Preparation method of locally plastic-packaged high-power alloy resistor

Through tape welding and local plastic sealing technology, combined with laser laser removal and nickel-tin plating, the temperature coefficient and oxidation resistance of high-power alloy resistance during welding is solved, and high-power, low-temperature drift and diversified specifications are achieved, reducing the temperature coefficient and anti-oxidation problems of high-power, low-temperature drift and various specifications. Manufacturing costs and improves antioxidant properties.

CN119092238APending Publication Date: 2024-12-06SUZHOU PROSEMI MICRO-ELECTRONIC TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411368324.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-01-10
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

During the welding process, the temperature coefficient of existing high-power alloy resistors increases due to the high resistance temperature coefficient of copper, and traditional plastic sealing materials cannot meet the high temperature test conditions, resulting in poor oxidation resistance. The preparation process depends on molds and consumes a lot of power. Moreover, the accuracy of the spray area is difficult to control, affecting the resistance value.

Method used

Welding, punching and local plastic sealing are used to carry out full coverage plastic sealing with high-temperature resistant polyimide materials, and unnecessary plastic sealing materials are removed by laser laser to form a high-power alloy resistor for local plastic sealing, and at the ends and welding Nickel-tin electroplating is carried out in the area to achieve anti-oxidation effect.

Benefits of technology

It has achieved high power, low temperature drifting, wave soldering, reduced manufacturing costs, and significantly improved oxidation resistance, getting rid of the dependence on molds. The overall plastic sealing and electroplating of the product are combined to ensure high temperature performance and diversified specifications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092238A_ABST
    Figure CN119092238A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a locally plastic-packaged high-power alloy resistor, which comprises the following steps of: punching a material strip to form a plurality of alloy resistor bodies on the material strip; the whole material belt is subjected to plastic packaging operation, the whole material belt is soaked in a plastic packaging material or the whole material belt is coated with the plastic packaging material in a spraying mode so that the whole material belt can be subjected to complete plastic packaging, and the outer surface of the alloy resistor body is completely covered with the plastic packaging material; removing a plastic package material on a subsequent welding area corresponding to an electrode on the alloy resistor body by adopting a laser mode, wherein the welding area is the surface of the bottom of the electrode; longitudinally cutting the connection position between the electrode on the plastically packaged material belt and the belt material along the thickness direction of the material belt so as to separate the alloy resistor body from the material belt and form a single locally plastically packaged high-power alloy resistor; and the residual surfaces of the high-power alloy resistor except the two end surfaces in the length direction and the electrode for subsequent welding parts are covered with a plastic package material.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the invention patent application with application date of January 10, 2023, application number 2023100377100, and invention name “A partially plastic-sealed anti-oxidation high-power alloy resistor and its preparation method”. Technical Field

[0002] The invention belongs to the technical field of alloy resistors, and in particular relates to a method for preparing a partially plastic-sealed, oxidation-resistant high-power (at least 7W) alloy resistor. Background Art

[0003] High-power alloy resistors have the advantages of high power and low resistance precision compared to traditional plastic-sealed resistors. Since they are pure alloy materials, there are no products and processes for plastic-sealing high-power alloy resistors in the existing technology. The disadvantage of this structure is that the client cannot perform wave soldering, and the tin creep during the welding process will have a certain impact on the resistance and temperature drift. However, the plastic sealing of traditional plastic-sealed resistors is highly dependent on molds, and the debugging of different product equipment is cumbersome and consumes a lot of power. In addition, traditional high-power alloy resistors are stamped and bent into an arch shape. Since the resistance temperature coefficient of copper is much larger than that of the alloy, the proportion of copper in the arch bridge greatly increases the temperature coefficient of the product.

[0004] The existing high-power alloy resistor products have a heating temperature of 500-700℃ when the products are short-term tested under load. The existing plastic packaging materials cannot meet the requirements of this test condition. Therefore, the current high-power shunts all adopt the method of forming a passivation layer on the surface to solve the anti-oxidation problem before use.

