioxide supplier and the nitrogen supplier to adjust the flow of the corresponding gas, and the flow control box and the steam supplier are connected to the reactor through a pipeline assembly.

[0022] In order to achieve the above-mentioned object and other related objects, the present invention also provides a testing method, which is tested by the testing device for simulating the reaction in a hydrogen-based shaft furnace as described above, comprising the following steps:

[0023] Laying a first corundum single ball layer, an iron ore sample layer, and a second corundum single ball layer in sequence from bottom to top in the reaction chamber;

[0024] The iron ore sample layer in the reactor is heated to a first preset temperature T1 by the electric heating furnace, and nitrogen is introduced during the heating process;

[0025] The iron ore sample layer is maintained at the first preset temperature T1, and a mixed reducing gas of steam and hydrogen, methane, carbon monoxide, carbon dioxide and nitrogen is introduced into the reaction chamber; a load is applied to the iron ore sample layer by the load mechanism, and a sponge iron sample is obtained after the iron ore sample layer is reduced;

[0026] Stop applying load to the sponge iron sample, stop heating, stop introducing the steam and stop introducing the mixed reducing gas, and introduce nitrogen to cool the sponge iron sample;

[0027] The cooled sponge iron sample is pushed out of the reaction chamber by the load mechanism, and the bonding index of the sponge iron sample and / or the metallization rate of the sponge iron sample are detected.

[0028] Optionally, the particle sizes of the first corundum single ball layer, the iron ore sample layer and the second corundum single ball layer are all D, 10 mm ≤ D ≤ 12.5 mm;

[0029] The iron ore sample layer is heated to a first preset temperature T1 at a heating rate V1, and the flow rate of the nitrogen during the heating process is G1, 8°C / min≤V1≤12°C / min, 900°C≤T1≤1100°C, 8L / min≤G1≤12L / min;

[0030] When the duration of the introduction of the steam and the mixed reducing gas reaches H1, a load is applied to the iron ore sample layer, and the ratio of the iron ore sample layer to the mixed reducing gas is F, 0.5h≤H1≤1.5h, 45g / (L / min)≤F≤55g / (L / min);

[0031] The duration of the load applied to the iron ore sample layer is H2, and the magnitude of the load is P, 2.5h≤H2≤3.5h, 0≤P≤0.3MPa;

[0032] The flow rate of nitrogen introduced into the sponge iron sample during the cooling process is G2 until the sponge iron sample is cooled to the second preset temperature T2, 8L / min≤G2≤12L / min; 40℃≤T2≤60℃.

[0033] Optionally, detecting the bonding index of the sponge iron sample includes:

[0034] The sponge iron sample comprises sponge iron particles and sponge iron agglomerates, wherein the sponge iron agglomerates are formed by bonding two or more sponge iron particles, and the total mass M1 of the sponge iron sample and the total mass M2 of the sponge iron agglomerates are weighed;

[0035] The sponge iron agglomerates are placed in a rotating drum and rotated to disperse at least a portion of the sponge iron agglomerates into sponge iron particles, and the total mass M3 of the remaining sponge iron agglomerates is weighed;

[0036] Calculate the bonding index of the sponge iron sample, the bonding index of the sponge iron sample is K,

[0037]

[0038] Optionally, detecting the metallization rate of the sponge iron sample includes:

[0039] crushing the sponge iron sample until the particle size is less than 0.074 mm;

[0040] The total iron content in the sponge iron sample is detected as N1, and the metallic iron content in the sponge iron sample is detected as N2;

[0041] Calculate the metallization ratio MR of the sponge iron sample,

[0042]

[0043] Optionally, the rotation speed of the drum is V2, 25r / min≤V2≤35r / min; the diameter of the drum is d1, the ratio of the diameter d1 of the drum to the total mass M1 of the sponge iron sample is W1, 0.5mm / g≤W1≤0.6mm / g; the height of the drum is d2, the ratio of the height d2 of the drum to the total mass M1 of the sponge iron sample is W2, 0.8mm / g≤W2≤0.9mm / g.

[0044] As described above, the test device and test method for simulating the reaction in a hydrogen-based vertical furnace of the present invention have at least the following beneficial effects: (1) The reducing gas generating mechanism and the steam supply device are used in combination to provide reducing gas and steam to the reaction chamber, so that the reducing gas generating mechanism, the steam supply device, the load mechanism, the reactor and the electric heating furnace cooperate to more accurately simulate the reaction in the hydrogen-based vertical furnace, which is beneficial to improve the accuracy of the test results; (2) The inner wall of the inner tube of the reactor has an inclined wall, so that the inner wall of the reactor in contact with the sponge iron sample has an inclination, which does not damage the sponge iron sample, makes it easier to capture the bonding state of the sponge iron sample, and more accurately determines the bonding index of the sponge iron sample; (3) The mass of the iron ore sample used in the test method is variable and proportional to the reducing gas flow rate, which meets the test requirements of different scales. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 It is a schematic structural diagram of an embodiment of a test device for simulating a reaction in a hydrogen-based vertical furnace according to the present invention;

[0046] Figure 2 Display as Figure 1 Schematic diagram of the structure of the reactor.

