Quinoxaline-based polymer electrochromic electrode material and preparation method and application thereof

Through the electrochemical oxidation polymerization method of quinoxalinyl polymer, combined with electroactive monomers, a network structure is formed, which solves the problem of low capacitance of electrochromic materials of conductive polymers, and achieves high specific capacitance and superior electrochromicity performance.

CN119092306APending Publication Date: 2024-12-06SOUTH CHINA UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411242871.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing conductive polymer electrochromic materials have slower electron transport and weaker charge transport in molecules, resulting in lower capacitance in the field of energy storage materials. D-A copolymers are more used in the field of electrochromic but are used in energy storage. Less material.

Method used

Homopolymers and copolymers were prepared by electrochemical oxidation polymerization method using quinoxalinyl polymer, and electroactive monomers were introduced to form a network structure to improve the redox reaction speed and electrochromic properties.

Benefits of technology

Fast intramolecular charge transfer and high specific capacitance are achieved, improving the performance and energy storage capacity of electrochromic materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092306A_ABST
    Figure CN119092306A_ABST
Patent Text Reader

Abstract

The invention discloses a quinoxaline-based polymer electrochromic electrode material and a preparation method and application thereof, and the preparation method of the material comprises the following steps: preparing an intermediate monomer quinoxaline derivative through a Suzuki coupling method, adding the intermediate monomer quinoxaline derivative into an organic solvent containing electrolyte, and carrying out electrochemical oxidation polymerization on a conductive substrate to obtain a homopolymer. And under the same condition, adding an electroactive monomer as a comonomer, and carrying out electrochemical oxidation copolymerization to obtain the bithiophene bridged quinoxaline electrochromic copolymer. The preparation process is simple, the reaction conditions are mild, the specific capacitance of the prepared homopolymer material reaches 1.73 mF cm <-2 >, the specific capacitance of the copolymer material reaches 4.65 mF cm <-2 >, and a constant potential polarization test shows that the homopolymer is purple in a normal state, is caesious when being changed into 1V potential and is light blue when being changed into 1.3 V potential; the copolymer is brownish red in a normal state, is grey black in color change under the potential of 1.2 V, and is blue in color change under the potential of 1.4 V.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of preparation of electrochromic electrode materials, and in particular relates to quinoxaline-based polymer electrochromic electrode materials and preparation methods and applications thereof. Background Art

[0002] In recent years, the scientific community has begun to think more seriously about how to manage energy consumption and protect natural resources. A lot of research is currently being done on renewable energy, but as the population continues to grow, people must also pay attention to how to improve or replace the energy storage methods currently used. The development of renewable energy (solar energy, tidal energy, geothermal energy, wind energy, and biofuels, etc.) has also received widespread attention, but these renewable energy sources have peak seasons and times that energy storage devices must adapt to. This means that energy storage devices must be able to store a large amount of energy during peak hours to provide energy for low-peak seasons. New energy storage devices such as lithium batteries, fuel cells, and supercapacitors have become the first choice for storing this energy. Among them, supercapacitors have attracted the interest of a large number of researchers as emerging energy storage devices due to their characteristics of fast charging and discharging with large currents, high power density, and high cycle efficiency. The following are currently used as electrode materials for supercapacitors: metal oxides (hydroxides), conductive polymers, carbon materials, and electroactive organic small molecules. Conductive polymers have been the focus of researchers since their discovery. Now researchers have developed many types of conductive polymers and a variety of methods to improve conductive polymers. Conductive polymers such as polypyrrole, polyaniline, and polythiophene have shown good capabilities in electrode research, but their electron transport is still slow and the charge transport within the molecule is also weak, resulting in their performance as electrochromic materials being not superior. Tong et al. synthesized an electrochromic polymer material with thiophene as the main chain. Due to its structural rigidity and linear structure, the cyclic stability of difunctional polymers is extremely poor, and the trifunctional polymers have improved, but are still poor (Tong T., Yao Z., Shuo W. et al. Materials Chemistry and Physics, 2024, 128544). In the molecular design strategy of polymer donors, since it was proposed in 1992, the D–A copolymerization of electron-donating (D) units and electron-accepting (A) units has been proven to be the most important and effective method for constructing high-performance polymer donors. At present, almost all high-efficiency polymer donors for PSCs are designed based on the D–A strategy. The optical and electronic properties of D–A copolymers can be easily adjusted by controlling the intramolecular charge transfer (ICT) from the D unit to the A unit. Zhu et al. synthesized three quinoxaline-based DA copolymers with different substituents (Zhu, J.; Wang, W.; Chen, H et al. Journal of Solid State Chemistry 2022, 307), which have good electrochromic ability but low capacitance. DA copolymers are widely used in the field of electrochromic, but are rarely used in the field of energy storage materials. Therefore, it is of practical significance to develop a new type of polymer electrochromic material with good cycle and high capacitance. Summary of the invention