[0005] For example, the invention patent application with application number CN109102973A discloses a resistor and a method for manufacturing a resistor, but only the position below the resistor body is coated with paint or epoxy resin by spraying, printing, roller coating or other common methods of similar coating materials. Not only is the coating area boundary unclear, but the spraying area accuracy is difficult to control, which in turn affects the product resistance, especially for resistance-sensitive low-resistance resistor products. Moreover, the anti-oxidation layer of the product prepared by the product will be cracked during the reflow soldering process, and the product will lose its protective effect. Summary of the invention

[0006] In view of this, in order to overcome the defects of the prior art, the purpose of the present invention is to provide a method for preparing a partially plastic-sealed anti-oxidation high-power alloy resistor to achieve full protection of the high-power alloy resistor.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions:

[0008] A method for preparing a partially plastic-sealed high-power alloy resistor comprises the following steps:

[0009] Welding the electrode strip and the alloy strip to obtain a material strip;

[0010] Punching the material strip to form a plurality of alloy resistors on the material strip;

[0011] Performing a plastic sealing operation on the entire material strip so that the outer surface of the alloy resistor is completely covered with the plastic sealing material;

[0012] Remove the plastic sealing material on the area of ​​the electrode on the alloy resistor body corresponding to the subsequent welding;

[0013] Separating the alloy resistor from the material strip to form the partially plastic-sealed high-power alloy resistor;

[0014] The partially plastic-sealed high-power alloy resistor is roll-plated with nickel-tin, so that a coating is formed on the end surfaces of both ends of the alloy resistor and the welding area.

[0015] According to some preferred implementation aspects of the present invention, during welding, the length extension direction of the electrode strip and the alloy strip is the same, and the welding is performed by electron beam welding to weld the electrode strip to the side surface of the alloy strip in the width direction.

[0016] According to some preferred embodiments of the present invention, the electrode strip is used to form an electrode of a high-power alloy resistor, and the alloy strip is used to form a resistor body of a high-power alloy resistor; the thickness of the electrode strip is greater than the thickness of the alloy strip.

[0017] According to some preferred embodiments of the present invention, on one side of the material strip in the thickness direction, the electrode strip is flush with the alloy strip; on the other side of the material strip in the thickness direction, the surface of the electrode strip is higher than the surface of the alloy strip to form a welding area.

[0018] According to some preferred implementation aspects of the present invention, the plastic sealing is to immerse the entire material strip in a plastic sealing material or spray the plastic sealing material onto the entire material strip, and then dry and solidify the material strip so that the entire material strip is completely plastic sealed. The material strip product is immersed in a high temperature resistant polyimide material, which is simple, easy to operate, and low in cost.

[0019] According to some preferred implementation aspects of the present invention, the removal is to remove the plastic encapsulation material on the welding area by laser. Laser can be used to selectively remove electrode polymer to achieve low-cost, high-efficiency and high-yield plastic encapsulation products.

[0020] According to some preferred implementation aspects of the present invention, the plastic packaging material is a polyimide material, preferably a high temperature resistant polyimide material, and its thermal decomposition temperature is 500-600°C.

[0021] According to some preferred implementation aspects of the present invention, the width of the electrode is greater than the width of the resistor body.

[0022] According to some preferred implementation aspects of the present invention, the working power of the high-power alloy resistor is greater than or equal to 7W, and the power of products with the same specifications is higher than that of traditional plastic-sealed resistors.

[0023] According to some preferred implementation aspects of the present invention, the separation is performed by longitudinal cutting along the thickness direction of the material strip to form a single bridge-shaped partial plastic-sealed resistor.

[0024] The present invention also provides a partially plastic-sealed high-power alloy resistor prepared by the above-mentioned preparation method.