[0047] Part Number Description

[0048] Electric heating furnace 1, furnace body 11, transverse thermocouple 12, reactor 2, outer tube 21, first bending portion 211, inner tube 22, lower tube section 221, upper tube section 222, lower port 223, second bending portion 224, support seat 23, reaction chamber 24, air inlet channel 25, top cover 26, reducing gas inlet 261, top coal gas outlet 262, first sealing member 27, second sealing member 28, load mechanism 3, driving member 31, pressure rod 32, pressure head 33, longitudinal thermocouple 34, air compressor 35, reducing gas generating mechanism 4, hydrogen supplier 41, methane supplier 42, carbon monoxide supplier 43, carbon dioxide supplier 44, nitrogen supplier 45, flow control box 46, pipeline assembly 47, iron ore sample layer 5, first corundum single ball layer 6, second corundum single ball layer 7, gas washing bottle 8, steam supplier 91, measuring cylinder 92. DETAILED DESCRIPTION

[0049] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0050] It should be noted that the diagram provided in the present embodiment only illustrates the basic concept of the present invention in a schematic manner, so the diagram only shows the components related to the present invention rather than drawing according to the number, shape and size of the components during actual implementation. The type, quantity and ratio of each component during actual implementation can be a random change, and the component layout type may also be more complicated. The structure, ratio, size, etc. illustrated in the drawings of the present specification are only used to match the content disclosed in the specification for people familiar with this technology to understand and read, and are not used to limit the limiting conditions that the present invention can implement, so they have no technical substantive significance. Any modification of the structure, change of the proportional relationship or adjustment of the size should still fall within the scope of the technical content disclosed by the present invention without affecting the effect that the present invention can produce and the purpose that can be achieved. At the same time, the terms such as "upper", "lower", "left", "right", "middle" and "one" quoted in this specification are only for the convenience of narration, and are not used to limit the scope of the present invention. The change or adjustment of its relative relationship should also be regarded as the scope of the present invention without substantially changing the technical content.

[0051] Before describing the embodiments of the present invention in detail, the application environment of the present invention is described first. The technology of the present invention is mainly applied to the field of hydrogen metallurgy technology, especially to simulate the reaction in a hydrogen-based vertical furnace, reduce the difference from the reaction in the furnace in actual production, make the reaction of the pellet sample in the reaction chamber closer to the reaction in actual working conditions, so that the sponge iron sample obtained after the reaction is also closer to the sponge iron sample in actual working conditions, and then make the detected bonding index and metallization rate of the sponge iron sample more accurate.

[0052] See also Figure 1 and Figure 2 In an optional embodiment, the present application provides a test device for simulating the reaction in a hydrogen-based vertical furnace, comprising an electric heating furnace 1, a reactor 2, a load mechanism 3, a reducing gas generating mechanism 4 and a steam supplier 91. The reactor 2 is placed in the electric heating furnace 1, and the reactor 2 has a reaction chamber 24 for accommodating an iron ore sample layer 5, and the iron ore sample layer 5 includes a pellet layer or a lump layer; at least a portion of the load mechanism 3 extends into the reaction chamber 24 to apply a load to the iron ore sample layer 5. The reducing gas generating mechanism 4 is connected to the reactor 2 and is used to introduce reducing gas into the reaction chamber 24, and the reducing gas generating mechanism 4 includes a hydrogen supplier 41, a methane supplier 42, a carbon monoxide supplier 43, a carbon dioxide supplier 44 and a nitrogen supplier 45, that is, the reducing gas introduced into the reaction chamber 24 can be a mixed reducing gas including a mixture of hydrogen, methane, carbon monoxide, carbon dioxide and nitrogen.

[0053] Optionally, the electric heating furnace 1 includes a furnace body 11, a transverse thermocouple 12 and a heating device. The furnace body 11 has a chamber for accommodating the reactor 2. The reactor 2 is placed in the chamber of the furnace body 11. The transverse thermocouple 12 passes through the furnace body 11 from the outside and then extends into the furnace body 11 to measure the temperature of the reactor 2. The heating device adjusts the heating temperature according to the temperature measurement information fed back by the transverse thermocouple 12, thereby realizing controllable heating of the iron ore sample layer.

[0054] Optionally, the hydrogen supplier 41 may be a gas cylinder filled with hydrogen, the methane supplier 42 may be a gas cylinder filled with methane, the carbon monoxide supplier 43 may be a gas cylinder filled with carbon monoxide, the carbon dioxide supplier 44 may be a gas cylinder filled with carbon dioxide, and the nitrogen supplier 45 may be a gas cylinder filled with nitrogen.