[0003] In order to overcome the problems that the above-mentioned traditional conductive polymers have poor electrochromic ability, DA copolymers are rarely used in the field of energy storage materials, and have low capacitance, the purpose of the present invention is to provide a quinoxaline-based polymer electrochromic electrode material and its preparation method and application. A quinoxaline derivative is added to an organic solvent containing an electrolyte, and a homopolymer is obtained by electrochemical oxidation polymerization. Under the same conditions, an electroactive monomer is added as a comonomer for electrochemical oxidation copolymerization to obtain a quinoxaline-based polymer electrochromic electrode material. The obtained homopolymer, as a DA-type polymer, has a fast intramolecular charge transfer, which enables it to undergo a fast redox reaction, so the homopolymer has good electrochromic ability and a higher specific capacitance; the obtained copolymer of quinoxaline derivatives and electroactive monomers has a faster redox process due to the introduction of an electroactive group as an electron donor, and the electrons are dispersed by the electron-withdrawing quinoxaline monomer, and the copolymer can form a network structure, has better film-forming properties, and has more superior electrochromic performance and a higher specific capacitance.

[0004] The purpose of the present invention is specifically achieved through the following technical solutions.

[0005] A method for preparing a quinoxaline-based polymer electrochromic electrode material comprises one of the following methods:

[0006] (1) Preparation of thiophene-bridged quinoxaline-based polymers: A quinoxaline derivative is added to an organic solvent containing an electrolyte, a platinum column electrode is used as a counter electrode, and an Ag / AgCl electrode is used as a reference electrode. After electrochemical oxidative polymerization, washing, and drying, a homopolymer is obtained on a cleaned conductive substrate.

[0007] (2) Preparation of thiophene-bridged quinoxaline electrochromic copolymer: A quinoxaline derivative and an electroactive monomer are added as two copolymer monomers in different proportions into an organic solvent containing an electrolyte. A platinum column electrode is used as a counter electrode and an Ag / AgCl electrode is used as a reference electrode. After electrochemical oxidation polymerization, washing and drying on a cleaned conductive substrate, a thiophene-bridged quinoxaline electrochromic copolymer is obtained.

[0008] Preferably, in method (1), the quinoxaline derivative is one of 5,8-di(3-hexylthiophene)quinoxaline, 5,8-di(bithiophene)quinoxaline and 5,8-dithiophenequinoxaline.

[0009] More preferably, in method (1), the quinoxaline derivative is 5,8-dithiophenequinoxaline.

[0010] Preferably, in method (2), the added electroactive monomer is one of a thiophene derivative, an aniline derivative, a pyrrole derivative, and tri(4-thienyl)triphenylamine (3TPA).

[0011] More preferably, in method (2), the electroactive monomer is tri(4-thienyl)triphenylamine.

[0012] Preferably, in method (2), the ratio of the quinoxaline derivative to the electroactive monomer is 20:1-1:20.

[0013] Further preferably, in method (2), the ratio of the quinoxaline derivative to the electroactive monomer is 1.5:1.

[0014] Preferably, in methods (1) and (2), the square resistance of the ITO glass is 10-100Ω.

[0015] Further preferably, in methods (1) and (2), the ITO glass has a square resistance of 10Ω.