[0025] Due to the adoption of the above technical scheme, compared with the prior art, the advantages of the present invention are as follows: the preparation method of the partially plastic-sealed high-power alloy resistor of the present invention adopts material strip welding, punching, plastic sealing, and then granulation and plastic sealing, which is convenient to prepare and gets rid of the dependence on molds; the product is plastic-sealed as a whole, and the end and welding area of ​​the product are electroplated with nickel and tin to achieve anti-oxidation performance during the product reflow soldering process. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0027] Figure 1 It is a schematic diagram of the cross-sectional structure of a partially plastic-sealed anti-oxidation high-power alloy resistor in an embodiment of the present invention;

[0028] Figure 2 It is a schematic diagram of the top view of the structure of a partially plastic-sealed anti-oxidation high-power alloy resistor in an embodiment of the present invention;

[0029] Figure 3 Schematic diagram of the material strip structure when preparing the oxidation-resistant high-power alloy resistor in the embodiment of the present invention

[0030] In the attached figure, 1: partially plastic-sealed anti-oxidation high-power alloy resistor; 2: strip; 3: alloy resistor body; 4: spacing area; 5: connection; 8: plastic sealing material; 9: resistor body; 10: electrode; 11: Ni plating layer; 12: Sn plating layer. DETAILED DESCRIPTION

[0031] In order to enable those skilled in the art to better understand the technical solution of the present invention, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0032] Example 1 High Power Alloy Resistor

[0033] like Figure 1-3 As shown, the partially plastic-sealed high-power alloy resistor 1 in this embodiment includes a resistor body 9, electrodes 10 located on both sides of the resistor body 9, a plastic sealing material 8 covering a partial surface of the alloy resistor, and nickel-tin layers 11 and 12 covering the remaining surface. The electrode 10 is welded on both sides of the length direction of the resistor body 9 by electron beam welding. The width of the electrode 10 is greater than the width of the resistor body 9, and the width direction here refers to the width direction of the high-power alloy resistor 1.

[0034] The thickness of the electrode 10 is greater than that of the resistor body 9. Specifically, on one side of the high-power alloy resistor 1 in the thickness direction, the electrode 10 is flush with the resistor body 9; on the other side of the high-power alloy resistor 1 in the thickness direction, the surface of the electrode 10 is higher than the surface of the resistor body 9 and extends outward.

[0035] In this embodiment, the high-power alloy resistor 1 is covered with a plastic packaging material 8 except for the two end faces in the length direction and the portion of the electrode 10 used for subsequent welding (welding area), and the remaining surface is covered with a nickel-plated layer 11 and a tin-plated layer 12, which can effectively achieve anti-oxidation performance during the product reflow soldering process.

[0036] The partially plastic-sealed high-power alloy resistor 1 in this embodiment has the advantages of high power, high resistance value accuracy, low temperature drift, wave soldering capability, and low manufacturing cost.

[0037] Example 2 Preparation method

[0038] This embodiment provides a method for preparing a partially plastic-sealed high-power alloy resistor 1 based on the embodiment 1, which specifically includes the following steps:

[0039] Step 1: Prepare the strip

[0040] According to the required resistance value, a suitable alloy strip and a suitable electrode strip are selected. The alloy strip is usually a Mn-Cu alloy, etc.; the electrode strip is a copper material with low resistivity. The electrode strip and the alloy strip are welded by electron beam welding to obtain an arched strip of electrode + alloy + electrode. The middle of the strip is electrode + alloy + electrode, and the two sides are strips 2 connected to the electrode.

[0041] During welding, the length extension direction of the electrode strip and the alloy strip is the same, and the two electrode strips are welded on the side of the alloy strip in the width direction. Among them, the thickness of the electrode strip is greater than the thickness of the alloy strip. The electrode strip is used to form the electrode 10 of the high-power alloy resistor 1, and the alloy strip is used to form the resistor body 9 of the high-power alloy resistor 1. The width of the electrode 10 finally formed is greater than the width of the resistor body 9.

[0042] On one side in the thickness direction of the material strip, the electrode strip is flush with the alloy strip; on the other side in the thickness direction of the material strip, the surface of the electrode strip is higher than the surface of the alloy strip to form a welding area.