[0055] Optionally, the load mechanism 3 includes a driving member 31, a pressure head 33 and a longitudinal thermocouple 34 extending into the reaction chamber 24. The driving member 31 is connected to the pressure head 33 through a pressure rod 32, and drives the pressure head 33 to move longitudinally in the reaction chamber 24 to adjust the load on the iron ore sample layer 5. The longitudinal thermocouple 34 passes through the driving member 31, the pressure rod 32 and the pressure head 33 and then extends into the iron ore sample layer 5. The longitudinal thermocouple 34 can measure the temperature of the iron ore sample layer 5. The longitudinal thermocouple 34 and the transverse thermocouple 12 cooperate to measure the temperature at different positions. The heating device of the electric heating furnace 1 adjusts the heating temperature according to the temperature measurement information fed back by the longitudinal thermocouple 34 and the transverse thermocouple 12, so as to timely adjust the heating temperature. The heating temperature is highly controllable and the adjustment is more precise. Among them, the pressure rod 32 and the pressure head 33 can be moved and adjusted along the thickness direction of the iron ore sample layer 5 so as to adapt to the testing requirements of different amounts of iron ore sample layers 5. For example, the lower end of the pressure rod 32 is provided with a first mounting hole, and the upper end of the pressure head 33 is provided with a plurality of second mounting holes arranged along its axial direction. The upper end of the pressure head 33 is sleeved on the lower end of the pressure rod 32, and the pressure head 33 is lifted and moved along its axial direction so that the second mounting holes located at different heights are aligned with the first mounting holes and locked by a pin so that the pressure head 33 and the pressure rod 32 are relatively fixed, thereby realizing the relative movement adjustment of the pressure head 33 and the pressure rod 32. The relative movement adjustment range of the pressure head 33 and the pressure rod 32 can be between 30 mm and 70 mm, for example, it can be any value among 30 mm, 50 mm or 70 mm. Furthermore, the load mechanism 3 further includes an air compressor 35, the driving member 31 may be a cylinder, the air compressor 35 is connected to the cylinder to provide operating power for the cylinder, the cylinder is installed at the top of the reactor 2 through a bracket, and the output end of the cylinder is connected to the pressure rod 32 extending into the reaction chamber 24 to drive the pressure rod 32 to move up and down. The lower end of the longitudinal thermocouple 34 passes through the cylinder, the pressure rod 32 and the pressure head 33, and can be coaxially arranged with the cylinder, the pressure rod 32 and the pressure head 33, with a compact layout, which is beneficial to saving occupied space.

[0056] Optionally, the reducing gas generating mechanism 4 further includes a flow control box 46, which is respectively connected to the hydrogen supplier 41, the methane supplier 42, the carbon monoxide supplier 43, the carbon dioxide supplier 44 and the nitrogen supplier 45 to adjust the flow of the corresponding gas, that is, the output flow of each supplier can be adjusted and controlled by the flow control box 46, thereby controlling the flow of hydrogen, methane, carbon monoxide, carbon dioxide and nitrogen to meet the test requirements of different reducing atmospheres. Further, the flow control box 46 and the steam supplier 91 are connected to the reactor 2 through the pipeline assembly 47, wherein the pipeline assembly 47 includes a metal pipe and a steam heating belt, and the steam heating belt is an electric heating belt, and the heating temperature can exceed 150°C. Specifically, the flow control box 46 and the steam supplier 91 are both connected to the reactor 2 through the metal pipe, and the steam heating belt is independently wound around the metal pipe.

[0057] Optionally, the steam supplier 91 is connected to a measuring cylinder 92 . The steam supplier 91 may be a steam generator whose vaporization temperature is higher than 200° C. The measuring cylinder 92 is connected to the steam generator to provide a water source. The measuring cylinder 92 may contain liquid distilled water.

[0058] In the test device for simulating the reaction in a hydrogen-based vertical furnace in the above-mentioned embodiment, the reducing gas generating mechanism 4 can provide a mixed reducing gas of hydrogen, methane, carbon monoxide, carbon dioxide and nitrogen, and the steam supplier 91 can provide steam. The in-situ reforming of methane and steam at the tuyere is fully considered, and the simulated reaction conditions are closer to the actual production conditions, which is conducive to improving the accuracy of the test results.

[0059] See also Figure 1 and Figure 2 In an optional embodiment, the reactor 2 includes an inner tube 22 and an outer tube 21, the outer tube 21 includes an outer tube bottom wall and an outer tube side wall, the inner tube 22 is located in the outer tube 21 and supported on the outer tube bottom wall, the inner side wall of the inner tube 22 and the outer tube bottom wall together define a reaction chamber 24, an air inlet channel 25 is formed between the outer side wall of the inner tube 22 and the outer tube side wall, a ventilation structure is provided at the lower part of the inner tube 22 or between the inner tube 22 and the outer tube bottom wall, and the air inlet channel 25 is connected to the reaction chamber 24 through the ventilation structure.

[0060] Optionally, the ventilation structure is a through hole provided on the lower side wall of the inner tube 22 .

[0061] Optionally, the gap between the lower end wall of the inner tube 22 and the bottom wall of the outer tube is formed as a ventilation structure, and there is no need to open additional through holes. The assembly gap between the inner tube 22 and the bottom wall of the outer tube can be used to achieve the circulation of reducing gas and steam, which is conducive to simplifying the structure and improving the structural strength of the inner tube 22.

