High-contrast wafer positioning calibration marker and preparation method thereof

The wafer positioning calibration standards for multilayer films of dielectrics are prepared through electron beam thermal evaporation and exposure technology, which solves the problems of metal pollution and positioning accuracy, and achieves high contrast and high-precision positioning calibration, avoids metal pollution and improves the flow stripping Yield rate.

CN119092486AInactive Publication Date: 2024-12-06METRIC OPTICS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411226997.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In existing integrated circuit measurement equipment, the positioning markers of metal graphic structures are likely to cause metal contamination of the instruments and equipment during use, reducing the yield rate of the flow sheet, and the positioning accuracy is difficult to meet the high requirements.

Method used

The electron beam thermal evaporation technology is used to prepare non-metallic multilayer films, combined with electron beam exposure technology and inductive coupling-reactive ion etching technology, high contrast wafer positioning calibration standards are prepared, and the dielectric multilayer film is used to provide high reflectivity , avoid metal contamination, and remove photoresist residues through a plasma demolifier to ensure nano-scale processing accuracy.

Benefits of technology

It effectively avoids the risk of metal contamination, improves the graphical positioning accuracy and automated recognition capabilities of wafer positioning calibration standards, and ensures high contrast and high-precision positioning calibration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092486A_ABST
    Figure CN119092486A_ABST
Patent Text Reader

Abstract

The invention discloses a high-contrast wafer positioning calibration marker and a preparation method thereof. The preparation method comprises the following steps: S1, preparing a medium multilayer film by adopting an electron beam thermal evaporation technology; s2, spin-coating photoresist on the surface of the dielectric multilayer film; s3, exposing by adopting an electron beam exposure technology, sequentially putting the exposed sample into a developing solution and a fixing solution, and removing the photoresist in an exposed area to obtain a photoresist pattern with the same shape as the design pattern; s4, completely etching the Si layer on the top layer by adopting an inductive coupling-reactive ion etching technology; s5, removing the residual photoresist on the surface through a plasma photoresist removing machine; and S6, carrying out subsequent cleaning on the surface by using the photoresist removing solution to obtain the wafer positioning calibration marker. According to the high-contrast wafer positioning calibration marker and the preparation method thereof, the dielectric material provides high contrast and has no metal pollution risk, and the high-contrast wafer positioning calibration marker has the advantage of high pattern positioning precision by utilizing the nanoscale processing precision of electron beam exposure patterning.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of integrated circuit manufacturing, and in particular to a high-contrast wafer positioning calibration mark and a preparation method thereof. Background Art

[0002] In the field of integrated circuit manufacturing, measurement and analysis using integrated circuit measurement equipment is an essential part of daily monitoring on the process line. By monitoring the accuracy of online tape-out and different process nodes, the process and product yield can be guaranteed. However, there are often errors in integrated circuit measurement equipment, so it is very necessary to calibrate the integrated circuit measurement equipment regularly to improve the measurement accuracy and precision of the equipment and ensure that the measurement results meet the standard requirements.

[0003] During the calibration process, a standard object is usually needed to help calibrate the device. A positioning standard object is an object with known size and characteristics. By comparing the value measured by the device after the positioning standard object is measured with the standard value, the positioning error of the device's translation stage can be determined and calibration adjustments can be made.

[0004] Wafer positioning calibration marks are the main tool and necessary condition for the current chip manufacturing position accuracy calibration. Through a sufficient number of characteristic patterns with the same shape in a specific position of the wafer, and based on scanning methods such as stage mapping, it can realize its monitoring wafer function as a metrological performance evaluation and tracking. Usually, the positioning mark mode includes two dimensions and can be used for positioning calibration in both X and Y directions.

[0005] In the prior art, there are two main performance requirements for positioning markers:

[0006] (1) To make the calibration of automatic metrology tools easier, the characteristic pattern of the positioning target needs to have high contrast under the optical microscope to facilitate automatic recognition and calibration;

[0007] (2) The positioning accuracy between any feature patterns should be as high as possible, which places high demands on the processing accuracy of the positioning mark.