[0043] Step 2: Punching

[0044] The material strip is punched according to the required resistance value and predetermined size, so that a plurality of alloy resistors 3 are formed on the material strip, and the terminal connection 5 of the electrodes 10 at both ends of each resistor alloy body is connected to the strip 2 to form the material strip. The plurality of alloy resistors 3 are arranged in sequence along the length direction of the material strip, and there is a spacing area 4 formed by punching between adjacent alloy resistors 3.

[0045] Step 3: Plastic sealing

[0046] The entire strip is plastic-sealed by immersing the entire strip in plastic-sealing material 8 or spraying the plastic-sealing material 8 onto the entire strip, and then drying and curing the strip to completely plastic-seale the entire strip, so that the outer surface of the alloy resistor 3 is completely covered with plastic-sealing material 8 .

[0047] The plastic encapsulation material 8 is a high temperature resistant polyimide material with a tensile strength of 250-500 MPa, a thermal decomposition temperature of 500-600°C, and a thermal expansion coefficient of 1×10 -6 / ℃, and the smoke rate is extremely low, and the carbon residue rate after high temperature combustion is above 50%.

[0048] Step 4: Laser

[0049] Laser is used to remove the plastic encapsulation material 8 corresponding to the welding area (i.e. the bottom of the electrode 10) on the alloy resistor 3 to expose the copper substrate, which is convenient for subsequent welding with the pad. The accuracy of laser can be controlled within ±0.2mm.

[0050] Step 5: Grain separation

[0051] The connection position 5 between the electrode 10 and the strip 2 on the plastic-sealed material strip is granulated, and the material strip is longitudinally cut along the thickness direction to separate the alloy resistor 3 from the material strip to form a partially plastic-sealed high-power alloy resistor 1, whose working power is greater than or equal to 7W.

[0052] The obtained partially plastic-sealed high-power alloy resistor 1 has a resistor body 9 and two welding electrodes 10. The high-power alloy resistor 1 has a plastic-sealed layer on the surface (welding area) at the bottom of the electrode 10 and the two end faces in the length direction.

[0053] Step 6: Electroplating

[0054] The product is rolled nickel-tin plated, so that the two end faces and the welding area of ​​the product form nickel-tin plating layers 11 and 12, and a partially plastic-sealed anti-oxidation high-power alloy resistor 1 is obtained. That is, the two end faces and the welding area of ​​the electrode of the obtained high-power alloy resistor 1 have a nickel plating layer 11 and an outer tin plating layer 12, and the surface of the remaining parts has a plastic sealing layer 8.

[0055] The electrical properties of the product made by the above method are as follows: power is 7~9w, resistance accuracy is 0.5%, and short-time overload test is 5 times rated power.

[0056] The preparation method of the partially plastic-sealed high-power alloy resistor of the present application changes the traditional stamping and bending process of the high-power alloy resistor, selects the material with electrode thickness greater than the alloy thickness to be directly welded into an arch material, greatly reduces the proportion of copper in the arch bridge and thus reduces the product resistance temperature coefficient. In addition, the high-power alloy resistor is selectively plastic-sealed to reduce manufacturing costs and diversify the specifications of the plastic-sealed products. Finally, the copper exposed position is electroplated, which has a better anti-oxidation effect, and the partially plastic-sealed high-power alloy resistor prepared has high power characteristics and low resistance temperature coefficient, and avoids the influence of tin climbing to the main part of the resistor during welding, which causes resistance value and temperature drift, and can be welded by wave soldering process. Compared with the prior art, the present application adopts a step welding method to achieve a low-temperature drift product; the product is immersed in a high-temperature resistant polyimide material, the method is simple and easy to operate, and the cost is low. The use of precisely controlled (±0.2mm) laser can selectively remove electrode polymers to achieve low-cost, high-efficiency, and high-yield plastic-sealed products; the flexibility in selecting applicable product sizes is relatively large and does not rely on molds; the high-temperature resistant polyimide material of the resistor body can achieve high-power resistance of the product; nickel-tin electroplating of the resistor ends and welding areas achieves antioxidant properties during the product reflow soldering process; the overall plastic sealing + electroplating of the product achieves good antioxidant properties.

