Improved method for measuring heat conductivity coefficient of heat-conducting film based on steady-state electrothermal method

By optimizing the test process of steady-state electric heating method, combined with experiments and simulations, the problems of large errors and high uncertainties in thermal conductivity measurement technology are solved, and efficient and accurate thermal conductivity measurement is achieved, which simplifies the operation steps and improves the repeatability .

CN119086638APending Publication Date: 2024-12-06ZHEJIANG UNIV +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411222530.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing thermal conductivity measurement technology has problems such as complex testing process, long time, poor repetition of results and limited application scope of samples. Especially in the steady-state electric heating method, the test error is large, the uncertainty is high, and the sample preparation is difficult, which seriously affects the test. Accuracy and reliability of results.

Method used

By combining experiments and simulations, the testing process of the steady-state electrothermal method is optimized. The specific steps include collecting surface temperature data under steady-state conditions, fitting curves, calculating temperature difference and thermal conductivity, controlling sample size and device conditions, reducing measurement errors and Uncertainty, the heating power and temperature difference curves are fitted using a positive proportional function to calculate the thermal conductivity to ensure measurement accuracy and repeatability.

Benefits of technology

Achieve a reduction in measurement error to 3.0%, uncertainty to 0.5%, and response time to milliseconds, improving the accuracy and repeatability of test results, simplifying the operation steps, eliminating the measurement of thermal conductivity of thermal radiation and thermal convection The impact of

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119086638A_ABST
    Figure CN119086638A_ABST
Patent Text Reader

Abstract

The invention designs the improved method for measuring the heat conduction coefficient of the heat conduction film based on the steady-state electrothermal method, and the precision and efficiency of heat conduction measurement are remarkably improved. An improved steady-state electrothermal method is adopted, and the in-plane heat conduction coefficient is obtained based on temperature distribution of the surface of the heat conduction film under different powers. According to the method, the measurement error is lower than 3.0%, the uncertainty is reduced to 0.5%, and the response time reaches the millisecond level. The method provides beneficial guidance for accurately evaluating the heat-conducting property of the material, and also provides technical support for thermal management engineering application of the graphite film material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of thermal conductivity measurement, and in particular to a method for measuring thermal conductivity of a thermally conductive film material. Background Art

[0002] In the era of artificial intelligence, the integration and performance requirements of electronic devices are increasing. The research and development of efficient heat dissipation materials has become an important challenge for the innovation and replacement of electronic devices. As one of the key properties for evaluating thermal conductive films, the accuracy of thermal conductivity measurement results not only helps promote the development of basic research on heat transfer, but is also crucial for product design optimization in practical engineering applications.

[0003] Existing thermal conductivity measurement technologies can be divided into steady-state methods and non-steady-state (transient) methods according to the test principles. When using steady-state methods (such as heat flow method, protected hot plate method, etc.) for measurement, the sample temperature does not change with time, the signal analysis is simple, in line with the actual application scenario, and the authenticity is high. However, it is necessary to design a measuring device that matches the sample size, and there are problems such as long test time, large contact thermal resistance, and limited test range. Non-steady-state methods (such as laser flash method, planar heat source method, etc.) can be measured during the heating process, with rapid and efficient measurements, but difficult data processing, higher uncertainty, and more influencing factors. In short, the existing commercial thermal measurement technology is limited by factors such as test principles, sample size, and device structure, resulting in a complex test process, long test time, poor repeatability of test results, and a limited range of sample applications.

[0004] Steady-state electrothermal method is a widely used thermal conductivity measurement method for micro-nano materials. The basic principle is to apply current to the sample to generate Joule heat, and calculate the thermal conductivity based on the steady-state temperature distribution of the sample. At present, there is no detailed basic research on the steady-state electrothermal method, so there are a series of problems such as large test errors, high uncertainty, and difficulty in sample preparation, which seriously affect the accuracy and reliability of the test results. Summary of the invention

[0005] In view of the above problems, the present invention provides a method for testing the thermal conductivity of a thermally conductive film. The method combines experiments and simulations, analyzes the basic principles of testing, and ingeniously constrains the testing process from three aspects: sample size, device conditions, and data processing, thereby reducing the test error to 3.0%, the test uncertainty to 0.5%, and the response time to milliseconds. This makes the test method have good accuracy and repeatability, and high test efficiency.