[0016] Preferably, in methods (1) and (2), the cleaning process of the conductive substrate is ultrasonically treated in acetone, anhydrous ethanol, water, 0.5 wt% NaOH aqueous solution, water, anhydrous ethanol, acetone, and anhydrous ethanol for 15 minutes respectively.

[0017] Preferably, in methods (1) and (2), the total monomer concentration is 0.0005-1 mol / L.

[0018] More preferably, in methods (1) and (2), the total monomer concentration is 0.001 mol / L.

[0019] Preferably, in methods (1) and (2), the electrolyte concentration is 0.001-5 mol / L.

[0020] Further preferably, in methods (1) and (2), the electrolyte concentration is 0.1 mol / L.

[0021] Preferably, in methods (1) and (2), the electrolyte is one of tetrabutylammonium perchlorate, lithium perchlorate, lithium tetrafluoroborate, and tetrabutylammonium hexafluorophosphate.

[0022] More preferably, in methods (1) and (2), the electrolyte is tetrabutylammonium hexafluorophosphate.

[0023] Preferably, in methods (1) and (2), the conductive substrate is at least one of glassy carbon, indium tin oxide (ITO) glass, carbon cloth, and carbon paper.

[0024] Further preferably, in methods (1) and (2), the conductive substrate is ITO glass.

[0025] Preferably, in methods (1) and (2), the CV scanning cycle number of the electrochemical oxidative polymerization reaction is 5-100.

[0026] Further preferably, in methods (1) and (2), the CV scanning cycle number of the electrochemical oxidative polymerization reaction is 15.

[0027] Preferably, in methods (1) and (2), the CV scanning potential range of the electrochemical oxidative polymerization reaction is -1-2V.

[0028] Further preferably, in methods (1) and (2), the CV scanning potential range of the electrochemical oxidative polymerization reaction is 0-1.6V.

[0029] Preferably, in methods (1) and (2), the electrochemical oxidative polymerization method is cyclic voltammetry with a scan rate of 20-200 mV s -1 .

[0030] Further preferably, in methods (1) and (2), the electrochemical oxidative polymerization method is cyclic voltammetry with a scan rate of 100 mV s -1 .

[0031] Preferably, in methods (1) and (2), the washing is washing with dichloromethane.

[0032] Preferably, in methods (1) and (2), the drying environment is vacuum, the temperature is 20-60° C., and the drying time is 6-48 hours.

[0033] Further preferably, in methods (1) and (2), the drying environment is vacuum, the temperature is 40° C., and the drying time is 12 h.

[0034] The quinoxaline-based polymer electrochromic electrode material was prepared by the above-mentioned preparation method, and the specific capacitance of the homopolymer material reached 1.73mF cm -2 The specific capacitance of the copolymer material is as high as 4.65mF cm -2 Through constant potential polarization test, it was found that the homopolymer is purple in normal state, changes to blue-gray at a potential of 1V, and changes to light blue at 1.3V; the copolymer is brown-red in normal state, changes to gray-black at a potential of 1.2V, and changes to blue at 1.4V.

[0035] Application of the quinoxaline-based polymer electrochromic electrode material in electrochromic devices.

[0036] Application of the quinoxaline-based polymer electrochromic electrode material in energy storage devices.

[0037] Compared with the prior art, the present invention has the following advantages and technical effects:

[0038] (1) The optimal performance of the quinoxaline-based copolymer synthesized by the present invention is 4.65 mF cm-2 It has a high specific capacitance and is an energy storage electrode material with a high specific capacitance.

[0039] (2) The present invention synthesizes quinoxaline derivatives containing thiophene groups and utilizes electrochemical polymerization methods to bridge quinoxaline with thiophene groups, thereby providing a fast electron transfer path, increasing specific capacitance, and also having rich color changes.

[0040] (3) The present invention introduces electroactive monomer copolymerization to form a network node during polymerization, so that the DA copolymer chain is uniformly attached to the ITO glass surface in a network structure, thereby increasing the specific surface area of ​​the composite material and further increasing the contact area between the electrolyte and the electrode; at the same time, the electroactive monomer serves as a site for redox reaction, which can provide more pseudocapacitance, and the electroactive monomer can better disperse the charge, which is beneficial to charge transfer.

