Semiconductor device
The semiconductor device's innovative layer structure addresses electrical and reliability issues in large, high-resolution displays by optimizing layer overlaps and resistance regions, resulting in improved transistor performance and reliability.
Patent Information
- Application Number
- CN202411208055.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2018-10-10
- Filing Date
- 2019-09-27
- Publication Date
- 2024-12-06
AI Technical Summary
Existing semiconductor devices face challenges in achieving good electrical characteristics and high reliability, particularly in large and high-resolution display devices, due to increased wiring resistance and the need for improved transistor performance.
A semiconductor device design featuring a specific layer structure with a semiconductor layer, first and second insulating layers, a metal oxide layer, and a conductive layer, where the insulating and metal oxide layers overlap the semiconductor layer in a controlled manner, with distinct resistance regions and tapered ends, and a functional layer to enhance adhesion and reduce defects.
The design achieves improved electrical characteristics and reliability by reducing wiring resistance, suppressing defects, and enhancing the source-drain withstand voltage, enabling high-performance transistors and display devices.
Smart Images

Figure CN119092554A_ABST
Abstract
Description
This application is a divisional application of the invention patent application with the invention name “Semiconductor Device”, the international application date of September 27, 2019, and the application number 201980065656.2 (the international application number is PCT / IB2019 / 058211). Technical Field
[0001] One embodiment of the present invention relates to a semiconductor device. One embodiment of the present invention relates to a display device. One embodiment of the present invention relates to a method for manufacturing a semiconductor device or a display device.
[0002] Note that one embodiment of the present invention is not limited to the above-mentioned technical field. As an example of the technical field of one embodiment of the present invention disclosed in this specification, etc., a semiconductor device, a display device, a light-emitting device, a power storage device, a storage device, an electronic device, a lighting device, an input device, an input-output device, a driving method thereof, or a manufacturing method thereof can be cited. A semiconductor device refers to any device that can work by utilizing semiconductor characteristics. Background Art
[0003] As a semiconductor material that can be used for transistors, oxide semiconductors using metal oxides have attracted attention. For example, Patent Document 1 discloses a semiconductor device in which a plurality of oxide semiconductor layers are stacked, in which an oxide semiconductor layer used as a channel contains indium and gallium, and the ratio of indium is higher than that of gallium, thereby improving field effect mobility (sometimes referred to as mobility or μFE).
[0004] Since the metal oxide that can be used for the semiconductor layer can be formed by sputtering or the like, it can be used for the semiconductor layer of the transistor constituting the large display device. In addition, since part of the production equipment of the transistor using polycrystalline silicon or amorphous silicon can be improved and used, the equipment investment can also be suppressed. In addition, compared with the transistor using amorphous silicon, the transistor using metal oxide has a high field effect mobility, so a high-performance display device provided with a driving circuit can be realized.
[0005] In addition, as the screen size of display devices tends to be larger, the development of display devices is even aimed at screens with a diagonal of 60 inches or more, and then a diagonal of 120 inches or more. In addition, the screen also tends to be higher resolution, such as Full High Definition (1920×1080 pixels, also called "2K", etc.), Ultra High-Definition (3840×2160 pixels, also called "4K", etc.), Super High-Definition (7680×4320 pixels, also called "8K", etc.).
[0006] The increase in screen size and resolution tends to increase the wiring resistance in the display unit. Patent Document 2 discloses a technique for forming a low-resistance wiring layer using copper (Cu) in order to suppress the increase in wiring resistance in a liquid crystal display device using amorphous silicon transistors. [Prior technical literature] [Patent Document]
[0007] [Patent Document 1] Japanese Patent Application Publication No. 2014-7399 [Patent Document 2] Japanese Patent Application Publication No. 2004-163901 Summary of the invention Technical problem to be solved by the invention
[0008] One object of one embodiment of the present invention is to provide a semiconductor device having good electrical characteristics. Another object of one embodiment of the present invention is to provide a semiconductor device having high reliability. Another object of one embodiment of the present invention is to provide a novel semiconductor device.
[0009] Note that the description of these purposes does not prevent the existence of other purposes. Furthermore, one embodiment of the present invention does not need to achieve all of the above purposes. In addition, purposes other than the above can be extracted from the description of the specification, drawings, claims, etc. Solutions to technical problems
[0010] One embodiment of the present invention is a semiconductor device, comprising a semiconductor layer, a first insulating layer, a second insulating layer, a metal oxide layer and a conductive layer, wherein the first insulating layer, the metal oxide layer and the conductive layer are sequentially stacked on the semiconductor layer, an end of the first insulating layer is located inside an end of the semiconductor layer, an end of the metal oxide layer is located inside an end of the first insulating layer, an end of the conductive layer is located inside an end of the metal oxide layer, the second insulating layer is arranged in a manner covering the semiconductor layer, the first insulating layer, the metal oxide layer and the conductive layer, the semiconductor layer has a first region, a pair of second regions and a pair of third regions, the first region overlaps with the first insulating layer and the metal oxide layer, the second region sandwiches the first region and overlaps with the first insulating layer and does not overlap with the metal oxide layer, the third region sandwiches the first region and the pair of second regions and does not overlap with the first insulating layer, the third region contacts the second insulating layer, the third region has a portion whose resistance is lower than that of the first region, and the second region has a portion whose resistance is higher than that of the third region.
[0011] In the above semiconductor device, the second region preferably has a portion having a lower resistance than that of the first region.
[0012] In the above semiconductor device, the second region preferably has a sheet resistance of 1×10 3Ω / □ or more and 1×10 9 The part below Ω / □.
[0013] In the above semiconductor device, the width of the second region in the cross section in the channel length direction is preferably not less than 100 nm and not more than 2 μm.
[0014] In the above semiconductor device, the second insulating layer is preferably a silicon nitride film.
[0015] In the semiconductor device described above, preferably, both the end of the first insulating layer and the end of the metal oxide layer have a tapered shape, and the taper angle of the end of the metal oxide layer is smaller than the taper angle of the end of the first insulating layer.
[0016] In the above semiconductor device, preferably, a functional layer is included between the metal oxide layer and the conductive layer, wherein the functional layer has conductivity, and an end of the functional layer is roughly aligned with an end of the metal oxide layer or located between the end of the metal oxide layer and the end of the conductive layer.
[0017] In the above semiconductor device, the semiconductor layer, the metal oxide layer, and the functional layer preferably all contain the same metal element.
[0018] In the above semiconductor device, the metal element is preferably at least one of indium and zinc. Effects of the Invention
[0019] According to one embodiment of the present invention, a semiconductor device having good electrical characteristics can be provided. In addition, a semiconductor device having high reliability can be provided. In addition, a novel semiconductor device can be provided.
[0020] Note that the description of the above effects does not prevent the existence of other effects. In addition, one mode of the present invention does not necessarily have all the above effects. In addition, effects other than the above can be extracted from the description of the specification, drawings, claims, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1A is a plan view showing a structural example of a semiconductor device. Figure 1B , Figure 1C is a cross-sectional view showing a structural example of a semiconductor device. Figure 2 is a cross-sectional view showing a structural example of a semiconductor device. Figure 3A , Figure 3B is a cross-sectional view showing a structural example of a semiconductor device. Figure 4A , Figure 4B is a cross-sectional view showing a structural example of a semiconductor device. Figure 5A , Figure 5B , Figure 5C is a cross-sectional view showing a structural example of a semiconductor device. Fig. 6A , Figure 6B , Figure 6C is a cross-sectional view showing a structural example of a semiconductor device. Fig. 7A , Figure 7B , Figure 7C It is a diagram for explaining a method for manufacturing a semiconductor device. Fig. 8A , Figure 8B It is a diagram for explaining a method for manufacturing a semiconductor device. Fig. 9A , Fig. 9B It is a diagram for explaining a method for manufacturing a semiconductor device. Fig. 10A , Fig. 10B It is a diagram for explaining a method for manufacturing a semiconductor device. Fig.11A , Fig. 11B It is a diagram for explaining a method for manufacturing a semiconductor device. Fig. 12A , Fig. 12B , Fig. 12C is a top view of the display device. Fig.13 is a cross-sectional view of a display device. Fig.14 is a cross-sectional view of a display device. Fig.15 is a cross-sectional view of a display device. Fig.16 is a cross-sectional view of a display device. Fig.17A is a block diagram of a display device. Fig. 17B , Fig. 17C is a circuit diagram of a display device. Fig.18A , Fig.18C , Fig.18D is a circuit diagram of a display device. Fig.18B It is a timing diagram of the display device. Fig.19A , Fig.19B This is an example of the structure of the display module. Fig. 20A , Fig. 20B It is an example of the structure of an electronic device. Fig.21A , Fig. 21B , Fig. 21C , Fig.21D , Fig.21E It is an example of the structure of an electronic device. Fig.22A , Fig. 22B , Fig. 22C , Fig.22D , Fig.22E , Fig.22F , Figure 22G It is an example of the structure of an electronic device. Fig.23A , Fig. 23B , Fig.23C , Fig.23D It is an example of the structure of an electronic device. Fig.24A is a cross-sectional STEM image of a transistor. Fig. 24B It is a graph showing the ID-VD characteristics of a transistor. Fig.25A is a cross-sectional STEM image of a transistor. Fig.25B It is a graph showing the ID-VD characteristics of a transistor. Fig.26 It is a graph showing the ID-VD characteristics of a transistor. Fig. 27 It is a graph showing the ID-VD characteristics of a transistor. Fig.28 It is a graph showing the ID-VD characteristics of a transistor. Fig.29 : is a graph showing the relationship between the wet etching time and the width L2. Fig. 30A , Fig. 30B It is a graph showing the amount of gas released from the insulating film. Fig. 30C is a graph showing the spin density of an insulating film. Modes for Carrying Out the Invention
[0022] The following describes the embodiments with reference to the accompanying drawings. Note that the embodiments can be implemented in a number of different ways, and a person skilled in the art can easily understand that the methods and details can be transformed into various forms without departing from the purpose and scope of the present invention. Therefore, the present invention should not be interpreted as being limited to the contents described in the following embodiments.
[0023] In the drawings described in this specification, the size of each component, the thickness of a layer, or a region may be exaggerated for the sake of clarity of description.
[0024] The ordinal numbers such as “first”, “second” and “third” used in this specification and the like are added to avoid confusion among constituent elements and are not intended to limit the number.
[0025] In this specification, for the sake of convenience, words and phrases such as "upper" and "lower" are used to indicate the positional relationship of the components with reference to the drawings. In addition, the positional relationship of the components is appropriately changed according to the direction in which each structure is described. Therefore, the words and phrases described in this specification are not limited and can be appropriately replaced according to the situation.
[0026] In this specification, etc., when transistors with different polarities are used or the direction of current changes during circuit operation, the functions of the source and drain included in the transistor may be interchanged. Therefore, the source and drain may be interchanged.
[0027] Note that in this specification, etc., the channel length direction of a transistor refers to one of the directions parallel to the straight line connecting the source region and the drain region at the shortest distance. That is, the channel length direction is equivalent to one of the directions of the current flowing through the semiconductor layer when the transistor is in the on state. In addition, the channel width direction refers to a direction orthogonal to the channel length direction. In addition, depending on the structure and shape of the transistor, the channel length direction and the channel width direction are sometimes not limited to one value.
[0028] In this specification, "electrical connection" includes connection through "an element having some kind of electrical function". Here, "an element having some kind of electrical function" is not particularly limited as long as it can transmit and receive electrical signals between the connected objects. For example, "an element having some kind of electrical function" includes not only electrodes and wiring, but also switching elements such as transistors, resistors, inductors, capacitors, and other elements having various functions.
[0029] In this specification, "film" and "layer" may be interchanged. For example, "conductive layer" and "insulating layer" may be replaced with "conductive film" and "insulating film".
[0030] In addition, in this specification, etc., unless otherwise specified, the off-state current refers to the drain current when the transistor is in the off state (also called the non-conducting state or the blocking state). Unless otherwise specified, in an n-channel transistor, the off state refers to the voltage V between the gate and the source. gs Below the threshold voltage V th (In a p-channel transistor, V gs Higher than V th ) status.
[0031] In this specification, etc., a display panel which is one form of a display device refers to a panel which can display (output) an image etc. on a display surface. Therefore, a display panel is one form of an output device.
[0032] In addition, in this specification, etc., a structure in which a connector such as an FPC (Flexible Printed Circuit) or TCP (Tape Carrier Package) is installed on a display panel substrate, or a structure in which an IC is directly mounted on a substrate using a COG (Chip On Glass) method, etc. is sometimes referred to as a display panel module or display module, or simply as a display panel, etc.
[0033] Note that in this specification, a touch panel, which is one form of a display device, has the following functions: a function of displaying an image on a display surface; and a function of acting as a touch sensor that detects when a detected object such as a finger or a stylus pen touches, is pressed, or approaches the display surface. Therefore, a touch panel is one form of an input / output device.
[0034] A touch panel may also be referred to as a display panel (or display device) having a touch sensor, or a display panel (or display device) having a touch sensor function. A touch panel may also include a display panel and a touch sensor panel. Alternatively, a structure may have a touch sensor function inside or on the surface of a display panel.
[0035] In this specification and the like, a structure in which a connector or an IC is mounted on a substrate of a touch panel may be referred to as a touch panel module, a display module, or simply as a touch panel.
[0036] (Implementation Method 1) In this embodiment, a semiconductor device, a display device, and a method for manufacturing the same, which are one embodiment of the present invention, are described. In particular, in this embodiment, a transistor using an oxide semiconductor in a semiconductor layer forming a channel is described as an example of a semiconductor device.
[0037] One embodiment of the present invention is a transistor including, on a formed surface, a semiconductor layer forming a channel, a gate insulating layer (also referred to as a first insulating layer) on the semiconductor layer, a metal oxide layer on the gate insulating layer, and a conductive layer (also referred to as a first conductive layer) on the metal oxide layer used as a gate electrode. The semiconductor layer preferably includes a metal oxide (hereinafter referred to as an oxide semiconductor) exhibiting semiconductor characteristics.
[0038] Preferably, the end of the first insulating layer is located inside the end of the semiconductor layer, the end of the metal oxide layer is located inside the end of the first insulating layer, and the end of the conductive layer is located inside the end of the metal oxide layer.
[0039] It is preferable that a second insulating layer is provided so as to cover the semiconductor layer, the first insulating layer, the metal oxide layer, and the conductive layer.
[0040] The semiconductor layer has a first region, a pair of second regions, and a pair of third regions. The first region overlaps with the first insulating layer and the metal oxide layer. The second region is a region that overlaps with the first insulating layer while sandwiching the first region and does not overlap with the metal oxide layer. In addition, the third region is a region that sandwiches the first region and the pair of second regions and does not overlap with the first insulating layer. The third region is in contact with the second insulating layer. The third region preferably has a portion whose resistance is lower than that of the first region, and the second region preferably has a portion whose resistance is higher than that of the third region.
[0041] Hereinafter, more specific examples will be described with reference to the drawings.
[0042] <Structural Example 1> Figure 1A is a top view of transistor 100, Figure 1B It is along Figure 1A The cross-sectional view along the dotted line A1-A2 shown in FIG. Figure 1C It is along Figure 1A The cross-sectional view is shown along the dotted line B1-B2. Figure 1A In the diagram, a portion of the components of transistor 100 (protective layer, etc.) is omitted. The dot-dash line A1-A2 direction corresponds to the channel length direction, and the dot-dash line B1-B2 direction corresponds to the channel width direction. Figure 1A Similarly, some of the components are omitted.
[0043] The transistor 100 is provided on a substrate 102 and includes an insulating layer 103, a semiconductor layer 108, an insulating layer 110, a metal oxide layer 114, a conductive layer 112, an insulating layer 116, and an insulating layer 118. The island-shaped semiconductor layer 108 is provided on the insulating layer 103. The insulating layer 110 is provided in a manner covering a portion of the top surface of the insulating layer 103 and a portion of the top surface of the semiconductor layer 108. The metal oxide layer 114 and the conductive layer 112 are provided on the insulating layer 110 in this order and have a portion overlapping with the semiconductor layer 108. Figure 2 Show Figure 1B An enlarged view of the area P surrounded by a dot-dashed line in FIG.
[0044] The ends of the conductive layer 112 and the metal oxide layer 114 are located inside the ends of the insulating layer 110. In other words, the insulating layer 110 has a portion protruding outside the ends of the conductive layer 112 and the metal oxide layer 114 at least on the semiconductor layer 108. In addition, the end of the conductive layer 112 is located inside the end of the metal oxide layer 114. In other words, the metal oxide layer 114 has a portion protruding outside the end of the conductive layer 112 at least on the semiconductor layer 108.
[0045] The semiconductor layer 108 includes a pair of regions 108L sandwiching a channel formation region and a pair of regions 108N outside thereof. The region 108L is a region of the semiconductor layer 108 that overlaps with the insulating layer 110 and does not overlap with the conductive layer 112. Figure 2 In FIG. 1 , the width of the channel formation region of the transistor 100 in the channel length direction is denoted as L1, and the width of the region 108L is denoted as L2.
[0046] The region 108L can be said to be a region having the same or lower resistance than the channel formation region, a region having the same or higher carrier concentration, a region having the same or higher oxygen vacancy density, or a region having the same or higher impurity concentration.
[0047] The region 108L can be said to be a region having the same or higher resistance, the same or lower carrier concentration, the same or lower oxygen vacancy density, or the same or lower impurity concentration than the region 108N.
[0048] The sheet resistance of region 108L is preferably 1×10 3 Ω / □ or more and 1×10 9 Ω / □ or less, more preferably 1×10 3 Ω / □ or more and 1×10 8 Ω / □ or less, more preferably 1×10 3 Ω / □ or more and 1×10 7 Ω / □ or less. By setting the above resistance range, a transistor with good electrical characteristics and high reliability can be realized. Note that the sheet resistance can be calculated from the value of the resistance. By providing the above region 108L between the region 108N and the channel formation region, the source-drain withstand voltage of the transistor 100 can be improved.
[0049] Note that the carrier concentration in the region 108L is not necessarily uniform, and may have a concentration gradient in which the carrier concentration decreases from the region 108N side toward the channel formation region. For example, either or both of the hydrogen concentration and the oxygen vacancy concentration in the region 108L may have a concentration gradient in which the concentration decreases from the region 108N side toward the channel formation region side.
[0050] Part of the end portion of the insulating layer 110 is located on the semiconductor layer 108. The insulating layer 110 has a portion overlapping with the conductive layer 112 and serving as a gate insulating layer and a portion not overlapping with the conductive layer 112 and the metal oxide layer 114 (that is, a portion overlapping with the region 108L).
[0051] The insulating layer 116 is provided so as to cover the top and side surfaces of the conductive layer 112, the side surfaces of the metal oxide layer 114, the top and side surfaces of the insulating layer 110, the top and side surfaces of the semiconductor layer 108, and the top surface of the insulating layer 103. The insulating layer 116 has a function of suppressing diffusion of impurities from above the insulating layer 116 to the semiconductor layer 108. In addition, the insulating layer 116 has a function of reducing the resistance of the semiconductor layer 108 in contact with the insulating layer 116 during film formation. The region 108N is in contact with the insulating layer 116. Since the region 108L is not in contact with the insulating layer 116 due to the presence of the insulating layer 110 therebetween, the hydrogen supplied from the insulating layer 116 is less than that of the region 108N. In addition, the impurity concentration is also lower than that of the region 108N, so that the region 108L can be made to have a higher resistance than that of the region 108N.
[0052] As described later, since the region 108L can be formed in a self-aligned manner, a photomask for forming the region 108L is not required, and the manufacturing cost can be reduced. In addition, when the region 108L is formed in a self-aligned manner, there is no relative misalignment between the region 108L and the conductive layer 112, so that the width of the region 108L in the semiconductor layer 108 can be roughly uniform.
[0053] A region 108L used as a bias region to which a gate electric field is not applied (or to which a gate electric field is less likely to be applied than in the channel formation region) can be uniformly and stably formed between the channel formation region and the low-resistance region 108N in the semiconductor layer 108. As a result, the source-drain withstand voltage of the transistor can be increased, and a highly reliable transistor and semiconductor device can be realized.
[0054] The width L2 of region 108L is preferably greater than 100nm and less than 2μm, more preferably greater than 150nm and less than 1μm, and further preferably greater than 200nm and less than 1μm. By providing region 108L, the electric field concentration near the drain can be alleviated, so the degradation of the transistor in a state where the drain voltage is high can be suppressed. In addition, in particular, by making the width L2 of region 108L greater than the thickness of the insulating layer 110, the electric field concentration near the drain can be effectively suppressed. On the other hand, when the width L2 is greater than 2μm, the source-drain resistance increases and the driving speed of the transistor sometimes decreases. By setting the width L2 to the above range, transistors and semiconductor devices with high reliability and high driving speed can be manufactured. In addition, the width L2 of region 108L can be determined according to the thickness of the semiconductor layer 108, the thickness of the insulating layer 110, and the size of the voltage applied between the source and the drain when driving the transistor 100.
[0055] By providing region 108L between the channel formation region and the low resistance region 108N, the current density at the boundary between the channel formation region and region 108N can be reduced, and the heat generated at the boundary between the channel and the source or drain can be suppressed, thereby manufacturing a transistor or semiconductor device with high reliability.
[0056] The conductive layer 112 is preferably made of a low-resistance material. By using a low-resistance material as the conductive layer 112, the parasitic resistance can be reduced so that the transistor has a high on-state current, thereby realizing a semiconductor device with a high on-state current. In addition, by reducing the wiring resistance in a large display device or a high-definition display device, signal delay can be suppressed and high-speed driving can be realized. For example, copper, silver, gold, or aluminum can be used as the conductive layer 112. In particular, copper is preferred because of its good mass productivity.
[0057] When the end of the formed layer forming the conductive layer 112 becomes a shape located inside the end of the conductive layer 112, that is, when undercut occurs, the coverage of the layer to be formed later decreases and defects such as disconnection or voids occur in the layer. When shape defects such as undercut occur, there is a concern that defects such as uneven electrical characteristics of the transistor may occur.
[0058] like Figure 1B , Figure 1C and Figure 2 As shown, it is preferred that the functional layer 113 is provided as a layer to be formed of the conductive layer 112, and the etching speed of the functional layer 113 by the etchant used when processing the conductive layer 112 is substantially equal to or lower than that of the conductive layer 112. By adopting the above structure, the occurrence of undercutting can be suppressed and a transistor that is not prone to shape defects can be realized. In addition, a transistor and a semiconductor device with good electrical characteristics can be realized.
[0059] like Figure 1B , Figure 1C As shown in the figures, it is preferred to provide a functional layer 113 between the conductive layer 112 and the metal oxide layer 114. In particular, it is preferred to use a material having conductivity for the functional layer 113. In addition, it is preferred to use a material having high adhesion to the conductive layer 112 for the functional layer 113. When the adhesion between the functional layer 113 and the conductive layer 112 is high, it is possible to prevent the etching agent from entering between the two layers when forming the functional layer 113 and the conductive layer 112 and generating a gap between the functional layer 113 and the conductive layer 112.