[0062] Optionally, the reactor 2 also includes a top cover 26, the lower end of the inner tube 22 extends into the outer tube 21, the upper end of the inner tube 22 and the upper end of the outer tube 21 are sealed by a first seal 27, the top cover 26 is sealed with the upper end of the inner tube 22 by a second seal 28, and the top cover 26 is provided with a reducing gas inlet 261 connected to the air inlet channel 25 and a top coal gas outlet 262 connected to the reaction chamber 24. Furthermore, the upper end of the outer tube 21 is bent outward and extended to form a first bending portion 211, and the upper end of the inner tube 22 is bent outward and extended to form a second bending portion 224, the second bending portion 224 is located above the first bending portion 211, and the first sealing member 27 is clamped between the first bending portion 211 and the second bending portion 224, and the first bending portion 211 and the second bending portion 224 cooperate to extrude the first sealing member 27 to achieve sealing; the top cover 26 is located above the second bending portion 224, and the second sealing member 28 is clamped between the top cover 26 and the second bending portion 224, and the top cover 26 and the second bending portion 224 cooperate to extrude the second sealing member 28 to achieve sealing, wherein the first sealing member 27 and the second sealing member 28 can be rubber gaskets, which are easy to deform and have good sealing performance; the first bending portion 211, the second bending portion 224, and the top cover 26 can be flanges, which are easy to connect and assemble.

[0063] Optionally, a support seat 23 located in the reaction chamber 24 is provided on the bottom wall of the outer tube, that is, the bottom end of the inner tube 22 is open to form a lower port 223, the inner tube 22 is located in the outer tube 21 and covers the support seat 23, wherein the inner tube 22 and the outer tube 21 can be coaxially arranged, and the support seat 23 is used to support the iron ore sample layer 5. Specifically, the support seat 23 includes a support plate and a plurality of support columns, the top of the support column is welded and fixed to the support plate, the bottom of the support column is welded and fixed to the bottom wall of the outer tube, the support column supports the support plate for supporting the iron ore sample layer 5, and the support plate is provided with air holes for the passage of reducing gas and steam, the reducing gas and steam enter the air inlet 25 from the reducing gas inlet 261, and are discharged to the washing bottle 8 from the top gas outlet 262 after flowing through the ventilation structure, the air holes, and the reaction chamber 24 in sequence. This structural design allows the reducing gas and steam to flow from top to bottom first, enter the reaction chamber 24 from the lower port 223 of the inner tube 22, and then flow from bottom to top out of the reaction chamber 24. The reducing gas and steam can be heated through the air inlet channel 25 before entering the reaction chamber 24, and the reaction efficiency is high. In particular, compared with the method of directly entering the reaction chamber 24, the reducing gas can be mixed and preheated in the air inlet channel 25 formed between the inner side wall of the inner tube 22 and the side wall of the outer tube before entering the reaction chamber 24, which is conducive to improving the reaction efficiency.

[0064] Optionally, the outer tube 21 is a stainless steel tube, which has good heat resistance, can withstand high temperatures above 1200° C., has deformation resistance, and has low cost.

[0065] Optionally, the inner tube 22 is a corundum tube, which has good heat resistance and is also beneficial to reducing the risk of bonding with the iron ore sample layer 5. The corundum tube is used in combination with the stainless steel tube, which can not only meet the use requirements of high temperature environment, but also helps to reduce costs.

[0066] Optionally, the inner wall of the inner tube 22 is an inclined wall. Further, the inner tube 22 can be a tapered tube, that is, the inner wall surface of the inner tube 22 is a tapered surface. The inclined setting of the inner wall of the inner tube 22 makes it easier to capture the agglomeration state of the sponge iron sample, and more accurately measure the bonding index and metallization rate; specifically, during the test, the sponge iron particles will bond with each other, so that the sponge iron sample will also bond with the inner wall surface of the inner tube 22, and the bonding state of the sponge iron sample is easily destroyed when it is taken out, and the inclined wall with an inclined design is conducive to reducing the risk of the sponge iron sample bonding with the inner wall of the inner tube 22, especially compared with the reaction tube of the existing direct reduction test equipment being a straight tube, the inclined setting of the inner wall of the inner tube 22 makes it possible to take out the sponge iron sample without using strong external force, reducing the difficulty of pushing the sponge iron sample out of the inner tube 22 and reducing the risk of damaging the bonding state of the sponge iron sample, thereby making it easier to capture the bonding state of the sponge iron sample, thereby improving the accuracy of the sponge iron sample bonding index detection.

[0067] Optionally, the inner tube 22 includes an upper tube section 222 and a lower tube section 221, the upper tube section 222 is located above the lower tube section 221, the upper tube section 222 is connected to the lower tube section 221 and is coaxially arranged, the upper tube section 222 is a straight tube, the inner side wall of the lower tube section 221 is an inclined wall, and the lower end of the upper tube section 222 is aligned with and connected to the upper end of the lower tube section 221. Further, the lower tube section 221 can be a tapered tube, that is, the inner wall surface of the lower tube section 221 is a tapered surface. Since the ambient temperature of the upper pipe section 222 is lower than that of the lower pipe section 221, the risk of adhesion between the upper pipe section 222 and the sponge iron sample is lower than that of the lower pipe section 221. The use of a straight pipe for the upper pipe section 222 is beneficial to reducing processing difficulty and cost, and the inner wall of the lower pipe section 221 is an inclined wall, which is beneficial to reducing the risk of adhesion between the sponge iron sample and the inner wall of the lower pipe section 221, reducing the difficulty of pushing the sponge iron sample out of the lower pipe section 221 and reducing the risk of damaging the bonding state of the sponge iron sample.