[0006] The thermally conductive film of the present invention includes, but is not limited to, various films and fiber materials such as graphene film, artificial carbon film, graphene fiber, carbon fiber, and metal.

[0007] Under steady-state conditions, based on the heat conduction formula and the energy conservation theorem, the following equation can be obtained:

[0008]

[0009] Where λ(T(x)) is the thermal conductivity of the thermally conductive film at temperature T(x), A C is the cross-sectional area, L is the half-length of the sample, P is the perimeter of the sample cross section, ε is the emissivity, σ is the Stefan-Boltzmann constant, and Ta is the ambient temperature. The traditional steady-state electrothermal method usually directly ignores the change of thermal conductivity with temperature (i.e. ) and heat loss due to thermal radiation and convection, the above formula can be simplified to But this can easily lead to huge measurement errors.

[0010] Therefore, the technical solution of the present invention is to provide a method for testing the thermal conductivity of a thermally conductive film improved based on a steady-state electrothermal method, and the specific steps are as follows:

[0011] (1) placing the thermal conductive film to be tested on two heat sinks with a spacing of 2L; heating the thermal conductive film to be tested with a heating power P;

[0012] (2) forming multiple measurement points along the length direction of the thermal conductive film between the two heat sinks, collecting the surface temperature values ​​of different measurement points, and obtaining measurement data (x, T), where x is the coordinate value of the measurement point and T is the measured temperature of the measurement point;

[0013] Using the quadratic equation T(x)=ax 2 +T o Fit the measured data (x, T) to obtain the Tx fitting curve;

[0014] (3) Changing the heating power to form multiple fitting curves, the multiple fitting curves intersect at two points, the two intersection points have the same temperature value Ts, and the distance between the two intersection points is 2L OA ;

[0015] Calculate the temperature T corresponding to the highest point of each fitting curve o , get T o and T s The temperature difference △T;

[0016] (4) Using different heating powers P and temperature differences △T, a direct proportional function is used to fit the heating power P-temperature difference △T curve to obtain the slope b;

[0017] (5) According to the formula λ=bL OA / 4A C Calculate the thermal conductivity λ of the sample being tested; where A C is the cross-sectional area, A C =thickness*width.

[0018] In the embodiment of the present invention, the heating method of step 2 is: inputting a constant current power supply to the thermal conductive film to be tested; testing the voltage at both ends, and then calculating the heating power P, P=UI.

[0019] In an embodiment of the present invention, a layer of spray with known emissivity can be sprayed onto the surface of the thermal conductive film and heat sink to be tested. The spray is coated with graphite, gold or platinum to keep the sample emissivity uniform and stable, and the thickness is less than 30% of the sample thickness to prevent affecting the electrical and thermal conductivity of the sample.

[0020] In the embodiment of the present invention, the maximum value T of the thermal conductive film to be tested o The range is controlled between room temperature and 60°C to ensure that the thermal conductivity of the thermal conductive film changes negligibly within this temperature range, that is, the second term of formula 1 satisfy Where K is a constant. And control the temperature rise △T OA <40℃, the fourth and fifth items of formula 1 can be controlled, that is, the heat loss caused by thermal radiation and thermal convection is less than 0.5% of the heat loss caused by thermal conduction, which can reduce the measurement error and improve the test accuracy.

[0021] In the embodiment of the present invention, initialization is performed in the following manner to ensure the stability of the test: when the sample temperature changes by less than 0.1°C and does not change monotonically, data is formally collected to ensure that the sample reaches a steady-state temperature and improve test accuracy.

[0022] In an embodiment of the present invention, the midpoints of the two heat sinks are taken as the origin, and the temperature distribution data within the range of 0 to 0.8L on both sides of the origin are collected to construct the sample surface temperature distribution curve. Because simulation calculations show that the temperature distribution in the sample thickness direction outside the range of 0.8L will cause the measurement results to be biased, especially for thick film samples, the error can even be several times. The internal isothermal surfaces of the sample within the range of 0 to 0.8L on both sides of the center point O of the sample segment being measured are parallel to each other and perpendicular to the length direction of the sample. The results of fitting this part of the data have higher measurement accuracy and smaller errors.