[0060] It is preferable to have a shape in which the cross section of each of the conductive layer 112 and the functional layer 113 is continuous. When the cross section of the conductive layer 112 and the functional layer 113 is continuous, the coverage of the layer (for example, the insulating layer 116) formed on the conductive layer 112 and the functional layer 113 is improved, thereby preventing defects such as disconnection or voids in the layer.
[0061] The end of the insulating layer 110 and the end of the metal oxide layer 114 preferably have a tapered shape. In addition, the taper angle of the end of the metal oxide layer 114 is preferably smaller than the taper angle of the end of the insulating layer 110. By adopting the above structure, the coverage of the layer (for example, the insulating layer 116) formed on the insulating layer 110 and the metal oxide layer 114 is improved, and the occurrence of defects such as disconnection or voids in the layer can be suppressed.
[0062] In this specification, etc., "the top surface shapes are substantially consistent" means that at least a portion of the edge of each layer in the stack overlaps. For example, it refers to the case where a part or all of the upper layer and the lower layer are processed by the same mask pattern. However, strictly speaking, sometimes the outlines do not overlap and the end of the upper layer is located inside the end of the lower layer or the end of the upper layer is located outside the end of the lower layer, and these cases are also included in the case of "the top surface shapes are substantially consistent".
[0063] In this specification and the like, the taper angle refers to an inclination angle formed by the side surface and the bottom surface of a layer when the target layer is observed from a direction perpendicular to a cross section (for example, a plane perpendicular to the surface of a substrate).
[0064] The insulating layer 116 is provided to cover the top surface and side surfaces of the conductive layer 112, the top surface and side surfaces of the functional layer 113, the side surfaces of the metal oxide layer 114, the top surface and side surfaces of the insulating layer 110, the top surface and side surfaces of the semiconductor layer 108, and the top surface of the insulating layer 103. The insulating layer 118 is provided to cover the insulating layer 116. The insulating layer 116 and the insulating layer 118 function as protective layers and can suppress diffusion of impurities from the outside.
[0065] Part of the conductive layer 112 , the functional layer 113 , and the metal oxide layer 114 functions as a gate electrode. Part of the insulating layer 110 functions as a gate insulating layer. The transistor 100 is a so-called top-gate transistor in which a gate electrode is provided over the semiconductor layer 108 .
[0066] like Figure 1A and Figure 1B As shown, the transistor 100 may also include a conductive layer 120a and a conductive layer 120b on the insulating layer 118. The conductive layer 120a and the conductive layer 120b are used as a source electrode or a drain electrode. The conductive layer 120a and the conductive layer 120b are electrically connected to a region 108N described later through an opening 141a and an opening 141b provided in the insulating layer 118 and the insulating layer 116, respectively.
[0067] The semiconductor layer 108 preferably includes a metal oxide.
[0068] For example, the semiconductor layer 108 preferably contains indium, an element M (M is one or more selected from gallium, aluminum, silicon, boron, yttrium, tin, copper, vanadium, beryllium, titanium, iron, nickel, germanium, zirconium, molybdenum, lanthanum, cerium, neodymium, hafnium, tantalum, tungsten and magnesium) and zinc. In particular, M is preferably one or more selected from aluminum, gallium, yttrium and tin.
[0069] In particular, as the semiconductor layer 108, an oxide containing indium, gallium, and zinc is preferably used.
[0070] The semiconductor layer 108 may have a stacked-layer structure in which layers having different compositions, layers having different crystallinity, or layers having different impurity concentrations are stacked.
[0071] As the conductive layer 112, one or more selected from copper, silver, gold, and aluminum can be used. Copper is particularly preferred because it has advantages of low resistance and high productivity.
[0072] The metal oxide layer 114 located between the insulating layer 110 and the functional layer 113 is used as a barrier film for preventing oxygen contained in the insulating layer 110 from diffusing toward the conductive layer 112. Furthermore, the metal oxide layer 114 is also used as a barrier film for preventing hydrogen or water contained in the conductive layer 112 from diffusing toward the insulating layer 110. The metal oxide layer 114 can be made of a material that is less likely to transmit oxygen and hydrogen than the insulating layer 110, for example.
[0073] The metal oxide layer 114 can prevent oxygen from diffusing from the insulating layer 110 to the conductive layer 112 even if a metal material that easily absorbs oxygen, such as aluminum or copper, is used for the conductive layer 112. Furthermore, even if the conductive layer 112 contains hydrogen, hydrogen can be prevented from diffusing from the conductive layer 112 through the insulating layer 110 to the semiconductor layer 108. As a result, the carrier concentration in the channel formation region of the semiconductor layer 108 can be made extremely low.
[0074] An insulating material or a conductive material can be used as the metal oxide layer 114. When the metal oxide layer 114 has insulating properties, the metal oxide layer 114 is used as a part of a gate insulating layer. On the other hand, when the metal oxide layer 114 has conductive properties, the metal oxide layer 114 is used as a part of a gate electrode.
[0075] An insulating material having a higher dielectric constant than silicon oxide is preferably used as the metal oxide layer 114. In particular, an aluminum oxide film, a hafnium oxide film, a hafnium aluminate film, or the like is preferably used because a driving voltage can be reduced.
[0076] As the metal oxide layer 114, for example, a conductive oxide such as indium oxide, indium tin oxide (ITO), or indium tin oxide containing silicon (ITSO) can be used. In particular, a conductive oxide containing indium is preferably used because it has high conductivity.
[0077] As the metal oxide layer 114, an oxide material containing one or more elements that are the same as those of the semiconductor layer 108 is preferably used. In particular, an oxide semiconductor material that can be applied to the above-mentioned semiconductor layer 108 is preferably used. In this case, by using a metal oxide film formed using the same sputtering target as that of the semiconductor layer 108 as the metal oxide layer 114, equipment can be shared, which is preferred.
[0078] In addition, when a metal oxide material containing indium and gallium is used for both the semiconductor layer 108 and the metal oxide layer 114, it is preferable to use a material having a higher gallium composition (content ratio) than that used for the semiconductor layer 108 as the metal oxide layer 114, because the barrier property against oxygen can be improved. In this case, by using a material having a higher indium composition than that used for the metal oxide layer 114 as the semiconductor layer 108, the field effect mobility of the transistor 100 can be improved.
[0079] The metal oxide layer 114 is preferably formed using a sputtering device. For example, when an oxide film is formed using a sputtering device, oxygen can be appropriately added to the insulating layer 110 or the semiconductor layer 108 by forming the oxide film in an atmosphere including an oxygen gas.
[0080] It is preferable that a conductive material having oxidation resistance is used for the functional layer 113 located between the metal oxide layer 114 and the conductive layer 112. By using a material having oxidation resistance, an increase in the resistance of the functional layer 113 can be suppressed.
[0081] Preferably, the etching speed of the metal oxide layer 114 and the functional layer 113 by the etchant used when processing the conductive layer 112 is substantially equal to or lower than that of the conductive layer 112 .
[0082] When the etching rate of the metal oxide layer 114 and the functional layer 113 is higher than that of the conductive layer 112, undercutting is likely to occur, that is, the ends of the metal oxide layer 114 and the functional layer 113 are located inside the ends of the conductive layer 112. When undercutting occurs, the coverage of the insulating layer 116 and the insulating layer 118 formed later is reduced, and defects such as disconnection or low-density areas (also called voids) are generated in the insulating layer 116 and the insulating layer 118.
[0083] In one embodiment of the present invention, by making the etching rate of the metal oxide layer 114 and the functional layer 113 equal to or lower than that of the conductive layer 112, undercutting can be suppressed and a transistor that is less likely to have shape defects can be realized. In addition, a transistor with good electrical characteristics can be realized.
[0084] The functional layer 113, the metal oxide layer 114, and the conductive layer 112 can be formed in the same step using an etchant used for processing the conductive layer 112. The metal oxide layer 114, the functional layer 113, and the conductive layer 112 can have substantially the same top surface shape.
[0085] The etching rate of the insulating layer 110 is preferably lower than that of the metal oxide layer 114, the functional layer 113, and the conductive layer 112. By making the etching rate of the insulating layer 110 lower than that of the metal oxide layer 114, the functional layer 113, and the conductive layer 112, the amount of the insulating layer 110 etched when the metal oxide layer 114, the functional layer 113, and the conductive layer 112 are formed can be reduced.
[0086] Preferably, the functional layer 113 has high adhesion to the metal oxide layer 114 and the conductive layer 112. For example, when the adhesion between the above layers is low in a structure in which the conductive layer 112 is formed on the metal oxide layer 114, the etchant enters between the above two layers when the metal oxide layer 114 and the conductive layer 112 are formed, so that sometimes a gap is generated between the metal oxide layer 114 and the conductive layer 112. In one embodiment of the present invention, by providing the functional layer 113 between the metal oxide layer 114 and the conductive layer 112, the adhesion between the metal oxide layer 114, the functional layer 113 and the conductive layer 112 is improved, and the generation of gaps between the above layers can be suppressed, so that a transistor that is not prone to poor shape can be realized. In addition, a transistor with good electrical characteristics can be realized.
[0087] Preferably, the amount of impurities including hydrogen released from the functional layer 113 is small. Examples of impurities including hydrogen include hydrogen and water. When impurities including hydrogen are released from the functional layer 113, when the hydrogen reaches the channel formation region of the semiconductor layer 108, the hydrogen sometimes bonds to oxygen in the channel formation region and is released as water, thereby forming oxygen vacancies (hereinafter also referred to as V in the channel formation region). O In addition, there are oxygen vacancies (V O ) and hydrogen, sometimes hydrogen enters the oxygen vacancy (V O ) state (hereinafter, also referred to as V O H) V O H becomes a carrier generation source and may adversely affect the electrical characteristics and reliability of the transistor. By using the functional layer 113 which contains hydrogen and releases a small amount of impurities, good electrical characteristics and reliability can be obtained.
[0088] Preferably, the amount of impurities including oxygen released from the functional layer 113 is small. Examples of impurities including oxygen include oxygen and water. When impurities including oxygen are released from the functional layer 113, the resistance of the conductive layer 112 may increase when the oxygen reaches the conductive layer 112. By using the functional layer 113 that releases a small amount of impurities including oxygen, the increase in the resistance of the conductive layer 112 can be suppressed.
[0089] As the functional layer 113, a metal oxide can be used. For example, an oxide containing indium such as indium oxide, indium tin oxide (ITO), or indium tin oxide containing silicon (ITSO) can be used. ITSO is not easily crystallized by containing silicon, and has high flatness, so the adhesion with the film formed on ITSO is improved, so it is particularly preferred. In addition, a metal oxide such as indium zinc oxide, zinc oxide, or zinc oxide containing gallium can be used.
[0090] As the functional layer 113, oxides of indium, element M (element M is one or more selected from gallium, aluminum, silicon, boron, yttrium, tin, copper, vanadium, beryllium, titanium, iron, nickel, germanium, zirconium, molybdenum, lanthanum, cerium, neodymium, hafnium, tantalum, tungsten and magnesium) and zinc can be used. In particular, element M is preferably one or more selected from aluminum, gallium, yttrium and tin. For example, when the atomic number ratio of In to Ga in In-Ga-Zn oxide is greater than 1, the conductivity is improved, so it is preferred. In particular, the ratio of the number of atoms of In, element M and Zn in the functional layer 113 is preferably set to In:M:Zn=4:2:3 or thereabouts. Alternatively, the ratio of the number of atoms of In, element M and Zn is preferably set to In:M:Zn=5:1:6 or thereabouts. In addition, as the composition of the semiconductor layer 108, the ratio of the number of atoms of In, element M and Zn in the semiconductor layer 108 can also be made substantially equal. That is, a material in which the ratio of the number of atoms of In, the element M, and Zn is In:M:Zn=1:1:1 or a material in the vicinity thereof may be included.
[0091] The functional layer 113 can be made of a metal such as aluminum, titanium, chromium, nickel, copper, yttrium, zirconium, molybdenum, silver, tantalum, or tungsten, or an alloy containing these elements as a main component.
[0092] The functional layer 113 is preferably made of a material different from that of the metal oxide layer 114 and the conductive layer 112. Note that in this specification, different materials refer to materials having different constituent elements or materials having the same constituent elements but different compositions. Even if the metal oxide layer 114 and the conductive layer 112 have low adhesion, by providing a functional layer 113 including a material different from that of the metal oxide layer 114 between the metal oxide layer 114 and the conductive layer 112, adhesion to the metal oxide layer 114 and the conductive layer 112 can be improved.
[0093] The functional layer 113 may have a structure in which the above-mentioned materials are stacked in two or more layers.
[0094] The semiconductor layer 108 has a channel formation region that overlaps with the conductive layer 112 via the insulating layer 110. The semiconductor layer 108 also has a pair of regions 108N that sandwich the channel formation region. The regions 108N are regions of the semiconductor layer 108 that do not overlap with the conductive layer 112 and the insulating layer 110 and that are in contact with the insulating layer 116.
[0095] The region 108N may be considered to be a region having lower resistance than the channel formation region, a region having higher carrier concentration, a region having higher oxygen vacancy density, a region having higher impurity concentration, or a region exhibiting n-type.
[0096] Region 108N is a region containing an impurity element (hereinafter referred to as the first element). As the first element, for example, hydrogen, boron, carbon, nitrogen, fluorine, phosphorus, sulfur, arsenic, aluminum, magnesium or a rare gas can be cited. Typical examples of rare gases include helium, neon, argon, krypton and xenon. In particular, it is preferred to contain boron, phosphorus, magnesium or aluminum. In addition, two or more of these elements may be contained.
[0097] Here, the concentration of the first element in the region 108N preferably has a concentration gradient in which the concentration increases as it approaches the insulating layer 116. Therefore, compared with the case where the entire region 108N has a uniform concentration, the total amount of the first element in the region 108N can be further reduced, thereby keeping the amount of the first element that may diffuse into the channel formation region due to heating or the like in the manufacturing process at a low level. As a result, the closer to the upper part of the region 108N, the lower the resistance, and the contact resistance with the conductive layer 120a (or the conductive layer 120b) can be more effectively reduced.
[0098] As described later, the process of adding the first element to the region 108N can be performed using the insulating layer 110 as a mask. Thus, the region 108N can be formed in a self-aligned manner.
[0099] Region 108N preferably has a first element concentration of 1×10 19 atoms / cm 3 Above and 1×10 23 atoms / cm 3 Below, preferably 5×10 19 atoms / cm 3 Above and 5×10 22 atoms / cm 3 Below, more preferably 1×10 20 atoms / cm 3 Above and 1×10 22 atoms / cm3 The following area.
[0100] For example, the concentration of the first element contained in the region 108N can be analyzed by using secondary ion mass spectrometry (SIMS) or X-ray photoelectron spectroscopy (XPS). When XPS analysis technology is used, the concentration distribution in the depth direction can be obtained by combining ion sputtering from the surface side or the back side and XPS analysis.
[0101] The first element in region 108N preferably exists in an oxidized state. For example, as the first element, it is preferable to use an element that is easily oxidized, such as boron, phosphorus, magnesium, aluminum, and silicon. This easily oxidized element can stably exist in an oxidized state while bonding with oxygen in the semiconductor layer 108, so even if a high temperature (for example, above 400°C, above 600°C, or above 800°C) is applied in a subsequent process, detachment can be suppressed. In addition, the first element takes away oxygen in the semiconductor layer 108, thereby generating many oxygen vacancies in region 108N. The oxygen vacancies bond with hydrogen in the film to become a carrier supply source, so that region 108N becomes an extremely low resistance state.
[0102] In addition, when a high temperature treatment is performed in a later step, a large amount of oxygen may be supplied to the region 108N from the outside or from a film near the region 108N, causing an increase in resistance. Therefore, when a high temperature treatment is performed, it is preferable to perform the treatment in a state where the semiconductor layer 108 is covered with the insulating layer 116 having a high oxygen barrier property.
[0103] The insulating layer 116 is provided in contact with the region 108N of the semiconductor layer 108 .
[0104] The insulating layer 116 is used as a hydrogen supply source for the region 108N. For example, the insulating layer 116 is preferably a film that releases hydrogen by heating. By providing the insulating layer 116 in contact with the region 108N and performing a heat treatment after forming the insulating layer 116, hydrogen can be supplied to the region 108N to reduce resistance.
[0105] The insulating layer 116 is preferably formed using a gas containing hydrogen as a film-forming gas used in forming the film. Thus, hydrogen can be efficiently supplied to the region 108N even when the insulating layer 116 is formed.
[0106] As the insulating layer 116 , an insulating film of silicon nitride, silicon nitride oxide, silicon oxynitride, aluminum nitride, aluminum nitride oxide, or the like can be used, for example.
[0107] By adding the first element as described above, the region 108N includes a plurality of oxygen vacancies, and thus, the carrier concentration can be further increased by oxygen supplied from the insulating layer 116 in addition to hydrogen in the semiconductor layer 108 .
[0108] The insulating layer 118 is used as a protective layer for protecting the transistor 100. The insulating layer 118 can be made of, for example, an inorganic insulating material such as oxide or nitride. More specifically, an inorganic insulating material such as silicon nitride, silicon nitride oxide, silicon oxynitride, aluminum oxide, aluminum oxynitride, aluminum nitride, hafnium oxide, and hafnium aluminate can be used. In addition, the insulating layer 118 can also be used as a planarization layer. In this case, an organic resin material can be used as the insulating layer 118.
[0109] Note that although the protective layer has an example of a stacked-layer structure of the insulating layer 116 and the insulating layer 118, the insulating layer 118 may not be provided if not necessary. Alternatively, the insulating layer 118 may have a stacked-layer structure of two or more layers.
[0110] Here, the semiconductor layer 108 and oxygen vacancies that may be formed in the semiconductor layer 108 are described.
[0111] Oxygen vacancies formed in the channel formation region of the semiconductor layer 108 affect transistor characteristics and cause problems. For example, when oxygen vacancies are formed in the semiconductor layer 108, the oxygen vacancies sometimes bond with hydrogen to become a carrier supply source. When a carrier supply source is generated in the channel formation region, the electrical characteristics of the transistor 100 change, typically a shift in the threshold voltage. Therefore, in the channel formation region, the fewer oxygen vacancies, the better.
[0112] Therefore, in one embodiment of the present invention, the insulating film near the channel formation region of the semiconductor layer 108, specifically, the insulating layer 110 located above the channel formation region and the insulating layer 103 located below the channel formation region, includes an oxide film. By moving oxygen from the insulating layer 103 and the insulating layer 110 to the channel formation region by heating or the like in the manufacturing process, oxygen vacancies in the channel formation region can be reduced.
[0113] The semiconductor layer 108 preferably has a region where the atomic number ratio of In to the element M is greater than 1. The higher the In content, the higher the field effect mobility of the transistor can be.
[0114] Here, in the metal oxide containing In, Ga and Zn, the bonding force between In and oxygen is weaker than that between Ga and oxygen, so when the content of In is high, oxygen vacancies are easily formed in the metal oxide film. In addition, when the metal element represented by the element M is used instead of Ga, the same tendency also exists. When there are many oxygen vacancies in the metal oxide film, the electrical characteristics and reliability of the transistor are reduced.
[0115] However, in one embodiment of the present invention, a large amount of oxygen can be supplied to the channel formation region of the semiconductor layer 108 including metal oxide, thereby enabling the use of a metal oxide material having a high content of In. Therefore, a transistor having extremely high field effect mobility, stable electrical characteristics, and high reliability can be realized.
[0116] For example, a metal oxide in which the atomic number ratio of In to the element M is 1.5 or more, 2 or more, 3 or more, 3.5 or more, or 4 or more can be suitably used.
[0117] In particular, the ratio of the number of atoms of In, M, and Zn in the semiconductor layer 108 is preferably In:M:Zn=4:2:3 or in the vicinity thereof. Alternatively, the ratio of the number of atoms of In, M, and Zn in the semiconductor layer 108 is preferably In:M:Zn=5:1:6 or in the vicinity thereof. Furthermore, in the composition of the semiconductor layer 108, the ratio of the number of atoms of In, M, and Zn in the semiconductor layer 108 may be substantially equal. That is, the semiconductor layer 108 may include a material in which the ratio of the number of atoms of In, the element M, and Zn is In:M:Zn=1:1:1 or in the vicinity thereof.
[0118] For example, by using the transistor with high field effect mobility for a gate driver that generates a gate signal, a display device with a narrow frame width (also referred to as a narrow frame) can be provided. In addition, by using the transistor with high field effect mobility for a source driver (especially a demultiplexer connected to an output terminal of a shift register included in the source driver), a display device with a small number of wirings connected to the display device can be provided.
[0119] Note that even if the semiconductor layer 108 includes a region where the atomic number ratio of In to the element M is greater than 1, the field effect mobility may decrease when the crystallinity of the semiconductor layer 108 is high. The crystallinity of the semiconductor layer 108 can be analyzed, for example, by X-ray diffraction (XRD) or a transmission electron microscope (TEM).
[0120] Here, the carrier concentration in the film can be reduced by reducing the impurity concentration and defect state density (reducing oxygen vacancies) in the channel formation region of the semiconductor layer 108. A transistor using the metal oxide film in the channel formation region of the semiconductor layer rarely has an electrical characteristic of a negative threshold voltage (also called a normally-on characteristic). In addition, a transistor using the metal oxide film has a characteristic of extremely small off-state current.
[0121] By using a metal oxide film with high crystallinity for the semiconductor layer 108, damage can be suppressed when processing the semiconductor layer 108 or when forming the insulating layer 110, thereby realizing a highly reliable transistor. On the other hand, by using a metal oxide film with low crystallinity for the semiconductor layer 108, conductivity can be improved, thereby realizing a transistor with high field effect mobility.
[0122] For example, the semiconductor layer 108 is preferably formed using a metal oxide film having a CAAC (c-axis aligned crystal) structure described later, a metal oxide film having a nc (nano crystal) structure, or a metal oxide film having a mixture of a CAAC structure and a nc structure.
[0123] Alternatively, the semiconductor layer 108 may have a stacked structure of two or more layers.
[0124] For example, a semiconductor layer 108 formed by stacking two or more metal oxide films having different compositions may be used. For example, when an In-M-Zn oxide is used, it is preferable to stack two or more films formed using a sputtering target material having a ratio of the number of atoms of In, element M, and Zn of In:M:Zn=5:1:6, In:M:Zn=4:2:3, In:M:Zn=1:1:1, In:M:Zn=2:2:1, In:M:Zn=1:3:4, In:M:Zn=1:3:2 or the vicinity thereof.
[0125] Alternatively, a semiconductor layer 108 formed by stacking two or more metal oxide films having different crystallinity may be used. In this case, it is preferred that the metal oxide films are formed continuously using the same oxide target under different film formation conditions without being exposed to the air.
