Method for detecting concentration of brightener in electroplating solution and reagent for determining concentration of brightener in electroplating solution
By adding inhibitors and leveling agents to the electroplating solution, using the principle of brightener counter-inhibitors, and using linear fitting method to determine the brightener concentration, the problem of large error in the determination of brightener concentration in the prior art is solved, and the problem of large error in the determination of brightener concentration in the existing technology is realized. The stability and accuracy of the electroplating effect are achieved.
Patent Information
- Application Number
- CN202411457388.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-18
- Publication Date
- 2024-12-06
AI Technical Summary
During the electroplating process, the change in the brightener concentration affects the plating quality and the stability of the electroplating effect. It is difficult for the prior art to accurately determine the brightener concentration, especially in the presence of a leveling agent, which leads to large test errors and affects the electroplating effect.
By preparing the test auxiliary liquid, adding inhibitors and leveling agents, using the principle of brightener counter-inhibitors, the brightener concentration in the electroplating solution is determined, and the linear fitting method is used to determine the brightener concentration based on the electroplating deposition rate to avoid interference from the leveling agent. , reduce test errors.
The precise determination of brightener concentration in the presence of a leveling agent is achieved, which reduces the test error and ensures the stability and accuracy of the electroplating effect.
Smart Images

Figure CN119086840A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of electroplating solution detection, and in particular to a method for detecting the concentration of a brightener in an electroplating solution and a reagent for measuring the concentration of a brightener in an electroplating solution. Background Art
[0002] Printed circuit boards (PCBs) are an essential component of electronic products. Electroplating copper on PCBs can increase their electrical conductivity and welding performance, and can protect the circuits. When electroplating PCBs, it is necessary to select an electroplating solution. The electroplating solution generally includes an electrolytic support solution and additives. Among them, the electroplating solution mainly includes metal salt compounds such as copper sulfate and copper chloride, inorganic acids and additives.
[0003] Metal salt compounds can provide the metal ions needed in the electroplating process. Inorganic acids can further ensure the conductivity of the electroplating solution to maintain the stability of the electroplating solution. Additives mainly include levelers, brighteners, inhibitors, etc. The content of additives plays an important role in regulating the deposition rate of the plated metal and improving the quality and brightness of the plating layer. The concentration of levelers and inhibitors changes relatively slowly during the electroplating process; while brighteners are continuously consumed during the electroplating process, and their concentration changes with the increase of time and the number of electroplating times. Therefore, regular measurement of the concentration of brighteners and timely adjustment of the electroplating solution play an important role in ensuring the stability of the electroplating effect. Summary of the invention
[0004] Based on this, the present application provides a method for detecting the concentration of brightener in a plating solution and a reagent for determining the concentration of brightener in a plating solution. The method for detecting the concentration of brightener in a plating solution provided in the present application has the advantage of high accuracy and can effectively ensure the stability of the electroplating effect.
[0005] In a first aspect of the present application, a method for detecting the concentration of a brightener in an electroplating solution is provided, comprising the following steps:
[0006] Detection of electroplating deposition rate Q of test auxiliary liquid IN ;
[0007] Add the electroplating solution sample to be tested into the test auxiliary solution to prepare a first mixed solution, and detect the electroplating deposition rate Q of the first mixed solution. B ;
[0008] Adding a known brightener standard sample to the first mixed solution at least once, and detecting the electroplating deposition rate Q after each addition of the known brightener standard sample; wherein the brightener concentration included in the known brightener standard sample is known;
[0009] According to the electroplating deposition rate Q IN , electroplating deposition rate Q Band the electroplating deposition rate Q, to obtain the brightener concentration in the electroplating solution sample to be tested;
[0010] The preparation step of the test auxiliary solution includes: gradually adding an inhibitor to the electrolytic support solution, recording the total amount of the inhibitor added when the electroplating deposition rate of the electrolytic support solution after adding the inhibitor no longer decreases, and preparing a first electrolytic support solution;
[0011] The leveling agent is gradually added to the first electrolytic supporting solution, and the total amount of the leveling agent added when the electroplating deposition rate of the first electrolytic supporting solution after the leveling agent is added is recorded to prepare the test auxiliary solution.
[0012] In one embodiment, when the known brightener standard sample is added once to the first mixed solution, the electroplating deposition rate after adding the known brightener standard sample is recorded as Q1; according to the electroplating deposition rate Q IN , electroplating deposition rate Q B and the electroplating deposition rate Q1, the step of obtaining the brightener concentration in the electroplating solution sample to be tested comprises:
[0013] The electroplating deposition rate Q of the first mixed solution is B is the intercept,
[0014] Performing linear fitting on the brightener concentration C1 of the known brightener standard sample and the electroplating deposition rate Q1 after adding the known brightener standard sample, to obtain a linear equation reflecting the corresponding relationship between the brightener concentration and the electroplating deposition rate;
[0015] The electroplating deposition rate Q of the test auxiliary liquid IN Substituting into the linear equation, we get C S Value; among them, C S The absolute value of the value is determined as the brightener concentration of the electroplating solution sample to be tested.
[0016] In one embodiment, when a known brightener standard sample is added to the first mixed solution n times, the electroplating deposition rates Q1 to Qn after each addition of the known brightener standard sample are detected, where n≥2;
[0017] The brightener concentration of the known brightener standard sample added for the first time is recorded as C1, and the brightener concentration of the known brightener standard sample added for the nth time is recorded as C n .