[0023] In an embodiment of the present invention, the quadratic equation in step (5) is T(x)=ax 2 +T O ; where a is the coefficient, x is the distance from the measuring point to the origin O, and T is the surface temperature of the measuring point; T O is the temperature of the center point (i.e. x=0).

[0024] According to formula 1, the measurement error caused by thermal radiation and thermal convection is mainly related to the specific surface area and thermal conductivity of the sample. Simplifying formula 1, where the second term is 0, the surface temperature of the sample is expressed in the form of temperature rise ΔT(x) (=T(x)-Ta) to obtain make Where C and D are constants, we can get If and only if, PL 2 / (KA c )≤0.00228, when the sample surface temperature distribution curve is fitted by the quadratic equation in step (5), the correlation coefficient R 2 ≥0.995. Therefore, in the embodiment of the present invention, the length range of the thermal conductive film to be measured is controlled to be 2L∈[100·t, 0.0955·(λ 0 A C / C) 1 / 2 ], the width is less than 0.2*L; where t is the thickness of the thermal conductive film to be tested, C is the circumference of the cross section of the thermal conductive film to be tested, and A C is the cross-sectional area, the cross-sectional area is the plane formed by the thickness and width of the thermal conductive film to be measured, λ 0 is the estimated value of thermal conductivity of the film sample, and L is the half length of the sample.

[0025] In an embodiment of the present invention, two auxiliary heat sinks are further included, which are located on both sides of the aforementioned heat sink; the long film containing the thermally conductive film to be tested is placed on four heat sinks, and a constant DC current is applied to the thermally conductive film to be tested through the two auxiliary heat sinks. As a preferred solution, a conductive paste is evenly applied on the auxiliary heat sinks, and the thermally conductive film to be tested is placed on the conductive paste and fixed. The conductive paste uses high-purity silver paste with excellent thermal / electrical conductivity to reduce the contact thermal resistance and contact resistance between the sample and the heat sink.

[0026] Usually, the size of the thermal conductive film to be tested can be measured using a vernier caliper, a screw positioner, a scanning electron microscope, a thickness gauge, etc. Each sample size is measured 5 times and the arithmetic average is taken.

[0027] Generally, the heat sink has good electrical and thermal conductivity, and includes but is not limited to metal, alloy, graphite block, etc.

[0028] Typically, temperature measurement methods (temperature acquisition methods) include, but are not limited to, infrared thermometers, Raman confocal methods, heat flow meters, thermocouples, and the like.

[0029] In an embodiment of the present invention, the following steps are performed:

[0030] (1) Remove impurities, dust and other attachments on the surface of the sample, cut the thermal conductive film to be tested into specified sizes, and measure its dimensional parameters.

[0031] (2) Apply the conductive paste evenly on the heat sink and auxiliary heat sink, in the order of 1, 2, 3, 4, set the middle distance of the heat sink to 2L, and place the thermal conductive film to be tested on the conductive paste.

[0032] (3) Spray a layer of spray with known emissivity onto the thermal conductive film to be tested and the surface of the heat sink.

[0033] (4) The prepared sample is placed in a vacuum chamber and connected to four heat sinks by a four-wire method. The sample segment between the two middle heat sinks is the sample segment to be tested (i.e., the thermal conductive film to be tested in the present application). The four-wire method is used to connect the four heat sinks, wherein the auxiliary heat sinks 1 and 4 apply a constant current, and the heat sinks 2 and 3 are used to measure the voltage drop U of the sample segment to be tested.

[0034] (5) Control the power supply to apply a constant DC current to the sample segment under test, measure the voltage drop U on the sample segment under test, and calculate the heating power P. Measure the transverse temperature distribution (x, T) on the surface of the sample segment under test, where x is the coordinate value of the measurement point and T is the measured temperature of the measurement point. When the sample temperature deviation is less than 0.1°C and does not change monotonically, it is considered to have reached a steady state, and formally collect data Q = (x, T).