[0126] In this case, a stacked structure of a metal oxide film having an nc structure and a metal oxide film having a CAAC structure may be used as the semiconductor layer 108. Alternatively, a stacked structure of a metal oxide film having an nc structure and a metal oxide film having an nc structure may be used. In addition, the function or material structure of the metal oxides suitable for these metal oxide films may refer to the description of CAC (Cloud-Aligned Composite) described later.
[0127] For example, the oxygen flow rate ratio during the film formation of the first metal oxide film formed first is set to be smaller than the oxygen flow rate ratio during the film formation of the second metal oxide film formed later. Alternatively, a condition in which oxygen is not introduced during the film formation of the first metal oxide film is adopted. Thus, oxygen can be effectively supplied during the film formation of the second metal oxide film. In addition, the first metal oxide film can have a lower crystallinity than the second metal oxide film and a higher conductivity than the second metal oxide film. On the other hand, by making the crystallinity of the second metal oxide film disposed on the upper portion higher than the crystallinity of the first metal oxide film, damage caused during the processing of the semiconductor layer 108 or the film formation of the insulating layer 110 can be suppressed.
[0128] More specifically, the oxygen flow rate ratio during the formation of the first metal oxide film is 0% or more and less than 50%, preferably 0% or more and 30% or less, more preferably 0% or more and 20% or less, and typically 10%. The oxygen flow rate ratio during the formation of the second metal oxide film is 50% or more and 100% or less, preferably 60% or more and 100% or less, more preferably 80% or more and 100% or less, further preferably 90% or more and 100% or less, and typically 100%. In addition, although the conditions such as pressure, temperature, and power during the formation of the first metal oxide film and the second metal oxide film can be made different, it is preferred that the conditions other than the oxygen flow rate ratio be the same because the time required for the film formation process can be shortened.
[0129] By adopting the above structure, the transistor 100 having excellent electrical characteristics and high reliability can be realized.
[0130] An oxide film is preferably used for the insulating layer 103 and the insulating layer 110 that are in contact with the channel formation region of the semiconductor layer 108. For example, an oxide film such as a silicon oxide film, a silicon oxynitride film, or an aluminum oxide film can be used. Thus, oxygen released from the insulating layer 103 or the insulating layer 110 by heat treatment or the like in the manufacturing process of the transistor 100 is supplied to the channel formation region of the semiconductor layer 108, whereby oxygen vacancies in the semiconductor layer 108 can be reduced.
[0131] A portion of an end portion of the insulating layer 110 is located on the semiconductor layer 108. The insulating layer 110 has a region which overlaps with the conductive layer 112 and functions as a gate insulating layer.
[0132] The insulating layer 110 preferably has a stacked structure of two or more layers. Figure 2An example of a three-layer structure in which the insulating layer 110 has an insulating layer 110a, an insulating layer 110c on the insulating layer 110a, and an insulating layer 110b between the insulating layer 110a and the insulating layer 110c is shown. Note that the insulating layers 110a, 110b, and 110c may be made of insulating films of the same material, so the interfaces between the insulating layers 110a, 110b, and 110c may not be clearly observed. Therefore, in this embodiment, the interfaces between the insulating layers 110a, 110b, and 110c are shown by dotted lines.
[0133] It is preferable that the defect density in the vicinity of the interface with the channel formation region of the insulating layer 110a in contact with the channel formation region of the semiconductor layer 108 and in the film is low. In addition, it is preferable that the concentration of impurities including hydrogen in the insulating layer 110a is low. In addition, it is preferable that the damage to the semiconductor layer 108 during the formation of the insulating layer 110a is small. By using a film with low defect density and impurity concentration as the insulating layer 110a and adopting film formation conditions that cause little damage to the semiconductor layer 108, a transistor with good electrical characteristics can be realized.
[0134] For example, when a film containing silicon is formed by PECVD as the insulating layer 110, the insulating layer 110a can be formed under film forming conditions in which the ratio of the gas containing silicon to the film forming gas used in the film forming process is low. By using film forming conditions in which the ratio of the gas containing silicon to the film forming gas is low, the insulating layer 110a having a low defect density and impurity concentration can be formed. In addition, by reducing the film forming power when forming the insulating layer 110a, damage to the semiconductor layer 108 can be reduced.
[0135] Preferably, the etching speed of the insulating layer 110 c in contact with the metal oxide layer 114 by the etchant used when processing the conductive layer 112 is substantially equal to or lower than that of the conductive layer 112 .
[0136] The insulating layer 110c is preferably a denser film than the insulating layer 110a. The dense insulating layer 110c can be formed under film forming conditions where its film forming speed is lower than that of the insulating layer 110a. In addition, water adsorption on the surface of the dense insulating layer 110c is suppressed. In other words, by providing the insulating layer 110c on the top surface of the insulating layer 110, water adsorption on the surface of the insulating layer 110 can be suppressed.
[0137] When water is adsorbed on the surface of the insulating layer 110, hydrogen contained in the adsorbed water reaches the channel formation region and generates carriers in the channel formation region, which sometimes has a bad influence on the electrical characteristics and reliability of the transistor. By providing an insulating layer 110c on the top surface of the insulating layer 110, to which water is not easily adsorbed, it is possible to suppress the generation of carriers in the channel formation region, thereby obtaining good electrical characteristics and reliability.
[0138] The insulating layer 110c can be formed under film forming conditions in which the film forming speed is lower than that of the insulating layer 110a. For example, when a film containing silicon is used as the insulating layer 110, the insulating layer 110c can be formed under film forming conditions in which the ratio of the gas containing silicon to the film forming gas used in the film forming is low. In addition, by making the film forming power higher than that of the insulating layer 110a during the film forming, the insulating layer 110c can be an insulating layer that is not easily adsorbed with water.
[0139] The etching rate of the insulating layer 110c using one etchant is preferably lower than the etching rate of the insulating layer 110a. In addition, the film density of the insulating layer 110c is sometimes higher than that of the insulating layer 110a. The difference in film density between the insulating layer 110a and the insulating layer 110c can be evaluated by, for example, the concentration (brightness) of a TEM image.
[0140] The insulating layer 110b can be formed under film forming conditions at a higher film forming rate than the insulating layer 110a and the insulating layer 110c. By using the insulating layer 110b with a high film forming rate, the insulating layer 110 having a stacked structure can be formed with high productivity.
[0141] For example, when a film containing silicon is used as the insulating layer 110, the insulating layer 110b can be formed under film forming conditions in which the ratio of the gas containing silicon to the film forming gas used in the film formation is higher than that of the insulating layer 110a and the insulating layer 110c. In addition, the insulating layer 110b can be formed with less impurities by increasing the power during film formation. Furthermore, the insulating layer 110b can be formed with less impurities by increasing the pressure during film formation.
[0142] The etching speed of the insulating layer 110b when using a single etchant is preferably higher than the etching speeds of the insulating layer 110a and the insulating layer 110c. In addition, the film density of the insulating layer 110b is sometimes lower than that of the insulating layer 110a and the insulating layer 110c. The difference in film density among the insulating layer 110a, the insulating layer 110b, and the insulating layer 110c can be evaluated, for example, by the concentration (brightness) of a TEM image. In addition, the hydrogen concentration of the insulating layer 110b is sometimes higher than that of the insulating layer 110a and the insulating layer 110c. The difference in hydrogen concentration among the insulating layer 110a, the insulating layer 110b, and the insulating layer 110c can be evaluated, for example, by secondary ion mass spectrometry (SIMS).
[0143] When the conductive layer 112, the functional layer 113, and the metal oxide layer 114 are formed, the thickness of the insulating layer 110c in a region that does not overlap with the conductive layer 112 may be reduced. Figure 2As shown, the insulating layer 110c is preferably left in the region not overlapping with the conductive layer 112. By adopting a structure in which the insulating layer 110c is left in the region not overlapping with the conductive layer 112, it is possible to suppress water adsorption to the insulating layer 110. The thickness of the insulating layer 110c in the region overlapping with the conductive layer 112 is set to be greater than 1 nm and less than 50 nm, preferably greater than 2 nm and less than 40 nm, and more preferably greater than 3 nm and less than 30 nm.
[0144] like Figure 3A As shown, the insulating layer 110 may also have a two-layer structure of an insulating layer 110 a and an insulating layer 110 c on the insulating layer 110 a .
[0145] like Figure 3B As shown, the insulating layer 110 may have a single-layer structure. As the insulating layer 110, any one of the insulating layer 110a, the insulating layer 110b, and the insulating layer 110c described above may be appropriately selected according to the purpose.
[0146] The insulating layer 103 may have a stacked structure. Figure 4A and Figure 4B An example of a transistor in which the insulating layer 103 has a stacked-layer structure is shown. Figure 4A is a cross-sectional view of the transistor 100 in the channel length direction. Figure 4B is a cross-sectional view of the transistor 100 in the channel width direction.
[0147] The insulating layer 103 preferably has a stacked structure of an insulating layer 103a and an insulating layer 103b on the insulating layer 103a. For example, as the insulating layer 103a, a nitride or nitride oxide such as silicon nitride, silicon nitride oxide, aluminum nitride, or aluminum nitride oxide can be appropriately used. For example, as the insulating layer 103b, an oxide or nitride oxide such as silicon oxide, silicon oxynitride, aluminum oxide, aluminum oxynitride, hafnium oxide, or hafnium oxynitride can be appropriately used. By providing the insulating layer 103a on the lower side of the insulating layer 103, it is possible to suppress the diffusion of impurities from the lower layer of the insulating layer 103 to the upper layer of the insulating layer 103. At the same time, by providing the insulating layer 103b on the upper side of the insulating layer 103 in contact with the channel formation region, oxygen released from the insulating layer 103 can be supplied to the channel formation region. The insulating layer 103 can have a stacked structure of, for example, a silicon nitride film and a silicon oxynitride film on the silicon nitride film.
[0148] Note that in this specification, etc., oxynitride refers to a substance containing more oxygen than nitrogen in its composition, and oxynitride is included in the category of oxide. Nitride oxide refers to a substance containing more nitrogen than oxygen in its composition, and nitride oxide is included in the category of nitride.
[0149] like Figure 4A and Figure 4BAs shown in FIG. 1 , the transistor 100 preferably has a region where the insulating layer 103 a is in contact with the insulating layer 116. By having the region where the insulating layer 103 a is in contact with the insulating layer 116, diffusion of impurities from outside the transistor 100 into the transistor 100 can be suppressed.
[0150] The transistor 100 includes a conductive layer 106 between a substrate 102 and an insulating layer 103 . The conductive layer 106 has a region overlapping with a channel formation region of a semiconductor layer 108 , a metal oxide layer 114 , a functional layer 113 , and a conductive layer 112 .
[0151] In the transistor 100, the conductive layer 106 is used as a first gate electrode (also referred to as a bottom gate electrode), and the functional layer 113 and the conductive layer 112 are used as a second gate electrode (also referred to as a top gate electrode). In addition, a portion of the insulating layer 103 is used as a first gate insulating layer, and a portion of the insulating layer 110 is used as a second gate insulating layer.
[0152] A portion of the semiconductor layer 108 that overlaps with one or more of the functional layer 113, the conductive layer 112, and the conductive layer 106 is used as a channel formation region. Note that, for ease of description below, the portion of the semiconductor layer 108 that overlaps with the functional layer 113 and the conductive layer 112 is sometimes referred to as a channel formation region, but in fact, a channel may be formed in a portion that does not overlap with the functional layer 113 and the conductive layer 112 but overlaps with the conductive layer 106 (including the portion of the region 108N).
[0153] like Figure 1C and Figure 4B As shown, the conductive layer 106 may be electrically connected to the conductive layer 112 through an opening 142 provided in the functional layer 113, the metal oxide layer 114, the insulating layer 110, and the insulating layer 103. Thus, the conductive layer 106 and the conductive layer 112 can be supplied with the same potential.
[0154] The conductive layer 106 can be made of the same material as the conductive layer 112, the conductive layer 120a, or the conductive layer 120b. In particular, the conductive layer 106 is preferably made of a material containing copper, in which case wiring resistance can be reduced. In addition, when the conductive layer 106 is made of a material containing a high melting point metal such as tungsten or molybdenum, it can be processed at a high temperature in a subsequent step.
[0155] like Figure 1C and Figure 4B As shown, the functional layer 113, the conductive layer 112, and the conductive layer 106 preferably protrude outside the end of the semiconductor layer 108 in the channel width direction. At this time, a structure is formed in which the semiconductor layer 108 in the channel width direction is entirely covered by the functional layer 113, the conductive layer 112, and the conductive layer 106 via the insulating layer 110 and the insulating layer 103.
[0156] By adopting the above structure, the semiconductor layer 108 can be electrically surrounded by the electric field generated by the pair of gate electrodes. In this case, it is particularly preferable to supply the same potential to the conductive layer 106, the functional layer 113, and the conductive layer 112. Thus, an electric field for inducing a channel can be effectively applied to the semiconductor layer 108, so that the on-state current of the transistor 100 can be increased. Therefore, the transistor 100 can also be miniaturized.
[0157] Alternatively, a structure may be employed in which the functional layer 113, the conductive layer 112, and the conductive layer 106 are not connected. In this case, a constant potential may be supplied to one of the pair of gate electrodes, and a signal for driving the transistor 100 may be supplied to the other. In this case, the threshold voltage when the transistor 100 is driven by the other gate electrode can be controlled by the potential supplied to one gate electrode.
[0158] Hereinafter, a structural example of a transistor having a partially different structure from that of the structural example 1 described above will be described. Note that the description of the parts repeated in the structural example 1 described above may be omitted below. In addition, in the drawings shown below, parts having the same functions as those of the structural example 1 described above are denoted by the same hatching and sometimes without a reference numeral.
[0159] <Structure Example 2> Figure 5A is a cross-sectional view of the transistor 100A in the channel length direction. Figure 5B It is a cross-sectional view of the transistor 100A in the channel width direction. Figure 5C yes Figure 5A An enlarged view of the area Q surrounded by a dot-dashed line in FIG.
[0160] The transistor 100A is different from Structural Example 1 mainly in that the film thickness of the functional layer 113 in a region not overlapping with the conductive layer 112 is thinner than the film thickness of the functional layer 113 in a region overlapping with the conductive layer 112 .
[0161] Since the thickness of the functional layer 113 in a region not overlapping with the conductive layer 112 is thin, the step size is reduced and coverage of the layer formed on the functional layer 113 is improved, thereby suppressing occurrence of defects such as disconnection and voids in the layer.
[0162] The above is the description of Structural Example 2.
[0163] <Structure Example 3> Fig. 6A is a cross-sectional view of the transistor 100B in the channel length direction. Figure 6B It is a cross-sectional view of the transistor 100B in the channel width direction. Figure 6C yes Fig. 6A An enlarged view of the region R surrounded by a dot-dashed line in FIG.
[0164] The main differences between transistor 100B and structural example 1 are that the film thickness of the functional layer 113 in the area not overlapping with the conductive layer 112 is thinner than the film thickness of the functional layer 113 in the area overlapping with the conductive layer 112, and the film thickness of the metal oxide layer 114 in the area not overlapping with the conductive layer 112 is thinner than the film thickness of the metal oxide layer 114 in the area overlapping with the conductive layer 112.
[0165] The conductive layer 112 and the functional layer 113 preferably have continuous cross-sections. When the conductive layer 112 and the functional layer 113 have continuous cross-sections, the coverage of the layer formed on the conductive layer 112 and the functional layer 113 is improved, thereby preventing defects such as disconnection or voids in the layer.
[0166] The above is the description of Structural Example 3.
[0167] <Manufacturing method example 1> Hereinafter, a method for manufacturing a semiconductor device according to one embodiment of the present invention will be described with reference to the drawings. Here, the transistor 100 shown in the above structural example will be described as an example.
[0168] The thin film (insulating film, semiconductor film, conductive film, etc.) constituting the semiconductor device can be formed by sputtering, chemical vapor deposition (CVD: Chemical Vapor Deposition) method, vacuum evaporation method, pulsed laser deposition (PLD: Pulsed Laser Deposition) method, atomic layer deposition (ALD: Atomic Layer Deposition) method, etc. As the CVD method, plasma enhanced chemical vapor deposition (PECVD: Plasma Enhanced CVD) method, thermal CVD method, etc. can be cited. In addition, as one of the methods of thermal CVD method, metal organic chemical vapor deposition (MOCVD: Metal Organic CVD) method can be cited.
[0169] Thin films (insulating films, semiconductor films, conductive films, etc.) that constitute semiconductor devices can be formed by methods such as spin coating, dipping, spraying, inkjet, dispenser, screen printing, offset printing, doctor knife, slit coating, roll coating, curtain coating, and doctor blade coating.
[0170] In addition, when processing a thin film constituting a semiconductor device, it can be processed by photolithography or the like. In addition to the above methods, the thin film can also be processed by nanoimprinting, sandblasting, lift-off, etc. In addition, an island-shaped thin film can be directly formed by a film forming method using a shielding mask such as a metal mask.
[0171] There are two typical photolithography methods. One is to form a resist mask on a thin film to be processed, process the thin film by etching, etc., and remove the resist mask. The other is to form a photosensitive thin film, then perform exposure and development to process the thin film into a desired shape.
[0172] In the photolithography method, as the light used for exposure, for example, i-line (wavelength 365nm), g-line (wavelength 436nm), h-line (wavelength 405nm) or a mixture of these lights can be used. In addition, ultraviolet light, KrF laser or ArF laser, etc. can also be used. In addition, liquid immersion exposure technology can also be used for exposure. As the light used for exposure, extreme ultraviolet light (EUV: Extreme Ultra-violet) or X-rays can also be used. In addition, an electron beam can also be used instead of the light used for exposure. When extreme ultraviolet light, X-rays or electron beams are used, extremely fine processing can be performed, so it is preferred. Note that when exposure is performed by scanning with a light beam such as an electron beam, a photomask is not required.
[0173] As a method for etching the thin film, a dry etching method, a wet etching method, a sand blast method, or the like can be used.
[0174] 7A to 11B The figures show cross sections at various stages of the manufacturing process of the transistor 100A. In each figure, the left side of the central dotted line shows a cross section in the channel length direction, and the right side of the central dotted line shows a cross section in the channel width direction.
[0175] [Formation of Conductive Layer 106] A conductive film is formed over the substrate 102, and the conductive film is etched to obtain a conductive layer 106 serving as a first gate electrode (see Fig. 7A ).
[0176] [Formation of Insulating Layer 103] Next, an insulating layer 103 is formed so as to cover the substrate 102 and the conductive layer 106 (see Figure 7B ). The insulating layer 103 can be formed by a PECVD method, an ALD method, a sputtering method, or the like.
[0177] When the insulating layer 103 has a stacked-layer structure, insulating films serving as the insulating layer 103 are sequentially formed. For example, when a stacked-layer structure of a nitride film and an oxide film over the nitride film is used as the insulating layer 103, the nitride film and the oxide film are sequentially formed.
[0178] The nitride film included in the insulating layer 103 may have a stacked structure of two or more layers. When a stacked structure of, for example, a first silicon nitride film, a second silicon nitride film on the first silicon nitride film, a third silicon nitride film on the second silicon nitride film, and an oxynitride silicon film on the third silicon nitride film is used as the insulating layer 103, the first silicon nitride film, the second silicon nitride film, the third silicon nitride film, and the oxynitride silicon film are formed in sequence.
[0179] When the insulating layer 103 has a stacked structure of a first silicon nitride film, a second silicon nitride film, a third silicon nitride film and an oxynitride silicon film, the first silicon nitride film preferably has a function of blocking impurities. By providing the first silicon nitride film, it is possible to suppress the diffusion of impurities from the lower layer of the insulating layer 103 to the upper layer of the insulating layer 103. It is preferred that the second silicon nitride film has a small stress and a high insulating withstand voltage. By providing the second silicon nitride film, an insulating layer 103 with a small stress and a high insulating withstand voltage can be formed. It is preferred that the third silicon nitride film releases a small amount of impurities containing hydrogen and has a function of blocking impurities containing hydrogen. By providing the third silicon nitride film, it is possible to suppress the diffusion of hydrogen into the channel formation region. It is preferred that the oxynitride silicon film has a low defect density and releases a small amount of impurities containing hydrogen.
[0180] For example, as the formation of the insulating layer 103, a first silicon nitride film having a function of blocking impurities is formed by a plasma CVD method using a mixed gas of silane, nitrogen and ammonia. Then, a second silicon nitride film having low stress and high insulation withstand voltage is formed using a mixed gas having a larger ammonia flow rate than the first silicon nitride film. Then, a third silicon nitride film having a function of blocking impurities including hydrogen and releasing a small amount of impurities including hydrogen is formed using a mixed gas having a smaller ammonia flow rate than the second silicon nitride film. Then, an oxynitride silicon film having a low defect density and releasing a small amount of impurities including hydrogen is formed using a mixed gas of silane and nitrous oxide, thereby forming the insulating layer 103. In addition, by switching the film forming conditions in the same processing chamber, the first silicon nitride film, the second silicon nitride film, the third silicon nitride film and the oxynitride silicon film can be continuously formed in a vacuum, thereby forming the insulating layer 103 with high productivity.
[0181] Alternatively, after forming the third silicon nitride film, plasma treatment is performed in an atmosphere including oxygen to oxidize the surface of the third silicon nitride film, whereby a silicon oxynitride film can be formed on the third silicon nitride film.
[0182] Sometimes the film density of the second silicon nitride film is lower than that of the first silicon nitride film and the third silicon nitride film. The difference in film density among the first silicon nitride film, the second silicon nitride film, and the third silicon nitride film can be evaluated, for example, by the concentration (brightness) of a TEM image. In addition, sometimes the hydrogen concentration of the second silicon nitride film is higher than that of the first silicon nitride film and the third silicon nitride film. The difference in hydrogen concentration among the first silicon nitride film, the second silicon nitride film, and the third silicon nitride film can be evaluated, for example, by secondary ion mass spectrometry (SIMS).
[0183] After forming the insulating layer 103, a process for supplying oxygen to the insulating layer 103 may be performed. For example, plasma treatment or heat treatment may be performed in an oxygen atmosphere. Alternatively, oxygen may be supplied to the insulating layer 103 by a plasma ion doping method or an ion implantation method. In addition, the heat treatment may not be performed after forming the insulating layer 103.
[0184] [Formation of Semiconductor Layer 108] Next, a metal oxide film is formed on the insulating layer 103 and processed to form an island-shaped semiconductor layer 108 (see Figure 7C ).
[0185] The metal oxide film is preferably formed by a sputtering method using a metal oxide target.
[0186] When forming a metal oxide film, oxygen gas and an inert gas (e.g., helium gas, argon gas, xenon gas, etc.) may also be mixed. Note that the higher the ratio of oxygen gas to the entire film-forming gas when forming a metal oxide film (oxygen flow ratio), the higher the crystallinity of the metal oxide film can be, and a transistor with high reliability can be realized. On the other hand, the lower the oxygen flow ratio, the lower the crystallinity of the metal oxide film, and a transistor with high on-state current can be realized.
