Silicon-carbon negative electrode material for lithium ion battery and preparation method of silicon-carbon negative electrode material

Modify mesoporous silica by high-energy ball milling and abrasive agent, and introduce organic carbon cladding and nitrogen doping during sintering, the volume expansion problem of silicon-based negative electrode material is solved, and the first Coulomb efficiency and reversible capacity of the electrode are improved. , extends the battery capacity retention rate.

CN119092666APending Publication Date: 2024-12-06天能新能源(湖州)有限公司
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411179510.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing silicon-based anode materials have volume expansion problems during the charge and discharge cycle, resulting in blockage of electron transport, SEI film rupture, first Coulomb efficiency reduction, reversible capacity reduction and rapid attenuation of battery capacity.

Method used

Mesoporous silica is surface modified by high-energy ball mill and abrasive agent, and organic carbon coating and nitrogen doping are introduced during sintering to form a crosslinked polymer with conductive effect, improving electrochemical performance, and reserved The structure expands the space to prevent the electrode structure from collapse.

Benefits of technology

The first reversible capacity and cycle stability of silicon carbon electrodes are improved, the lithium ion transfer efficiency is improved, the battery capacity retention rate is extended, and the first Coulomb efficiency is significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention belongs to the technical field of lithium battery negative electrode materials, and particularly relates to a silicon-carbon negative electrode material for a lithium ion battery and a preparation method of the silicon-carbon negative electrode material. The preparation method of the silicon-carbon negative electrode material comprises the following steps: carrying out particle size optimization and surface modification on mesoporous silica by using a grinding aid through a high-energy ball milling method; preparing electrode slurry; and drying and sintering to prepare the silicon-carbon negative electrode material. Through surface modification, mesoporous silica is combined with a polymer layer with a self-repairing effect and a good lithium ion transfer effect, a nitrogen atom-doped organic carbon coating layer is formed on the surface after sintering, and the electrochemical performance of the electrode material is optimized. The obtained silicon-carbon negative electrode material has the advantages of high initial coulombic efficiency, high reversible capacity and high battery capacity retention rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium battery negative electrode materials, and in particular relates to a silicon-carbon negative electrode material for lithium ion batteries and a preparation method thereof. Background Art

[0002] Rechargeable lithium-ion batteries (LIBs) have many significant advantages as the core energy storage devices of contemporary portable electronic products, power tools and future electric vehicles. The commonly used negative electrode materials for lithium-ion batteries are mainly graphite, silicon, lithium titanate, etc. Silicon-based negative electrode materials have the advantages of high energy density, excellent fast charging performance and strong lithium storage capacity, and are widely used in the fields of power batteries and consumer batteries. Chinese patent CN114824224B provides a silicon-based negative electrode material and a preparation method thereof, and a lithium-ion battery. The outer layer of the silicon-based negative electrode material has a carbon coating layer with a special structure. The carbon coating layer structure comes from a soluble organic carbon source. The molecular structure of the soluble organic carbon source is rich in aromatic carbon rings and aliphatic carbon structures, and is attached with connected oxygen-containing or nitrogen-containing groups. The aromatic carbon content is not less than 10wt% of the total carbon content, and the ratio of the aromatic carbon content to the aliphatic carbon content is greater than 1. The mass of the carbon coating layer accounts for 0.01-30wt% of the mass of the silicon-based negative electrode material. Chinese patent CN114122339B discloses a silicon-based composite material, a preparation method thereof and a lithium-ion battery. The silicon-based composite material comprises a graphite-like carbon material, nano-active particles and amorphous carbon; the nano-active particles comprise nano-silicon and a coating layer formed on the surface of the nano-silicon, the coating layer comprises silicate and metal nano-particles, and the metal nano-particles are dispersed in the silicate.

[0003] However, existing silicon-based negative electrode materials still have the problem of volume expansion during the charge and discharge cycle. The advantage of silicon-based electrodes is that the upper limit of lithium insertion capacity is high, but in the actual lithium insertion / de-lithiation reaction, silicon needs to change the lattice structure to complete the alloying / de-alloying with lithium, and the volume change during this phase transition process reaches 300%. This volume difference destroys the original lattice structure and affects the transmission of electrons in the electrode; the SEI film on the outer layer of the electrode is repeatedly broken and generated, and after breaking, it loses its original functional structure. The process of generating a new passivation film not only consumes electrolyte and lithium source but also hinders the diffusion of lithium ions; in terms of battery performance, it is manifested as a decrease in the first coulomb efficiency, a decrease in the first reversible capacity, and a rapid decay of battery capacity with cycles. Summary of the invention

[0004] In view of this, the present invention hopes to solve the problem of volume expansion of silicon-based negative electrode materials and obtain negative electrode materials with high coulombic efficiency, high reversible capacity and high battery capacity retention rate for the first time.