[0008] To meet the above two requirements, the current mainstream technical solution is to use metal graphic structures to improve optical contrast using the high reflectivity of metal. However, during the manufacturing process, metal residues are inevitably present on the surface of the wafer, which greatly increases the risk of metal contamination to instruments and equipment during the use of positioning markers, thereby reducing the yield rate of wafer production, and in severe cases, will bring immeasurable economic losses. Summary of the invention

[0009] The purpose of the present invention is to provide a high-contrast wafer positioning calibration mark and a preparation method, which utilizes dielectric materials to provide high contrast, effectively avoiding the risk of metal contamination to instruments and equipment caused by wafer marks with metal patterns during use. The nanometer-level processing accuracy of electron beam exposure patterning ensures that the final wafer positioning calibration mark has extremely high pattern positioning accuracy.

[0010] To achieve the above object, the present invention provides a method for preparing a high-contrast wafer positioning calibration mark, comprising the following steps:

[0011] S1. Using electron beam thermal evaporation technology to prepare a non-metallic dielectric multilayer film of a predetermined thickness on the surface of a cleaned wafer substrate;

[0012] S2, spin-coating a photoresist having a thickness not less than 1 / 3 of the thickness of the top Si layer on the surface of the dielectric multilayer film obtained in step S1, and baking to solidify it, thereby obtaining a photoresist-dielectric multilayer film sample;

[0013] S3, exposing the photoresist-dielectric multilayer film sample obtained in step S2 by electron beam exposure technology, wherein the exposure pattern is the design pattern of the wafer positioning calibration mark, placing the exposed sample in a developer and a fixer in sequence, removing the photoresist in the exposed area, and obtaining a photoresist pattern having the same shape as the design pattern;

[0014] S4, using the photoresist pattern obtained in step S3 as a mask, using inductively coupled-reactive ion etching technology to completely etch the top Si layer to obtain a multilayer film sample with a desired pattern structure;

[0015] S5, using a plasma stripper to remove the remaining photoresist on the surface of the multilayer film sample obtained in step S4 using oxygen ions;

[0016] S6. Post-cleaning the surface of the multilayer film sample obtained in step S5 using a degumming solution to remove organic matter and particles remaining on the surface, thereby obtaining a wafer positioning calibration standard.

[0017] Preferably, in step S1, the thickness of the dielectric multilayer film is controlled by an optical monitoring method.

[0018] Preferably, in step S1, the process parameters of the electron beam evaporation technology are: voltage 200-250V, current 500mA, Si deposition rate The SiO2 deposition rate is The wafer substrate heating temperature is 150°C and the background vacuum is less than 5×10 -4 pa.

[0019] Preferably, in step S2, the photoresist is PMMA or ZEP;

[0020] The process parameters of the photoresist spin coating are as follows: the rotation speed of the photoresist spin coating machine is 3000-4000 r / min, the baking uses a hot plate, the temperature is 178-182° C., and the time is 8-12 min.

[0021] Preferably, in step S3, the process parameters of the electron beam exposure technology are: electron acceleration voltage is 100 kV, beam spot current is 49.5-50.5 nA, beam spot size is 35-45 nm, and exposure dose is 950-1250 μC / cm2;

[0022] The developer is a mixed solution of methyl isobutyl ketone MIBK and isopropyl alcohol IPA in a mixing ratio of 1:3, the developing temperature is 22.8-23.2° C., and the developing time is 1-5 min;

[0023] The fixing solution is an IPA solution, and the image is rinsed in the fixing solution for 0.5 to 1 min and blown dry with a nitrogen gun.

[0024] Preferably, in step S4, the process parameters of the inductively coupled reactive ion etching technology are: trifluoromethane with a flow rate of 50 sccm and sulfur hexafluoride with a flow rate of 15 sccm as etching gas, a pressure of 15 mTorr, an RF source power of 25 W, an inductively coupled plasma power of 1200 W, a bias voltage of 380 V, an operating temperature of 5° C., and an etching rate of 10 nm / s.