[0187] In the case where the semiconductor layer 108 has a stacked structure, it is preferred to continuously form films in the same film forming chamber using the same sputtering target because a good interface can be obtained. In particular, although the conditions of pressure, temperature, power, etc. during the film formation of each metal oxide film can be made different, it is preferred to shorten the time required for the film forming process by making the conditions other than the oxygen flow rate ratio the same. In addition, in the case of stacking metal oxide films with different compositions, it is preferred to continuously form the films without being exposed to the atmosphere.
[0188] Here, the metal oxide film is preferably formed under film forming conditions so as to form a metal oxide film having a CAAC structure, a metal oxide film having an nc structure, or a metal oxide film having a mixture of a CAAC structure and an nc structure. Note that the film forming conditions for forming a metal oxide film having a CAAC structure and the film forming conditions for forming an nc structure differ depending on the composition of the sputtering target used, so the substrate temperature, oxygen flow ratio, pressure, power, etc. may be appropriately set according to the composition.
[0189] As a film forming condition of the metal oxide film, the substrate temperature can be set to be higher than room temperature and lower than 450° C., preferably higher than room temperature and lower than 300° C., more preferably higher than room temperature and lower than 200° C., and further preferably higher than room temperature and lower than 140° C. For example, when a large glass substrate or a resin substrate is used as the substrate 102, the substrate temperature is preferably higher than room temperature and lower than 140° C., because productivity can be improved. In addition, by forming the metal oxide film at room temperature or in a state where the substrate temperature is not heated, crystallinity can be reduced.
[0190] In addition, it is preferable to perform a treatment for removing water, hydrogen, organic matter, etc. attached to the surface of the insulating layer 103 or a treatment for supplying oxygen to the insulating layer 103 before forming the metal oxide film. For example, a heat treatment may be performed at a temperature of 70° C. to 200° C. in a reduced pressure atmosphere. Alternatively, a plasma treatment may be performed in an oxygen-containing atmosphere. In addition, when a plasma treatment is performed in an atmosphere containing nitrous oxide gas, organic matter on the surface of the insulating layer 103 can be appropriately removed. It is preferable that, after such treatment, a metal oxide film is continuously formed in a manner that does not expose the surface of the insulating layer 103 to the atmosphere.
[0191] When the metal oxide film is processed, a wet etching method and / or a dry etching method can be used. At this time, a portion of the insulating layer 103 which does not overlap with the semiconductor layer 108 may be etched and thinned.
[0192] In addition, heat treatment may be performed after the metal oxide film is formed or after the metal oxide film is processed into the semiconductor layer 108 to remove hydrogen or water in the metal oxide or the semiconductor layer 108. Typically, the temperature of the heat treatment may be set to be 150° C. or higher and lower than the strain point of the substrate, 250° C. or higher and 450° C. or higher and 300° C. or lower. In addition, heat treatment may not be performed after the metal oxide film is formed or after the metal oxide film is processed into the semiconductor layer 108. In addition, heat treatment may be performed at any stage after the metal oxide film is formed. In addition, it may also serve as a subsequent heat treatment or heat application process.
[0193] The heat treatment can be performed in an atmosphere containing a rare gas or nitrogen. Alternatively, the heating can be performed in the atmosphere and then in an atmosphere containing oxygen. As a nitrogen-containing atmosphere or an oxygen-containing atmosphere, ultra-dry air (CDA: Clean Dry Air) can also be used. In addition, the atmosphere of the above-mentioned heat treatment preferably does not contain hydrogen, water, etc. In addition, by using a high-purity gas with a dew point of less than -60°C, preferably less than -100°C, it is possible to prevent hydrogen, water, etc. from mixing into the semiconductor layer 108 as much as possible. In addition, the heat treatment can be performed using an electric furnace, a rapid thermal annealing (RTA: Rapid Thermal Annealing) device, etc. By using an RTA device, the heat treatment time can be shortened.
[0194] It is also preferable to form the insulating film 110f immediately after forming the semiconductor layer 108. When the surface of the semiconductor layer 108 is exposed, water may adhere to the surface of the semiconductor layer 108. When water adheres to the surface of the semiconductor layer 108, hydrogen may diffuse into the semiconductor layer 108 by subsequent heat treatment, etc., and V may be formed. O H.V O Since H may become a source of carrier generation, the less water attached to the semiconductor layer 108 the better.
[0195] [Formation of Insulating Film 110f, Metal Oxide Film 114f, and Functional Film 113f] Next, an insulating film 110 f and a metal oxide film 114 f are formed so as to cover the insulating layer 103 and the semiconductor layer 108 .
[0196] The insulating film 110f is a film that later becomes the insulating layer 110. As the insulating film 110f, for example, an oxide film such as a silicon oxide film or a silicon oxynitride film is preferably formed by using a plasma enhanced chemical vapor deposition apparatus (referred to as a PECVD apparatus or simply referred to as a plasma CVD apparatus). Alternatively, it can be formed by a PECVD method using microwaves.
[0197] When the insulating layer 110 has a stacked structure, the insulating films that become the insulating layer 110 are formed in sequence. Figure 2 As shown, when the insulating layer 110 has a three-layer structure of the insulating layer 110a, the insulating layer 110b, and the insulating layer 110c, an insulating film to become the insulating layer 110a, an insulating film to become the insulating layer 110b, and an insulating film to become the insulating layer 110c are sequentially formed.
[0198] For example, the insulating film to be the insulating layer 110a is formed by a plasma CVD method using a mixed gas of silane and nitrous oxide, thereby forming the insulating layer 110. Next, the insulating film to be the insulating layer 110b is formed under conditions of high power using a mixed gas having a higher flow rate ratio of silane to nitrous oxide than the insulating film to be the insulating layer 110a. Next, the insulating film to be the insulating layer 110c is formed under conditions of low pressure using a mixed gas having a lower flow rate ratio of silane to nitrous oxide than the insulating film to be the insulating layer 110b. In addition, by switching the film forming conditions in the same processing chamber, the insulating film to be the insulating layer 110a, the insulating film to be the insulating layer 110b, and the insulating film to be the insulating layer 110c can be continuously formed in a vacuum, thereby forming the insulating film 110f with high productivity.
[0199] For example, Figure 3A As shown, when the insulating layer 110 has a two-layer structure of the insulating layer 110 a and the insulating layer 110 c , an insulating film to become the insulating layer 110 a and an insulating film to become the insulating layer 110 c are formed in sequence.
[0200] For example, an insulating film to be the insulating layer 110a is formed by a plasma CVD method using a mixed gas of silane and nitrous oxide to form the insulating layer 110. Next, an insulating film to be the insulating layer 110c is formed under conditions of lower pressure and higher power than those of the insulating film to be the insulating layer 110a to form the insulating film to be the insulating layer 110. In addition, by switching film forming conditions in the same processing chamber, the insulating film to be the insulating layer 110a and the insulating film to be the insulating layer 110c can be continuously formed in a vacuum, thereby forming the insulating film 110f with high productivity.
[0201] Heat treatment may be performed after the insulating film 110f is formed. By performing heat treatment, impurities in the insulating film 110f and water on the surface of the insulating film 110f can be removed. The heat treatment may be performed at a temperature of 200° C. to 400° C. in an atmosphere containing one or more of nitrogen, oxygen, and a rare gas. In addition, heat treatment may not be performed after the insulating film 110f is formed. In addition, heat treatment may be performed at any stage after the insulating film 110f is formed. In addition, it may also serve as a subsequent heat treatment or heat application process.
[0202] The metal oxide film 114f is a film that later becomes the metal oxide layer 114. In particular, the metal oxide film 114f is preferably formed by sputtering in an atmosphere containing oxygen, for example. Thus, oxygen can be supplied to the insulating film 110f when the metal oxide film 114f is formed.
[0203] When the metal oxide film 114 f is formed by a sputtering method using an oxide target containing a metal oxide similarly to the semiconductor layer 108 , the above description can be applied.
[0204] For example, the metal oxide film 114f can be formed by a reactive sputtering method using oxygen as a film-forming gas and a metal target. When aluminum is used as the metal target, an aluminum oxide film can be formed.
[0205] When the metal oxide film 114f is formed, the higher the ratio of the oxygen flow rate to the total flow rate of the film forming gas introduced into the film forming chamber of the film forming apparatus (oxygen flow rate ratio) or the oxygen partial pressure in the film forming chamber is, the greater the amount of oxygen supplied to the insulating film 110f can be. The oxygen flow rate ratio or the oxygen partial pressure is, for example, 50% or more and 100% or less, preferably 65% or more and 100% or less, more preferably 80% or more and 100% or less, and further preferably 90% or more and 100% or less. In particular, it is preferred to set the oxygen flow rate ratio to 100% to make the oxygen partial pressure as close to 100% as possible.
[0206] In this way, by forming the metal oxide film 114f by sputtering in an atmosphere containing oxygen, oxygen can be supplied to the insulating film 110f while preventing oxygen from being separated from the insulating film 110f when the metal oxide film 114f is formed. As a result, a large amount of oxygen can be enclosed in the insulating film 110f. In addition, by supplying a large amount of oxygen to the channel formation region of the semiconductor layer 108 through the subsequent heat treatment, oxygen vacancies in the channel formation region can be reduced, thereby realizing a transistor with high reliability.
[0207] As the film formation condition of the metal oxide film 114f, the substrate temperature is set to be higher than room temperature and lower than 450°C, preferably higher than room temperature and lower than 300°C, more preferably higher than room temperature and lower than 200°C, and further preferably higher than room temperature and lower than 140°C. For example, when a large glass substrate or a resin substrate is used as the substrate 102, it is preferred that the substrate temperature is higher than room temperature and lower than 140°C because productivity is improved. In addition, when the temperature when the metal oxide film 114f is formed is high, the crystallinity of the metal oxide film 114f is improved and the etching rate is sometimes reduced. When the film formation temperature of the metal oxide film 114f is low, the crystallinity of the metal oxide film 114f is reduced and the etching rate is sometimes increased. In addition, the film formation temperature of the metal oxide film 114f can also be appropriately selected so as to obtain an etching rate that is very suitable for the etchant used when processing the metal oxide film 114f.
[0208] In addition, heat treatment may be performed after the metal oxide film 114f is formed so as to supply oxygen from the insulating film 110f to the semiconductor layer 108. The heat treatment may be performed at a temperature of 200° C. to 400° C. in an atmosphere containing one or more of nitrogen, oxygen, and a rare gas. In addition, heat treatment may not be performed after the metal oxide film 114f is formed. In addition, heat treatment may be performed at any stage after the metal oxide film 114f is formed. In addition, it may also serve as a subsequent heat treatment or heat application step.
[0209] Next, a functional film 113f (see FIG. 114 ) serving as the functional layer 113 is formed on the metal oxide film 114f. Fig. 8A ) The functional film 113f is preferably formed by a sputtering method using a sputtering target of a metal or alloy.
[0210] In addition, heat treatment may be performed after the functional film 113f is formed. When a material containing oxygen is used as the functional film 113f, oxygen can be supplied from the functional film 113f to the semiconductor layer 108 by performing heat treatment after the functional film 113f is formed. The heat treatment may be performed at a temperature of 200° C. to 400° C. in an atmosphere containing one or more of nitrogen, oxygen, and a rare gas. Note that heat treatment may not be performed after the functional film 113f is formed.
[0211] Next, the functional film 113f, the metal oxide film 114f, the insulating film 110f, and a portion of the insulating layer 103 are etched to form an opening 142 that reaches the conductive layer 106 (see FIG. 14A ). Figure 8B Thus, the conductive layer 112 to be formed later can be electrically connected to the conductive layer 106 through the opening 142.
[0212] [Formation of Conductive Film 112f] Next, a conductive film 112f (see FIG. 112 ) serving as the conductive layer 112 is formed on the functional film 113f. Fig. 9A ) The conductive film 112f is preferably formed by a sputtering method using a sputtering target of a metal or alloy.
[0213] [Formation of Insulating Layer 110, Metal Oxide Layer 114, Functional Layer 113, and Conductive Layer 112] Next, a resist mask 115 is formed on the conductive film 112f (see Fig. 9B Then, the conductive film 112f, the functional film 113f, and the metal oxide film 114f in the area not covered by the resist mask 115 are removed to form the conductive layer 112, the functional layer 113, and the metal oxide layer 114 (see Fig. 10A ).
[0214] When forming the conductive layer 112, the functional layer 113, and the metal oxide layer 114, a wet etching method can be appropriately used. As the wet etching method, for example, an etchant containing hydrogen peroxide can be used. For example, an etchant containing one or more of phosphoric acid, acetic acid, nitric acid, hydrochloric acid, and sulfuric acid can be used. In particular, when a material containing copper is used as the conductive layer 112, an etchant containing phosphoric acid, acetic acid, and nitric acid can be appropriately used.
[0215] By adopting a structure in which the etching rate of the metal oxide layer 114 and the functional layer 113 is lower than that of the conductive layer 112, the functional layer 113, the metal oxide layer 114, and the conductive layer 112 can be formed in the same process. In addition, the end of the conductive layer 112 can be located inside the end of the metal oxide layer 114 and the functional layer 113. In addition, since the same process can be used, the process can be simplified and the productivity can be improved.
[0216] The conductive layer 112, the functional layer 113, and the metal oxide layer 114 are processed so that the ends thereof are located inside the outline of the resist mask 115. The conductive layer 112, the functional layer 113, and the metal oxide layer 114 are preferably formed by wet etching. The width of the region 108L can be controlled by adjusting the etching time.
[0217] When forming the conductive layer 112, the functional layer 113, and the metal oxide layer 114, the conductive film 112f, the functional film 113f, and the metal oxide film 114f may be etched using an anisotropic etching method, and then the side surfaces of the conductive film 112f, the functional film 113f, and the metal oxide film 114f may be etched using an isotropic etching method to cause the end surfaces to recede (also referred to as side etching). In this way, the conductive layer 112, the functional layer 113, and the metal oxide layer 114 may be formed such that the end portions thereof are located inside the insulating layer 110 in a plan view.
[0218] When the conductive layer 112, the functional layer 113, and the metal oxide layer 114 are formed, the conductive layer 112 is retracted relative to the functional layer 113 and the metal oxide layer 114, and the thickness of the functional layer 113 in a region not overlapping with the conductive layer 112 is sometimes thinner than the thickness of the functional layer 113 in a region overlapping with the conductive layer 112 (see Figure 5A , Figure 5B and Figure 5C ). In addition, the thickness of the metal oxide layer 114 in a region not overlapping with the conductive layer 112 is sometimes thinner than the thickness of the metal oxide layer 114 in a region overlapping with the conductive layer 112 and the functional layer 113 (see Fig. 6A , Figure 6B and Figure 6C ).
[0219] In addition, when forming the conductive layer 112, the functional layer 113, and the metal oxide layer 114, etching may be performed at least twice using different etching conditions or methods. For example, the conductive film 112f may be etched first, and then the functional film 113f and the metal oxide film 114f may be etched using different etching conditions.
[0220] Next, the insulating film 110f is removed in the region not covered by the resist mask 115 to form the insulating layer 110 (see Fig. 10B ). When forming the insulating layer 110, either a wet etching method or a dry etching method or both can be used. Note that the insulating layer 110 can be formed in a state where the resist mask 115 is removed, but by not removing the resist mask 115, a reduction in the film thickness of the conductive layer 112 can be suppressed.
[0221] After the insulating layer 110 is formed, the resist mask 115 is removed.
[0222] [Formation of Insulating Layer 116 and Region 108N (Hydrogen Supply Process)] Next, a process of supplying hydrogen to the exposed region of the semiconductor layer 108 is performed. Here, hydrogen is supplied by forming an insulating layer 116 containing hydrogen so as to be in contact with the exposed region of the semiconductor layer 108 (see Fig.11A ).
[0223] The insulating layer 116 is preferably formed by a plasma CVD method using a film-forming gas containing hydrogen. For example, a silicon nitride film is formed by using a film-forming gas containing silane gas and ammonia gas. By using ammonia gas in addition to silane gas, a large amount of hydrogen can be contained in the film. In addition, hydrogen can also be supplied to the exposed portion of the semiconductor layer 108 during film formation.
[0224] Preferably, a portion of hydrogen released from the insulating layer 116 is supplied to a portion of the semiconductor layer 108 by performing heat treatment after forming the insulating layer 116. The heat treatment is preferably performed at a temperature of 150° C. to 450° C., preferably 200° C. to 400° C., in an atmosphere containing one or more of nitrogen, oxygen, and a rare gas.
[0225] By supplying hydrogen as described above, a region 108N having a very low resistance can be formed in the semiconductor layer 108 .
[0226] By performing the heat treatment, oxygen can be supplied from the insulating layer 110 to the channel formation region of the semiconductor layer 108 .
[0227] [Formation of Insulating Layer 118] Next, an insulating layer 118 is formed on the insulating layer 116 .
[0228] When the insulating layer 118 is formed by a plasma CVD method, if the film formation temperature is too high, impurities contained in the region 108N and the like may diffuse to the peripheral portion of the channel formation region including the semiconductor layer 108. As a result, there is a concern that the resistance of the channel formation region decreases or the resistance of the region 108N increases. The film formation temperature of the insulating layer 116 or the insulating layer 118 is, for example, preferably 150° C. to 400° C., more preferably 180° C. to 360° C., and further preferably 200° C. to 250° C. By forming the insulating layer 118 at a low temperature, good electrical characteristics can be obtained even for a transistor with a short channel length.
[0229] Alternatively, heat treatment may be performed after the insulating layer 118 is formed.
[0230] [Formation of Openings 141a and 141b] Next, a mask is formed at a desired position of the insulating layer 118 by photolithography, and then the insulating layer 118 and the insulating layer 116 are partially etched, thereby forming the opening 141 a and the opening 141 b reaching the region 108N.
[0231] [Formation of Conductive Layer 120a and Conductive Layer 120b] Next, a conductive film is formed on the insulating layer 118 so as to cover the openings 141a and 141b, and the conductive film is processed into a desired shape to form the conductive layers 120a and 120b (see FIG. 1 ). Fig. 11B ).
[0232] Through the above steps, the transistor 100 can be manufactured.
[0233] <Components of a semiconductor device> Next, components included in the semiconductor device of this embodiment will be described in detail.
[0234] [Substrate] Although there is no particular limitation on the material of the substrate 102, it is at least required to have heat resistance sufficient to withstand subsequent heat treatment. For example, a single crystal semiconductor substrate or polycrystalline semiconductor substrate made of silicon or silicon carbide, a compound semiconductor substrate such as silicon germanium, an SOI substrate, a glass substrate, a ceramic substrate, a quartz substrate, a sapphire substrate, or the like can be used as the substrate 102. In addition, a substrate having a semiconductor element provided thereon can also be used as the substrate 102.
[0235] In addition, a flexible substrate may be used as the substrate 102, and the transistor 100 and the like may be directly formed on the flexible substrate. Alternatively, a peeling layer may be provided between the substrate 102 and the transistor 100 and the like. The peeling layer may be used when a part or all of a semiconductor device is manufactured on the peeling layer, and then separated from the substrate 102 and transferred to another substrate. In this case, the transistor 100 and the like may also be transferred to a substrate with low heat resistance or a flexible substrate.
[0236] [Insulating layer 103] The insulating layer 103 can be formed using a sputtering method, a CVD method, an evaporation method, a pulsed laser deposition (PLD) method, or the like as appropriate. In addition, the insulating layer 103 can be formed using, for example, a single layer or a stack of oxide insulating films or nitride insulating films. Note that in order to improve the interface characteristics between the insulating layer 103 and the semiconductor layer 108, at least a region in contact with the semiconductor layer 108 in the insulating layer 103 is preferably formed using an oxide insulating film. In addition, the insulating layer 103 is preferably formed using a film that releases oxygen by heating.
[0237] The insulating layer 103 can be made of, for example, silicon oxide, silicon oxynitride, silicon nitride oxide, silicon nitride, aluminum oxide, hafnium oxide, gallium oxide, or Ga—Zn oxide, and can be provided in a stacked layer or a single layer.
[0238] When a film other than an oxide film such as a silicon nitride film is used on the side of the insulating layer 103 in contact with the semiconductor layer 108, the surface in contact with the semiconductor layer 108 is preferably subjected to pretreatment such as oxygen plasma treatment to oxidize the surface or the vicinity of the surface.
[0239] [Conductive film] The conductive layer 106 and the conductive layer 112 used as the drain electrode, the conductive layer 120a used as one of the source electrode and the drain electrode, and the conductive layer 120b used as the other of the source electrode and the drain electrode can be formed respectively using a metal element selected from chromium, copper, aluminum, gold, silver, zinc, molybdenum, tantalum, titanium, tungsten, manganese, nickel, iron, and cobalt, or an alloy containing the above metal elements, or an alloy combining the above metal elements.
[0240] In addition, as the conductive layer 106, the conductive layer 112, the conductive layer 120a and the conductive layer 120b, an oxide conductor or a metal oxide film such as In-Sn oxide, In-W oxide, In-W-Zn oxide, In-Ti oxide, In-Ti-Sn oxide, In-Zn oxide, In-Sn-Si oxide, In-Ga-Zn oxide can be used.
[0241] Here, an oxide conductor (OC) is described. For example, an oxide conductor is obtained by forming oxygen vacancies in a metal oxide having semiconductor properties, and adding hydrogen to the oxygen vacancies to form donor energy levels near the conduction band. As a result, the conductivity of the metal oxide increases, and the metal oxide becomes a conductor. A metal oxide that can become a conductor is called an oxide conductor.
[0242] In addition, as the conductive layer 106, a stacked structure of a conductive film containing the above-mentioned oxide conductor (metal oxide) or a conductive film containing a metal or alloy may be used. By using a conductive film containing a metal or an alloy, wiring resistance can be reduced. In this case, it is preferred to use a conductive film containing an oxide conductor as a portion in contact with the insulating layer used as a gate insulating film.
[0243] In addition, the conductive layer 106, the conductive layer 112, the conductive layer 120a, and the conductive layer 120b preferably contain any one or more selected from the above-mentioned metal elements, titanium, tungsten, tantalum, and molybdenum. In particular, a tantalum nitride film is preferably used. The tantalum nitride film has conductivity and high barrier properties against copper, oxygen, or hydrogen, and the amount of hydrogen released from the tantalum nitride film itself is small, so the tantalum nitride film can be appropriately used as a conductive film in contact with the semiconductor layer 108 or a conductive film near the semiconductor layer 108.
[0244] [Insulating layer 110] The insulating layer 110 used as a gate insulating film of the transistor 100 or the like can be formed using a PECVD method, a sputtering method, or the like. As the insulating layer 110, an insulating layer including one or more of a silicon oxide film, a silicon oxynitride film, a silicon nitride oxide film, a silicon nitride film, an aluminum oxide film, a hafnium oxide film, a yttrium oxide film, a zirconium oxide film, a gallium oxide film, a tantalum oxide film, a magnesium oxide film, a lanthanum oxide film, a cerium oxide film, and a neodymium oxide film can be used. In addition, the insulating layer 110 may have a stacked structure of two layers or a stacked structure of three or more layers.