[0068] Optionally, the inner diameter of the pipe section with the inner side wall of the inner tube 22 being the inclined wall gradually increases from top to bottom, that is, the inner diameter of the pipe section with the inclined wall gradually increases from the end away from the lower port 223 to the end close to the lower port 223. Further, the angle between the inclined wall and the axis of the inner tube 22 is α, 2°≤α<10°; specifically, α can be any value among 2°, 5°, 7° or 9.5°.

[0069] In the test device for simulating the reaction in a hydrogen-based vertical furnace in the above-mentioned embodiment, the reactor 2 guides the flow direction of the reducing gas, and the inner tube 22 with an inclined structure can reduce the damage to the sponge iron sample, making it easier to capture the bonding state of the sponge iron sample, thereby improving the accuracy of the sponge iron bonding index measurement.

[0070] See also Figure 1 and Figure 2 In some optional embodiments, the present application further provides a test method, which is tested using a test device for simulating the reaction in a hydrogen-based vertical furnace as in any of the above embodiments, and includes the following steps:

[0071] The first corundum single ball layer 6, the iron ore sample layer 5 and the second corundum single ball layer 7 are sequentially laid from bottom to top in the reaction chamber 24. The iron ore sample layer 5 includes a pellet layer or a block layer. The particle sizes of the first corundum single ball layer 6, the iron ore sample layer 5 and the second corundum single ball layer 7 are all D, 10mm≤D≤12.5mm. The iron ore sample layer 5 is arranged between the first corundum single ball layer 6 and the second corundum single ball layer 7, which is beneficial to avoid the risk of the iron ore sample layer 5 adhering to the pressure head 33 and the support seat 23, and can also promote the uniform distribution of the reducing gas;

[0072] The iron ore sample layer 5 in the reactor is controllably heated by the electric heating furnace 1 to a first preset temperature T1, and nitrogen is introduced during the heating process. The iron ore sample layer 5 is heated to the first preset temperature T1 at a heating rate V1, and the flow rate of nitrogen during the heating process is G1, wherein 8°C / min≤V1≤12°C / min, 900°C≤T1≤1100°C, 8L / min≤G1≤12L / min, specifically, V1 can be any of 8°C / min, 10°C / min or 12°C / min, T1 can be any of 900°C, 1000°C or 1100°C, G1 can be any of 8L / min, 10L / min or 12L / min, and nitrogen is first introduced into the iron ore sample layer 5 during the heating process, which is beneficial to discharge the air in the reactor 2 and avoid the reduction of the iron ore sample layer 5 being affected by the air, thereby affecting the accuracy of the detection result;

[0073] The iron ore sample layer 5 is maintained at a first preset temperature T1, and steam and a mixed reducing gas including hydrogen, methane, carbon monoxide, carbon dioxide and nitrogen are introduced into the reaction chamber 24. When the introduction time of the steam and the mixed reducing gas reaches H1, a load is applied to the iron ore sample layer 5, and the ratio of the iron ore sample layer 5 to the mixed reducing gas is F, wherein 0.5h≤H1≤1.5h, 45g / (L / min)≤F≤55g / (L / min), specifically, H1 can be any value among 0.5h, 1h or 1.5h, and F can be any value among 45g / (L / min), 50g / (L / min) or 55g / (L / min);

[0074] A load is applied to the iron ore sample layer 5 by the load mechanism 3, and a sponge iron sample is obtained after the iron ore sample layer 5 is reduced. The time for applying the load to the iron ore sample layer 5 is H2, and the magnitude of the load is P, wherein 2.5h≤H2≤3.5h, 0≤P≤0.3MPa, specifically, H2 can be any value among 2.5h, 3h or 3.5h, and P can be any value among 0MPa, 0.1MPa or 0.3MPa, etc.;

[0075] After the load application time reaches H2, stop applying the load to the sponge iron sample, stop heating, stop introducing steam and stop introducing the mixed reducing gas, introduce nitrogen to cool the sponge iron sample, and the flow rate of nitrogen introduced into the sponge iron sample during the cooling process is G2 until the sponge iron sample is cooled to a second preset temperature T2, wherein 8L / min≤G2≤12L / min, T2 does not exceed 60°C, for example, 40°C≤T2≤60°C, specifically, G2 can be any value among 8L / min, 10L / min or 12L / min, and T2 can be any value among 40°C, 50°C or 60°C;

[0076] The cooled sponge iron sample is pushed out of the reaction chamber by a load mechanism, and the bonding index and / or the metallization rate of the sponge iron sample are detected.

[0077] Optional, testing of the bonding index of sponge iron specimens includes:

[0078] The sponge iron sample includes sponge iron particles and sponge iron agglomerates. The sponge iron agglomerates are formed by bonding two or more sponge iron particles. The total mass M1 of the sponge iron sample and the total mass M2 of the sponge iron agglomerates are weighed.