[0025] Preferably, in step S5, the relevant parameters of the plasma stripping machine are: using an oxygen flow rate of 50 sccm, a pressure of 15 mTorr, an RF source power of 25 W, an inductively coupled plasma power of 1000 W, a bias voltage of 380 V, an operating temperature of 5° C., and an etching time of 2 min.

[0026] To achieve the above-mentioned purpose, the present invention also provides a high-contrast wafer positioning calibration mark, including a wafer substrate and a dielectric multilayer film arranged on the surface of the wafer substrate, wherein the surface array of the wafer substrate is arranged with a plurality of units, and characteristic patterns are arranged between adjacent units, and the characteristic patterns are arranged in a grid shape for establishing a grid coordinate system.

[0027] Preferably, the characteristic pattern is one or more of a cross, a square and a windmill.

[0028] Preferably, the dielectric multilayer film comprises a plurality of alternating high refractive index material layers and low refractive index material layers, the top layer of the dielectric multilayer film is a high refractive index material layer, the high refractive index material layer is Si, the low refractive index material layer is SiO2, the number of layers of the dielectric multilayer film is 2 to 10, and the thickness of each film layer is determined by optimizing the design using thin film design software.

[0029] Therefore, the present invention adopts the above-mentioned high-contrast wafer positioning calibration standard and preparation method, and the beneficial effects are as follows:

[0030] (1) The present invention has no metal pollution: The present invention utilizes dielectric multilayer films to replace traditional metals, thereby fundamentally avoiding the risk of metal contamination that may be caused to instruments and equipment by wafer markers with metal patterns during use. Thin film design software is used to optimize the high reflectivity of the multilayer film in the entire visible spectrum. The dielectric multilayer film provides high reflectivity in the entire visible spectrum to ensure that the feature patterns processed on the wafer substrate have high contrast when observed under an optical microscope, which is convenient for automatic identification.

[0031] (2) The present invention has high pattern positioning accuracy: The present invention adopts a processing method based on electron beam lithography technology, and its nanometer-level processing accuracy ensures that the final wafer positioning calibration mark can have extremely high pattern positioning accuracy. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 It is a schematic flow chart of an embodiment of a high-contrast wafer positioning calibration standard and a preparation method of the present invention;

[0033] Figure 2 Schematic diagram of the effect of characteristic patterns of a high-contrast wafer positioning calibration mark and a preparation method embodiment of the present invention, wherein (a) is a square, (b) is a windmill, and (c) is a cross;

[0034] Figure 3 It is a microscopic schematic diagram of the surface of a wafer substrate according to an embodiment of a high-contrast wafer positioning calibration mark and a preparation method of the present invention. DETAILED DESCRIPTION

[0035] The technical solution of the present invention is further described below through the accompanying drawings and embodiments.

[0036] Unless otherwise defined, technical or scientific terms used in the present invention shall have the common meanings understood by one having ordinary skills in the field to which the present invention belongs.

[0037] Embodiment 1

[0038] like Figure 1 As shown, a method for preparing a high-contrast wafer positioning calibration mark includes the following steps:

[0039] S1. Prepare a SiO2 / Si multilayer film of predetermined thickness on the surface of the cleaned wafer substrate using electron beam thermal evaporation technology. The thickness of the SiO2 / Si multilayer film is controlled by optical monitoring method. The process parameters are: voltage 200V, current 500mA, Si deposition rate The SiO2 deposition rate is The heating temperature of the wafer substrate is 150°C, and the background vacuum degree is less than 5×10 -4 pa.

[0040] S2, spin-coating photoresist on the surface of the SiO2 / Si multilayer film obtained in step S1, and baking to solidify it, to obtain a photoresist-SiO2 / Si multilayer film sample. The photoresist is PMMA, and the photoresist spin coating process parameters are set as follows: the speed of the coating machine is 3000r / min, the thickness is 200nm, and the baking is done on a hot plate at a temperature of 180°C for 10min;

[0041] S3, using electron beam exposure technology to expose the photoresist on the surface of the photoresist-SiO2 / Si multilayer film sample obtained in step S2, the exposure pattern is the design pattern of the wafer positioning calibration mark, the exposed sample is placed in the developer and fixer in turn, the photoresist in the exposed area is removed, and a photoresist pattern with the same shape as the design pattern is obtained. The electron acceleration voltage is 100 kV, the beam spot current is 50 nA, the beam spot size is 45 nm, and the exposure dose is 1100 μC / cm 2 The developer is a mixed solution of methyl isobutyl ketone MIBK and isopropyl alcohol IPA, with a mixing ratio of 1:3, a developing temperature of 23°C, and a developing time of 1 min. After development, rinse in the IPA solution for 0.5 min and blow dry with a nitrogen gun.