[0245] In addition, the insulating layer 110 in contact with the semiconductor layer 108 is preferably an oxide insulating film, and more preferably has a region where the oxygen content exceeds the stoichiometric composition. In other words, the insulating layer 110 is an insulating layer that can release oxygen. For example, oxygen can be supplied to the insulating layer 110 by forming the insulating layer 110 in an oxygen atmosphere; by performing heat treatment, plasma treatment, etc. on the formed insulating layer 110 in an oxygen atmosphere; or by forming an oxide film on the insulating layer 110 in an oxygen atmosphere.
[0246] As the insulating layer 110, a material such as hafnium oxide having a higher relative dielectric constant than silicon oxide or silicon oxynitride may be used. Thus, the thickness of the insulating layer 110 can be increased to suppress leakage current caused by tunnel current. In particular, crystalline hafnium oxide is preferably used because its relative dielectric constant is higher than that of amorphous hafnium oxide.
[0247] [Semiconductor layer] When the semiconductor layer 108 is an In-M-Zn oxide, the atomic number ratio of In to the element M in the sputtering target used to form the In-M-Zn oxide is preferably greater than 1. Examples of the atomic number ratio of the metal element in the sputtering target include In:M:Zn=1:1:1, In:M:Zn=1:1:1.2, In:M:Zn=2:1:3, In:M:Zn=3:1:2, In:M:Zn=4:2:3, In:M:Zn=4:2:4.1, In:M:Zn=5:1:6, In:M:Zn=5:1:7, In:M:Zn=5:1:8, In:M:Zn=6:1:6, In:M:Zn=5:2:5, and the like.
[0248] In addition, it is preferable to use a target containing polycrystalline oxide as a sputtering target, which is preferred because it is easy to form a crystalline semiconductor layer 108. Note that the atomic number ratio of the formed semiconductor layer 108 is within the range of ±40% of the atomic number ratio of the metal element in the above-mentioned sputtering target. For example, when the composition of the sputtering target used for the semiconductor layer 108 is In:Ga:Zn=4:2:4.1 [atomic number ratio], the composition of the formed semiconductor layer 108 is sometimes In:Ga:Zn=4:2:3 [atomic number ratio] or its vicinity.
[0249] Note that when the atomic number ratio is described as In:Ga:Zn=4:2:3 or in the vicinity thereof, the following cases are included: when In is 4, Ga is 1 or more and 3 or less, and Zn is 2 or more and 4 or less. In addition, when the atomic number ratio is described as In:Ga:Zn=5:1:6 or in the vicinity thereof, the following cases are included: when the In ratio is 5, Ga is greater than 0.1 and 2 or less, and Zn is 5 or more and 7 or less. In addition, when the atomic number ratio is described as In:Ga:Zn=1:1:1 or in the vicinity thereof, the following cases are included: when In is 1, Ga is greater than 0.1 and 2 or less, and Zn is greater than 0.1 and 2 or less.
[0250] The energy gap of the semiconductor layer 108 is 2 eV or more, preferably 2.5 eV or more. In this way, by using a metal oxide having a wider energy gap than silicon, the off-state current of the transistor can be reduced.
[0251] A metal oxide with a low carrier concentration is preferably used for the semiconductor layer 108. In order to reduce the carrier concentration of the metal oxide, the impurity concentration in the metal oxide is reduced to reduce the defect state density. In this specification, etc., a state in which the impurity concentration is low and the defect state density is low is referred to as "high-purity intrinsic" or "substantially high-purity intrinsic". In addition, examples of impurities in the metal oxide include hydrogen, nitrogen, alkali metals, alkaline earth metals, iron, nickel, silicon, and the like.
[0252] In particular, since the hydrogen contained in the metal oxide reacts with the oxygen bonded to the metal atom to become water, oxygen vacancies are sometimes formed in the metal oxide. When the channel formation region in the metal oxide includes oxygen vacancies, the transistor sometimes has a normally-on characteristic. Furthermore, sometimes the defects formed by hydrogen entering the oxygen vacancies are used as donors to generate electrons as carriers. In addition, sometimes a part of the hydrogen is bonded to the oxygen bonded to the metal atom to generate electrons as carriers. Therefore, transistors using metal oxides containing a large amount of hydrogen tend to have normally-on characteristics.
[0253] Defects in which hydrogen enters oxygen vacancies may be used as donors for metal oxides. However, it is difficult to quantitatively evaluate this defect. Therefore, in metal oxides, evaluation is sometimes performed not by donor concentration but by carrier concentration. Therefore, in this specification, etc., sometimes as a parameter of the metal oxide, instead of using donor concentration, carrier concentration assuming a state where no electric field is applied is used. That is, the "carrier concentration" recorded in this specification, etc. may sometimes be referred to as "donor concentration".
[0254] Therefore, it is preferable to reduce the amount of hydrogen in the metal oxide as much as possible. Specifically, in the metal oxide, the hydrogen concentration measured by secondary ion mass spectrometry (SIMS) is less than 1×10 20 atoms / cm 3 , preferably less than 1×10 19 atoms / cm 3 , more preferably less than 5×10 18 atoms / cm 3 , and more preferably less than 1×10 18 atoms / cm 3 By using a metal oxide in which impurities such as hydrogen are sufficiently reduced in the channel formation region of a transistor, the transistor can have stable electrical characteristics.
[0255] The carrier concentration of the metal oxide in the channel formation region is preferably 1×10 18 cm -3 Below, more preferably below 1×10 17 cm -3 , and more preferably less than 1×1016 cm -3 , and further preferably less than 1×10 13 cm -3 , and further preferably less than 1×10 12 cm -3 Note that there is no particular restriction on the lower limit of the carrier concentration of the metal oxide in the channel formation region, and it may be, for example, 1×10 - 9-3 cm.
[0256] The semiconductor layer 108 preferably has a non-single crystal structure. The non-single crystal structure includes, for example, a CAAC structure, a polycrystalline structure, a microcrystalline structure, or an amorphous structure described below. Among the non-single crystal structures, the amorphous structure has the highest defect state density, and the CAAC structure has the lowest defect state density.
[0257] CAAC (c-axis aligned crystal) is described below. CAAC is an example of a crystal structure.
[0258] The CAAC structure refers to one of the crystalline structures of a thin film including a plurality of nanocrystals (a crystalline region with a maximum diameter of less than 10 nm), and has the following characteristics: the c-axis of each nanocrystal is oriented in a specific direction, the a-axis and the b-axis thereof are not oriented, and the nanocrystals are continuously connected without forming grain boundaries. In particular, in a thin film having a CAAC structure, the c-axis of each nanocrystal is easily oriented in the thickness direction of the thin film, the normal direction of the formed surface, or the normal direction of the thin film surface.
[0259] CAAC-OS (Oxide Semiconductor) is an oxide semiconductor with high crystallinity. On the other hand, no clear grain boundaries are observed in CAAC-OS, so the decrease in electron mobility caused by grain boundaries is not likely to occur. In addition, the crystallinity of oxide semiconductors is sometimes reduced due to the mixing of impurities or the generation of defects, so it can be said that CAAC-OS is an oxide semiconductor with few impurities or defects (oxygen vacancies, etc.). Therefore, the physical properties of oxide semiconductors containing CAAC-OS are stable. Therefore, oxide semiconductors containing CAAC-OS have high heat resistance and high reliability.
[0260] In the unit lattice of crystallography, the c-axis is generally the more special axis among the three axes (crystal axes) constituting the unit lattice, namely, the a-axis, the b-axis, and the c-axis. In particular, in a crystal having a layered structure, generally speaking, the two axes parallel to the plane direction of the layer are the a-axis and the b-axis, and the axis intersecting the layer is the c-axis. As a typical example of such a crystal having a layered structure, there is graphite classified as a hexagonal system, in which the a-axis and the b-axis of the unit lattice are parallel to the cleavage plane, and the c-axis is orthogonal to the cleavage plane. For example, a crystal of InGaZnO4 with a layered structure and a YbFe2O4 type crystal structure can be classified as a hexagonal system, in which the a-axis and the b-axis of the unit lattice are parallel to the plane direction of the layer, and the c-axis is orthogonal to the layer (i.e., the a-axis and the b-axis).
[0261] In an oxide semiconductor film having a microcrystalline structure (microcrystalline oxide semiconductor film), the crystal part cannot be clearly confirmed in the image observed by TEM. The size of the crystal part contained in the microcrystalline oxide semiconductor film is mostly greater than 1nm and less than 100nm or greater than 1nm and less than 10nm. In particular, an oxide semiconductor film having nanocrystals (nc: nanocrystal) with a size of greater than 1nm and less than 10nm or greater than 1nm and less than 3nm is called an nc-OS (nanocrystalline Oxide Semiconductor) film. For example, when observing an nc-OS film using TEM, the grain boundary cannot be clearly confirmed.
[0262] In the nc-OS film, the atomic arrangement in a tiny area (for example, an area above 1 nm and below 10 nm, especially an area above 1 nm and below 3 nm) has periodicity. In addition, the regularity of the crystal orientation is not observed between different crystalline parts of the nc-OS film. Therefore, no orientation is observed in the entire film. Therefore, sometimes the nc-OS film is no different from the amorphous oxide semiconductor film in certain analysis methods. For example, when the nc-OS film is structurally analyzed by the out-of-plane method of an XRD device using X-rays whose beam diameter is larger than the crystalline part, no peak representing the crystalline plane is detected. In addition, in the electron diffraction pattern (also called selected area electron diffraction pattern) of the nc-OS film obtained using electron rays whose beam diameter is larger than the crystalline part (for example, more than 50 nm), a halo pattern is observed. On the other hand, when the nc-OS film is subjected to electron diffraction (also called nanobeam electron diffraction) using an electron beam whose electron beam diameter is close to the size of the crystalline portion or smaller than the crystalline portion (for example, greater than 1 nm and less than 30 nm), a ring-shaped (annular) area with high brightness is observed, and sometimes multiple spots are observed within the annular area.
[0263] The defect state density of the nc-OS film is lower than that of the amorphous oxide semiconductor film. However, the regularity of the crystal orientation is not observed between different crystalline parts of the nc-OS film. Therefore, the defect state density of the nc-OS film is higher than that of the CAAC-OS film. Therefore, the nc-OS film sometimes has a higher carrier concentration and electron mobility than the CAAC-OS film. As a result, transistors using the nc-OS film sometimes have a higher field effect mobility.
[0264] The nc-OS film can be formed at a smaller oxygen flow rate ratio than when the CAAC-OS film is formed. In addition, the nc-OS film can be formed at a lower substrate temperature than when the CAAC-OS film is formed. For example, the nc-OS film can be formed when the substrate temperature is a relatively low temperature (e.g., a temperature below 130°C) or when the substrate is not heated, so it is suitable for large glass substrates, resin substrates, etc., and can improve productivity.
[0265] Below, an example of the crystal structure of a metal oxide is described. Note that a metal oxide formed by sputtering using an In-Ga-Zn oxide target (In:Ga:Zn=4:2:4.1 [atomic number ratio]) is used as an example for description. The metal oxide formed by sputtering using the above target at a substrate temperature of 100°C or higher and 130°C or lower tends to have a crystal structure of either a nc (nano crystal) structure or a CAAC structure, or a mixed structure thereof. The metal oxide formed by sputtering at a substrate temperature of room temperature (RT) tends to have a nc crystal structure. Note that the room temperature (RT) here refers to a temperature including a temperature when the substrate is not heated.
[0266] <Composition of Metal Oxide> Hereinafter, a configuration of a CAC (Cloud-Aligned Composite)-OS that can be used for a transistor disclosed in one embodiment of the present invention will be described.
[0267] In this specification, CAAC (c-axis aligned crystal) or CAC (Cloud-Aligned Composite) may be described. Note that CAAC is an example of a crystal structure, and CAC is an example of a function or a material configuration.
[0268] CAC-OS or CAC-metal oxide has a conductive function in a part of the material, an insulating function in another part of the material, and has a semiconductor function as a whole. In addition, when CAC-OS or CAC-metal oxide is used in the active layer of a transistor, the conductive function is to allow electrons (or holes) used as carriers to flow through, and the insulating function is to prevent electrons used as carriers from flowing through. Through the complementary effects of the conductive function and the insulating function, CAC-OS or CAC-metal oxide can have a switching function (a function of controlling on / off). By separating each function in CAC-OS or CAC-metal oxide, each function can be maximized.
[0269] In addition, CAC-OS or CAC-metal oxide includes a conductive region and an insulating region. The conductive region has the function of the above-mentioned conductivity, and the insulating region has the function of the above-mentioned insulation. In addition, in the material, the conductive region and the insulating region are sometimes separated with a nanoparticle level. In addition, the conductive region and the insulating region are sometimes distributed unevenly in the material. In addition, sometimes the conductive region whose edge is fuzzy and connected with a cloud shape is observed.
[0270] In CAC-OS or CAC-metal oxide, the conductive region and the insulating region may be dispersed in the material with a size of 0.5 nm to 10 nm, preferably 0.5 nm to 3 nm.
[0271] In addition, CAC-OS or CAC-metal oxide is composed of components with different band gaps. For example, CAC-OS or CAC-metal oxide is composed of a component with a wide gap caused by an insulating region and a component with a narrow gap caused by a conductive region. In this structure, when carriers are allowed to flow through, the carriers mainly flow through the component with the narrow gap. In addition, the component with a narrow gap complements the component with a wide gap, and the carriers flow through the component with the wide gap in conjunction with the component with the narrow gap. Therefore, when the above-mentioned CAC-OS or CAC-metal oxide is used in the channel formation region of a transistor, a high current driving force, that is, a large on-state current and a high field effect mobility can be obtained in the on state of the transistor.
[0272] That is, CAC-OS or CAC-metal oxide may also be referred to as a matrix composite material (matrix composite) or a metal matrix composite material (metal matrix composite).
[0273] The above is the description of the components.
[0274] At least a part of this embodiment mode can be implemented in combination with other embodiment modes described in this specification as appropriate.
[0275] (Implementation Method 2) In this embodiment, an example of a display device including the transistor described as an example in the above embodiment will be described.
[0276] <Structure example> Fig. 12A 7 shows a top view of a display device 700. The display device 700 includes a first substrate 701 and a second substrate 705 bonded together by a sealant 712. In a region sealed by the first substrate 701, the second substrate 705, and the sealant 712, a pixel portion 702, a source driver circuit portion 704, and a gate driver circuit portion 706 are provided on the first substrate 701. The pixel portion 702 is provided with a plurality of display elements.
[0277] In addition, a portion of the first substrate 701 that does not overlap with the second substrate 705 is provided with an FPC terminal portion 708 connected to an FPC 716 (FPC: Flexible printed circuit). The FPC 716 provides various signals to the pixel portion 702, the source driver circuit portion 704, and the gate driver circuit portion 706 through the FPC terminal portion 708 and the signal line 710.
[0278] A plurality of gate drive circuits 706 may be provided. In addition, the gate drive circuit 706 and the source drive circuit 704 may be separately formed on a semiconductor substrate or the like, or may be packaged as an IC chip. The IC chip may be mounted on the first substrate 701 or mounted on the FPC 716.
[0279] As transistors included in the pixel portion 702 , the source driver circuit portion 704 , and the gate driver circuit portion 706 , transistors of the semiconductor device of one embodiment of the present invention can be used.
[0280] As display elements provided in the pixel portion 702, liquid crystal elements, light-emitting elements, etc. can be cited. As liquid crystal elements, transmissive liquid crystal elements, reflective liquid crystal elements, semi-transmissive liquid crystal elements, etc. can be used. In addition, as light-emitting elements, self-luminous light-emitting elements such as LED (Light Emitting Diode), OLED (Organic LED), QLED (Quantum-dot LED), semiconductor lasers, etc. can be cited. In addition, MEMS (Micro Electro Mechanical Systems) elements of a shutter method or an optical interference method, or display elements using a microcapsule method, an electrophoresis method, an electrowetting method, or an electronic powder fluid (registered trademark) method, etc. can be used.
[0281] Fig. 12B The display device 700A shown is an example of a display device that can be used as a flexible display using a resin layer 743 having flexibility instead of the first substrate 701.
[0282] The pixel portion 702 of the display device 700A is not a rectangular shape but has arc-shaped corners. Fig. 12B As shown in the region P1 in FIG. 1 , the pixel portion 702 and a portion of the resin layer 743 have a cutout portion. A pair of gate drive circuit portions 706 are provided on both sides of the pixel portion 702. The gate drive circuit portion 706 is provided at the corner of the pixel portion 702 along the inner side of the arc-shaped contour.
[0283] The portion of the resin layer 743 provided with the FPC terminal portion 708 protrudes. The portion of the resin layer 743 including the FPC terminal portion 708 may be along Fig. 12B By folding a portion of the resin layer 743 to the back, the display device 700A can be mounted on an electronic device in a state where the FPC 716 and the back of the pixel portion 702 are overlapped, thereby saving space in the electronic device.
[0284] In addition, the FPC 716 connected to the display device 700A is mounted with an IC 717. The IC 717 has, for example, a function of a source driver circuit. Here, the source driver circuit unit 704 in the display device 700A may have a structure including at least one of a protection circuit, a buffer circuit, a demultiplexer circuit, and the like.
[0285] Fig. 12C The display device 700B shown is a display device suitable for electronic devices with a large screen. For example, the display device 700B can be suitable for television devices, monitor devices, personal computers (including notebook and desktop), tablet terminals, digital signage, etc.
[0286] The display device 700B includes a plurality of source driver ICs 721 and a pair of gate driver circuit units 722 .
[0287] A plurality of source driver ICs 721 are mounted on the FPCs 723. In addition, one terminal of each of the FPCs 723 is connected to the first substrate 701, and another terminal is connected to the printed circuit board 724. By bending the FPCs 723, the printed circuit board 724 can be arranged on the back side of the pixel portion 702 and installed in the electronic device, thereby reducing the space for installing the electronic device.
[0288] On the other hand, the gate driving circuit portion 722 is formed on the first substrate 701. Thus, an electronic device with a narrow frame can be realized.
[0289] By adopting the above structure, a large and high-resolution display device can be realized. For example, a display device with a screen size of 30 inches or more, 40 inches or more, 50 inches or more, or 60 inches or more can be realized. In addition, a display device with extremely high resolution such as 4K2K and 8K4K can be realized.
[0290] <Cross-sectional structure example> Refer to the following Figures 13 to 16 A structure using a liquid crystal element and a structure using an EL element as a display element are described. Figures 13 to 15 are respectively along Fig. 12A A cross-sectional view along the dashed line QR is shown. Fig.16 It is along Fig. 12B A cross-sectional view taken along dashed line ST in the display device 700A is shown. Fig.13 and Fig.14 This is a structure that uses a liquid crystal element as a display element. Fig.15 and Fig.16 This is a structure using EL elements.
[0291] [Description of Common Parts of Display Devices] Figures 13 to 16 The display device shown includes a routing wiring section 711, a pixel section 702, a source driver circuit section 704, and an FPC terminal section 708. The routing wiring section 711 includes a signal line 710. The pixel section 702 includes a transistor 750 and a capacitor 790. The source driver circuit section 704 includes a transistor 752. Fig.14 A case where the capacitor 790 is not included is shown.
[0292] The transistor 750 and the transistor 752 can use the transistor described in Embodiment 1.
[0293] The transistor used in this embodiment includes a highly purified oxide semiconductor film in which the formation of oxygen vacancies is suppressed. The transistor can have a low off-state current. Therefore, the retention time of an electrical signal such as an image signal can be extended, and the writing interval of the image signal can be extended. Therefore, the frequency of the refresh operation can be reduced, thereby achieving the effect of reducing power consumption.
[0294] In addition, the transistor used in this embodiment can obtain a higher field effect mobility, so it can be driven at high speed. For example, by using such a transistor capable of high-speed driving in a display device, a switching transistor of a pixel portion and a driving transistor for a driving circuit portion can be formed on the same substrate. That is, a structure that does not use a driving circuit formed by a silicon wafer or the like can be adopted, thereby reducing the number of components of the display device. In addition, by also using a transistor capable of high-speed driving in the pixel portion, a high-quality image can be provided.
[0295] Fig.13 , Fig.15 and Fig.16 The capacitor 790 shown includes a lower electrode formed by processing the same film as the first gate electrode included in the transistor 750 and an upper electrode formed by processing the same metal oxide as the semiconductor layer. The upper electrode is low-resistance in the same manner as the source region and the drain region of the transistor 750. In addition, a portion of an insulating film used as a first gate insulating layer of the transistor 750 is provided between the lower electrode and the upper electrode. That is, the capacitor 790 has a stacked structure in which an insulating film used as a dielectric film is sandwiched between a pair of electrodes. In addition, the upper electrode is connected to a wiring formed by processing the same film as the source electrode and the drain electrode of the transistor.
[0296] In addition, a planarization insulating film 770 is provided over the transistor 750 , the transistor 752 , and the capacitor 790 .
[0297] In addition, the transistor 750 included in the pixel portion 702 and the transistor 752 included in the source driver circuit portion 704 may also use transistors of different structures. For example, a structure in which one side uses a top-gate transistor and the other side uses a bottom-gate transistor may be adopted. In addition, the gate driver circuit portion 706 is also the same as the source driver circuit portion 704.
[0298] The signal line 710 is formed of the same conductive film as the source electrode and the drain electrode of the transistors 750 and 752. Here, a low-resistance material such as a material containing copper is preferably used, thereby reducing signal delay caused by wiring resistance, thereby achieving large-screen display.
[0299] The FPC terminal portion 708 includes a wiring 760, a portion of which is used as a connection electrode, an anisotropic conductive film 780, and an FPC 716. The wiring 760 is electrically connected to the terminal of the FPC 716 via the anisotropic conductive film 780. Here, the wiring 760 is formed of the same conductive film as the source electrode and the drain electrode of the transistors 750 and 752.
[0300] A flexible substrate such as a glass substrate or a plastic substrate can be used as the first substrate 701 and the second substrate 705. When a flexible substrate is used as the first substrate 701, an insulating layer having a barrier property against water or hydrogen is preferably provided between the first substrate 701 and the transistor 750 or the like.
[0301] A light-shielding film 738, a coloring film 736, and an insulating film 734 in contact with these are provided on the second substrate 705 side.
[0302] [Structural Example of Display Device Using Liquid Crystal Element] Fig.13 The display device 700 shown includes a liquid crystal element 775 and a spacer 778. The liquid crystal element 775 includes a conductive layer 772, a conductive layer 774, and a liquid crystal layer 776 between the conductive layer 772 and the conductive layer 774. The conductive layer 774 is provided on the side of the second substrate 705 and serves as a common electrode. In addition, the conductive layer 772 is electrically connected to a source electrode or a drain electrode included in the transistor 750. The conductive layer 772 is formed on the planarization insulating film 770 and serves as a pixel electrode.