[0079] The sponge iron agglomerates are placed in a rotating drum and rotated to disperse at least a portion of the sponge iron agglomerates into sponge iron particles, and the total mass M3 of the remaining sponge iron agglomerates is weighed;

[0080] Calculate the bonding index of the sponge iron sample. The bonding index of the sponge iron sample is K.

[0081]

[0082] The number of revolutions of the drum can be set according to demand, for example, it can be any number such as 3 revolutions, 5 revolutions or 8 revolutions.

[0083] Optionally, testing the metallization rate of sponge iron samples includes:

[0084] Crushing the sponge iron sample until the particle size is less than 0.074 mm;

[0085] The total iron (TFe) content in the sponge iron sample is detected as N1, and the metallic iron (MFe) content in the sponge iron sample is N2;

[0086] Calculate the metallization ratio MR of the sponge iron sample,

[0087]

[0088] Optionally, the rotation speed of the drum is V2, 25r / min≤V2≤35r / min, the diameter of the drum is d1, the ratio of the diameter of the drum d1 to the total mass M1 of the sponge iron sample is W1, 0.5mm / g≤W1≤0.6mm / g, the height of the drum is d2, the ratio of the height of the drum d2 to the total mass M1 of the sponge iron sample is W2, 0.8mm / g≤W2≤0.9mm / g, specifically, V2 can be any value such as 25r / min, 30r / min or 35r / min, W1 can be any value such as 0.5mm / g, 0.55mm / g or 0.6mm / g, and W2 can be any value such as 0.8mm / g, 0.86mm / g or 0.9mm / g.

[0089] In the test method in the above embodiment, the mass of the iron ore sample layer can be changed according to demand, and the flow rate of the mixed reducing gas can be adjusted according to a certain flow rate ratio based on the mass of the iron ore sample layer, which can meet the test needs of different scales and is conducive to more accurate simulation of the reaction in the hydrogen-based vertical furnace.

[0090] The specific operation of the testing method is further described below with specific examples. It should be understood that the specific implementation methods of the present application are not limited to the following examples.

[0091] Embodiment 1:

[0092] The test method includes the following steps:

[0093] A first corundum single ball layer with a particle size of 10 mm to 12.5 mm is laid on the upper surface of the support seat, a 300 g iron ore sample layer with a particle size of 10 mm to 12.5 mm is placed on the upper surface of the first corundum single ball layer, and a second corundum single ball layer with a particle size of 10 mm to 12.5 mm is laid on the uppermost layer of the iron ore sample layer;

[0094] The outer tube, the inner tube and the load mechanism with the longitudinal thermocouple are connected, the longitudinal thermocouple is inserted into the center of the iron ore sample layer, and the pressure head touches the surface of the second corundum single ball layer lightly, and no load is applied at this time;

[0095] The electric heating furnace heats the iron ore sample layer in the reactor to 900°C, and nitrogen is introduced during the heating process with a flow rate of 10L / min and a heating rate of 10°C / min;

[0096] When the temperature of the iron ore sample layer reaches 900°C, start the steam supply device and the flow control box to introduce steam and a mixed reducing gas including hydrogen, carbon monoxide, carbon dioxide, methane and nitrogen into the reactor, and maintain the total flow of steam and mixed reducing gas at 6L / min;

[0097] After 1 hour of reduction, turn on the air compressor and start adding weight. The pressure of adding weight is 0 MPa, that is, no load is actually applied.

[0098] After loading for 3 hours, the load was removed, the steam was stopped, and the mixed reducing gas was switched to nitrogen. In other words, the hydrogen, carbon monoxide, carbon dioxide and methane in the mixed reducing gas were stopped, and the nitrogen flow rate was 10 L / min.

[0099] After the sample is cooled to 50°C, the sponge iron sample obtained after the reaction is gently pushed out from the lower end of the inner tube using a pressure rod to test the bonding index of the sponge iron sample;

[0100] The sponge iron samples were crushed to a particle size of <0.074 mm, and the TFe content and MFe content of the sponge iron samples were detected by chemical analysis, and the metallization rate of the sponge iron samples was calculated.

[0101] The test results show that the bonding index of the sponge iron sample before drumming is 8.32%, the bonding index after drumming is 0, and the average value is 4.16%; the TFe content of the sponge iron sample is 89.08%, the MFe content is 85.66%, and the metallization rate is 96.16%.

[0102] Example 2

[0103] The test method includes the following steps:

[0104] A first corundum single ball layer with a particle size of 10 mm to 12.5 mm is laid on the upper surface of the support seat, a 300 g iron ore sample layer with a particle size of 10 mm to 12.5 mm is placed on the upper surface of the first corundum single ball layer, and a second corundum single ball layer with a particle size of 10 mm to 12.5 mm is laid on the uppermost layer of the iron ore sample layer;

[0105] The outer tube, the inner tube and the load mechanism with the longitudinal thermocouple are connected through flanges, the longitudinal thermocouple is inserted into the center of the iron ore sample layer, and the pressure head touches the surface of the second corundum single ball layer lightly, and no load is applied at this time;

[0106] The electric heating furnace heats the iron ore sample layer in the reactor to 1100°C, and nitrogen is introduced during the heating process with a flow rate of 10L / min and a heating rate of 10°C / min;

[0107] When the temperature of the iron ore sample layer reaches 1100°C, start the steam generator and the flow control box to introduce steam and a mixed reducing gas including hydrogen, carbon monoxide, carbon dioxide, methane and nitrogen into the reactor, and maintain the total flow of steam and mixed reducing gas at 6L / min;

[0108] After 1 hour of reduction, turn on the air compressor and start adding weight. The pressure of the added weight is 0.3MPa.