[0042] S4, using the photoresist pattern of the sample in step S3 as a mask, the top Si layer is completely etched by inductively coupled-reactive ion etching technology to obtain a SiO2 / Si multilayer film sample with the expected pattern structure. The etching gas and flow rate are trifluoromethane (CHF3): 50sccm and sulfur hexafluoride (SF6): 15sccm, the pressure is 15mTorr, the RF source power is 25W, the inductively coupled plasma power is 1200W, the bias voltage is 380V, the operating temperature is 5°C, and the etching rate is 10nm / s.

[0043] S5. Using a plasma stripper, remove the remaining photoresist on the surface of the SiO2 / Si multilayer film sample obtained in step S4 using oxygen ions, wherein the oxygen flow rate is 50 sccm, the pressure is 15 mTorr, the RF source power is 25 W, the inductively coupled plasma power is 1000 W, the bias voltage is 380 V, the operating temperature is 5° C., and the etching time is 2 min.

[0044] S6. Use a degumming solution (acetone) to perform post-cleaning on the surface of the SiO2 / Si multilayer film sample obtained in step S5 to remove organic matter and particles remaining on the surface to obtain a high-contrast wafer positioning calibration standard.

[0045] A high contrast wafer positioning calibration mark includes a wafer substrate and a dielectric multilayer film arranged on the surface of the wafer substrate. A plurality of units are arranged in an array on the surface of the wafer substrate, and the array covers the entire surface of the wafer substrate. A characteristic pattern is arranged between adjacent units. The characteristic pattern includes a cross, a square and a windmill, such as Figure 2 As shown; and all feature graphics are arranged in a grid to establish a grid coordinate system, such as Figure 3 As shown. The dielectric multilayer film structure replaces the traditional metal. The dielectric multilayer film structure provides high reflectivity in the full visible spectrum to ensure that the feature patterns processed on the wafer substrate have high contrast when observed under an optical microscope, which is convenient for automatic identification. The dielectric multilayer film includes a plurality of alternating high-refractive index material layers and low-refractive index material layers. The high-refractive index material layer is Si (polycrystalline or amorphous silicon), the low-refractive index material layer is SiO2, and the top layer is fixed to Si thin film material. In this embodiment, the dielectric multilayer film is two layers, and the thickness of each layer is determined by optimizing the design through thin film design software.

[0046] Therefore, the present invention adopts the above-mentioned high-contrast wafer positioning calibration mark and preparation method, uses dielectric materials to provide high contrast, and effectively avoids the risk of metal contamination to instruments and equipment caused by wafer marks with metal patterns during use. The nanometer-level processing precision of electron beam exposure patterning ensures that the final wafer positioning calibration mark has extremely high pattern positioning accuracy.

[0047] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for preparing a high-contrast wafer positioning calibration mark, characterized in that: The following steps are involved: S1. Using electron beam thermal evaporation technology to prepare a non-metallic dielectric multilayer film of a predetermined thickness on the surface of a cleaned wafer substrate; S2, spin-coating a photoresist having a thickness not less than 1 / 3 of the thickness of the top Si layer on the surface of the dielectric multilayer film obtained in step S1, and baking to solidify it, thereby obtaining a photoresist-dielectric multilayer film sample; S3, exposing the photoresist-dielectric multilayer film sample obtained in step S2 by electron beam exposure technology, wherein the exposure pattern is the design pattern of the wafer positioning calibration mark, placing the exposed sample in a developer and a fixer in sequence, removing the photoresist in the exposed area, and obtaining a photoresist pattern having the same shape as the design pattern; S4, using the photoresist pattern obtained in step S3 as a mask, using inductively coupled reactive ion etching technology to completely etch the top Si layer to obtain a multilayer film sample with a desired pattern structure; S5, using a plasma stripper to remove the remaining photoresist on the surface of the multilayer film sample obtained in step S4 using oxygen ions; S6. Post-cleaning the surface of the multilayer film sample obtained in step S5 using a degumming solution to remove organic matter and particles remaining on the surface, thereby obtaining a wafer positioning calibration standard.