[0303] A material that is translucent or reflective to visible light can be used for the conductive layer 772. As the translucent material, for example, an oxide material containing indium, zinc, tin, or the like can be used. As the reflective material, for example, a material containing aluminum, silver, or the like can be used.
[0304] When a reflective material is used as the conductive layer 772, the display device 700 is a reflective liquid crystal display device. On the other hand, when a light-transmitting material is used as the conductive layer 772, the display device 700 is a transmissive liquid crystal display device. In the case of a reflective liquid crystal display device, a polarizing plate is provided on the viewing side. On the other hand, in the case of a transmissive liquid crystal display device, a pair of polarizing plates are provided so as to sandwich a liquid crystal element.
[0305] Fig.14 The display device 700 shown in the figure shows an example of a liquid crystal element 775 using a lateral electric field method (for example, FFS mode). A conductive layer 774 serving as a common electrode is provided on the conductive layer 772 via an insulating layer 773. The alignment state of the liquid crystal layer 776 can be controlled by an electric field generated between the conductive layer 772 and the conductive layer 774.
[0306] exist Fig.14 In the embodiment, a storage capacitor can be formed by a stacked structure of a conductive layer 774, an insulating layer 773, and a conductive layer 772. Therefore, there is no need to provide a separate capacitor, and the aperture ratio can be increased.
[0307] In addition, although Fig.13 and Fig.14 Although not shown in the figure, an alignment film may be provided in contact with the liquid crystal layer 776. In addition, an optical member (optical substrate) such as a polarizing member, a phase difference member, an antireflection member, and a light source such as a backlight or a sidelight may be provided as appropriate.
[0308] The liquid crystal layer 776 may use thermotropic liquid crystal, low molecular liquid crystal, polymer liquid crystal, polymer dispersed liquid crystal (PDLC: Polymer Dispersed Liquid Crystal), polymer network liquid crystal (PNLC: Polymer Network Liquid Crystal), ferroelectric liquid crystal, antiferroelectric liquid crystal, etc. In addition, when the transverse electric field method is adopted, liquid crystal exhibiting a blue phase that does not require an alignment film may also be used.
[0309] As the mode of the liquid crystal element, a TN (Twisted Nematic) mode, a VA (Vertical Alignment) mode, an IPS (In-Plane-Switching) mode, an FFS (Fringe Field Switching) mode, an ASM (Axially Symmetric aligned Micro-cell) mode, an OCB (Optically Compensated Birefringence) mode, an ECB (Electrically Controlled Birefringence) mode, a guest-host mode, or the like can be used.
[0310] The liquid crystal layer 776 may be a dispersed liquid crystal using polymer dispersed liquid crystal, polymer network liquid crystal, or the like. In this case, a structure may be used for black and white display without providing the color film 736, or a structure may be used for color display using the color film 736.
[0311] In addition, as a driving method of the liquid crystal element, a time-sharing display method (also called a field sequential driving method) that uses a sequential additive color mixing method to perform color display can be applied. In this case, a structure without a color film 736 can be adopted. When the time-sharing display method is adopted, for example, there is no need to provide sub-pixels that respectively display R (red), G (green), and B (blue), so there is an advantage that the aperture ratio and resolution of the pixel can be improved.
[0312] [Display device using light-emitting element] Fig.15 The display device 700 shown includes a light-emitting element 782. The light-emitting element 782 includes a conductive layer 772, an EL layer 786, and a conductive film 788. The EL layer 786 includes an organic compound or an inorganic compound such as quantum dots.
[0313] Examples of materials that can be used for the organic compound include fluorescent materials and phosphorescent materials, etc. Examples of materials that can be used for quantum dots include colloidal quantum dot materials, alloy quantum dot materials, core-shell quantum dot materials, and core-type quantum dot materials.
[0314] Fig.15 The display device 700 shown in the figure has an insulating film 730 covering a portion of a conductive layer 772 on a planarizing insulating film 770. Here, the light emitting element 782 includes a light-transmitting conductive film 788 and is a top-emitting light emitting element. Alternatively, the light emitting element 782 may have a bottom-emitting structure that emits light to the conductive layer 772 side or a double-sided emission structure that emits light to both the conductive layer 772 side and the conductive film 788 side.
[0315] The coloring film 736 is provided at a position overlapping with the light emitting element 782, and the light shielding film 738 is provided at a position overlapping with the insulating film 730, in the routing wiring portion 711, and in the source driver circuit portion 704. In addition, the coloring film 736 and the light shielding film 738 are covered by the insulating film 734. In addition, the space between the light emitting element 782 and the insulating film 734 is filled with the sealing film 732. In addition, when the EL layer 786 is formed in an island shape in each pixel or in a strip shape in each pixel column, that is, by separate coating, a structure without providing the coloring film 736 may be adopted.
[0316] Fig.16 The structure of a display device suitable for a flexible display is shown. Fig.16 It is along Fig. 12B A cross-sectional view taken along dashed line ST in the display device 700A is shown.
[0317] Fig.16The display device 700A shown in the figure adopts a stacked structure of a supporting substrate 745, an adhesive layer 742, a resin layer 743 and an insulating layer 744 instead of Fig.15 The first substrate 701 is shown. The transistor 750, the capacitor 790, and the like are provided on an insulating layer 744 formed on a resin layer 743.
[0318] The support substrate 745 is a flexible thin substrate including an organic resin, glass, or the like. The resin layer 743 is a layer of an organic resin including polyimide, acrylic resin, or the like. The insulating layer 744 includes an inorganic insulating film including silicon oxide, silicon oxynitride, silicon nitride, or the like. The resin layer 743 and the support substrate 745 are bonded together by an adhesive layer 742. The resin layer 743 is preferably thinner than the support substrate 745.
[0319] Fig.16 The display device 700 shown includes a protective layer 740 instead of Fig.15 The substrate 705 shown. The protective layer 740 is bonded to the sealing film 732. The protective layer 740 may be a glass substrate, a resin film, etc. In addition, the protective layer 740 may also be an optical component such as a polarizing plate, a scattering plate, an input device such as a touch sensor panel, or a stacked structure of two or more of the above.
[0320] The EL layer 786 included in the light-emitting element 782 is provided in an island shape on the insulating film 730 and the conductive layer 772. By forming the EL layer 786 separately in a manner that the luminescent color in each sub-pixel is different, color display can be achieved without using the coloring film 736. In addition, a protective layer 741 is provided to cover the light-emitting element 782. The protective layer 741 can prevent impurities such as water from diffusing into the light-emitting element 782. The protective layer 741 is preferably an inorganic insulating film. In addition, it is more preferable to adopt a stacked structure in which the inorganic insulating film and the organic insulating film are each one or more.
[0321] Fig.16 7 shows a foldable region P2. The region P2 includes a portion where no inorganic insulating film such as a supporting substrate 745, an adhesive layer 742, and an insulating layer 744 is provided. In addition, in the region P2, a resin layer 746 is provided to cover the wiring 760. By not providing an inorganic insulating film in the foldable region P2 as much as possible and adopting a structure in which only a conductive layer containing a metal or alloy and a layer containing an organic material are stacked, cracks can be prevented from being generated when the display device 700A is bent. In addition, by not providing a supporting substrate 745 in the region P2, a portion of the display device 700A can be bent with an extremely small radius of curvature.
[0322] [Configuration Example of Providing Input Device in Display Device] In addition, you can also Figures 13 to 16 The display device shown is provided with an input device. As the input device, for example, a touch sensor or the like can be cited.
[0323] For example, various sensor types may be used, such as electrostatic capacitance type, resistance film type, surface acoustic wave type, infrared type, optical type, pressure sensitive type, etc. Furthermore, two or more of the above types may be used in combination.
[0324] In addition, touch panels have the following structures: so-called In-Cell touch panels in which the input device is formed between a pair of substrates; so-called On-Cell touch panels in which the input device is formed on the display device; so-called Out-Cell touch panels in which the input device is bonded to the display device; and so on.
[0325] At least a part of the structural examples described in this embodiment mode and the drawings and the like corresponding to these examples can be implemented in combination with other structural examples, drawings and the like as appropriate.
[0326] At least a part of this embodiment mode can be implemented in combination with other embodiment modes described in this specification as appropriate.
[0327] (Implementation 3) In this embodiment, a display device including a semiconductor device which is one embodiment of the present invention is described with reference to FIG. 17 .
[0328] Fig.17A The display device shown in FIG. 5 includes a pixel portion 502, a driver circuit portion 504, a protection circuit 506, and a terminal portion 507. Note that a structure without providing the protection circuit 506 may also be adopted. Fig.17A In order to distinguish the protection circuit 506 from the pixel circuit 501, the pixel circuit 501 is shaded.
[0329] The transistor of one embodiment of the present invention can be used as a transistor included in the pixel portion 502 or the driver circuit portion 504. Furthermore, the transistor of one embodiment of the present invention can be used for the protection circuit 506.
[0330] The pixel portion 502 includes a plurality of pixel circuits 501 that drive a plurality of display elements arranged in X rows and Y columns (X and Y are each an independent natural number of 2 or more).
[0331] The driving circuit unit 504 includes a gate driver 504a that outputs scanning signals to the scanning lines GL_1 to GL_X, a source driver 504b that supplies data signals to the data lines DL_1 to DL_Y, and other driving circuits. The gate driver 504a may be configured to include at least a shift register. In addition, the source driver 504b may be configured to include, for example, a plurality of analog switches. In addition, the source driver 504b may also be configured to include a shift register.
[0332] The terminal portion 507 is a portion where terminals for inputting power, control signals, image signals, and the like from an external circuit to the display device are provided.
[0333] The protection circuit 506 is a circuit that causes the wiring connected thereto to be in a conductive state with other wirings when a potential outside a certain range is supplied thereto. Fig.17A The protection circuit 506 shown is connected to various wirings such as scanning lines GL_1 to GL_X between the gate driver 504 a and the pixel circuit 501 or data lines DL_1 to DL_Y between the source driver 504 b and the pixel circuit 501 .
[0334] In addition, a structure in which the gate driver 504a and the source driver 504b are each arranged on the same substrate as the pixel portion 502 can be adopted, or a structure in which another substrate having a gate driving circuit or a source driving circuit formed thereon (for example, a driving circuit board formed using a single crystal semiconductor or a polycrystalline semiconductor) is installed on the substrate using COG or TAB (Tape Automated Bonding) can be adopted.
[0335] also, Fig.17A The plurality of pixel circuits 501 shown may be, for example, Fig. 17B , Fig. 17C The structure shown.
[0336] Fig. 17B The pixel circuit 501 shown includes a liquid crystal element 570, a transistor 550, and a capacitor 560. In addition, the pixel circuit 501 is connected to a data line DL_n, a scanning line GL_m, a potential supply line VL, and the like.
[0337] The potential of one of the pair of electrodes of the liquid crystal element 570 is appropriately set according to the specification of the pixel circuit 501. The orientation state of the liquid crystal element 570 is set according to the written data. In addition, a common potential may be supplied to one of the pair of electrodes of the liquid crystal element 570 included in each of the plurality of pixel circuits 501. In addition, a different potential may be supplied to one of the pair of electrodes of the liquid crystal element 570 included in each of the pixel circuits 501 of each row.
[0338] Fig. 17C The pixel circuit 501 shown includes transistors 552 and 554, a capacitor 562, and a light emitting element 572. In addition, the pixel circuit 501 is connected to a data line DL_n, a scanning line GL_m, a potential supply line VL_a, a potential supply line VL_b, and the like.
[0339] In addition, a high power supply potential VDD is applied to one of the potential supply lines VL_a and VL_b, and a low power supply potential VSS is applied to the other. According to the potential applied to the gate of the transistor 554, the current flowing through the light emitting element 572 is controlled, thereby controlling the brightness of light emitted from the light emitting element 572.
[0340] At least a part of the structural examples described in this embodiment mode and the drawings and the like corresponding to these examples can be implemented in combination with other structural examples, drawings and the like as appropriate.
[0341] At least a part of this embodiment mode can be implemented in combination with other embodiment modes described in this specification as appropriate.
[0342] (Implementation 4) A pixel circuit including a memory for correcting grayscale displayed by a pixel and a display device including the pixel circuit are described below. The transistor described in Embodiment Mode 1 can be used as a transistor used in a pixel circuit described below.
[0343] <Circuit Structure> Fig.18A : shows a circuit diagram of a pixel circuit 400. The pixel circuit 400 includes a transistor M1, a transistor M2, a capacitor C1, and a circuit 401. In addition, the pixel circuit 400 is connected to a wiring S1, a wiring S2, a wiring G1, and a wiring G2.
[0344] The gate of the transistor M1 is connected to the wiring G1, one of the source and the drain is connected to the wiring S1, and the other of the source and the drain is connected to one electrode of the capacitor C1. The gate of the transistor M2 is connected to the wiring G2, one of the source and the drain is connected to the wiring S2, and the other of the source and the drain is connected to the other electrode of the capacitor C1 and the circuit 401.
[0345] The circuit 401 includes at least one display element. Various elements can be used as the display element, and typically, a light-emitting element such as an organic EL element or an LED element, a liquid crystal element, or a MEMS (Micro Electro Mechanical Systems) element can be used.
[0346] A node connecting the transistor M1 and the capacitor C1 is referred to as a node N1 , and a node connecting the transistor M2 and the circuit 401 is referred to as a node N2 .
[0347] The pixel circuit 400 can maintain the potential of the node N1 by turning off the transistor M1. In addition, the potential of the node N2 can be maintained by turning off the transistor M2. In addition, when a predetermined potential is written to the node N1 through the transistor M1 while the transistor M2 is in the off state, the potential of the node N2 can be changed in accordance with the potential change of the node N1 due to capacitive coupling through the capacitor C1.
[0348] Here, as one or both of the transistor M1 and the transistor M2, the transistor using an oxide semiconductor illustrated in Embodiment 1 can be used. Since the transistor has an extremely low off-state current, the potentials of the nodes N1 and N2 can be maintained for a long time. In addition, when the potential holding period of each node is short (specifically, when the frame frequency is 30 Hz or more, etc.), a transistor using a semiconductor such as silicon can also be used.
[0349] <Drive method example> Next, refer to Fig.18B An example of an operation method of the pixel circuit 400 will be described. Fig.18B 4 is a timing chart of the operation of the pixel circuit 400. Note that for the sake of convenience, the influence of various resistances such as wiring resistance, parasitic capacitance of transistors and wiring, and threshold voltage of transistors are not considered here.
[0350] exist Fig.18B In the operation shown, one frame period is divided into a period T1 and a period T2. The period T1 is a period for writing a potential to the node N2, and the period T2 is a period for writing a potential to the node N1.
[0351] [Period T1] During the period T1, a potential that turns on the transistor is supplied to both the wiring G1 and the wiring G2. In addition, a fixed potential V is supplied to the wiring S1. ref , providing the first data potential V to the wiring S2 w .
[0352] The node N1 is supplied with a potential V from the wiring S1 via the transistor M1. ref In addition, the node N2 is supplied with the first data potential V from the wiring S2 through the transistor M2. w Therefore, capacitor C1 becomes to maintain the potential difference V w -V ref status.
[0353] [Period T2] Next, in period T2, a potential for turning on the transistor M1 is supplied to the wiring G1, and a potential for turning off the transistor M2 is supplied to the wiring G2. The second data potential V dataIn addition, the wiring S2 may be supplied with a predetermined constant potential or may be in a floating state.
[0354] The node N1 is supplied with the second data potential V from the wiring S1 through the transistor M1. data At this time, due to the capacitive coupling through the capacitor C1, the corresponding second data potential V data The potential of the node N2 changes by a potential dV. That is, the circuit 401 receives the first data potential V w The potential added to the potential dV. Note that although Fig.18B The potential dV is shown as a positive value, but it can also be a negative value. data It can also be compared with the second data potential V ref Low.
[0355] Here, the potential dV is basically determined by the capacitance value of the capacitor C1 and the capacitance value of the circuit 401. When the capacitance value of the capacitor C1 is sufficiently larger than the capacitance value of the circuit 401, the potential dV becomes close to the second data potential V data The potential.
[0356] As described above, since the pixel circuit 400 can combine two types of data signals to generate a potential supplied to the circuit 401 including a display element, grayscale correction can be performed within the pixel circuit 400 .
[0357] In addition, the pixel circuit 400 can generate a potential exceeding the maximum potential that can be supplied to the wiring S1 and the wiring S2. For example, when a light-emitting element is used, high dynamic range (HDR) display can be performed. In addition, when a liquid crystal element is used, overdrive can be achieved.
[0358] <Application Examples> [Example of using liquid crystal element] Fig.18C The pixel circuit 400LC shown includes a circuit 401LC. The circuit 401LC includes a liquid crystal element LC and a capacitor C2.
[0359] One electrode of the liquid crystal element LC is connected to the other electrode of the capacitor C1, the other of the source and drain of the transistor M2, and one electrode of the capacitor C2, and the other electrode is connected to the potential V com2 The other electrode of capacitor C2 is connected to the supply potential V com1 Wiring connections.
[0360] Capacitor C2 is used as a storage capacitor. In addition, capacitor C2 can be omitted when not needed.
[0361] Since the pixel circuit 400LC can provide a high voltage to the liquid crystal element LC, high-speed display can be achieved by overdriving, and a liquid crystal material with a high driving voltage can be used. In addition, by providing a correction signal to the wiring S1 or the wiring S2, grayscale correction can be performed according to the use temperature or the degradation state of the liquid crystal element LC.
[0362] [Example of using light emitting element] Fig.18D The pixel circuit 400EL shown includes a circuit 401EL. The circuit 401EL includes a light emitting element EL, a transistor M3, and a capacitor C2.
[0363] The gate of the transistor M3 is connected to one electrode of the capacitor C2, and one of the source and the drain is connected to the supplied potential V H The other of the source and drain is connected to one electrode of the light emitting element EL. The other electrode of the capacitor C2 is connected to the supply potential V com The other electrode of the light emitting element EL is connected to the wiring supplied with the potential V L Wiring connections.
[0364] The transistor M3 has a function of controlling the current supplied to the light emitting element EL. The capacitor C2 is used as a storage capacitor. The capacitor C2 may be omitted when not required.
[0365] In addition, although the structure in which the anode side of the light emitting element EL is connected to the transistor M3 is shown here, a structure in which the cathode side is connected to the transistor M3 may also be adopted. In this case, the potential V H With potential V L The value of .
[0366] In the pixel circuit 400EL, a large current can flow through the light emitting element EL by applying a high potential to the gate of the transistor M3, so that HDR display can be realized. In addition, by providing a correction signal to the wiring S1 or the wiring S2, the electrical characteristic deviation of the transistor M3 and the light emitting element EL can be corrected.
[0367] In addition, not limited to Fig.18C and Fig.18D The circuit shown may also adopt a structure in which transistors or capacitors are additionally added.
[0368] At least a part of this embodiment mode can be implemented in combination with other embodiment modes described in this specification as appropriate.
[0369] (Implementation 5) In this embodiment, a display module that can be manufactured using one embodiment of the present invention is described.
[0370] Fig.19A The display module 6000 shown includes a display device 6006 connected to an FPC 6005 , a frame 6009 , a printed circuit board 6010 , and a battery 6011 between an upper cover 6001 and a lower cover 6002 .
[0371] For example, a display device manufactured using one embodiment of the present invention can be used as the display device 6006. By using the display device 6006, a display module with extremely low power consumption can be implemented.
[0372] The shapes and sizes of the upper cover 6001 and the lower cover 6002 may be appropriately changed according to the size of the display device 6006 .
[0373] The display device 6006 may also function as a touch panel.
[0374] The frame 6009 has a function of protecting the display device 6006, a function of blocking electromagnetic waves generated by the operation of the printed circuit board 6010, a function of a heat sink, and the like.
[0375] The printed circuit board 6010 has a power supply circuit, a signal processing circuit for outputting a video signal and a clock signal, a battery control circuit, and the like.
[0376] Fig.19B FIG. 6 is a schematic cross-sectional view of a display module 6000 having an optical touch sensor.
[0377] The display module 6000 includes a light emitting portion 6015 and a light receiving portion 6016 provided on a printed circuit board 6010. In addition, a pair of light guide portions (light guide portion 6017a, light guide portion 6017b) are provided in the area surrounded by the upper cover 6001 and the lower cover 6002.
[0378] The display device 6006 overlaps with the printed circuit board 6010 and the battery 6011 via the frame 6009. The display device 6006 and the frame 6009 are fixed to the light guide portions 6017a and 6017b.
[0379] Light 6018 emitted from the light emitting unit 6015 passes through the light guiding unit 6017a, the upper part of the display device 6006, and the light guiding unit 6017b to reach the light receiving unit 6016. For example, when the light 6018 is blocked by a detection object such as a finger or a stylus pen, a touch operation can be detected.
[0380] For example, a plurality of light emitting units 6015 are provided along two adjacent sides of the display device 6006. A plurality of light receiving units 6016 are arranged at positions facing the light emitting units 6015. Thus, information on the position of the touch operation can be obtained.
[0381] As the light emitting unit 6015, for example, a light source such as an LED element can be used, and in particular, a light source that emits infrared rays is preferably used. As the light receiving unit 6016, a photoelectric element that receives the light emitted by the light emitting unit 6015 and converts it into an electrical signal can be used. Preferably, a photodiode that can receive infrared rays is used.
[0382] By using the light guide 6017a and the light guide 6017b that transmit the light 6018, the light emitting unit 6015 and the light receiving unit 6016 can be arranged on the lower side of the display device 6006, and it is possible to suppress the malfunction of the touch sensor caused by the external light reaching the light receiving unit 6016. In particular, it is preferable to use a resin that absorbs visible light and transmits infrared light, thereby more effectively suppressing the malfunction of the touch sensor.
[0383] At least a part of this embodiment mode can be implemented in combination with other embodiment modes described in this specification as appropriate.
[0384] (Implementation method 6) In this embodiment, an example of electronic equipment in which a display device according to one embodiment of the present invention can be used is described.
[0385] Fig. 20A The electronic device 6500 shown is a portable information terminal device that can be used as a smartphone.
[0386] The electronic device 6500 includes a housing 6501, a display portion 6502, a power button 6503, a button 6504, a speaker 6505, a microphone 6506, a camera 6507, a light source 6508, and the like. The display portion 6502 has a touch panel function.
[0387] As the display portion 6502 , a display device which is one embodiment of the present invention can be used.
[0388] Fig. 20B 65 is a schematic cross-sectional view of an end portion of a housing 6501 on one side of a microphone 6506 .
[0389] A light-transmitting protective component 6510 is provided on the display surface side of the housing 6501, and a display panel 6511, an optical component 6512, a touch sensor panel 6513, a printed circuit board 6517, a battery 6518, etc. are provided in the space surrounded by the housing 6501 and the protective component 6510.
[0390] The protection member 6510 is fixed to the display panel 6511 , the optical member 6512 , and the touch sensor panel 6513 via an adhesive layer (not shown).