[0109] After loading for 3 hours, the load was removed, the steam was stopped, and the mixed reducing gas was switched to nitrogen. In other words, the hydrogen, carbon monoxide, carbon dioxide and methane in the mixed reducing gas were stopped, and the nitrogen flow rate was 10 L / min.

[0110] After the sample is cooled to 50°C, the sponge iron sample obtained after the reaction is gently pushed out from the lower end of the inner tube using a pressure rod to test the bonding index of the sponge iron sample;

[0111] The sponge iron was crushed to a particle size of <0.074 mm, and the TFe content and MFe content of the sponge iron sample were detected by chemical analysis, and the metallization rate of the sponge iron sample was calculated.

[0112] The test results show that the bonding index of the sponge iron sample before drumming is 39.46%, the bonding index after drumming is 19.83%, and the average value is 29.65%; the TFe content of the sponge iron sample is 88.72%, the MFe content is 87.71%, and the metallization rate is 98.86%.

[0113] From the comparison between Example 1 and Example 2, it can be seen that increasing the temperature is beneficial to improving the metallization rate of the sponge iron sample, but it also strengthens the bonding of the particles of the sponge iron sample, affecting the discharge of the vertical furnace.

[0114] The test device and test method for simulating the reaction in a hydrogen-based vertical furnace of the present application contain methane and steam in the reducing gas, which improves the authenticity of the reducing gas composition and the accuracy of the characterization index, is more conducive to understanding the reaction mechanism in the hydrogen-based vertical furnace, and provides a reliable technical basis for actual working conditions.

[0115] In the description of this specification, the description with reference to the terms "this embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0116] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A test device for simulating the reaction in a hydrogen-based shaft furnace, characterized in that: include: Electric heating furnace; A reactor, the reactor being placed in the electric heating furnace, the reactor having a reaction chamber for accommodating an iron ore sample layer; A load mechanism, at least a portion of which extends into the reaction chamber to apply a load to the iron ore sample layer; A reducing gas generating mechanism, connected to the reactor and used to introduce reducing gas into the reaction chamber; A steam supplier is connected to the reactor and is used to introduce steam into the reaction chamber.

2. The test device for simulating the reaction in a hydrogen-based vertical furnace according to claim 1, characterized in that: The reactor comprises an inner tube and an outer tube, the outer tube comprises an outer tube bottom wall and an outer tube side wall, the inner tube is located inside the outer tube and supported on the outer tube bottom wall, the inner side wall of the inner tube and the outer tube bottom wall together define the reaction chamber, an air inlet channel is formed between the outer side wall of the inner tube and the outer tube side wall, a ventilation structure is provided at the lower part of the inner tube or between the inner tube and the outer tube bottom wall, and the air inlet channel is connected to the reaction chamber through the ventilation structure.

3. The test device for simulating the reaction in a hydrogen-based shaft furnace according to claim 2, characterized in that: The ventilation structure is a through hole arranged on the lower side wall of the inner tube, or the ventilation structure is formed by the gap between the lower end wall of the inner tube and the bottom wall of the outer tube.

4. The test device for simulating the reaction in a hydrogen-based shaft furnace according to claim 2, characterized in that: A support base located in the reaction chamber is provided on the bottom wall of the outer tube, and the support base includes a support plate and a plurality of support columns, the top and bottom of the support columns are respectively welded and fixed to the support plate and the bottom wall of the outer tube, the support plate is used to support the iron ore sample layer, and the support plate is provided with air holes for the reducing gas and the steam to pass through.

5. The test device for simulating the reaction in a hydrogen-based vertical furnace according to claim 2, characterized in that: The outer tube is a stainless steel tube, and the inner tube is a corundum tube.

6. The test device for simulating the reaction in a hydrogen-based vertical furnace according to claim 2, characterized in that: The inner side wall of the inner tube is an inclined wall.

7. The test device for simulating the reaction in a hydrogen-based vertical furnace according to claim 2, characterized in that: The inner tube comprises an upper tube section and a lower tube section which are connected to each other. The upper tube section is a straight tube, and the inner side wall of the lower tube section is an inclined wall.

8. The test device for simulating the reaction in a hydrogen-based vertical furnace according to claim 6 or 7, characterized in that: The inner diameter of the pipe section whose inner side wall is an inclined wall gradually increases from top to bottom.

9. The test device for simulating the reaction in a hydrogen-based shaft furnace according to claim 8, characterized in that: The angle between the inclined wall and the axis of the inner tube is α, 2°≤α<10°.