[0018] According to the electroplating deposition rate Q IN , electroplating deposition rate Q B , electroplating deposition rate Q1~Qn, the step of obtaining the brightener concentration in the electroplating solution sample to be tested comprises:
[0019] The electroplating deposition rate Q of the first mixed solution isB is the intercept,
[0020] Linear fitting is performed on the brightener concentration C1 of the first known brightener standard sample added, the electroplating deposition rate Q1 after adding the known brightener standard sample once, the total brightener concentration N of the known brightener standard sample added n times, and the electroplating deposition rate Qn after adding the known brightener standard sample n times, to obtain a linear equation reflecting the corresponding relationship between the brightener concentration and the electroplating deposition rate; wherein, the total brightener concentration N=C1+ …… +C n .
[0021] The electroplating deposition rate Q of the test auxiliary liquid IN Substituting into the linear equation, we get C S Value; among them, C S The absolute value of the value is determined as the brightener concentration of the electroplating solution sample to be tested.
[0022] In one embodiment, in the test auxiliary solution, the volume concentration of the inhibitor is 1 mL / L~300 mL / L.
[0023] In one embodiment, in the test auxiliary liquid, the volume concentration of the leveling agent is 1 mL / L~200 mL / L.
[0024] In one embodiment, the electrolyte support solution includes a metal salt compound and an inorganic acid;
[0025] Optionally, the metal salt compound includes one or more of copper sulfate, copper chloride, copper bromide, copper iodide, copper sulfide, copper acetate, copper nitrate, copper fluoroborate, copper methanesulfonate, copper benzenesulfonate, copper toluenesulfonate, ferrous sulfate, ferrous sulfate, sodium chloride and potassium chloride;
[0026] Optionally, the inorganic acid includes one or more of sulfuric acid, hydrochloric acid, acetic acid, phosphoric acid, benzenesulfonic acid, phenolsulfonic acid, toluenesulfonic acid and aminosulfonic acid.
[0027] In one embodiment, the test method of the electroplating deposition rate includes one or more of cyclic voltammetry scanning method, cyclic voltammetry stripping analysis method and cyclic pulse voltammetry stripping analysis method.
[0028] In one embodiment, the detection method includes one or more of the following features:
[0029] (1) The inhibitor includes one or more of butyl polyoxyethylene polyoxypropylene ether, polyethylene glycol, polypropylene glycol, ethylene oxide / propylene oxide block copolymer, isooctyl alcohol polyoxyethylene ether, polyoxyethylene lauryl ether and polyoxyethylene nonylphenyl ether;
[0030] (2) The brightener includes one or more of propane sulfonate pyridinium salt, N-propane benzene sulfonate, polydisulfide propane sulfonate, 3-mercapto-1-propane sulfonate, N,N-dimethyl-dithiocarbamoyl propyl sulfonate, 3-thio-isothiourea propyl sulfonate, 3-(benzothiazolyl-2-mercapto)-propyl sulfonate, alkyl polyalkoxy propyl sulfonate potassium salt, linear polyepoxy naphthol propyl sulfonate potassium salt, thiourea, 1,3-dimethyl thiourea, trimethyl thiourea, diethyl thiourea and allyl thiourea;
[0031] (3) The leveling agent includes one or more of dialkylamine, trialkylamine, arylalkylamine, diarylamine, imidazole, triazole, tetrazole, benzimidazole, benzotriazole, thiazole, benzothiazole, piperidine, morpholine, guanidine compounds, piperazine, pyridine, oxazole, benzoxazole, pyrimidine, quinoline and isoquinoline, polyethyleneimine, quaternized polyvinylimidazole cationic polymer, diethylenetriamine cationic polymer, imidazoline quaternary ammonium salt cationic polymer, imidazoline quaternary ammonium salt cationic derivative, copolymer of imidazole and 1,4-butanediol diglycidyl ether and organic dye.
[0032] The second aspect of the present application provides a computer-readable storage medium having a computer program stored thereon. When the computer program is executed by a processor, at least one step of the method for detecting the concentration of brightener in the electroplating solution described in any embodiment of the first aspect of the present application is implemented.
[0033] In a third aspect of the present application, a reagent for determining the concentration of a brightener in a plating solution is provided, wherein the reagent comprises the test auxiliary solution described in any one of the embodiments of the first aspect of the present application.
[0034] The beneficial effects of the method for detecting the concentration of brightener in the electroplating solution provided by the present application include at least:
[0035] The present application prepares a test auxiliary liquid so that the plating solution contains an inhibitor and a leveler, wherein the presence of the inhibitor can facilitate the testing of the content of the brightener by utilizing the action principle of the brightener anti-inhibitor; in addition, since the leveler interferes with the ability of the brightener anti-inhibitor; the present application adds a sufficient amount of the leveler to the test auxiliary liquid, thereby avoiding the introduction of an additional leveler into the plating solution sample to be tested, which may cause the weakening of the ability of the brightener anti-inhibitor, thereby reducing the test error of the brightener concentration.