[0391] A portion of the display panel 6511 is folded in a region outside the display portion 6502. The folded portion is connected to an FPC 6515. An IC 6516 is mounted on the FPC 6515. The FPC 6515 is connected to a terminal provided on a printed circuit board 6517.
[0392] The display panel 6511 may use a flexible display panel of one embodiment of the present invention. Thus, an extremely lightweight electronic device may be realized. In addition, since the display panel 6511 is extremely thin, a large-capacity battery 6518 may be mounted while suppressing the thickness of the electronic device. In addition, by folding a portion of the display panel 6511 to provide a connection portion with the FPC 6515 on the back of the pixel portion, an electronic device with a narrow frame may be realized.
[0393] At least a part of this embodiment mode can be implemented in combination with other embodiment modes described in this specification as appropriate.
[0394] (Implementation 7) In this embodiment, an electronic device including a display device manufactured using one embodiment of the present invention is described.
[0395] The electronic device exemplified below is an electronic device including a display device of one embodiment of the present invention in a display unit. Therefore, the electronic device exemplified below is an electronic device that can achieve high resolution. In addition, it is an electronic device that can achieve both high resolution and a large screen.
[0396] On the display unit of an electronic device according to one embodiment of the present invention, for example, images having a resolution of full HD, 4K2K, 8K4K, 16K8K, or higher can be displayed.
[0397] Electronic devices include, for example, television devices, notebook personal computers, display devices, digital signage, pinball machines, game consoles, and other electronic devices with relatively large screens, as well as digital cameras, digital video cameras, digital photo frames, mobile phones, portable game consoles, portable information terminals, and sound reproduction devices.
[0398] An electronic device using one embodiment of the present invention can be assembled along a flat or curved surface such as an inner wall or outer wall of a house or building, or an interior or exterior of a car or the like.
[0399] Fig.21A 1 is a diagram showing the appearance of a camera 8000 to which a viewfinder 8100 is attached.
[0400] The camera 8000 includes a housing 8001 , a display portion 8002 , operation buttons 8003 , a shutter button 8004 , etc. The camera 8000 is also provided with a detachable lens 8006 .
[0401] In the camera 8000, the lens 8006 and the housing may also be formed as one body.
[0402] The camera 8000 can perform imaging by pressing a shutter button 8004 or touching a display portion 8002 serving as a touch panel.
[0403] The housing 8001 includes an embedder having electrodes, and can be connected to a flash device or the like in addition to the viewfinder 8100 .
[0404] The viewfinder 8100 includes a housing 8101 , a display portion 8102 , a button 8103 , and the like.
[0405] The housing 8101 is attached to the camera 8000 via an inserter that fits into the camera 8000. The viewfinder 8100 can display an image received from the camera 8000 on the display portion 8102.
[0406] Button 8103 is used as a power button or the like.
[0407] The display device according to one embodiment of the present invention can be used for the display portion 8002 of the camera 8000 and the display portion 8102 of the viewfinder 8100. Alternatively, the camera 8000 may include a built-in viewfinder.
[0408] Fig. 21B 8200 is a diagram showing the appearance of a head mounted display 8200 .
[0409] The head mounted display 8200 includes a mounting portion 8201 , a lens 8202 , a main body 8203 , a display portion 8204 , a cable 8205 , and the like. In addition, a battery 8206 is built in the mounting portion 8201 .
[0410] Power is supplied from a battery 8206 to a main body 8203 via a cable 8205. The main body 8203 includes a wireless receiver and the like, and can display received image information and the like on a display portion 8204. In addition, the main body 8203 includes a camera, thereby making it possible to use the movement of the user's eyeballs and eyelids as an input method.
[0411] In addition, multiple electrodes may be provided at the position of the mounting portion 8201 touched by the user to detect the current flowing through the electrodes according to the movement of the user's eyeballs, thereby realizing the function of recognizing the user's line of sight. In addition, the mounting portion 8201 may have a function of monitoring the user's pulse according to the current flowing through the electrodes. In addition, the mounting portion 8201 may have various sensors such as a temperature sensor, a pressure sensor, an acceleration sensor, and may also have a function of displaying the user's biological information on the display portion 8204 or a function of changing the image displayed on the display portion 8204 in synchronization with the movement of the user's head.
[0412] The display device which is one embodiment of the present invention can be used for the display portion 8204 .
[0413] Fig. 21C , Fig.21D and Fig.21E 8300 is a diagram showing the appearance of a head-mounted display 8300. The head-mounted display 8300 includes a housing 8301, a display portion 8302, a belt-shaped fixing tool 8304, and a pair of lenses 8305.
[0414] The user can see the display on the display unit 8302 through the lens 8305. It is preferable to configure the display unit 8302 in a curved manner because the user can experience a high sense of reality. In addition, by viewing images displayed on different areas of the display unit 8302 through the lens 8305, three-dimensional display using parallax can be performed. In addition, one embodiment of the present invention is not limited to a structure in which one display unit 8302 is provided, and two display units 8302 may be provided so that one display unit is provided for each pair of eyes of the user.
[0415] A display device which is one embodiment of the present invention can be used for the display portion 8302. Since a display device including a semiconductor device which is one embodiment of the present invention has extremely high resolution, even if Fig.21E By using lens 8305 to enlarge in this way, a more realistic image can be displayed without causing the user to see the pixels.
[0416] FIG. 22A to FIG. 22G The electronic device shown includes a housing 9000, a display portion 9001, a speaker 9003, operation keys 9005 (including a power switch or an operation switch), a connecting terminal 9006, a sensor 9007 (the sensor has the function of measuring the following factors: force, displacement, position, speed, acceleration, angular velocity, rotation speed, distance, light, liquid, magnetism, temperature, chemical substance, sound, time, hardness, electric field, current, voltage, electricity, radiation, flow, humidity, inclination, vibration, smell or infrared), a microphone 9008, etc.
[0417] FIG. 22A to FIG. 22GThe electronic device shown has various functions. For example, it may have the following functions: a function of displaying various information (static images, dynamic images, text images, etc.) on a display unit; a function of a touch panel; a function of displaying a calendar, date, or time, etc.; a function of controlling processing by using various software (programs); a function of wireless communication; a function of reading out programs or data stored in a storage medium for processing; etc. Note that the functions of the electronic device are not limited to the above functions, but may have various functions. The electronic device may include a plurality of display units. In addition, a camera or the like may be provided in the electronic device so that it has the following functions: a function of taking a static image or a dynamic image and storing it in a storage medium (an external storage medium or a storage medium built into the camera); a function of displaying the taken image on a display unit; etc.
[0418] Below, we explain in detail FIG. 22A to FIG. 22G Electronic equipment shown.
[0419] Fig.22A 1 is a perspective view showing a television set 9100. The television set 9100 can be incorporated with a large display portion 9001 having a size of, for example, 50 inches or more or 100 inches or more.
[0420] Fig. 22B 9101 is a perspective view showing a portable information terminal 9101. The portable information terminal 9101 can be used as a smart phone, for example. The portable information terminal 9101 can also be provided with a speaker 9003, a connection terminal 9006, a sensor 9007, etc. In addition, the portable information terminal 9101 can display text or image information on multiple faces thereof. Fig. 22B An example of displaying three icons 9050 is shown. In addition, information 9051 represented by a dotted rectangle may be displayed on the other surface of the display unit 9001. Examples of information 9051 include information indicating that an email, SNS, or phone call has been received; a title of the email or SNS; a sender's name; a date; a time; a remaining battery level; and an antenna receiving signal strength. Alternatively, icon 9050 may be displayed at a location where information 9051 is displayed.
[0421] Fig. 22C9102 is a three-dimensional diagram showing a portable information terminal 9102. The portable information terminal 9102 has a function of displaying information on three or more surfaces of the display unit 9001. Here, an example is shown in which information 9052, information 9053, and information 9054 are displayed on different surfaces. For example, the user can also check the information 9053 displayed at a position that can be viewed from above the portable information terminal 9102 while the portable information terminal 9102 is placed in the pocket of a coat. The user can check the display without taking the portable information terminal 9102 out of the pocket, thereby being able to determine, for example, whether to answer a call.
[0422] Fig.22D is a stereoscopic diagram showing a watch-type portable information terminal 9200. The portable information terminal 9200 can be used as a smart watch (registered trademark), for example. In addition, the display surface of the display unit 9001 is curved, and display can be performed on the curved display surface. For example, by communicating with a headset capable of wireless communication, the portable information terminal 9200 can make a hands-free call. In addition, the portable information terminal 9200 includes a connection terminal 9006, which can exchange data with other information terminals or charge. In addition, the charging work can also be performed using wireless power supply.
[0423] Fig.22E , Fig.22F and Figure 22G 9201 is a perspective view showing a foldable portable information terminal. Fig.22E is a perspective view of the portable information terminal 9201 in an unfolded state. Figure 22G is a perspective view of the portable information terminal 9201 in a folded state, and Fig.22F The portable information terminal 9201 is from Fig.22E and Figure 22G The portable information terminal 9201 is a three-dimensional diagram of a state in which one state changes to another state. The portable information terminal 9201 has good portability in the folded state, and has excellent display overview in the unfolded state because it has a large display area with seamless splicing. The display unit 9001 included in the portable information terminal 9201 is supported by three housings 9000 connected by hinges 9055. For example, the display unit 9001 can be bent with a curvature radius of more than 1 mm and less than 150 mm.
[0424] Fig.23A 100 shows an example of a television set. A display portion 7500 of a television set 7100 is incorporated in a housing 7101. Here, a structure in which the housing 7101 is supported by a stand 7103 is shown.
[0425] The operation can be performed by using the operation switch provided in the housing 7101 or the remote control operation machine 7111 provided separately. Fig.23AThe television set 7100 shown in the figure can be operated. Alternatively, a touch panel may be used for the display portion 7500, and the television set 7100 can be operated by touching the display portion 7500 with a finger or the like. Furthermore, the remote control unit 7111 may include a display portion in addition to the operation buttons.
[0426] Alternatively, the television set 7100 may include a television broadcast receiver or a communication device for connecting to a communication network.
[0427] Fig. 23B The notebook personal computer 7200 is shown. The notebook personal computer 7200 includes a housing 7211 , a keyboard 7212 , a pointing device 7213 , an external connection port 7214 , and the like. A display portion 7500 is incorporated in the housing 7211 .
[0428] Fig.23C and Fig.23D An example of digital signage is shown.
[0429] Fig.23C The digital signage 7300 shown includes a housing 7301, a display unit 7500, a speaker 7303, etc. In addition, it may also include an LED lamp, operation keys (including a power switch or an operation switch), a connection terminal, various sensors, a microphone, etc.
[0430] Fig.23D The digital signage 7400 is shown to be disposed on a cylindrical pillar 7401. The digital signage 7400 includes a display portion 7500 disposed along a curved surface of the pillar 7401.
[0431] The larger the display unit 7500 is, the more information can be provided at one time and the easier it is to attract people's attention, thereby improving the advertising effect, for example.
[0432] A touch panel is preferably used for display portion 7500 so that the user can operate the display portion 7500. This allows the display portion 7500 to be used not only for advertisements but also for providing information required by the user, such as route information, traffic information, and guidance of commercial facilities.
[0433] like Fig.23C and Fig.23D As shown, the digital signage 7300 or the digital signage 7400 can be linked with the information terminal device 7311 such as a smartphone carried by the user preferably through wireless communication. For example, the advertisement information displayed on the display unit 7500 can be displayed on the screen of the information terminal device 7311, and the display of the display unit 7500 can be switched by operating the information terminal device 7311.
[0434] Furthermore, the game can be executed on the digital signage 7300 or the digital signage 7400 using the information terminal device 7311 as an operation unit (controller). Thus, an unspecified number of users can participate in the game at the same time and enjoy the game.
[0435] A display device according to one embodiment of the present invention can be applied to FIG. 23A to FIG. 23D Display unit 7500 is shown.
[0436] Although the electronic device of this embodiment has a structure including a display portion, one embodiment of the present invention can also be applied to an electronic device that does not have a display portion.
[0437] At least a part of this embodiment mode can be implemented in combination with other embodiment modes described in this specification as appropriate. [Example 1]
[0438] In this embodiment, samples (sample A1 and sample A2) corresponding to the transistor 100 shown in Fig. 1 were manufactured to evaluate the cross-sectional shape and drain current-drain voltage characteristics (ID-VD characteristics) of the transistor. Note that a transistor without the conductive layer 106 was manufactured here.
[0439] <Sample production> First, a first silicon nitride film with a thickness of 50 nm, a second silicon nitride film with a thickness of 150 nm, a third silicon nitride film with a thickness of 100 nm, and a first silicon oxynitride film with a thickness of 3 nm are sequentially formed on a glass substrate.
[0440] The first silicon nitride film and the third silicon nitride film were formed by PECVD using a mixed gas of silane gas with a flow rate of 200 sccm, nitrogen gas with a flow rate of 2000 sccm, and argon gas with a flow rate of 100 sccm. During the film formation, the pressure was 100 Pa, the power was 2000 W, and the substrate temperature was 350°C.
[0441] The second silicon nitride film was formed by PECVD using a mixed gas of silane gas with a flow rate of 290 sccm, nitrogen gas with a flow rate of 2000 sccm, and argon gas with a flow rate of 2000 sccm. During the film formation, the pressure was 200 Pa, the power was 3000 W, and the substrate temperature was 350°C.
[0442] The first silicon oxynitride film was formed by PECVD using a mixed gas of silane gas at a flow rate of 20 sccm and nitrous oxide gas at a flow rate of 3000 sccm. During the film formation, the pressure was 40 Pa, the power was 3000 W, and the substrate temperature was 350°C.
[0443] Next, a first metal oxide film with a thickness of 25 nm is formed on the first silicon oxynitride film. The first metal oxide film is formed by a sputtering method using an In-Ga-Zn oxide target (In:Ga:Zn=4:2:4.1 [atomic number ratio]). During film formation, the pressure is 0.6 Pa, the power is 2.5 kW, and the substrate temperature is room temperature. As a film-forming gas, a mixed gas of oxygen gas and argon gas is used, and the oxygen flow ratio is 10%.
[0444] Next, heat treatment was performed at 370° C. for 1 hour in a nitrogen atmosphere, and then heat treatment was performed at 370° C. for 1 hour in a mixed gas atmosphere of nitrogen and oxygen (nitrogen gas flow rate: oxygen gas flow rate=4:1). An oven device was used for the heat treatment.
[0445] Next, the first metal oxide film is processed into an island shape to form a first metal oxide layer.
[0446] Next, a second silicon oxynitride film with a thickness of 5 nm, a third silicon oxynitride film with a thickness of 130 nm, and a fourth silicon oxynitride film with a thickness of 5 nm were sequentially formed as a gate insulating layer.
[0447] The second silicon oxynitride film is formed by a PECVD method using a mixed gas of silane gas with a flow rate of 24 sccm and nitrous oxide gas with a flow rate of 18000 sccm. During the film formation, the pressure is 200 Pa, the power is 130 W, and the substrate temperature is 350° C. Note that the second silicon oxynitride film corresponds to the insulating layer 110 a described in Embodiment 1.
[0448] The third silicon oxynitride film is formed by a PECVD method using a mixed gas of silane gas with a flow rate of 200 sccm and nitrous oxide gas with a flow rate of 10000 sccm. During the film formation, the pressure is 300 Pa, the power is 750 W, and the substrate temperature is 350° C. Note that the third silicon oxynitride film corresponds to the insulating layer 110 b described in Embodiment 1.
[0449] The fourth silicon oxynitride film is formed by a PECVD method using a mixed gas of silane gas with a flow rate of 20 sccm and nitrous oxide gas with a flow rate of 3000 sccm. During the film formation, the pressure is 40 Pa, the power is 500 W, and the substrate temperature is 350° C. Note that the fourth silicon oxynitride film corresponds to the insulating layer 110 c described in Embodiment 1.
[0450] Next, a heat treatment was performed at 370° C. for 1 hour in a nitrogen atmosphere. An oven apparatus was used for the heat treatment.
[0451] Next, a second metal oxide film with a thickness of 20 nm was formed on the fourth silicon oxynitride film. The second metal oxide film was formed by a sputtering method using an In-Ga-Zn oxide target (In:Ga:Zn=4:2:4.1 [atomic number ratio]). During film formation, the pressure was 0.8 Pa, the power was 3.5 kW, and the substrate temperature was 200° C. As a film-forming gas, an oxygen gas (oxygen flow ratio was 100%) was used.
[0452] Next, a heat treatment was performed at 370° C. for 1 hour in an atmosphere of a mixed gas of nitrogen and oxygen (nitrogen gas flow rate: oxygen gas flow rate=4:1). An oven apparatus was used for the heat treatment.
[0453] Next, an ITSO film with a thickness of 10 nm and a copper film with a thickness of 100 nm are sequentially formed on the second metal oxide film. The ITSO film and the copper film are formed by sputtering. The ITSO film is formed using an ITSO target (In2O3:SnO2:SiO2=85:10:5 [weight ratio]). The copper film is formed using a Cu target.
[0454] Next, a resist mask is formed on the copper film, and the second metal oxide film, ITSO film, and copper film are processed to form a second metal oxide layer, ITSO layer, and copper layer. A wet etching method is used for processing. As an etchant, a solution obtained by mixing two solutions of solution A and solution B at a volume ratio of 5:1 before use is used. As solution A, an aqueous solution of phosphoric acid (less than 5 weight%), hydrofluoric acid (less than 1 weight%), nitric acid (less than 10 weight%), and an additive (less than 22 weight%) is used. As solution B, an aqueous solution of hydrogen peroxide (31 weight%) is used. The etchant temperature during etching is 30°C.
[0455] Here, the wet etching processing time of sample A1 and sample A2 is different so that the width L2 of the region 108L in the channel length direction of sample A1 and sample A2 is different. The wet etching processing time of sample A1 is 110 seconds, and the wet etching processing time of sample A2 is 60 seconds.
[0456] Next, the second silicon oxynitride film, the third silicon oxynitride film, and the fourth silicon oxynitride film are etched using the resist mask as a mask to form a gate insulating layer. A dry etching method is used for processing. Then, the resist mask is removed.
[0457] Next, a fourth silicon nitride film with a thickness of 100 nm and a fifth silicon oxynitride film with a thickness of 300 nm were sequentially formed as protection layers covering the transistors.
[0458] The fourth silicon nitride film is formed by PECVD using a mixed gas of silane gas with a flow rate of 150 sccm, nitrogen gas with a flow rate of 5000 sccm, and argon gas with a flow rate of 100 sccm. During film formation, the pressure is 200 Pa, the power is 2000 W, and the substrate temperature is 350 °C.
[0459] The fifth silicon oxynitride film is formed by PECVD using a mixed gas of silane gas with a flow rate of 290 sccm and nitrous oxide gas with a flow rate of 4000 sccm. During film formation, the pressure is 133 Pa, the power is 1000 W, and the substrate temperature is 350 °C.
[0460] Next, an opening is formed in a part of the protective layer covering the transistor, and a titanium film with a thickness of 30 nm, a copper film with a thickness of 100 nm, and a titanium film with a thickness of 50 nm are sequentially formed by sputtering, and then the film is processed to obtain source electrodes and drain electrodes. Then, an acrylic resin film with a thickness of about 1.5 μm is formed as a planarization layer, and a heat treatment is performed at a temperature of 250 °C for 1 hour in a nitrogen atmosphere.
[0461] Through the above process, transistors (sample A1 and sample A2) formed on a glass substrate are obtained.
[0462] <Cross-sectional observation> Next, sample A1 and sample A2 are thinned by a focused ion beam (FIB: Focused Ion Beam), and the cross-sections of sample A1 and sample A2 are observed by STEM.
[0463] <Evaluation of ID-VD characteristics> Next, the ID-VD characteristics of the transistors manufactured above are measured.
[0464] The measurement conditions for the ID-VD characteristics of the transistors are as follows: the source potential is set to the ground potential (GND), and the drain voltage (VD) is scanned at intervals of 0.25 V in the range of 0 V to 30 V. ID-VD measurements are continuously performed on the same transistors under four conditions of gate voltage (VG) of 0 V, 2 V, 4 V, and 6 V. Transistors with a channel length of 3 μm and a channel width of 10 μm are used as the transistors, and the ID-VD characteristics of 20 transistors are measured in each sample.
[0465] Fig.24A A cross-sectional STEM image of sample A1 is shown. Fig.24A It is a transmission electron image (TE image: Transmission Electron Image) with a magnification of 80,000 times. As Fig.24AAs shown in FIG. 1 , the width L2 of region 108L in sample A1 is 583 nm. Fig.24A , a glass substrate is denoted as Glass, each silicon nitride film is denoted as SiN, each silicon oxynitride film is denoted as SiON, each metal oxide film is denoted as IGZO, an ITSO film is denoted as ITSO, and a copper film is denoted as Cu.
[0466] Fig. 24B The ID-VD characteristics of sample A1 are shown in Figure 1. Fig. 24B In the graph, the horizontal axis represents the drain voltage (VD) and the vertical axis represents the drain current (ID). Fig. 24B As shown, it was confirmed that sample A1 exhibited good ID-VD characteristics under the conditions of gate voltage (VG) of 2V, 4V, and 6V.
[0467] Fig.25A A cross-sectional STEM image of sample A2 is shown. Fig.25A This is a transmission electron image (TE image) with a magnification of 80,000 times. Fig.25A As shown, in sample A2, the width L2 of region 108L is 238 nm. Fig.25A , a glass substrate is denoted as Glass, each silicon nitride film is denoted as SiN, each silicon oxynitride film is denoted as SiON, each metal oxide film is denoted as IGZO, an ITSO film is denoted as ITSO, and a copper film is denoted as Cu.
[0468] Fig.25B The ID-VD characteristics of sample A2 are shown in Figure 2. Fig.25B In the graph, the horizontal axis represents the drain voltage (VD) and the vertical axis represents the drain current (ID). Fig.25B As shown in the figure, it was confirmed that the on-state current of sample A2 decreased when the gate voltage (VG) was 4V and 6V. No decrease in on-state current was confirmed when the gate voltage (VG) was 2V, so it is estimated that the transistor deteriorated in the high drain voltage region when the gate voltage (VG) was 2V. No decrease in on-state current was confirmed in the above sample A1, so since the width of region 108L is large, the transistor degradation can be suppressed when the drain voltage is high in sample A1. [Example 2]
[0469] In this example, samples (sample B1 to sample B5) corresponding to the transistor 100 shown in FIG. 1 were manufactured and the drain current-drain voltage characteristics (ID-VD characteristics) of the transistors were evaluated.
[0470] <Sample production> First, a titanium film with a thickness of 30 nm and a copper film with a thickness of 100 nm were sequentially formed on a glass substrate by sputtering, and these were processed to obtain a first gate electrode (bottom gate).
[0471] Next, a first silicon nitride film with a thickness of 50 nm, a second silicon nitride film with a thickness of 150 nm, a third silicon nitride film with a thickness of 100 nm, and a first oxynitride silicon film with a thickness of 3 nm are sequentially formed as a first gate insulating layer. The first silicon nitride film to the third silicon nitride film and the first oxynitride silicon film can refer to the description of Example 1, so their detailed description is omitted.