[0035] (6) Repeat step (5) by sequentially changing the constant current applied by the power supply to obtain the voltage U and the sample surface temperature distribution curve Q under different currents.

[0036] (7) Use a quadratic equation to fit different temperature distributions to obtain fitting curves. The fitting curves of sample surface temperature distribution under different current conditions will intersect at two points A. 1 (L OA , T s ) and A 2 (-L OA , T s ). Where L OA is the effective half length of the sample, T s is the stable temperature of the sample in contact with the heat sink. According to the highest point O of each fitting curve, the corresponding temperature is T o , calculate T at different currents o and T s The temperature difference △T and the heating power P of the sample section being tested, P=UI.

[0037] (8) A proportional function is used to fit the heating power P-temperature difference △T curve under different currents, and the slope b is obtained.

[0038] P=b*△T (2)

[0039] (9) The thermal conductivity λ of the sample is calculated by the following formula.

[0040] λ=bL OA / 4A C (3)

[0041] Among them, A C A is the cross-sectional area of ​​the sample segment being tested, C =thickness*width.

[0042] The sample to be tested should have good electrical conductivity and remain uniform, complete and consistent.

[0043] The length range of the sample segment to be tested should be controlled to be 2L∈[100·t,0.0955·(λ 0 A C / C) 1 / 2 ], the width should be less than 0.2*L. Where t is the thickness of the sample to be tested, A C is the cross-sectional area of ​​the sample segment under test, C is the perimeter of the cross-sectional area of ​​the sample segment under test, and L is the half length of the sample segment under test.

[0044] The maximum value T of the transverse temperature of the sample section under test o The range should be controlled between room temperature and 60℃.

[0045] The step (7) comprises the following steps:

[0046] (71) Select the temperature distribution data within the range of 0 to 0.8 L on both sides of the center point O of the sample segment to be measured, and use the following quadratic equation to fit the temperature T and distance x:

[0047] T(x)=ax 2 +T o (3)

[0048] (72) The transverse temperature distribution curves under different given current conditions are summarized and intersect at two points A 1 (L OA , T s ) and A 2 (-L OA , T s ). Among them, L OA is the effective half length of the sample segment being tested, T s is the temperature at both ends of the sample segment being tested.

[0049] The beneficial effects of the present invention are as follows: by optimizing three aspects, namely, sample size control, test device design and data processing optimization, the measurement error is controlled within 3.0%, the uncertainty is reduced to 0.5%, the steady-state response time reaches the millisecond level, and the influence of heat loss such as thermal radiation and thermal convection on the thermal conductivity measurement can be eliminated. The operation steps are simple and the test results are accurate. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] Figure 1 It is a schematic diagram of thermal conductivity test of the present invention;

[0051] Figure 2 It is a flow chart of thermal conductivity test of the present invention;

[0052] Figure 3 is the surface temperature distribution curve of the sample at different powers in Example 1;

[0053] Figure 4 is the fitting curve of sample surface temperature at different powers in Example 1;

[0054] Figure 5 is the power and sample surface temperature difference fitting curve of Example 1;

[0055] Figure 6 is a temperature response diagram of a sample in a thermal conductivity test in Example 1;

[0056] Figure 7 These are the test results of multiple samples cut from the same film in Example 1;

[0057] Figure 8 The results are compared between Example 1 and a common commercial thermal conductivity tester;

[0058] Fig. 9 It is the temperature distribution curve under different sample size parameters. DETAILED DESCRIPTION

[0059] The present invention is specifically described below through examples. The examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art may make some non-essential changes and adjustments based on the contents of the above invention, which all fall within the scope of protection of the present invention.

[0060] In the present invention, the half length is the distance from the center of the sample to the end point of the sample, that is, half the length of the thermal conductive film to be tested.

[0061] Embodiment 1:

[0062] Taking a graphene film with a thickness of 25 μm as an example, the thermal conductivity measurement method of the present invention comprises the following steps:

[0063] (1) Cut the complete and uniform graphene film into strip samples of 40 mm x 1 mm.