[0041] (4) The synthesis process of the present invention is simple to operate, has mild reaction conditions, low energy consumption, and is suitable for large-scale industrial applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 Schematic diagram of the reaction process of an embodiment of the present invention.

[0043] Figure 2 This is the polymerization CV diagram of the quinoxaline-based homopolymer material prepared in Example 2 of the present invention.

[0044] Figure 3 The quinoxaline-based homopolymer material prepared in Example 2 of the present invention is subjected to the following tests at 25, 50, 75, 100, 150, and 200 mV s -1 CV graph of.

[0045] Figure 4 The graph is a current response (CA) graph of the quinoxaline-based homopolymer material prepared in Example 2 of the present invention at potentials of 1V and 0V.

[0046] Figure 5 The quinoxaline-based copolymer material prepared in Example 3 of the present invention has a thermal conductivity of 25, 50, 75, 100, 150, and 200 mVs -1 CV graph of.

[0047] Figure 6 The bithiophene-bridged quinoxaline-based copolymer material prepared in Example 3 of the present invention has a conductivity of 0.05, 0.1, 0.2, 0.5, 0.7, and 1 mA cm -2 Comparison chart of constant current charge and discharge (GCD) under the same conditions. DETAILED DESCRIPTION

[0048] The specific implementation of the present invention is further described below in conjunction with examples and drawings, but the implementation of the present invention is not limited thereto.

[0049] Figure 1 The schematic diagram of the reaction process of the quinoxaline-based polymer electrochromic electrode material proposed in the present invention is shown in the following examples. Figure 1 The process operation is shown.

[0050] Example 1

[0051] (1) Preparation of quinoxaline-based homopolymer material: 5,8-di(3-hexylthiophene)quinoxaline and tetrabutylammonium hexafluorophosphate were added to 30 ml of dichloromethane, with the initial concentration of tetrabutylammonium hexafluorophosphate being 0.001 mol / L and the initial concentration of 5,8-di(3-hexylthiophene)quinoxaline being 0.5 mmol / L. Then, electrochemical oxidative polymerization was carried out by cyclic voltammetry using a platinum column electrode as the counter electrode, ITO glass as the working electrode, and Ag / AgCl electrode as the reference electrode at a scan rate of 20 mV s -1 , the number of cycles is 30, and the potential range is -1-1.4 V. Finally, the obtained polymer film is washed and dried to obtain the thiophene-bridged quinoxaline-based polymer.

[0052] (2) Preparation of quinoxaline-based copolymer materials: 5,8-dithiophenequinoxaline, 3,4-ethylenedioxythiophene and tetrabutylammonium hexafluorophosphate were added to dichloromethane, the initial concentration of the electrolyte was 0.001 mol / L, the initial total concentration of the monomer was 0.5 mmol / L, and the ratio was 1:1. Then, a platinum column electrode was used as the counter electrode, ITO glass was used as the working electrode, and Ag / AgCl electrode was used as the reference electrode. Electrochemical oxidation polymerization was carried out by cyclic voltammetry, with a cycle number of 50 and a scan rate of 20 mV s -1 , the potential range is -1-1.6 V. Finally, the obtained polymer film is washed and dried to obtain the quinoxaline-based electrochromic copolymer material.

[0053] Example 2

[0054] (1) Preparation of quinoxaline-based homopolymer material: 5,8-dithiophenequinoxaline and tetrabutylammonium hexafluorophosphate were added to 30 ml of dichloromethane, with the initial concentration of tetrabutylammonium hexafluorophosphate being 0.1 mol / L and the initial concentration of 5,8-dithiophenequinoxaline being 1 mmol / L. Then, electrochemical oxidative polymerization was carried out by cyclic voltammetry using a platinum column electrode as the counter electrode, ITO glass as the working electrode, and Ag / AgCl electrode as the reference electrode. The cycle number was 15 and the scan rate was 100 mV s -1 , the potential range is 0-1.6V. Figure 2As shown in the figure, the first CV curve has an obvious oxidation peak at about 1.2V, proving that the monomer has free radicals available for polymerization at 1.2V, and as the number of scans increases, the monomer that originally did not have a redox peak begins to have a combined redox peak, and the area around the curve increases with the number of scans, proving that the monomer has undergone a polymerization reaction within this potential range, and the polymer was successfully prepared. Finally, the obtained polymer film was washed and dried to obtain a quinoxaline-based homopolymer material.