[0005] The present invention provides a method for preparing a silicon-carbon negative electrode material for a lithium ion battery, comprising the following steps: S1. According to the mass fraction, 1 to 3 parts of mesoporous silica, 0.01 to 0.05 parts of a grinding aid, and 15 to 45 parts of a ball milling medium are mixed and ball milled to obtain modified silica particles; S2. According to the weight ratio, 1 to 5 parts of a dispersant, 25 to 65 parts of a carbon source, 15 to 20 parts of a nitrogen source, and 90 to 100 parts of the modified silicon dioxide particles are mixed and homogenized in a dispersion medium to obtain an electrode slurry; S3, drying the electrode slurry, sintering and then cooling to obtain a silicon-carbon negative electrode material.

[0006] Preferably, the preparation method of the grinding aid is as follows: by weight, 15 to 30 parts of ethanolamine thioglycolate (CAS: 126-97-6), 0.05 to 0.5 parts of (di-n-butyl) (vinyl) borate (CAS: 2245893-16-5), 0.03 to 0.6 parts of lithium acrylate, and 1 to 3 parts of a catalyst are added to 100 to 150 parts of a solvent, stirred at 70 to 80° C. for 6 to 10 hours, and the solvent is removed by distillation to obtain a grinding aid. Further preferably, the catalyst is at least used to catalyze the Michael addition reaction, and the solvent is DMF.

[0007] Preferably, the ball milling medium is at least one of zirconia balls, agate balls and stainless steel balls.

[0008] Preferably, the parameters of the ball milling step are a rotation speed of 1000 to 1400 rpm, a ball milling time of 8 to 12 h, and a protective atmosphere of at least one of argon and nitrogen.

[0009] Preferably, the dispersant is one of polyethylene glycol, polyvinyl pyrrolidone or polyvinylidene fluoride.

[0010] Preferably, the carbon source is at least one of glucose, fructose, sucrose, cellulose, starch, polyimide, polyacrylonitrile, polystyrene, polythiophene, polyaniline and polypyrrole. Preferably, the nitrogen source is at least one of urea, melamine, dicyandiamide, dopamine, thiourea, ethylenediamine, aniline, triethanolamine and triethylenetetraethylamine.

[0011] Preferably, the mixing and homogenizing step is to first add the dispersant, carbon source and nitrogen source into the dispersion medium and stir, and then add the modified silicon dioxide particles and stir and sonicate together.

[0012] Preferably, the drying method in step S3 is vacuum freeze drying at -30°C.

[0013] Preferably, the sintering step is to heat to 550-650°C at a heating rate of 1-3 min / °C and keep the temperature for 6-10 hours.

[0014] The present invention also provides a silicon-carbon negative electrode material prepared by any of the above preparation methods.

[0015] The present invention performs surface modification on mesoporous silica by high-energy ball milling and grinding aids, and introduces an organic carbon coating layer and nitrogen doping during sintering to improve electrochemical performance. In the grinding aid, the thiol provided by ethanolamine thioglycolate combines with the vinyl part of the borate to obtain an addition product containing thiol and borate. Under the synergistic effect of the Michael addition catalyst and the lithium ion self-catalysis, the lithium acrylate further undergoes a thiol-Michael addition reaction to form a cross-linked polymer with good conductive effect. The particle size of the mesoporous silica is about 1 to 10 μm, and it has a uniform pore structure with a pore size of 2 to 100 nm, which can provide a fast ion transmission channel, and the large specific surface area increases the reaction activity of the material. When no grinding aid is added, high-energy ball milling can nano-size the particle size of the mesoporous silica and improve the first reversible capacity of the electrode. When the grinding aid is added, the high-energy spherical graphite can additionally guide the polymer layer to covalently adhere to the surface of the mesoporous silica to achieve the modification effect. After modification, the carboxyl groups contained in the polymer stabilize the SEI film and improve the efficiency of lithium ion transfer; the borate bonds of the polymer have high stretchability and show self-repairing properties during the charge and discharge reaction, improving the initial reversible capacity and cycle stability of the silicon-carbon electrode. After sintering, a nitrogen-doped organic carbon coating layer is formed on the outside of the modified silica particles, which reserves sufficient space for the structural expansion of the modified silica particles during the charge and discharge process, preventing the collapse of the electrode structure caused by uncontrollable expansion. DETAILED DESCRIPTION

[0016] The present invention is further described below in conjunction with specific embodiments. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should belong to the scope of protection of the present invention.