[0036] In summary, the detection method provided in the present application can accurately test the concentration of brightener when a leveling agent is present in the electroplating solution sample to be tested. It has the advantages of small test error and high accuracy, which is beneficial to control the content of brightener during the electroplating process, and can effectively ensure the stability of the electroplating effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 This is a flow chart of a method for detecting the concentration of brightener in an electroplating solution according to an example of the present application;
[0038] Figure 2 A linear equation fitting curve of the corresponding relationship between the concentration of the reactive brightener and the electroplating deposition rate in an example of the present application;
[0039] Figure 3 The linear equation fitting curve of the corresponding relationship between the concentration of reactive brightener and the electroplating deposition rate is another example of the present application. DETAILED DESCRIPTION
[0040] The following is a further complete and clear description of the method for detecting the concentration of brightener in the electroplating solution and the reagent for measuring the concentration of brightener in the electroplating solution of the present application in combination with specific examples. The present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present application more thoroughly understood.
[0041] The conventional improved linear approximation method for determining the brightener concentration comprises the following steps: (1) adding a certain amount of additive without brightener to the electroplating base solution (without additives) to obtain the cut-off charge Q of the test auxiliary solution. intercept , the total volume is V1; after adding V2 volume of the plating solution sample to be tested, the charge is Q bath Then add two known brightener standard samples C and record the quantity Q1 and Q2 respectively. intercept As the vertical axis, connect Q bath , Q1, Q2, the extended line intersects with the horizontal axis, and the corresponding concentration value is the sample concentration. In the traditional brightener concentration test, since the performance of the leveling agent at that time was not strong, the experimenters would assume that the leveling agent had little interference with the brightener test and its influence could be ignored. However, with the advancement of electroplating technology, the leveling agent will interfere with the ability of the brightener to resist the inhibitor, and the influence of the leveling agent on the test has reached a level that cannot be ignored. If the original method is continued to be used for measurement, a large error will occur.
[0042] Among the test methods that take the influence of leveling agents into consideration, there are methods that require the concentration of leveling agents to be measured before testing brighteners, and the measured brightener concentration is highly dependent on the accuracy of the tested leveling agent concentration. This makes the brightener test not an independent part and must be combined with the leveling agent test.
[0043] See also Figure 1 In a first aspect of the present application, a method for detecting the concentration of a brightener in a plating solution is provided, comprising the following steps:
[0044] Detection of electroplating deposition rate Q of test auxiliary liquid IN ;
[0045] Add the electroplating solution sample to be tested into the test auxiliary solution to prepare a first mixed solution, and detect the electroplating deposition rate Q of the first mixed solution. B ;
[0046] Adding a known brightener standard sample to the first mixed solution at least once, and detecting the electroplating deposition rate Q after each addition of the known brightener standard sample; wherein the brightener concentration included in the known brightener standard sample is known;
[0047] According to the electroplating deposition rate Q IN , electroplating deposition rate Q B and the electroplating deposition rate Q, to obtain the brightener concentration in the electroplating solution sample to be tested.
[0048] The preparation step of the test auxiliary solution includes: gradually adding an inhibitor to the electrolytic support solution, recording the total amount of the inhibitor added when the electroplating deposition rate of the electrolytic support solution after adding the inhibitor no longer decreases, and preparing a first electrolytic support solution;
[0049] The leveling agent is gradually added to the first electrolytic supporting solution, and the total amount of the leveling agent added when the electroplating deposition rate of the first electrolytic supporting solution after the leveling agent is added is recorded to prepare the test auxiliary solution.
[0050] The present application prepares a test auxiliary liquid so that the plating solution contains an inhibitor and a leveler, wherein the presence of the inhibitor can facilitate the testing of the content of the brightener by utilizing the action principle of the brightener anti-inhibitor; in addition, since the leveler interferes with the ability of the brightener anti-inhibitor; the present application adds a sufficient amount of the leveler to the test auxiliary liquid, thereby avoiding the introduction of an additional leveler into the plating solution sample to be tested, which may cause the weakening of the ability of the brightener anti-inhibitor, thereby reducing the test error of the brightener concentration.
[0051] In summary, the detection method provided in the present application can accurately test the concentration of brightener when a leveling agent is present in the electroplating solution sample to be tested. It has the advantages of small test error and high accuracy, which is beneficial to control the content of brightener during the electroplating process, and can effectively ensure the stability of the electroplating effect.
[0052] In one example, when the known brightener standard sample is added once to the first mixed solution, the electroplating deposition rate after adding the known brightener standard sample is recorded as Q1.
[0053] At this time, according to the electroplating deposition rate Q IN , electroplating deposition rate Q B and the electroplating deposition rate Q1 after adding a known brightener standard sample, the step of obtaining the brightener concentration in the electroplating solution sample to be tested comprises:
[0054] The electroplating deposition rate Q of the first mixed solution is B is the intercept,
[0055] Performing linear fitting on the brightener concentration C1 and the electroplating deposition rate Q1 of the known brightener standard sample to obtain a linear equation reflecting the corresponding relationship between the brightener concentration and the electroplating deposition rate;
[0056] The electroplating deposition rate Q of the test auxiliary liquid IN Substituting into the linear equation, we get C S Value; among them, C S The absolute value of the value is determined as the brightener concentration of the electroplating solution sample to be tested.