10. The test device for simulating the reaction in a hydrogen-based vertical furnace according to claim 2, characterized in that: The reactor also includes a top cover, the lower end of the inner tube extends into the outer tube, the upper end of the inner tube is sealed with the upper end of the outer tube by a first seal, the top cover is sealed with the upper end of the inner tube by a second seal, and the top cover is provided with a reducing gas inlet connected to the air inlet channel and a top coal gas outlet connected to the reaction chamber.

11. The test device for simulating the reaction in a hydrogen-based vertical furnace according to claim 1, characterized in that: The load-bearing mechanism includes a driving member, a pressure head and a longitudinal thermocouple extending into the reaction chamber. The driving member is connected to the pressure head through a pressure rod, and drives the pressure head to move longitudinally in the reaction chamber to adjust the load on the iron ore sample layer. The longitudinal thermocouple passes through the driving member, the pressure rod and the pressure head and then extends into the iron ore sample layer.

12. The test device for simulating the reaction in a hydrogen-based vertical furnace according to claim 1, characterized in that: The reducing gas generating mechanism includes a hydrogen supplier, a methane supplier, a carbon monoxide supplier, a carbon dioxide supplier, a nitrogen supplier and a flow control box. The flow control box is respectively connected to the hydrogen supplier, the methane supplier, the carbon monoxide supplier, the carbon dioxide supplier and the nitrogen supplier to adjust the flow of the corresponding gas. The flow control box and the steam supplier are connected to the reactor through a pipeline assembly.

13. A testing method, using the testing device for simulating the reaction in a hydrogen-based shaft furnace as claimed in any one of claims 1 to 12, characterized in that: The following steps are involved: Laying a first corundum single ball layer, an iron ore sample layer, and a second corundum single ball layer in sequence from bottom to top in the reaction chamber; The iron ore sample layer in the reactor is heated to a first preset temperature T1 by the electric heating furnace, and nitrogen is introduced during the heating process; The iron ore sample layer is maintained at the first preset temperature T1, and a mixed reducing gas of steam and hydrogen, methane, carbon monoxide, carbon dioxide and nitrogen is introduced into the reaction chamber; a load is applied to the iron ore sample layer by the load mechanism, and a sponge iron sample is obtained after the iron ore sample layer is reduced; Stop applying load to the sponge iron sample, stop heating, stop introducing the steam and stop introducing the mixed reducing gas, and introduce nitrogen to cool the sponge iron sample; The cooled sponge iron sample is pushed out of the reaction chamber by the load mechanism, and the bonding index of the sponge iron sample and / or the metallization rate of the sponge iron sample are detected.

14. The testing method according to claim 13, characterized in that: The particle sizes of the first corundum single spherical layer, the iron ore sample layer and the second corundum single spherical layer are all D, 10 mm≤D≤12.5 mm; The iron ore sample layer is heated to a first preset temperature T1 at a heating rate V1, and the flow rate of the nitrogen during the heating process is G1, 8°C / min≤V1≤12°C / min, 900°C≤T1≤1100°C, 8L / min≤G1≤12L / min; When the duration of the introduction of the steam and the mixed reducing gas reaches H1, a load is applied to the iron ore sample layer, and the ratio of the iron ore sample layer to the mixed reducing gas is F, 0.5h≤H1≤1.5h, 45g / (L / min)≤F≤55g / (L / min); The duration of the load applied to the iron ore sample layer is H2, and the magnitude of the load is P, 2.5h≤H2≤3.5h, 0≤P≤0.3MPa; The flow rate of nitrogen introduced into the sponge iron sample during the cooling process is G2 until the sponge iron sample is cooled to the second preset temperature T2, 8L / min≤G2≤12L / min; 40℃≤T2≤60℃.

15. The testing method according to claim 13, characterized in that: Testing the bonding index of the sponge iron sample includes: The sponge iron sample comprises sponge iron particles and sponge iron agglomerates, wherein the sponge iron agglomerates are formed by bonding two or more sponge iron particles, and the total mass M1 of the sponge iron sample and the total mass M2 of the sponge iron agglomerates are weighed; The sponge iron agglomerates are placed in a rotating drum and rotated to disperse at least a portion of the sponge iron agglomerates into sponge iron particles, and the total mass M3 of the remaining sponge iron agglomerates is weighed; Calculate the bonding index of the sponge iron sample, the bonding index of the sponge iron sample is K, 16. The testing method according to claim 13, characterized in that: Detecting the metallization rate of the sponge iron sample includes: crushing the sponge iron sample until the particle size is less than 0.074 mm; The total iron content in the sponge iron sample is detected as N1, and the metallic iron content in the sponge iron sample is detected as N2; Calculate the metallization ratio MR of the sponge iron sample, 17. The testing method according to claim 15, characterized in that: The rotation speed of the drum is V2, 25r / min≤V2≤35r / min; the diameter of the drum is d1, and the ratio of the diameter d1 of the drum to the total mass M1 of the sponge iron sample is W1, 0.5mm / g≤W1≤0.6mm / g; the height of the drum is d2, and the ratio of the height d2 of the drum to the total mass M1 of the sponge iron sample is W2, 0.8mm / g≤W2≤0.9mm / g.