[0055] (2) Preparation of quinoxaline-based copolymer materials: 5,8-dithiophenequinoxaline, pyrrole and tetrabutylammonium perchlorate were added to dichloromethane, the initial concentration of tetrabutylammonium perchlorate was 1 mol / L, the initial total concentration of monomers was 0.5 mol / L, and the ratio was 1:10. Then, a platinum column electrode was used as the counter electrode, a glassy carbon electrode was used as the working electrode, and an Ag / AgCl electrode was used as the reference electrode. The electrochemical oxidation polymerization was carried out by cyclic voltammetry, with a cycle number of 50 and a scan rate of 50 mV s -1 , the potential range is -1-1.6 V. Finally, the obtained polymer film is washed and dried to obtain the quinoxaline-based electrochromic copolymer material.

[0056] The quinoxaline-based homopolymer material prepared in this embodiment was subjected to a CV curve test in order to test its current response changes at different scan rates. Figure 3 As shown, at 25mV s -1 The initial oxidation potential is 0.42V at a scan rate, and then it begins to have a peak shape at 0.9V. During the reverse scan, the reduction peak is not obvious enough. When the scan rate is gradually increased, the oxidation peak and the reduction peak become more and more obvious, proving that the material has a good electrochemical response.

[0057] The bithiophene-bridged quinoxaline-based polymer material prepared in this example was subjected to a constant potential polarization test to analyze its response time and charge amount to the color change caused by the potential change. Figure 4 As shown in the figure, it can be seen that the time for the current to decay to 90% at 1V is 3.39s, and the time for the current to decay to 90% at 0V is 1.12s, and the electric charges are 4.1mC and 3.8mC respectively, indicating that the electrochromic response is excellent.

[0058] Example 3

[0059] (1) Preparation of quinoxaline-based homopolymer material: 5,8-dithiophenequinoxaline and lithium tetrafluoroborate were added to 30 ml of dichloromethane, with the initial concentration of lithium tetrafluoroborate being 5 mol / L and the initial concentration of 5,8-dithiophenequinoxaline being 1 mol / L. Then, electrochemical oxidative polymerization was carried out by cyclic voltammetry using a platinum column electrode as the counter electrode, ITO glass as the working electrode, and Ag / AgCl electrode as the reference electrode at a scan rate of 50 mV s -1 , the number of cycles is 5, and the potential range is 0-2 V. Finally, the obtained polymer film is washed and dried to obtain a quinoxaline-based homopolymer material.

[0060] (2) Preparation of quinoxaline-based copolymer materials: 5,8-dithiophenequinoxaline, tri(4-thienyl)triphenylamine and tetrabutylammonium hexafluorophosphate were added to dichloromethane. The initial concentration of the electrolyte was 0.1 mol / L, the initial total concentration of the monomer was 1 mmol / L, and the ratio was 1.5:1. Then, a platinum column electrode was used as the counter electrode, ITO glass was used as the working electrode, and Ag / AgCl electrode was used as the reference electrode. Electrochemical oxidative polymerization was carried out by cyclic voltammetry. The number of cycles was 15 and the scan rate was 100 mV s -1 , the potential range is 0-1.6V. Finally, the obtained polymer film is washed and dried to obtain a quinoxaline-based copolymer material. The obtained material was tested and found to have a high conductivity at 0.05mA cm -2 The specific capacitance can reach 4.65mF cm at a current density of -2 .

[0061] The quinoxaline-based copolymer material prepared in this embodiment was subjected to a CV curve test to analyze its response changes to different scanning rates. Figure 5 As shown in the figure, it can be seen that at 25mV s -1 The initial oxidation potential is 0.55V at the scan rate, and then it starts to have a peak shape at 0.95V. During the reverse scan, the reduction peak is obvious, and when the scan rate gradually increases, the oxidation peak and the reduction peak become more and more obvious, proving that the material has an excellent electrochemical response.