[0057] When the known brightener standard sample is added once to the first mixed solution, the linear equation fitting curve of the corresponding relationship between the brightener concentration and the electroplating deposition rate is as follows: Figure 2 In the test auxiliary liquid, there is sufficient inhibitor and leveler, at this time, the electroplating deposition rate is the lowest. Figure 2 Specifically, Q IN After adding the electroplating solution sample to be tested, the brightener can weaken the inhibitory effect of the inhibitor due to the action of the brightener against the inhibitor, thereby increasing the electroplating deposition rate of the first mixed solution. Figure 2 Specifically, Q B Further adding a known brightener standard sample, whose brightener concentration is C1, further weakens the inhibition effect, so that the electroplating deposition rate after adding the brightener standard sample increases to Figure 2 Q1 in the first mixed solution. B As the intercept, the brightener concentration C1 and the electroplating deposition rate Q1 of the known brightener standard sample are linearly fitted to obtain a linear equation fitting curve reflecting the corresponding relationship between the brightener concentration and the electroplating deposition rate; the electroplating deposition rate Q1 of the test auxiliary liquid is substituted into IN After that, we get C S Since the determination method of this application uses the brightener anti-inhibitor principle, the C S The value is negative, C S The absolute value of the value can be determined as the brightener concentration of the electroplating solution sample to be tested.
[0058] In one example, a known brightener standard sample is added to the first mixed solution n times, and the electroplating deposition rates Q1 to Qn after each addition of the known brightener standard sample are detected, where n≥2;
[0059] The brightener concentration of the known brightener standard sample added for the first time is recorded as C1, and the brightener concentration of the known brightener standard sample added for the nth time is recorded as C n .
[0060] According to the electroplating deposition rate Q IN , electroplating deposition rate Q B , electroplating deposition rate Q1~Qn, the step of obtaining the brightener concentration in the electroplating solution sample to be tested comprises:
[0061] The electroplating deposition rate Q of the first mixed solution is B is the intercept,
[0062] Linear fitting is performed on the brightener concentration C1 of the first known brightener standard sample added, the electroplating deposition rate Q1 after adding the known brightener standard sample once, the total brightener concentration N of the known brightener standard sample added n times, and the electroplating deposition rate Qn after adding the known brightener standard sample n times, to obtain a linear equation reflecting the corresponding relationship between the brightener concentration and the electroplating deposition rate; the total brightener concentration N=C1+ …… +C n .
[0063] The electroplating deposition rate Q of the test auxiliary liquid IN Substituting into the linear equation, we get C S Value; among them, C S The absolute value of the value is determined as the brightener concentration of the electroplating solution sample to be tested.
[0064] It can be understood that the concentration of the brightener in the known brightener standard samples added n times to the first mixed solution can be the same or different. When the concentration of the brightener in the known brightener standard samples added n times is the same, the total brightener concentration N is nC1. For example, when the concentration of the brightener in the known brightener standard samples added twice is the same, the total brightener concentration N is 2C1. When the concentration of the brightener in the known brightener standard samples added n times is different, the total brightener concentration N=C1+ …… +C n .
[0065] It can be understood that when the values of brightener concentration C and electroplating deposition rate Q are greater, the linear equation reflecting the corresponding relationship between brightener concentration and electroplating deposition rate obtained by linear fitting is more accurate.
[0066] In order to coordinate accuracy and processing efficiency, preferably, the number of times the known brightener standard is added to the first mixed solution is twice. At this time, the brightener concentration of the known brightener standard added for the first time is recorded as C1, and the brightener concentration of the known brightener standard added for the second time is recorded as C2. IN , electroplating deposition rate Q B , electroplating deposition rate Q1~Qn, the step of obtaining the brightener concentration in the electroplating solution sample to be tested comprises: using the electroplating deposition rate Q1~Qn of the first mixed solution B is the intercept,
[0067] Linear fitting was performed on the brightener concentration C1 and electroplating deposition rate Q1 of the known brightener standard sample added for the first time, and the total brightener concentration N and electroplating deposition rate Q2 of the known brightener standard sample added for the second time, to obtain a linear equation reflecting the corresponding relationship between the brightener concentration and the electroplating deposition rate; the total brightener concentration N=C1+C2.
[0068] The electroplating deposition rate Q of the test auxiliary liquid IN Substituting into the linear equation, we get C S Value; among them, C S The absolute value of the value is determined as the brightener concentration of the electroplating solution sample to be tested. When the known brightener standard sample is added twice to the first mixed solution, the linear equation fitting curve of the corresponding relationship between the brightener concentration and the electroplating deposition rate is as follows: Figure 3 shown.
[0069] In one example, in the step of adding the electroplating solution sample to be tested to the test auxiliary liquid, the ratio of the volume of the test auxiliary liquid to the volume of the electroplating solution sample to be tested is (0.5-500): 1. It can be understood that the volume ratio of the test auxiliary liquid to the electroplating solution sample to be tested includes but is not limited to 0.5: 1, 1: 1, 2: 1, 3: 1, 4: 1, 5: 1, 6: 1, 7: 1, 8: 1, 9: 1, 10: 1, 10.5: 1, 15: 1, 20: 1, 25: 1, 30: 1, 80: 1, 100: 1, 150: 1, 200: 1, 220: 1, 260: 1, 280: 1, 300: 1, 350: 1, 400: 1, 450: 1 or 500: 1.
[0070] Furthermore, in the step of adding the electroplating solution sample to be tested into the test auxiliary liquid, the ratio of the volume of the test auxiliary liquid to the volume of the electroplating solution sample to be tested is (1-10):1.
[0071] In one example, the test method of the electroplating deposition rate includes one or more of cyclic voltammetry scanning method, cyclic voltammetry stripping analysis method and cyclic pulse voltammetry stripping analysis method.