[0064] (2) Thermal conductivity test schematic diagram Figure 1 , set the distance between the heat sink and the auxiliary heat sink, that is, the distance between copper blocks 1, 2 and 3, 4 is 10mm, and the distance between the heat sinks, that is, the distance between copper blocks 2, 3 is 10mm. Apply high-purity silver glue evenly on the heat sink and the auxiliary heat sink, and place the strip thermal conductive film sample on the silver glue, and wait for the silver glue to solidify.

[0065] (3) Spray a thin layer of amorphous graphite spray onto the surface of the test sample and the heat sink, and set the infrared camera emissivity value to 0.85.

[0066] (4) Place the heat sink in the vacuum chamber and connect the four heat sinks in sequence using the four-wire method. The length of the sample between the two middle heat sinks is the sample segment to be tested. In this embodiment, the length of the sample segment to be tested is 2L, which is 10 mm. Set the vacuum degree of the chamber to 10 -4 Entrust.

[0067] (5) The control power supply applies a constant DC current of 800 mA to the sample segment under test, measures the voltage drop U on the sample segment under test, and uses an infrared thermometer to measure the lateral temperature distribution on the surface of the sample segment under test. When the temperature fluctuation on the sample surface is less than 0.1 K for 3 consecutive seconds and does not change monotonically, it is considered that a steady state has been reached. The voltage drop U on the sample segment under test and the surface temperature distribution curve Q are recorded.

[0068] (6) The current is increased by 300 mA until the constant current reaches 2900 mA, and step (5) is repeated to obtain the voltage U and sample surface temperature distribution curve Q under different currents, as shown in FIG. Figure 3 shown.

[0069] (7) Select the temperature distribution data within the range of 0 to 0.8 L on both sides of the center point O of the sample segment to be measured, and use the quadratic equation T(x) = ax 2 +T O Fit the temperature T and distance x, such as Figure 4 As shown in Figure 2, the fitting curves of the sample surface temperature distribution under different current conditions will intersect at two points A. 1 (4.5, 295.8) and A 2 (-4.5, 295.8). The effective half length of the sample is L OA The stable temperature T of the sample in contact with the heat sink is 4.5 mm. s is 295.8K. According to the highest point O of each fitting curve, the corresponding temperature is T o , calculate the temperature difference △T between points O and A and the heating power P of the sample section under different currents, P=UI.

[0070] (8) A proportional function is used to fit the heating power P-temperature difference ΔT curve under each current. According to the formula P = b*ΔT, the slope b is 0.02149, as shown in Figure 5 shown.

[0071] (9) According to the formula λ=bL OA / 4A C The thermal conductivity λ of the sample under test is calculated to be 967 W / mK.

[0072] The same film sample was used to perform thermal conductivity tests using different commonly used commercial thermal conductivity test instruments. The test results are as follows: Figure 8 As shown, the test results of this embodiment are similar to those of a commercial thermal conductivity tester, and the test results are reliable.

[0073] pass Figure 7 It can be seen that the results obtained by the thermal conductivity test of this embodiment have good measurement repeatability and accuracy. By testing the thermal conductivity test results of 10 samples of the same size made on the same film, it can be concluded that the deviation of the test results obtained by the present invention is less than 3.0%. And after test calculations, see Table 1, it is concluded that the uncertainty of the test of the present invention is less than 0.5%.

[0074] Table 1 Summary of uncertainty of each parameter

[0075] Test Parameters unit Test range Uncertainty Sample half length L mm 0~10 0.0002 Sample width w μm 0~1000 0.0001 Sample thickness t μm 0~500 0.002 Current I mA 0~7000 0.00015 Voltage U mV 0~5000 0.0002 Temperature rise △T K 0~40 0.005

[0076] Comparative Example 1:

[0077] Compared with Example 1, the only difference is:

[0078] Step (1) The same graphene film is cut into strips of 60 mm x 1 mm. This does not meet the requirement of 2L∈[100·t,0.0955·(λ 0 A C / C) 1 / 2 ]Require.

[0079] Step (2) sets the distance between heat sinks 1, 2 and 3, 4 and the auxiliary heat sink to 10 mm, and the distance between heat sinks 2, 3 to 30 mm.

[0080] Step (5) controls the power supply to apply a constant direct current of 500 mA to the sample segment under test.