[0062] The bithiophene-bridged quinoxaline-based polymer material prepared in this example was subjected to a GCD test. Figure 6 As shown in Figure 2, the potential window is 0.4-1.4 V. As the current density increases, it increases at 0.5 mA cm -2 The specific capacitance is still 0.05 mA cm at a current density of -2 67.6% at a current density of 1.3 Å, demonstrating its good rate performance.

[0063] Example 4

[0064] (1) Preparation of quinoxaline-based homopolymer material: 5,8-dithiophenequinoxaline and tetrabutylammonium hexafluorophosphate were added to 30 ml of acetonitrile, with the initial concentration of tetrabutylammonium hexafluorophosphate being 1 mol / L and the initial concentration of 5,8-dithiophenequinoxaline being 1 mmol / L. Then, electrochemical oxidation polymerization was carried out by cyclic voltammetry using a platinum column electrode as the counter electrode, a carbon cloth as the working electrode, and an Ag / AgCl electrode as the reference electrode, with a cycle number of 100 and a scan rate of 100 mV s -1 , the potential range is 0-1.8 V. Finally, the obtained polymer is washed and dried to obtain a quinoxaline-based homopolymer material.

[0065] (2) Preparation of quinoxaline-based copolymer materials: 5,8-dithiophenequinoxaline, aniline and tetrabutylammonium hexafluorophosphate were added to dichloromethane. The initial concentration of the electrolyte was 0.5 mol / L, the initial total concentration of the monomer was 0.05 mol / L, and the ratio was 20:1. Then, a platinum column electrode was used as the counter electrode, ITO glass was used as the working electrode, and Ag / AgCl electrode was used as the reference electrode. Electrochemical oxidative polymerization was carried out by cyclic voltammetry. The number of cycles was 20 and the scan rate was 200 mV s -1 , the potential range is -1-2 V. Finally, the obtained polymer film is washed and dried to obtain a quinoxaline-based copolymer material.

[0066] Example 5

[0067] (1) Preparation of quinoxaline-based homopolymer material: 5,8-dithiophenequinoxaline and tetrabutylammonium hexafluorophosphate were added to 30 ml of dichloromethane, with the initial concentration of lithium perchlorate being 0.1 mol / L and the initial concentration of 5,8-dithiophenequinoxaline being 0.005 mol / L. Then, electrochemical oxidation polymerization was carried out by cyclic voltammetry using a platinum column electrode as the counter electrode, ITO glass as the working electrode, and Ag / AgCl electrode as the reference electrode, with a cycle number of 100 and a scan rate of 200 mV s -1 , the potential range is 0-1.4 V. Finally, the obtained polymer film is washed and dried to obtain a quinoxaline-based homopolymer material.

[0068] (2) Preparation of quinoxaline-based copolymer materials: 5,8-dithiophenequinoxaline, tri(4-thienyl)triphenylamine and tetrabutylammonium hexafluorophosphate were added to dichloromethane. The initial concentration of the electrolyte was 0.1 mol / L, the initial total concentration of the monomer was 1 mmol / L, and the ratio was 3:1. Then, a platinum column electrode was used as the counter electrode, ITO glass was used as the working electrode, and Ag / AgCl electrode was used as the reference electrode. Electrochemical oxidative polymerization was carried out by cyclic voltammetry. The number of cycles was 40 and the scan rate was 100 mV s -1, the potential range is 0-1.5 V. Finally, the obtained polymer film is washed and dried to obtain a quinoxaline-based copolymer material.

[0069] Example 6

[0070] (1) Preparation of quinoxaline-based homopolymer material: 5,8-dithiophenequinoxaline and tetrabutylammonium hexafluorophosphate were added to 30 ml of dichloromethane, with the initial concentration of tetrabutylammonium hexafluorophosphate being 0.1 mol / L and the initial concentration of 5,8-dithiophenequinoxaline being 0.05 mol / L. Then, electrochemical oxidative polymerization was carried out by cyclic voltammetry using a platinum column electrode as the counter electrode, ITO glass as the working electrode, and Ag / AgCl electrode as the reference electrode. The number of cycles was 20 and the scan rate was 100 mV s -1 , the potential range is -0.6-1.5 V. Finally, the obtained polymer film is washed and dried to obtain a quinoxaline-based homopolymer material.