[0072] In one example, the variable for measuring the electroplating deposition rate includes one or more of the area of the electroplating metal dissolution peak outputted by the charge Q and the height of the electroplating metal dissolution peak outputted by the current i.
[0073] Preferably, the variable for measuring the electroplating deposition rate is the area of the electroplated copper dissolution peak outputted as charge Q. At this time, the reference standard for judging that the electroplating deposition rate of the electrolytic support solution no longer decreases is that the area of the electroplated copper dissolution peak no longer decreases. That is, the preparation steps of the test auxiliary liquid include: gradually adding an inhibitor to the electrolytic support liquid, recording the amount of the inhibitor added when the area of the electroplated copper dissolution peak of the electrolytic support liquid after adding the inhibitor no longer decreases, and preparing the first electrolytic support liquid; gradually adding a leveling agent to the first electrolytic support liquid, recording the amount of the leveling agent added when the area of the electroplated copper dissolution peak of the first electrolytic support liquid after adding the leveling agent no longer decreases, and preparing the test auxiliary liquid.
[0074] It is understandable that the volume concentration of the inhibitor added to the test auxiliary liquid is related to the composition of the electrolysis support liquid. In one example, in the test auxiliary liquid, the volume concentration of the inhibitor is 1 mL / L~300 mL / L. It is understandable that in the test auxiliary liquid, the volume concentration of the inhibitor includes but is not limited to 1 mL / L, 10 mL / L, 20 mL / L, 30 mL / L, 40 mL / L, 50 mL / L, 60 mL / L, 70 mL / L, 80 mL / L, 90 mL / L, 100 mL / L, 120 mL / L, 150 mL / L, 180 mL / L, 200 mL / L, 220 mL / L, 240 mL / L, 260 mL / L, 280 mL / L or 300 mL / L, or within the interval formed by any two of the above point values.
[0075] Furthermore, in the test auxiliary liquid, the volume concentration of the inhibitor is 28 mL / L~32 mL / L. It can be understood that in the test auxiliary liquid, the inhibitor is sufficient. At this time, only physical phenomena such as adsorption or desorption can occur in the test auxiliary liquid, and no obvious electroplating or dissolution occurs. Furthermore, the volume concentration of the inhibitor includes but is not limited to 28 mL / L, 29 mL / L, 30 mL / L, 31 mL / L or 32 mL / L, or within the interval formed by any two of the above point values.
[0076] It is understandable that the volume concentration of the leveling agent added to the test auxiliary liquid is related to the composition of the electrolytic support liquid. In one example, in the test auxiliary liquid, the volume concentration of the leveling agent is 1 mL / L~200 mL / L. It is understandable that in the test auxiliary liquid, the volume concentration of the leveling agent includes but is not limited to 1 mL / L, 10 mL / L, 20 mL / L, 30 mL / L, 40 mL / L, 50 mL / L, 60 mL / L, 70 mL / L, 80 mL / L, 90 mL / L, 100 mL / L, 120 mL / L, 150 mL / L, 180 mL / L or 200 mL / L, or within the interval formed by any two of the above point values.
[0077] In one example, in the test auxiliary liquid, the volume concentration of the leveler is 8 mL / L~12 mL / L. In the test auxiliary liquid, the leveler is added in sufficient amount. At this time, its interference with the inhibitor and the like interact sufficiently. Thus, the influence of the leveler contained in the subsequent electroplating solution sample to be tested or the known brightener standard on the test results can be effectively avoided. Furthermore, the volume concentration of the leveler includes but is not limited to 8 mL, 9 mL, 10 mL, 11 mL or 12 mL, or within the interval formed by any two of the above point values.
[0078] In one example, the electrolytic support solution includes a metal salt compound and an inorganic acid. It is understandable that the present application does not limit the type and source of the electroplating support solution, as long as it can play an electroplating role. Preferably, the above-mentioned electrolytic support solution does not include additives. The additives include one or more of a leveling agent, an inhibitor and a brightener.
[0079] In one example, the metal salt compound includes one or more of copper sulfate, copper chloride, copper bromide, copper iodide, copper sulfide, copper acetate, copper nitrate, copper fluoroborate, copper methanesulfonate, copper benzenesulfonate, copper toluenesulfonate, ferrous sulfate, ferrous sulfate, sodium chloride and potassium chloride.
[0080] In one example, the inorganic acid includes one or more of sulfuric acid, hydrochloric acid, acetic acid, phosphoric acid, benzenesulfonic acid, phenolsulfonic acid, toluenesulfonic acid and aminosulfonic acid.
[0081] In one specific example, a method for detecting the concentration of brightener in a plating solution comprises the following steps:
[0082] S100, preparation of a test auxiliary solution: gradually adding an inhibitor to an electrolytic support solution, recording the amount of the inhibitor added when the electroplating copper dissolution peak area of the electrolytic support solution measured by cyclic voltammetry scanning no longer decreases after the inhibitor is added, and preparing a first electrolytic support solution; gradually adding a leveling agent to the first electrolytic support solution, recording the amount of the leveling agent added when the electroplating copper dissolution peak area of the first electrolytic support solution measured by cyclic voltammetry scanning no longer decreases after the leveling agent is added, and preparing the test auxiliary solution.
[0083] S200, detection of electroplating deposition rate Q of test auxiliary liquid IN .