[0081] Step (6) increases the current by 200 mA successively until the constant current reaches 1500 mA.

[0082] At this time, the slope b calculated in step (8) is 0.06267.

[0083] Step (9) calculates the thermal conductivity λ of the sample to be tested to be 5641 W / mK.

[0084] The results of Example 1 and Comparative Example 1 show that Fig. 9 As shown, the beneficial effect of sample size control on detection accuracy in the present invention is verified. Two sizes of thermal conductive films are used for thermal conductivity testing. Example 1 meets the size requirements of the present invention, that is, the length range of the thermal conductive film to be tested in claim 1 is controlled to be 2L∈[100·t, 0.0955·(λ 0 A C / C) 1 / 2 ], the width is less than 0.2*L; where t is the thickness of the thermal conductive film to be tested, C is the circumference of the cross section of the thermal conductive film to be tested, and A C is the cross-sectional area, the cross-sectional area is the plane formed by the thickness and width of the thermal conductive film to be measured, λ 0is the estimated value of the thermal conductivity of the film sample, and L is the half length of the sample. Another comparative example 1 does not meet the size requirements of the present invention. Fig. 9 It can be seen that the thermal conductivity data fitting curve obtained by the sample meeting the size requirements of the present invention is better and the measurement result is more accurate. Figure 8 The results also proved the accuracy of the measurement after size adjustment.

[0085] Embodiment 3:

[0086] (1) A complete and uniform graphene film with a thickness of 25 μm was cut into strip samples of 40 mm x 1 mm.

[0087] (2) Thermal conductivity test sample stage settings see Figure 2 , set the distance between the copper blocks of heat sinks 1, 2 and 3, 4 to 10mm, and the distance between heat sinks 2, 3 to 8mm. Apply high-purity silver glue evenly on the four heat sinks, place the strip sample on the silver glue, and wait for the silver glue to solidify.

[0088] (3) Spray a thin layer of amorphous graphite spray onto the surface of the test sample and the heat sink, and set the infrared camera emissivity value to 0.85.

[0089] (4) Place the heat sink in the vacuum chamber and connect the four heat sinks in sequence using the four-wire method. The length of the sample between the two middle heat sinks is the sample segment to be tested. In this embodiment, the length of the sample segment to be tested is 8 mm. Set the vacuum degree of the chamber to 10 -4 Entrust.

[0090] (5) The control power supply applies a constant DC current of 450 mA to the sample segment under test, measures the voltage drop U on the sample segment under test, and uses an infrared thermometer to measure the lateral temperature distribution on the surface of the sample segment under test. When the temperature fluctuation on the sample surface is less than 0.1 K for 3 consecutive seconds and does not change monotonically, it is considered that a steady state has been reached, and the voltage drop and surface temperature distribution curve on the sample segment under test are recorded.

[0091] (6) The current was increased by 150 mA successively until the constant current reached 1650 mA, and step (5) was repeated to obtain the voltage U and sample surface temperature distribution curves under different currents.

[0092] (7) Select the temperature distribution data within the range of 0-0.8L on both sides of the center point O of the sample segment to be measured, and use the quadratic equation T(x) = ax 2 +T o Fitting the temperature T and distance x, the fitting curves of the sample surface temperature distribution under different current conditions will intersect at two points A 1 (4.2, 301.1) and A 2 (-4.2, 301.1). The effective half length of the sample is L OAThe stable temperature T of the sample in contact with the heat sink is 4.2 mm. s is 301.1K. According to the highest point O of each fitting curve, the corresponding temperature is T o , calculate the temperature difference △T between points O and A under different currents and the heating power P of the sample segment under test, P=UI.

[0093] (8) A proportional function is used to fit the heating power P-temperature difference ΔT curve under each current. According to the formula P=b*ΔT, the slope b is 0.02269.

[0094] (9) According to the formula λ=bL OA / 4A C The thermal conductivity λ of the sample under test is calculated to be 953 W / mK.

[0095] Embodiment 4:

[0096] (1) A complete and uniform graphene film with a thickness of 25 μm was cut into strip samples of 40 mm x 1 mm.