[0472] Next, a first metal oxide film with a thickness of 25 nm is formed on the first silicon oxynitride film. The first metal oxide film is formed by a sputtering method using an In-Ga-Zn oxide target (In:Ga:Zn=4:2:4.1 [atomic number ratio]). During film formation, the pressure is 0.3 Pa, the power is 4.5 kW, and the substrate temperature is room temperature. As a film-forming gas, a mixed gas of oxygen gas and argon gas is used, and the oxygen flow ratio is 10%.
[0473] Next, heat treatment was performed at 370° C. for 1 hour in a nitrogen atmosphere, and then heat treatment was performed at 370° C. for 1 hour in a mixed gas atmosphere of nitrogen and oxygen (nitrogen gas flow rate: oxygen gas flow rate=4:1). An oven device was used for the heat treatment.
[0474] Next, the first metal oxide film is processed into an island shape to form a first metal oxide layer.
[0475] Next, a second oxynitride silicon film with a thickness of 5 nm, a third oxynitride silicon film with a thickness of 130 nm, and a fourth oxynitride silicon film with a thickness of 5 nm are sequentially formed as gate insulating layers. The second to fourth oxynitride silicon films can refer to the description of Embodiment 1, so their detailed description is omitted.
[0476] Next, a heat treatment was performed at 370° C. for 1 hour in a nitrogen atmosphere. An oven apparatus was used for the heat treatment.
[0477] Next, a second metal oxide film with a thickness of 20 nm was formed on the fourth silicon oxynitride film. The second metal oxide film was formed by a sputtering method using an In-Ga-Zn oxide target (In:Ga:Zn=4:2:4.1 [atomic number ratio]). During film formation, the pressure was 0.8 Pa, the power was 3.5 kW, and the substrate temperature was 200° C. As a film-forming gas, an oxygen gas (oxygen flow ratio was 100%) was used.
[0478] Next, a heat treatment was performed at 370° C. for 1 hour in an atmosphere of a mixed gas of nitrogen and oxygen (nitrogen gas flow rate: oxygen gas flow rate=4:1). An oven apparatus was used for the heat treatment.
[0479] Next, an ITSO film with a thickness of 10 nm and a copper film with a thickness of 100 nm are sequentially formed on the second metal oxide film. The ITSO film and the copper film are formed by sputtering. The ITSO film is formed using an ITSO target (In2O3:SnO2:SiO2 = 85:10:5 [weight ratio]). The copper film is formed using a Cu target.
[0480] Next, a resist mask is formed on the copper film, and the second metal oxide film, the ITSO film, and the copper film are processed to form a second metal oxide layer, an ITSO layer, and a copper layer. The wet etching method is used for processing. The etchant used can refer to the description in Example 1, so its detailed description is omitted.
[0481] Here, the wet etching treatment time for each of sample B1 to sample B5 is made different so that the width L2 in the channel length direction of region 108L for each of sample B1 to sample B5 is different. The wet etching treatment times for sample B1, sample B2, sample B3, sample B4, and sample B5 are set to 60 sec, 75 sec, 90 sec, 105 sec, and 120 sec, respectively.
[0482] Next, the second silicon oxynitride film is etched using the above resist mask as a mask to form a second gate insulating layer. The dry etching method is used for processing. Then, the resist mask is removed.
[0483] Next, a fourth silicon nitride film with a thickness of 100 nm and a fifth silicon oxynitride film with a thickness of 300 nm are sequentially formed as a protective layer covering the transistor. The fourth silicon nitride film and the fifth silicon oxynitride film can refer to the description in Example 1, so their detailed descriptions are omitted.
[0484] Next, an opening is formed in a part of the protective layer covering the transistor, and a titanium film with a thickness of 30 nm, a copper film with a thickness of 100 nm, and a titanium film with a thickness of 50 nm are sequentially formed by sputtering, and then the film is processed to obtain source electrodes and drain electrodes. Then, an acrylic resin film with a thickness of about 1.5 μm is formed as a planarization layer and heat-treated at a temperature of 250 °C for 1 hour in a nitrogen atmosphere.
[0485] Through the above processes, transistors (sample B1 to sample B5) formed on a glass substrate are obtained.
[0486] <ID-VD characteristic evaluation> Next, the ID-VD characteristics of the transistors manufactured above are measured.
[0487] The measurement conditions of the ID-VD characteristics of the transistor are as follows: the source potential is set to the ground potential (GND) and the drain voltage (VD) is scanned at 0.25 V intervals in the range of 0 V to 30 V. The ID-VD measurement is continuously performed using the same transistor under four conditions of the gate voltage (VG) being 0 V, 2 V, 4 V, and 6 V. As the transistor, a transistor with a channel length of 3 μm and a channel width of 10 μm is used.
[0488] Fig.26 , Fig. 27 and Fig.28 The ID-VD characteristics of sample B1 to sample B5 are shown. Fig.26 , Fig. 27 and Fig.28 In each of , the horizontal axis represents the drain voltage (VD) and the vertical axis represents the drain current (ID).
[0489] exist Fig.26 In the figure, the results of sample B1 and sample B2 are shown horizontally. Fig. 27 , the results of sample B3 and sample B4 are shown in the horizontal direction. Fig.28 The results of sample B5 are shown. In addition, the width L2 of sample B1 is about 200nm, the channel length is 2.86μm, and the channel width is 10μm. The width L2 of sample B2 is about 300nm, the channel length is 2.63μm, and the channel width is 10μm. The width L2 of sample B3 is about 400nm, the channel length is 2.5μm, and the channel width is 10μm. The width L2 of sample B4 is about 500nm, the channel length is 3.32μm, and the channel width is 10μm. The width L2 of sample B5 is about 600nm, the channel length is 3.06μm, and the channel width is 10μm.
[0490] exist Figure 26 to Figure 28In each of the figures, conditions in which the structures of the transistors are different in the vertical direction are shown. The result denoted as Single Gate is the result of ID-VD measurement performed by applying a gate voltage (VG) to the conductive layer 112 in a transistor that does not include the conductive layer 106. The result denoted as Source Sync. is the result of ID-VD measurement performed by applying a gate voltage (VG) to the conductive layer 112 (top gate electrode) in a transistor that includes the conductive layer 106, with the conductive layer 106 (bottom gate electrode) being electrically connected to the source electrode (GND). The result denoted as Top Gate Sync. is the result of ID-VD measurement performed by applying a gate voltage (VG) to the conductive layer 112 (top gate electrode) in a transistor that includes the conductive layer 106, with the conductive layer 106 (bottom gate electrode) being electrically connected to the conductive layer 112 (top gate electrode).
[0491] like Figure 26 to Figure 28 As shown, in Single Gate, when the width L2 is about 200nm, the on-state current decreases, but when the width L2 is about 300nm or more, the on-state current decreases are not confirmed, and good ID-VD characteristics are shown. In Source Sync. and Top Gate Sync., when the width L2 is about 200nm, about 300nm, and about 400nm, the on-state current decreases, but when the width L2 is about 500nm or more, the on-state current decreases are not confirmed, and good ID-VD characteristics are shown. It can be confirmed that in any transistor structure, the decrease in the on-state current when a high drain voltage is applied can be suppressed by increasing the width L2.
[0492] Fig.29 The relationship between the wet etching time and the width L2 when the second metal oxide film, ITSO film and copper film are processed to form a second metal oxide layer, an ITSO layer and a copper layer is shown. Fig.29 In FIG. 1 , the horizontal axis represents the wet etching time and the vertical axis represents the width L2. Fig.29 In the figure, the black circle indicates the average value within the substrate surface, and the error bar indicates the maximum and minimum values within the substrate surface. Note that here, the measurement results of four locations within the substrate surface are shown for samples with wet etching processing time of 60 sec, 75 sec, and 105 sec, and the measurement results of one location within the substrate surface are shown for samples with wet etching processing time of 90 sec and 120 sec. Fig.29 As shown, it was confirmed that the wet etching process time and the width L2 showed an almost linear relationship, and the width L2 was controlled with high precision according to the wet etching process time. [Example 3]
[0493] In this embodiment, a sample in which a metal oxide film is formed on an insulating film is manufactured to evaluate the amount of oxygen and nitric oxide released from the insulating film and the spin density of the insulating film. A plurality of samples (samples C1 to C4, D1 to D4, E1 to E4, and F1 to F4) having different film forming conditions for the insulating film and the metal oxide film are manufactured.
[0494] <Sample production> First, an insulating film is formed on a substrate.
[0495] As the substrate, glass substrates were used for samples C1 to C4 and samples D1 to D4, and quartz substrates were used for samples E1 to E4 and samples F1 to F4.
[0496] In samples C1 to C4 and E1 to E4, a silicon oxynitride film with a thickness of about 140 nm was formed as an insulating film by plasma CVD. When forming the silicon oxynitride film, the flow rates of silane gas and nitrous oxide gas were 160 sccm and 4000 sccm, respectively, the pressure was 200 Pa, the power was 1500 W, and the substrate temperature was 220°C.
[0497] In samples D1 to D4 and F1 to F4, a first silicon oxynitride film having a thickness of about 5 nm, a second silicon oxynitride film having a thickness of about 130 nm, and a third silicon oxynitride film having a thickness of about 5 nm are formed as insulating films by plasma CVD. When forming the first silicon oxynitride film, the flow rates of silane gas and nitrous oxide gas are 24 sccm and 18000 sccm, respectively. During film formation, the pressure is 200 Pa, the power is 130 W, and the substrate temperature is 350°C. When forming the second silicon oxynitride film, the flow rates of silane gas and nitrous oxide gas are 200 sccm and 4000 sccm, respectively. During film formation, the pressure is 300 Pa, the power is 750 W, and the substrate temperature is 350°C. When forming the third silicon oxynitride film, the flow rates of silane gas and nitrous oxide gas are 20 sccm and 3000 sccm, respectively. During the film formation, the pressure is 40 Pa, the power is 500 W, and the substrate temperature is 350°C.
[0498] Next, heat treatment was performed at 370° C. for 1 hour in a nitrogen atmosphere.
[0499] Next, a metal oxide film with a thickness of about 20 nm is formed on the insulating film by sputtering. The metal oxide film is formed using a metal oxide target with an atomic ratio of metal elements of In:Ga:Zn = 4:2:3 [atomic ratio]. As the film-forming gas, a mixed gas of argon gas and oxygen gas is used.
[0500] The ratio of oxygen gas in the total flow rate of the film-forming gas (oxygen flow ratio) for sample C2, sample D2, sample E2, and sample F2 is 50%. The oxygen flow ratio for sample C3, sample D3, sample E3, and sample F3 is 70%. The oxygen flow ratio for sample C4, sample D4, sample E4, and sample F4 is 100%.
[0501] No metal oxide film is formed on sample C1, sample D1, sample E1, and sample F1.
[0502] Next, each sample is heat-treated at 370 °C for 1 hour in a mixed atmosphere of oxygen gas and nitrogen gas.
[0503] Then, in sample C2 to sample C4, sample D2 to sample D4, sample E2 to sample E4, sample F2 to sample F4, the metal oxide film is removed by wet etching.
[0504] Through the above processes, sample C1 to sample C4, sample D1 to sample D4, sample E1 to sample E4, and sample F1 to sample F4 are manufactured.
[0505] <TDS analysis> Each of the above sample C1 to sample C4 and sample D1 to sample D4 is subjected to thermal desorption spectroscopy (TDS) analysis. The TDS analysis is performed at a heating rate of 30 °C / min for the stage temperature.
[0506] Fig. 30A and Fig. 30B The TDS analysis results are shown. Fig. 30A The release amount of the gas with a mass-to-charge ratio (M / z) = 32 equivalent to an oxygen molecule is shown, Fig. 30B The release amount of the gas with a mass-to-charge ratio (M / z) = 30 equivalent to a nitric oxide molecule is shown. In Fig. 30A and Fig. 30B In , the horizontal axis represents the oxygen flow ratio (O2 ratio) when forming the metal oxide film, and the vertical axis represents the desorption of the gas. Additionally, in Fig. 30A and Fig. 30B the black squares represent the condition where the substrate temperature is 220 °C when forming the insulating film, and the black triangles represent the condition where the substrate temperature is 350 °C when forming the insulating film. Additionally, in Fig. 30A and Fig. 30B on the horizontal axis of, samples C1 and D1 that do not form the metal oxide film are represented by "none".
[0507] As Fig. 30A shown, by forming the metal oxide film on the insulating film, the amount of oxygen molecules released from the insulating film increases, from which it can be known that oxygen is supplied to the insulating film by forming the metal oxide film. Additionally, the higher the oxygen flow ratio when forming the metal oxide film, the more oxygen molecules are released from the insulating film. No difference in the oxygen desorption amount based on the different substrate temperatures when forming the insulating film is observed.
[0508] As Fig. 30B shown, by forming the metal oxide film on the insulating film, the amount of nitric oxide molecules released from the insulating film increases, which indicates that nitrogen oxides are formed in the insulating film by forming the metal oxide film. It was confirmed that: compared with the condition where the substrate temperature is 220 °C when forming the insulating film, the amount of nitric oxide molecules released is less under the condition of 350 °C. Additionally, under the condition where the substrate temperature is 350 °C when forming the insulating film, the higher the oxygen flow ratio when forming the metal oxide film, the less nitric oxide molecules are released from the insulating film. Under the condition where the substrate temperature is 220 °C when forming the insulating film, there is a tendency for the amount of nitric oxide molecules released to increase under the condition where the oxygen flow ratio is 70% compared to the condition where the oxygen flow ratio is 50% when forming the metal oxide film.
[0509] <ESR analysis> Samples E1 to E4 and samples F1 to F4 mentioned above were analyzed by electron spin resonance method (ESR: Electron Spin Resonance). When performing the ESR analysis, the measurement temperature was 85 K, the high-frequency power (microwave power) at 9.2 GHz was 10 mW, and the magnetic field direction was parallel to the film surface of the sample. The detection limit was 3.5×10 17 spins / cm 3 .
[0510] Fig. 30C The ESR analysis results are shown. Fig. 30CThe spin density of the signal caused by nitrogen dioxide (NO2) is shown. The signal caused by nitrogen dioxide (NO2) is divided into three signals by the nuclear spin of nitrogen, and the g values of the three signals are observed to be around 2.04, around 2.00, and around 1.96, respectively. Fig. 30C In the figure, the horizontal axis represents the oxygen flow ratio (O2ratio) when forming the metal oxide film, and the vertical axis represents the spin density (Spin density). Fig. 30C In the figure, the black squares indicate the condition where the substrate temperature is 220°C when the insulating film is formed, and the black triangles indicate the condition where the substrate temperature is 350°C when the insulating film is formed. In addition, the spin density indicates the number of spins per volume of the insulating film, and the spin density is calculated by dividing the number of spins obtained in the ESR analysis by the volume of the insulating film used for the ESR analysis. Fig. 30C The horizontal axis in FIG. 1 represents sample E1 and sample F1 on which no metal oxide film is formed, with “none”.
[0511] like Fig. 30C As shown in FIG. 1 , when a metal oxide film is formed on an insulating film, the spin density of nitrogen dioxide (NO2) caused by the insulating film increases. It was confirmed that the spin density caused by nitrogen dioxide (NO2) is less under the condition of a substrate temperature of 350°C than under the condition of a substrate temperature of 220°C when forming the insulating film. In addition, under the condition of a substrate temperature of 350°C when forming the insulating film, the higher the oxygen flow rate ratio when forming the metal oxide film, the less the spin density caused by nitrogen dioxide (NO2). [Explanation of symbols]
[0512] C1: capacitor, C2: capacitor, DL_n: data line, DL_Y: data line, DL_1: data line, EL: light emitting element, G1: wiring, G2: wiring, GL_m: scanning line, GL_X: scanning line, GL_1: scanning line, LC: liquid crystal element, M1: transistor, M2: transistor, M3: transistor, N1: node, N2: node, P: region, P1: region, P2: region, Q: region, R: region, S1: wiring, S2: wiring, T1: period, T2: period, 100: transistor, 100A: transistor, 100B: transistor, 102: substrate, 103: insulating layer, 103a: insulating layer, 103b: insulating layer, 106: conductive layer, 1 08: semiconductor layer, 108L: region, 108N: region, 110: insulating layer, 110a: insulating layer, 110b: insulating layer, 110c: insulating layer, 110f: insulating film, 112: conductive layer, 112f: conductive film, 113: functional layer, 113f: functional film, 114: metal oxide layer, 114f: metal oxide film, 115: resist mask, 116: insulating layer, 118: insulating layer, 120a: conductive layer, 120b: conductive layer, 141a: opening, 141b: opening, 142: opening, 400: pixel circuit, 400EL: pixel circuit, 400LC: pixel circuit, 401: circuit, 401EL: circuit, 401LC: circuit , 501: pixel circuit, 502: pixel portion, 504: driver circuit portion, 504a: gate driver, 504b: source driver, 506: protection circuit, 507: terminal portion, 550: transistor, 552: transistor, 554: transistor, 560: capacitor, 562: capacitor, 570: liquid crystal element, 572: light emitting element, 700: display device, 700A: display device, 700B: display device, 701: first substrate, 702: pixel portion, 704: source driver circuit portion, 705: second substrate, 706: gate driver circuit portion, 708: FPC terminal portion, 710: signal line, 711: wiring portion, 712: sealant, 716: FPC, 7 17: IC, 721: source driver IC, 722: gate driver circuit portion, 723: FPC, 724: printed circuit board, 730: insulating film, 732: sealing film, 734: insulating film, 736: coloring film, 738: light shielding film, 740: protective layer, 741: protective layer, 742: adhesive layer, 743: resin layer, 744: insulating layer, 745: supporting substrate, 746: resin layer, 750: transistor, 752: transistor, 760: wiring, 770: planarizing insulating film, 772: conductive layer, 773: insulating layer, 774: conductive layer, 775: liquid crystal element, 776: liquid crystal layer, 778: spacer, 780: anisotropic conductive film, 782: light emitting element,786: EL layer, 788: conductive film, 790: capacitor, 6000: display module, 6001: upper cover, 6002: lower cover, 6005: FPC, 6006: display device, 6009: frame, 6010: printed circuit board, 6011: battery, 6015: light emitting unit, 6016: light receiving unit, 6017a: light guiding unit, 6017b: light guiding unit, 6018: light, 6500: electronic device, 6501: housing, 6502: display unit, 6503: power button, 6504: button, 6505: speaker, 6506: microphone, 65 07: Camera, 6508: Light source, 6510: Protective member, 6511: Display panel, 6512: Optical member, 6513: Touch sensor panel, 6515: FPC, 6516: IC, 6517: Printed circuit board, 6518: Battery, 7100: Television device, 7101: Housing, 7103: Bracket, 7111: Remote control device, 7200: Notebook personal computer, 7211: Housing, 7212: Keyboard, 7213: Pointing device, 7214: External connection port, 7300: Digital signage, 7301: Housing, 7303: Speaker, 7311: Information terminal device, 7400: Digital signage, 7401: Pillar, 7500: Display unit, 8000: Camera, 8001: Housing, 8002: Display unit, 8003: Operation button, 8004: Shutter button, 8006: Lens, 8100: Viewfinder, 8101: Housing, 8102: Display unit, 8103: Button, 8200: Head-mounted display, 8201: Mounting unit, 8202: Lens, 8203: Main body, 8204: Display unit, 8205: Cable, 8206: Battery, 8300: Head-mounted display, 83 01: Housing, 8302: Display unit, 8304: Fixing tool, 8305: Lens, 9000: Housing, 9001: Display unit, 9003: Speaker, 9005: Operation key, 9006: Connection terminal, 9007: Sensor, 9008: Microphone, 9050: Icon, 9051: Information, 9052: Information, 9053: Information, 9054: Information, 9055: Hinge, 9100: Television device, 9101: Portable information terminal, 9102: Portable information terminal, 9200: Portable information terminal, 9201: Portable information terminal.
Claims
1. A semiconductor device comprising: Semiconductor layer; a first insulating layer; a second insulating layer; Metal oxide layer; as well as Conductive layer, The first insulating layer, the metal oxide layer and the conductive layer are sequentially stacked on the semiconductor layer. The first insulating layer has a stacked structure in which a first layer, a second layer and a third layer are stacked in sequence. In a cross section along the channel length direction, an end of the first insulating layer is located inside an end of the semiconductor layer. In a cross section along the channel length direction, an end of the metal oxide layer is located inside an end of the first insulating layer. In the cross section along the channel length direction, the end of the conductive layer is located inside the end of the metal oxide layer. The second insulating layer is provided in a manner of covering the semiconductor layer, the first insulating layer, the metal oxide layer and the conductive layer. The semiconductor layer comprises indium and oxygen, The film density of the second layer is lower than the film density of the first layer and the third layer, Furthermore, the hydrogen concentration of the second layer measured by secondary ion mass spectrometry is higher than the hydrogen concentrations of the first layer and the third layer measured by secondary ion mass spectrometry.
2. A semiconductor device comprising: Semiconductor layer; a first insulating layer; a second insulating layer; Metal oxide layer; as well as Conductive layer, The first insulating layer, the metal oxide layer and the conductive layer are sequentially stacked on the semiconductor layer. The first insulating layer has a stacked structure in which a first layer, a second layer and a third layer are stacked in sequence. In a cross section along the channel length direction, an end of the first insulating layer is located inside an end of the semiconductor layer. In a cross section along the channel length direction, an end of the metal oxide layer is located inside an end of the first insulating layer. In the cross section along the channel length direction, the end of the conductive layer is located inside the end of the metal oxide layer. The second insulating layer is provided in a manner of covering the semiconductor layer, the first insulating layer, the metal oxide layer and the conductive layer. The semiconductor layer has a first region, a pair of second regions, and a pair of third regions. The first region overlaps with the first insulating layer and the metal oxide layer, The second region sandwiches the first region and overlaps with the first insulating layer but does not overlap with the metal oxide layer. The third region sandwiches the first region and a pair of the second regions and does not overlap with the first insulating layer. The third region is arranged in contact with the second insulating layer, The third region has a portion having a lower resistance than the first region, The second region has a portion having a higher resistance than that of the third region, The semiconductor layer comprises indium and oxygen, The film density of the second layer is lower than the film density of the first layer and the third layer, Furthermore, the hydrogen concentration of the second layer measured by secondary ion mass spectrometry is higher than the hydrogen concentrations of the first layer and the third layer measured by secondary ion mass spectrometry.
3. The semiconductor device according to claim 1 or 2, The second insulating layer is a silicon nitride film.
4. The semiconductor device according to claim 1 or 2, wherein the end of the first insulating layer and the end of the metal oxide layer both have a tapered shape, And the taper angle of the end of the metal oxide layer is smaller than the taper angle of the end of the first insulating layer.
5. The semiconductor device according to claim 1 or 2, The semiconductor layer also includes gallium and zinc.