[0084] S300, adding the electroplating solution sample to be tested into the test auxiliary solution to prepare a first mixed solution, and detecting the electroplating deposition rate Q of the first mixed solution. B .
[0085] S400, adding a known brightener standard sample into the first mixed solution twice, and detecting the electroplating deposition rates Q1 and Q2 after adding the known brightener standard sample each time; wherein the brightener concentration in the known brightener standard sample is C1.
[0086] S500, electroplating deposition rate Q of the first mixed solution B As the intercept, linear fitting was performed on the brightener concentration C1 of the known brightener standard sample added for the first time and the electroplating deposition rate Q1 after the known brightener standard sample was added once, the total brightener concentration 2C1 of the known brightener standard sample added twice and the electroplating deposition rate Q2 after the known brightener standard sample was added twice, and the linear equation reflecting the corresponding relationship between the brightener concentration and the electroplating deposition rate was obtained.
[0087] S600, the electroplating deposition rate Q of the test auxiliary liquid IN Substituting into the linear equation, we get C S Value; among them, C S The absolute value of the value is determined as the brightener concentration of the electroplating solution sample to be tested.
[0088] In one example, the inhibitor includes one or more of butyl polyoxyethylene polyoxypropylene ether, polyethylene glycol, polypropylene glycol, ethylene oxide / propylene oxide block copolymer, isooctyl alcohol polyoxyethylene ether, polyoxyethylene lauryl ether and polyoxyethylene nonylphenyl ether.
[0089] In one example, the brightener includes one or more of propane sulfonate pyridinium salt, N-propanebenzene sulfonate, polydisulfide propane sulfonate, 3-mercapto-1-propane sulfonate, N,N-dimethyl-dithiocarbamoyl propyl sulfonate, 3-thio-isothiourea propyl sulfonate, 3-(benzothiazolyl-2-mercapto)-propyl sulfonate, alkyl polyalkoxy propyl sulfonate potassium salt, straight polyepoxy naphthol propyl sulfonate potassium salt, thiourea, 1,3-dimethylthiourea, trimethylthiourea, diethylthiourea and allylthiourea.
[0090] In one example, the leveler includes one or more of dialkylamine, trialkylamine, arylalkylamine, diarylamine, imidazole, triazole, tetrazole, benzimidazole, benzotriazole, thiazole, benzothiazole, piperidine, morpholine, guanidine compounds, piperazine, pyridine, oxazole, benzoxazole, pyrimidine, quinoline and isoquinoline, polyethyleneimine, quaternized polyvinylimidazole cationic polymer, diethylenetriamine cationic polymer, imidazoline quaternary ammonium salt cationic polymer, imidazoline quaternary ammonium salt cationic derivative, copolymer of imidazole and 1,4-butanediol diglycidyl ether and organic dye.
[0091] Illustratively, the organic dye includes, but is not limited to, Janus Green, Basic Brown, Phenylpyrazolium Dye, Malachite Green, Rose Aniline, or Crystal Violet.
[0092] To improve the accuracy of the test results, in one example, the known brightener standard sample does not include a leveler or an inhibitor.
[0093] The method for detecting the brightener concentration in the electroplating solution provided in the present application has high accuracy and good universality, and is applicable to most inhibitors, brighteners and levelers.
[0094] The second aspect of the present application provides a computer-readable storage medium having a computer program stored thereon. When the computer program is executed by a processor, at least one step of the method for detecting the concentration of brightener in the electroplating solution described in any example of the first aspect of the present application is implemented.
[0095] In a third aspect of the present application, a reagent for determining the concentration of a brightener in a plating solution is provided, wherein the reagent comprises the test auxiliary solution described in any example of the first aspect of the present application.
[0096] The following further specific examples are provided to explain the present application in detail. It should also be understood that the following examples are only used to further explain the present application and cannot be understood as limiting the scope of protection of the present application. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present application belong to the scope of protection of the present application. The specific process parameters of the following embodiments are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not necessarily limited to the specific values of the embodiments below.
[0097] [raw material]
[0098] Electrolysis support solution: Model VFP22; including commercially available AR grade copper sulfate, sulfuric acid and hydrochloric acid;
[0099] Inhibitors: polyethylene glycol;
[0100] Leveling agent: copolymer of imidazole and 1,4-butanediol diglycidyl ether;
[0101] Brightener: sodium polydisulfide dipropane sulfonate.
[0102] Example 1
[0103] The method for detecting the concentration of brightener in the electroplating solution comprises the following steps:
[0104] (1) Preparation of test auxiliary solution: gradually add inhibitor to the electrolytic support solution, and record the amount of inhibitor added when the peak area of electroplated copper dissolution of the electrolytic support solution measured by cyclic voltammetry scanning no longer decreases after the addition of the inhibitor. At this time, the concentration of the inhibitor is 30 mL / L; gradually add leveling agent to the electrolytic support solution containing an inhibitor concentration of 30 mL / L, and record the amount of leveling agent added when the peak area of electroplated copper dissolution of the first electrolytic support solution measured by cyclic voltammetry scanning no longer decreases after the addition of the leveling agent. At this time, the concentration of the leveling agent is 10 mL / L.
[0105] The test auxiliary solution was prepared by adding an inhibitor and a leveler to the electrolytic support solution; wherein the concentration of the inhibitor in the test auxiliary solution was 30 mL / L, and the concentration of the leveler was 10 mL / L; and the volume of the test auxiliary solution was 45 mL.