[0097] (2) Thermal conductivity test sample stage settings see Figure 2 , set the distance between the copper blocks of heat sinks 1, 2 and 3, 4 to 10mm, and the distance between heat sinks 2, 3 to 6mm. Apply high-purity silver glue evenly on the four heat sinks, place the strip sample on the silver glue, and wait for the silver glue to solidify.

[0098] (3) Spray a thin layer of amorphous graphite spray onto the surface of the test sample and the heat sink, and set the infrared camera emissivity value to 0.85.

[0099] (4) Place the heat sink in the vacuum chamber and connect the four heat sinks in sequence using the four-wire method. The length of the sample between the two middle heat sinks is the sample segment to be tested. In this embodiment, the length of the sample segment to be tested is 6 mm. Set the vacuum degree of the chamber to 10 -4 Entrust.

[0100] (5) The control power supply applies a constant DC current of 600 mA to the sample segment under test, measures the voltage drop U on the sample segment under test, and uses an infrared thermometer to measure the lateral temperature distribution on the surface of the sample segment under test. When the temperature fluctuation on the sample surface is less than 0.1 K for 3 consecutive seconds and does not change monotonically, it is considered that a steady state has been reached, and the voltage drop and surface temperature distribution curve on the sample segment under test are recorded.

[0101] (6) The current was increased by 300 mA successively until the constant current reached 2700 mA, and step (5) was repeated to obtain the voltage U and sample surface temperature distribution curves under different currents.

[0102] (7) Select the temperature distribution data within the range of 0-0.8L on both sides of the center point O of the sample segment to be measured, and use the quadratic equation T(x) = ax2 +To fits the temperature T and distance x, and the fitting curves of the sample surface temperature distribution under different current conditions will intersect at two points A1 (2.9, 297.9) and A2 (-2.9, 297.9). The effective half-length LOA of the sample is 2.9 mm, and the stable temperature T of the sample in contact with the heat sink is s is 297.9K. According to the highest point O of each fitting curve, the corresponding temperature is T o , calculate the temperature difference △T between points O and A and the heating power P of the sample section under different currents, P=UI.

[0103] (8) A proportional function is used to fit the heating power P-temperature difference △T curve under each current. According to the formula P=b*△T, the slope b is 0.03410.

[0104] (9) According to the formula λ=bL OA / 4A C The thermal conductivity λ of the sample under test is calculated to be 988.9 W / mK.

[0105] Embodiment 5:

[0106] (1) A complete and uniform graphene film with a thickness of 100 μm was cut into strip samples of 40 mm x 1 mm.

[0107] (2) Thermal conductivity test sample stage settings see Figure 2 , set the distance between the copper blocks of heat sinks 1, 2 and 3, 4 to 10mm, and the distance between heat sinks 2, 3 to 10mm. Apply high-purity silver glue evenly on the four heat sinks, place the strip sample on the silver glue, and wait for the silver glue to solidify.

[0108] (3) Spray a thin layer of amorphous graphite spray onto the surface of the test sample and the heat sink, and set the infrared camera emissivity value to 0.85.

[0109] (4) Place the heat sink in the vacuum chamber and connect the four heat sinks in sequence using the four-wire method. The length of the sample between the two middle heat sinks is the sample segment to be tested. In this embodiment, the length of the sample segment to be tested is 10 mm. Set the vacuum degree of the chamber to 10 -4 Entrust.

[0110] (5) The control power supply applies a constant DC current of 2000 mA to the sample segment under test, measures the voltage drop U on the sample segment under test, and uses an infrared thermometer to measure the lateral temperature distribution on the surface of the sample segment under test. When the temperature fluctuation on the sample surface is less than 0.1 K for 3 consecutive seconds and does not change monotonically, it is considered that a steady state has been reached, and the voltage drop and surface temperature distribution curve on the sample segment under test are recorded.

[0111] (6) The current was increased by 300 mA successively until the constant current reached 4100 mA, and step (5) was repeated to obtain the voltage U and sample surface temperature distribution curves under different currents.