[0057] The method for preparing a partially plastic-sealed high-power alloy resistor of the present invention adopts material strip welding, punching, plastic sealing, and then granulation and plastic sealing, which is convenient to prepare and gets rid of the dependence on molds; the product is plastic-sealed as a whole, and the end and welding area of ​​the product are electroplated with nickel and tin to achieve anti-oxidation performance during the product reflow soldering process.

[0058] The above embodiments prepared by the method of the present invention are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit and essence of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a partially plastic-sealed high-power alloy resistor, characterized in that: The steps include: Punching the material strip to form a plurality of alloy resistors on the material strip; Performing a plastic sealing operation on the entire material strip, immersing the entire material strip in a plastic sealing material or spraying the plastic sealing material on the entire material strip, and drying and curing the material, so that the entire material strip is completely plastic sealed, and the outer surface of the alloy resistor is completely covered with the plastic sealing material; Using laser to remove the plastic sealing material on the subsequent welding area corresponding to the electrode on the alloy resistor, the welding area is the surface of the bottom of the electrode; The connection position between the electrode and the strip on the plastic-sealed material strip is longitudinally cut along the thickness direction of the material strip to separate the alloy resistor body from the material strip to form a single partially plastic-sealed high-power alloy resistor; The remaining surface of the high-power alloy resistor except the two end faces in the length direction and the portion of the electrode used for subsequent welding is covered with a plastic packaging material.

2. The preparation method according to claim 1, characterized in that: The steps also include plating the partially plastic-sealed high-power alloy resistor with nickel and tin, so that an electroplating layer is formed in the welding area and the end faces of the alloy resistor, thereby forming a partially plastic-sealed anti-oxidation high-power alloy resistor; the two end faces in the length direction of the partially plastic-sealed anti-oxidation high-power alloy resistor and the welding area of ​​the electrode have a nickel-plated layer and an outer tin-plated layer, and the surface of the remaining part has a plastic-sealed layer.

3. The preparation method according to claim 1, characterized in that: The punching is to punch the material strip according to the predetermined size of the required resistance value, so that a plurality of alloy resistors are formed on the material strip, and the connection points of the two end electrodes of each resistor alloy body are connected to the strip; the plurality of alloy resistors are arranged in sequence along the length direction of the material strip, and there is a spacing area formed by punching between adjacent alloy resistors.

4. The preparation method according to claim 1, characterized in that: The material strip is obtained by electron beam welding an electrode strip and an alloy strip; during welding, the length extension direction of the electrode strip and the alloy strip is the same, and the two electrode strips are welded to the side surfaces in the width direction of the alloy strip to obtain an arched material strip of electrode+alloy+electrode.

5. The preparation method according to claim 4, characterized in that: The electrode strip is used to form an electrode of a high-power alloy resistor, and the alloy strip is used to form a resistor body of a high-power alloy resistor; the width of the electrode is greater than the width of the resistor body.

6. The preparation method according to claim 4, characterized in that: The alloy strip is made of Mn-Cu alloy, and the electrode strip is made of copper.

7. The preparation method according to claim 4, characterized in that: The thickness of the electrode strip is greater than the thickness of the alloy strip.

8. The preparation method according to claim 7, characterized in that: On one side of the material strip in the thickness direction, the electrode strip is flush with the alloy strip; on the other side of the material strip in the thickness direction, the surface of the electrode strip is higher than the surface of the alloy strip to form a welding area. 9 . The preparation method according to claim 1 , wherein the plastic packaging material is a polyimide material.

10. The preparation method according to claim 9, wherein the thermal decomposition temperature of the polyimide material is 500-600°C, the tensile strength is 250-500MPa, and the residual carbon rate after high-temperature combustion is above 50%.

11. The preparation method according to claim 1, wherein the accuracy of the laser is ±0.2 mm.

12. The preparation method according to any one of claims 1 to 11, characterized in that: The working power of the high-power alloy resistor is greater than or equal to 7W, the resistance accuracy is 0.5%, and the short-time overload test is 5 times the rated power.

Citation Information

Patent Citations

  • A resistor and a method for manufacturing the resistor