[0106] (2) The test auxiliary liquid is subjected to cyclic voltammetry scanning (equipment: Metrohm 894 Professional CVS, equipped with silver-silver chloride reference electrode), and the electroplated copper dissolution peak area is measured and recorded as the electroplating deposition rate Q of the test auxiliary liquid. IN .
[0107] (3) Add 5 mL of the electroplating solution sample to be tested in Example 1 to the test auxiliary solution to prepare a first mixed solution, perform cyclic voltammetry scanning on the first mixed solution, and detect the electroplating deposition rate Q of the first mixed solution. B .
[0108] (4) adding a known brightener standard sample (the brightener concentration in the known brightener standard sample is C1) to the first mixed solution twice, performing cyclic voltammetry scanning, and detecting the electroplating deposition rates Q1 and Q2 after each addition of the known brightener standard sample; wherein the brightener concentration in the known brightener standard sample is C1.
[0109] (5) Electroplating deposition rate Q of the first mixed solution B As the intercept, linear fitting is performed on the brightener concentration C1 of the first known brightener standard sample added and the electroplating deposition rate Q1 after the first addition of the known brightener standard sample, the total brightener concentration 2C1 of the second known brightener standard sample added and the electroplating deposition rate Q2 after the second addition of the known brightener standard sample, to obtain a linear equation reflecting the corresponding relationship between the brightener concentration and the electroplating deposition rate; the electroplating deposition rate Q IN Substituting into the linear equation, we get C S Value; among them, C S The absolute value of the value is determined as the brightener concentration of the electroplating solution sample to be tested.
[0110] Alternatively, the electroplating deposition rate Q of the first mixed solution may be B is the intercept, forming the ordinate and abscissa; mark the point values (C1, Q1) and (2C1, Q2), represented by point A and point B respectively. Connect Q B , point A and point B, forming a linear equation fitting curve, the ordinate of the linear equation fitting curve corresponds to Q IN The horizontal axis value is C S Value, C S The absolute value of the value is determined as the brightener concentration of the electroplating solution sample to be tested.
[0111] Embodiment 2 to Embodiment 8
[0112] The method for detecting the brightener concentration in the electroplating solution of Examples 2 to 8 is basically the same as that of Example 1, with the main difference being that the electroplating solution sample to be tested selected in step (4) is the electroplating solution sample to be tested of Examples 2 to 8.
[0113] In order to verify the effectiveness of the brightener concentration detection of the present application, the plating solution samples to be tested in Examples 1 to 8 of the present application are prepared samples (recorded as the actual concentration of the additive in the plating solution sample to be tested) and compared with the C S The absolute values of the values are compared to obtain the consistency of the test results.
[0114] The actual concentration of the additive in the electroplating solution samples to be tested in Examples 1 to 8, the C S The absolute values of the values and the test deviations are shown in Table 1.
[0115] Table 1
[0116]
[0117] As can be seen from Table 1, the test method provided in the present application can accurately test the concentration of the brightener based on the different concentrations of inhibitors and levelers contained in the electroplating solution sample to be tested; and the test deviation is within 4.2%.
[0118] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0119] The above-described embodiments only express several implementation methods of the present application, which is convenient for understanding the technical solution of the present application in detail, but it cannot be understood as limiting the scope of protection of the invention patent. It should be pointed out that for ordinary technicians in this field, without departing from the concept of the present application, several modifications and improvements can be made, which all belong to the scope of protection of the present application. It should be understood that the technical solutions obtained by those skilled in the art through logical analysis, reasoning or limited experiments on the basis of the technical solutions provided in the present application are all within the scope of protection of the claims attached to the present application. Therefore, the scope of protection of the patent of this application shall be based on the content of the attached claims, and the description can be used to interpret the content of the claims.
Claims
1. A method for detecting the concentration of brightener in an electroplating solution, characterized in that: The following steps are involved: Detection of electroplating deposition rate Q of auxiliary liquid IN ; Add the electroplating solution sample to be tested into the test auxiliary solution to prepare a first mixed solution, and detect the electroplating deposition rate Q of the first mixed solution. B ; Adding a known brightener standard sample to the first mixed solution at least once, and detecting the electroplating deposition rate Q after each addition of the known brightener standard sample; wherein the brightener concentration included in the known brightener standard sample is known; According to the electroplating deposition rate Q IN , electroplating deposition rate Q B and the electroplating deposition rate Q, to obtain the brightener concentration in the electroplating solution sample to be tested; The test auxiliary solution preparation step includes: gradually adding an inhibitor to an electrolytic support solution, recording the total amount of the inhibitor added when the electroplating deposition rate of the electrolytic support solution after adding the inhibitor no longer decreases, and preparing a first electrolytic support solution; The leveling agent is gradually added to the first electrolytic supporting solution, and the total amount of the leveling agent added when the electroplating deposition rate of the first electrolytic supporting solution after the leveling agent is added is recorded to prepare the test auxiliary solution.
2. The method for detecting the concentration of brightener in the electroplating solution according to claim 1, characterized in that: When the known brightener standard sample is added once to the first mixed solution, the electroplating deposition rate after adding the known brightener standard sample is recorded as Q1; according to the electroplating deposition rate Q IN , electroplating deposition rate Q B and the electroplating deposition rate Q1, the step of obtaining the brightener concentration in the electroplating solution sample to be tested comprises: The electroplating deposition rate Q of the first mixed solution is B is the intercept, Performing linear fitting on the brightener concentration C1 of the known brightener standard sample and the electroplating deposition rate Q1 after adding the known brightener standard sample, to obtain a linear equation reflecting the corresponding relationship between the brightener concentration and the electroplating deposition rate; The electroplating deposition rate Q of the test auxiliary liquid IN Substituting into the linear equation, we get C S Value; among them, C S The absolute value of the value is determined as the brightener concentration of the electroplating solution sample to be tested.