[0071] (2) Preparation of quinoxaline-based copolymer materials: 5,8-dithiophenequinoxaline, tri(4-thienyl)triphenylamine and tetrabutylammonium hexafluorophosphate were added to dichloromethane, the initial concentration of the electrolyte was 0.1 mol / L, the initial total concentration of the monomer was 0.1 mol / L, and the ratio was 3:1. Then, a platinum column electrode was used as the counter electrode, ITO glass was used as the working electrode, and Ag / AgCl electrode was used as the reference electrode. Electrochemical oxidative polymerization was carried out by cyclic voltammetry, with a cycle number of 40 and a scan rate of 100 mV s -1 , the potential range is 0-1.5 V. Finally, the obtained polymer film is washed and dried to obtain a quinoxaline-based copolymer material.

[0072] Example 7

[0073] (1) Preparation of quinoxaline-based homopolymer material: 5,8-dithiophenequinoxaline and tetrabutylammonium hexafluorophosphate were added to 30 ml of tetrahydrofuran, with the initial concentration of tetrabutylammonium hexafluorophosphate being 0.1 mol / L and the initial concentration of 5,8-dithiophenequinoxaline being 0.005 mol / L. Then, electrochemical oxidation polymerization was carried out by cyclic voltammetry using a platinum column electrode as the counter electrode, ITO glass as the working electrode, and Ag / AgCl electrode as the reference electrode, with a cycle number of 100 and a scan rate of 100 mV s -1 , the potential range is -0.3-1.8 V. Finally, the obtained polymer film is washed and dried to obtain a quinoxaline-based homopolymer material.

[0074] (2) Preparation of quinoxaline-based copolymer materials: 5,8-dithiophenequinoxaline, tri(4-thienyl)triphenylamine and tetrabutylammonium hexafluorophosphate were added to dichloromethane. The initial concentration of the electrolyte was 0.1 mol / L, the initial total concentration of the monomer was 1 mol / L, and the ratio was 1:20. Then, a platinum column electrode was used as the counter electrode, ITO glass was used as the working electrode, and Ag / AgCl electrode was used as the reference electrode. Electrochemical oxidative polymerization was carried out by cyclic voltammetry. The number of cycles was 5 and the scan rate was 200 mV s -1 , the potential range is 0-1.4 V. Finally, the obtained polymer film is washed and dried to obtain a quinoxaline-based copolymer material.

[0075] Example 8

[0076] (1) Preparation of quinoxaline-based homopolymer material: 5,8-dithiophenequinoxaline and tetrabutylammonium hexafluorophosphate were added to 30 ml of methanol, with the initial concentration of tetrabutylammonium hexafluorophosphate being 1 mol / L and the initial concentration of 5,8-dithiophenequinoxaline being 0.1 mol / L. Then, electrochemical oxidative polymerization was carried out by cyclic voltammetry using a platinum column electrode as the counter electrode, ITO glass as the working electrode, and Ag / AgCl electrode as the reference electrode. The number of cycles was 15 and the scan rate was 150 mV s -1 , the potential range is -0.3-1.8 V. Finally, the obtained polymer film is washed and dried to obtain a quinoxaline-based homopolymer material.

[0077] (2) Preparation of quinoxaline-based copolymer materials: 5,8-dithiophenequinoxaline, tri(4-thienyl)triphenylamine and tetrabutylammonium hexafluorophosphate were added to dichloromethane, the initial concentration of the electrolyte was 0.1 mol / L, the initial total concentration of the monomer was 0.0005 mol / L, and the ratio was 9:1. Then, a platinum column electrode was used as the counter electrode, carbon paper was used as the working electrode, and Ag / AgCl electrode was used as the reference electrode. Electrochemical oxidation polymerization was carried out by cyclic voltammetry, the number of cycles was 100, and the potential range was -0.3-1.7 V. Finally, the obtained polymer film was washed and dried to obtain the quinoxaline-based copolymer material.