[0112] (7) Select the temperature distribution data within the range of 0-0.8L on both sides of the center point O of the sample segment to be measured, and use the quadratic equation T(x) = ax 2 +To fits the temperature T and distance x. The fitting curves of the sample surface temperature distribution under different current conditions will intersect at two points A. 1 (6.2, 295.5) and A 2 (-6.2, 295.5). The effective half length of the sample is L OA The stable temperature T of the sample in contact with the heat sink is 6.2 mm. s is 295.5K. According to the highest point O of each fitting curve, the corresponding temperature is T o , calculate the temperature difference △T between points O and A under different currents and the heating power P of the sample segment under test, P=UI.

[0113] (8) A proportional function is used to fit the heating power P-temperature difference △T curve under each current. According to the formula P=b*△T, the slope b is 0.07751.

[0114] (9) According to the formula λ=bL OA / 4A C The thermal conductivity λ of the sample under test is calculated to be 1049 W / mK.

[0115] Although the embodiments of the present invention are disclosed for illustrative purposes, those skilled in the art will appreciate that various substitutions, changes and modifications are possible without departing from the spirit and scope of the present invention and the appended claims. Therefore, the scope of the present invention is not limited to the contents disclosed in the embodiments.

Claims

1. A method for measuring thermal conductivity of a thermally conductive film, characterized in that: The following steps are involved: (1) Place the thermal conductive film to be tested on two heat sinks with a spacing of 2L; The thermal conductive film to be tested is heated with a heating power P; (2) forming multiple measurement points along the length direction of the thermal conductive film between the two heat sinks, collecting the surface temperature values ​​of different measurement points, and obtaining measurement data (x, T), where x is the coordinate value of the measurement point and T is the measured temperature of the measurement point; Using the quadratic equation T(x)=ax 2 +T o Fit the measured data (x, T) to obtain the Tx fitting curve; (3) Changing the heating power to form multiple fitting curves, the multiple fitting curves intersect at two points, the two intersection points have the same temperature value Ts, and the distance between the two intersection points is 2L OA ; Calculate the temperature T corresponding to the highest point of each fitting curve o , get T o and T s The temperature difference △T; (4) Using different heating powers P and corresponding temperature differences ΔT, a direct proportional function is used to fit the heating power P-temperature difference ΔT curve to obtain the slope b; (5) According to the formula λ=bL OA / 4A C Calculate the thermal conductivity λ of the sample being tested; where A C is the cross-sectional area, A C =thickness*width.

2. The measuring method according to claim 1, characterized in that: The heating method of step 2 is: Input constant current power to the thermal conductive film to be tested; Test the voltage across the terminals and calculate the heating power.

3. The method according to claim 1, characterized in that It also includes two auxiliary heat sinks, which are located on both sides of the two heat sinks in claim 1; the long film containing the thermally conductive film to be tested is placed on the four heat sinks, and a constant direct current is applied to the thermally conductive film to be tested through the two auxiliary heat sinks.

4. The method according to claim 1, characterized in that Spray a layer of spray with known emissivity onto the surface of the thermal conductive film and heat sink to be tested.

5. The method according to claim 1, characterized in that The heat sink spacing satisfies 2L∈[100·t,0.0955·(λ0A C / C) 1 / 2 ], the width of the thermal conductive film to be tested is less than 0.2*L; Where t is the thickness of the thermal conductive film to be tested, C is the circumference of the cross section of the thermal conductive film to be tested, and A C is the cross-sectional area, the cross-sectional area is the plane formed by the thickness and width of the thermal conductive film to be tested, and λ0 is the estimated value of the thermal conductivity of the film sample.

6. The method according to claim 1, characterized in that T o Between room temperature and 60°C.

7. The method according to claim 1, characterized in that: The measuring points are located within a range of 0 to 0.8 L on both sides of the midpoints of the two heat sinks.

8. The method according to claim 1, characterized in that The coordinates of the measurement point are based on the midpoints of the two heat sinks as the origin, and the quadratic equation is T(x)=ax 2 +T o ; Where a is the coefficient, x is the distance from the measuring point to the center of the thermal conductive film to be measured, and T is the surface temperature of the measuring point; T o is the temperature of the center point (i.e. x=0).

9. The method according to claim 1, characterized in that: When the sample temperature changes by less than 0.1°C and does not change monotonically, data are formally collected.

Citation Information

Cited By