3. The method for detecting the concentration of brightener in the electroplating solution according to claim 1, characterized in that: When a known brightener standard sample is added to the first mixed solution n times, the electroplating deposition rate Q1~Qn after each addition of the known brightener standard sample is detected, where n≥2; The brightener concentration of the known brightener standard sample added for the first time is recorded as C1, and the brightener concentration of the known brightener standard sample added for the nth time is recorded as C n ; According to the electroplating deposition rate Q IN , electroplating deposition rate Q B , electroplating deposition rate Q1~Qn, the step of obtaining the brightener concentration in the electroplating solution sample to be tested comprises: The electroplating deposition rate Q of the first mixed solution is B is the intercept, Linear fitting is performed on the brightener concentration C1 of the first known brightener standard sample added, the electroplating deposition rate Q1 after adding the known brightener standard sample once, the total brightener concentration N of the known brightener standard sample added n times, and the electroplating deposition rate Qn after adding the known brightener standard sample n times, to obtain a linear equation reflecting the corresponding relationship between the brightener concentration and the electroplating deposition rate; wherein, the total brightener concentration N=C1+ …… +C n ; The electroplating deposition rate Q of the test auxiliary liquid IN Substituting into the linear equation, we get C S Value; among them, C S The absolute value of the value is determined as the brightener concentration of the electroplating solution sample to be tested.
4. The method for detecting the brightener concentration in the electroplating solution according to any one of claims 1 to 3, characterized in that: In the test auxiliary solution, the volume concentration of the inhibitor is 1 mL / L to 300 mL / L.
5. The method for detecting the brightener concentration in the electroplating solution according to any one of claims 1 to 3, characterized in that: In the test auxiliary liquid, the volume concentration of the leveling agent is 1 mL / L to 200 mL / L.
6. The method for detecting the brightener concentration in the electroplating solution according to any one of claims 1 to 3, characterized in that: The electrolytic support solution includes a metal salt compound and an inorganic acid; Optionally, the metal salt compound includes one or more of copper sulfate, copper chloride, copper bromide, copper iodide, copper sulfide, copper acetate, copper nitrate, copper fluoroborate, copper methanesulfonate, copper benzenesulfonate, copper toluenesulfonate, ferrous sulfate, ferrous sulfate, sodium chloride and potassium chloride; Optionally, the inorganic acid includes one or more of sulfuric acid, hydrochloric acid, acetic acid, phosphoric acid, benzenesulfonic acid, phenolsulfonic acid, toluenesulfonic acid and aminosulfonic acid.
7. The method for detecting the brightener concentration in the electroplating solution according to any one of claims 1 to 3, characterized in that: The test method of the electroplating deposition rate includes one or more of cyclic voltammetry scanning method, cyclic voltammetry stripping analysis method and cyclic pulse voltammetry stripping analysis.
8. The method for detecting the brightener concentration in the electroplating solution according to any one of claims 1 to 3, characterized in that: The detection method includes one or more of the following features: (1) The inhibitor includes one or more of butyl polyoxyethylene polyoxypropylene ether, polyethylene glycol, polypropylene glycol, ethylene oxide / propylene oxide block copolymer, isooctyl alcohol polyoxyethylene ether, polyoxyethylene lauryl ether and polyoxyethylene nonylphenyl ether; (2) The brightener includes one or more of propane sulfonate pyridinium salt, N-propane benzene sulfonate, polydisulfide propane sulfonate, 3-mercapto-1-propane sulfonate, N,N-dimethyl-dithiocarbamoyl propyl sulfonate, 3-thio-isothiourea propyl sulfonate, 3-(benzothiazolyl-2-mercapto)-propyl sulfonate, alkyl polyalkoxy propyl sulfonate potassium salt, linear polyepoxy naphthol propyl sulfonate potassium salt, thiourea, 1,3-dimethyl thiourea, trimethyl thiourea, diethyl thiourea and allyl thiourea; (3) The leveling agent includes one or more of dialkylamine, trialkylamine, arylalkylamine, diarylamine, imidazole, triazole, tetrazole, benzimidazole, benzotriazole, thiazole, benzothiazole, piperidine, morpholine, guanidine compounds, piperazine, pyridine, oxazole, benzoxazole, pyrimidine, quinoline and isoquinoline, polyethyleneimine, quaternized polyvinylimidazole cationic polymer, diethylenetriamine cationic polymer, imidazoline quaternary ammonium salt cationic polymer, imidazoline quaternary ammonium salt cationic derivative, copolymer of imidazole and 1,4-butanediol diglycidyl ether and organic dye.
9. A computer-readable storage medium having a computer program stored thereon, characterized in that: When the computer program is executed by a processor, at least one step in the method for detecting the concentration of brightener in the electroplating solution according to any one of claims 1 to 8 is implemented.
10. A reagent for determining the concentration of brightener in an electroplating solution, characterized in that: The reagent comprises the test auxiliary liquid according to any one of claims 1 to 8.