[0017] Example 1 S1, ball-milling 1 g of silica mesoporous molecular sieve SBA-15, 0.01 g of grinding aid, and 15 g of zirconium oxide balls in an argon atmosphere to obtain modified silica particles; S2, add 1g polyethylene glycol, 25g glucose, and 15g urea to deionized water and stir, then add 90g modified silica particles and stir at 200rpm for 30min, ultrasonicate for 10min, and freeze-dry at -30°C; S3. Sintering and carbonization are carried out in a tubular furnace in an argon atmosphere, and finally naturally cooled to room temperature to obtain a silicon-carbon negative electrode material.

[0018] The preparation method of the grinding aid is as follows: 15g of ethanolamine thioglycolate, 0.05g of (di-n-butyl)(vinyl) borate, 0.03g of lithium acrylate and 1g of triethylamine are added into 100g of DMF, stirred at 70°C for 6h, and DMF is removed by distillation to obtain the grinding aid.

[0019] In S1, the ball milling speed was 1000 rpm and the ball milling time was 12 h.

[0020] The sintering carbonization heating rate in S3 is 1 min / ℃, the temperature is raised to 550℃, and the temperature is kept for 10 hours.

[0021] Example 2 S1. Mill 2 g of silica mesoporous molecular sieve SBA-15, 0.025 g of grinding aid, and 30 g of agate balls in a nitrogen atmosphere to obtain modified silica particles; S2, adding 2.5 g polyvinyl pyrrolidone, 45 g polyimide, and 18 g melamine into deionized water and stirring, then adding 95 g modified silica particles and stirring at 250 rpm for 35 min, ultrasonicating for 13 min, and freeze-drying at -30 °C; S3. Sintering and carbonization are carried out in a tubular furnace in an argon atmosphere, and finally naturally cooled to room temperature to obtain a silicon-carbon negative electrode material.

[0022] The preparation method of the grinding aid is as follows: 23g of ethanolamine thioglycolate, 0.3g of (di-n-butyl)(vinyl) borate, 0.3g of lithium acrylate and 2g of triethylamine are added into 125g of DMF, stirred at 75°C for 8h, and DMF is removed by distillation to obtain the grinding aid.

[0023] In S1, the ball milling speed was 1200 rpm and the ball milling time was 10 h.

[0024] The carbonization heating rate in S3 is 2 min / °C, the temperature is raised to 600°C, and the temperature is kept for 8 h.

[0025] Example 3 S1. 3 g of silica mesoporous molecular sieve SBA-15, 0.05 g of grinding aid, and 45 g of stainless steel balls were ball-milled in an argon-nitrogen mixed atmosphere to obtain modified silica particles; S2, adding 5 g of polyvinylidene fluoride, 65 g of polythiophene, and 20 g of aniline into deionized water and stirring, then adding 100 g of modified silica particles and stirring at 300 rpm for 40 min, ultrasonicating for 15 min, and freeze-drying at -30°C; S3. Sintering and carbonization are carried out in a tubular furnace in a hydrogen-argon mixed atmosphere, and finally naturally cooled to room temperature to obtain a silicon-carbon negative electrode material.

[0026] The preparation method of the grinding aid is as follows: 30g of ethanolamine thioglycolate, 0.5g of (di-n-butyl)(vinyl) borate, 0.6g of lithium acrylate and 3g of triethylamine are added into 150g of DMF, stirred at 80°C for 10h, and DMF is removed by distillation to obtain the grinding aid.

[0027] The ball milling speed in S1 was 1400 rpm and the ball milling time was 8 h.

[0028] The carbonization heating rate in S3 is 3 min / °C, the temperature is raised to 650°C, and the temperature is kept for 6 hours.

[0029] Comparative Example 1 The operation steps are the same as those in Example 1, except that no grinding aid is added to S1.

[0030] Comparative Example 2 The operation steps are the same as those of Example 1, except that no (di-n-butyl)(vinyl) borate is added to the grinding aid.

[0031] Comparative Example 3 The operation steps are the same as those in Example 1, except that lithium acrylate is not added to the grinding aid.