Claims

1. A method for preparing a quinoxaline-based polymer electrochromic electrode material, characterized in that: This includes one of the following methods: (1) Preparation of thiophene-bridged quinoxaline-based polymers: A quinoxaline derivative is added to an organic solvent containing an electrolyte, a platinum column electrode is used as a counter electrode, and an Ag / AgCl electrode is used as a reference electrode. After electrochemical oxidative polymerization, washing, and drying, a homopolymer is obtained on a cleaned conductive substrate; (2) Preparation of thiophene-bridged quinoxaline electrochromic copolymers: A quinoxaline derivative and an electroactive monomer are added as two copolymers in different proportions into an organic solvent containing an electrolyte. A platinum column electrode is used as a counter electrode and an Ag / AgCl electrode is used as a reference electrode. After electrochemical oxidation polymerization, washing and drying on a cleaned conductive substrate, a thiophene-bridged quinoxaline electrochromic copolymer is obtained.

2. The method for preparing the quinoxaline-based polymer electrochromic electrode material according to claim 1, characterized in that: In method (1), the added quinoxaline derivative is one of 5,8-di(3-hexylthiophene)quinoxaline, 5,8-di(bithiophene)quinoxaline, and 5,8-dithiophenequinoxaline (DTQX); The initial monomer concentration of the quinoxaline derivative for electrochemical oxidative polymerization is 0.0005-1 mol / L, and the initial electrolyte concentration is 0.001-5 mol / L.

3. The method for preparing the quinoxaline-based polymer electrochromic electrode material according to claim 1, characterized in that: In method (2), the molar ratio of the quinoxaline derivative to the electroactive monomer is 20:1-1:20; The electroactive monomer is one of a thiophene derivative, an aniline derivative, a pyrrole derivative, and tri(4-thienyl)triphenylamine (3TPA); The total initial monomer concentration of the electrochemical oxidative polymerization of the quinoxaline derivative and the electroactive monomer is 0.0005-1 mol / L, and the initial concentration of the electrolyte is 0.001-5 mol / L.

4. The method for preparing the quinoxaline-based polymer electrochromic electrode material according to claim 1, characterized in that: In method (1) and method (2), the electrolyte is one of tetrabutylammonium perchlorate, lithium perchlorate, lithium tetrafluoroborate, and tetrabutylammonium hexafluorophosphate; The organic solvent is at least one of methanol, acetonitrile, dimethylformamide, dimethyl sulfoxide, propylene carbonate, tetrahydrofuran and dichloromethane.

5. The method for preparing the quinoxaline-based polymer electrochromic electrode material according to claim 1, characterized in that: In method (1) and method (2), the electrochemical oxidative polymerization method is cyclic voltammetry, the number of cycles is 5-100, and the potential range is -1-2V.

6. The method for preparing the quinoxaline-based polymer electrochromic electrode material according to claim 1, characterized in that: In method (1) and method (2), the electrochemical oxidative polymerization method is cyclic voltammetry (CV) with a scan rate of 20-200 mV s -1 .

7. The preparation method according to claim 1, characterized in that: In method (1) and method (2), the conductive substrate is one or more of glassy carbon, indium tin oxide (ITO) glass, carbon cloth, carbon paper, Prussian blue, and tungsten trioxide.

8. The quinoxaline-based polymer electrochromic electrode material prepared by the preparation method according to any one of claims 1 to 7, characterized in that: Homopolymer material specific capacitance reaches 1.73mF cm -2 The specific capacitance of the copolymer material is as high as 4.65mF cm -2 Through constant potential polarization test, it was found that the homopolymer is purple in normal state, changes to blue-gray at a potential of 1V, and changes to light blue at 1.3V; the copolymer is brown-red in normal state, changes to gray-black at a potential of 1.2V, and changes to blue at 1.4V.

9. Use of the quinoxaline-based polymer electrochromic electrode material according to claim 8 in an electrochromic device.

10. Use of the quinoxaline-based polymer electrochromic electrode material according to claim 8 in energy storage devices.