2. The method for preparing a high-contrast wafer positioning calibration mark according to claim 1, characterized in that: In step S1, the thickness of the dielectric multilayer film is controlled by an optical monitoring method.

3. The method for preparing a high-contrast wafer positioning calibration mark according to claim 1, characterized in that: In step S1, the process parameters of the electron beam evaporation technology are: voltage 200-250V, current 500mA, Si deposition rate The SiO2 deposition rate is The wafer substrate heating temperature is 150°C and the background vacuum is less than 5×10 -4 pa.

4. The method for preparing a high-contrast wafer positioning calibration mark according to claim 1, characterized in that: In step S2, the photoresist is PMMA or ZEP; The process parameters of the photoresist spin coating are as follows: the rotation speed of the photoresist spin coating machine is 3000-4000 r / min, the baking is performed using a hot plate at a temperature of 178-182° C., and the time is 8-12 min.

5. The method for preparing a high-contrast wafer positioning calibration mark according to claim 1, characterized in that: In step S3, the process parameters of the electron beam exposure technology are: electron acceleration voltage is 100 kV, beam spot current is 49.5-50.5 nA, beam spot size is 35-45 nm, and exposure dose is 950-1250 μC / cm2; The developer is a mixed solution of methyl isobutyl ketone MIBK and isopropyl alcohol IPA in a mixing ratio of 1:3, the developing temperature is 22.8-23.2° C., and the developing time is 1-5 min; The fixing solution is an IPA solution, and the image is rinsed in the fixing solution for 0.5 to 1 min and blown dry with a nitrogen gun.

6. The method for preparing a high-contrast wafer positioning calibration mark according to claim 1, characterized in that: In step S4, the process parameters of the inductively coupled reactive ion etching technology are: trifluoromethane with a flow rate of 50 sccm and sulfur hexafluoride with a flow rate of 15 sccm as etching gas, a pressure of 15 mTorr, an RF source power of 25 W, an inductively coupled plasma power of 1200 W, a bias voltage of 380 V, an operating temperature of 5° C., and an etching rate of 10 nm / s.

7. The method for preparing a high-contrast wafer positioning calibration mark according to claim 1, characterized in that: In step S5, the relevant parameters of the plasma stripping machine are: using an oxygen flow rate of 50 sccm, a pressure of 15 mTorr, an RF source power of 25 W, an inductively coupled plasma power of 1000 W, a bias voltage of 380 V, an operating temperature of 5° C., and an etching time of 2 min.

8. A high contrast wafer positioning calibration mark prepared by the method for preparing a high contrast wafer positioning calibration mark according to any one of claims 1 to 7, characterized in that: It includes a wafer substrate and a dielectric multilayer film arranged on the surface of the wafer substrate. The surface array of the wafer substrate is arranged with a plurality of units, and characteristic patterns are arranged between adjacent units. The characteristic patterns are arranged in a grid shape for establishing a grid coordinate system.

9. The high contrast wafer positioning calibration mark according to claim 8, characterized in that: The characteristic pattern is one or more of a cross, a square and a windmill.

10. The high contrast wafer positioning calibration mark according to claim 8, characterized in that: The dielectric multilayer film includes a plurality of alternating high-refractive index material layers and low-refractive index material layers, the top layer of the dielectric multilayer film is a high-refractive index material layer, the high-refractive index material layer is Si, the low-refractive index material layer is SiO2, the number of layers of the dielectric multilayer film is 2 to 10, and the thickness of each film layer is determined by optimizing the design using thin film design software.