[0032] Example 4 Button-type batteries were prepared using the silicon-carbon negative electrodes prepared in Examples 1 to 3 and Comparative Examples 1 to 3, and their electrochemical performance was tested.

[0033] Preparation method of button battery: take the silicon-carbon negative electrode obtained in the example: acetylene black: polyvinylidene fluoride = 8:1:1 (weight ratio), add appropriate amount of NMP to prepare battery slurry and place it in an agate mortar to grind and mix evenly; coat the mixture on copper foil, place it in a vacuum drying oven and dry it for 12 hours to make a negative electrode sheet; use metal lithium sheet as counter electrode and reference electrode, 1mol / LLiPF6EC:DMC:EMC=1:1:1 (mass ratio) as electrolyte, polypropylene microporous membrane as separator, and assemble it with the negative electrode sheet into a button battery. Constant current charge and discharge experiments were carried out in the blue battery test system, the charge and discharge voltage was limited to 0.005V~1.5V, and the battery charge and discharge rate was 0.2C.

[0034] The test results are as follows: According to the electrochemical performance test results, the first coulombic efficiency of the electrodes prepared in Examples 1 to 3 of the present invention is 94.3% to 95.8%, and the first reversible capacity is 1945.29 to 2392.88 mAh / g, which are significantly improved compared with Comparative Example 1 without adding a grinding aid. Comparative Examples 2 and 3 respectively verify the two situations where the grinding aid lacks (di-n-butyl)(vinyl) borate and lacks lithium acrylate. At this time, the grinding aid can still improve the electrochemical performance of the electrode to a certain extent, but the improvement effect is obviously not as good as the synergistic effect.

Claims

1. A method for preparing a silicon-carbon negative electrode material, characterized in that: The preparation method comprises the following steps: S1. Mix and ball-mill 1 to 3 parts of mesoporous silica, 0.01 to 0.05 parts of grinding aids and 15 to 45 parts of ball-milling media in proportions by mass to obtain modified silica particles; S2. Mix and homogenize 1 to 5 parts of dispersant, 25 to 65 parts of carbon source, 15 to 20 parts of nitrogen source and 90 to 100 parts of the modified silica particles in a dispersion medium in proportions by mass to obtain an electrode slurry; S3. Dry the electrode slurry, sinter and carbonize it, and then cool it to obtain a silicon-carbon negative electrode material.

2. The preparation method according to claim 1, characterized in that: The grinding aid preparation method comprises the following steps: by weight, adding 15 to 30 parts of ethanolamine thioglycolate, 0.05 to 0.5 parts of (di-n-butyl) (vinyl) borate, 0.03 to 0.6 parts of lithium acrylate and 1 to 3 parts of a catalyst into 100 to 150 parts of a solvent, stirring at 70 to 80° C. for 6 to 10 hours, and removing the solvent to obtain the grinding aid.

3. The preparation method according to claim 1, characterized in that: The parameters of the ball milling step are a rotation speed of 1000-1400 rpm, a ball milling time of 8-12 h, and a protective atmosphere of at least one of argon and nitrogen.

4. The preparation method according to claim 1, characterized in that: The dispersant is one of polyethylene glycol, polyvinyl pyrrolidone or polyvinylidene fluoride.

5. The preparation method according to claim 1, characterized in that: The mixing and homogenizing step in S2 is to first add the dispersant, the carbon source, and the nitrogen source into the dispersion medium and stir, and then add the modified silicon dioxide particles and stir and ultrasonicate them together.

6. The preparation method according to claim 1, characterized in that: The carbon source is at least one of glucose, fructose, sucrose, cellulose, starch, polyimide, polyacrylonitrile, polystyrene, polythiophene, polyaniline and polypyrrole.

7. The preparation method according to claim 1, characterized in that: The nitrogen source is at least one of urea, melamine, dicyandiamide, dopamine, thiourea, ethylenediamine, aniline, triethanolamine, and triethylenetetraethylamine.

8. The preparation method according to claim 1, characterized in that: In step S3, the drying method is vacuum freeze drying at below -30°C.

9. The preparation method according to claim 1, characterized in that: The sintering step comprises heating to 550-650° C. at a heating rate of 1-3 min / ° C. and keeping the temperature for 6-10 hours.

10. A silicon-carbon negative electrode material, characterized in that: Prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Artificial graphite negative electrode material of lithium ion battery, preparation method of artificial graphite negative electrode material and lithium ion solid-state battery

    CN120681753A