Modified titanium niobate coated ternary positive electrode material as well as preparation method and application thereof
By doping elements modified titanium niobate coating on the surface of high nickel and low cobalt ternary positive electrode materials, the battery performance problems caused by material structural instability are solved, higher capacity and cycling performance are achieved, and lithium batteries are improved. Overall performance.
Patent Information
- Application Number
- CN202411213022.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
AI Technical Summary
The high nickel and low cobalt ternary cathode material has poor battery performance due to its unstable structural structure, and structural damage and oxygen precipitation are prone to occur during cyclic charging and discharge. The existing cladding materials have limited improvement in performance.
The modified titanium niobate coated ternary positive electrode material is used to coat the surface of the nickel-cobalt lithium aluminum aluminate positive electrode material with elements such as dysprosium, molybdenum, manganese, zinc, cobalt and other metal oxides to improve the structural stability of the material. The coated material was prepared using the sol-gel method to enhance cell performance.
The structural stability and cyclic performance of high-nickel and low-cobalt positive electrode materials have been improved. The discharge specific capacity of the first circle has reached more than 210.5mAh/g, the 1C specific capacity is more than 200.5mAh/g, and the circulation retention rate is more than 95.2%, which has significantly improved three times. Capacity and rate performance of the lithium battery.
Smart Images

Figure CN119092680A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and in particular to a modified titanium niobate-coated ternary positive electrode material and a preparation method and use thereof. Background Art
[0002] Ternary lithium-ion batteries are considered to be the mainstay and future of automotive batteries due to their excellent energy density. High-nickel, low-cobalt ternary cathode materials have become one of the main development directions of ternary cathode materials due to their high theoretical specific capacity. However, high-nickel, low-cobalt cathode materials lack the stabilizing effect of cobalt, and are prone to structural instability, mechanical instability between and within primary particle crystals, and oxygen precipitation during cyclic charge and discharge.
[0003] To address the above issues, the cathode materials of ternary lithium-ion batteries are mainly improved by doping, coating, and optimizing the synthesis process. Coating technology is one of the most widely used and effective methods. However, ordinary coating materials have limited performance improvement on cathode materials of ternary lithium-ion batteries. Summary of the invention
[0004] In view of this, the present application provides a modified titanium niobate-coated ternary positive electrode material and its preparation method and use, in order to solve the problem that the high-nickel and low-cobalt ternary positive electrode material has an unstable structure, resulting in poor battery performance.
[0005] In a first aspect, the present application provides a modified titanium niobate-coated ternary positive electrode material.
[0006] In an optional embodiment, the modified titanium niobate coated ternary positive electrode material includes a nickel cobalt aluminum oxide lithium positive electrode material and a coating material coated on the surface of the nickel cobalt aluminum oxide lithium positive electrode material;
[0007] The chemical formula of the coating material is Ti x Nb y M z O 7 , wherein y=2x, z=0.02-0.08, x+y+z=3, and M includes at least one doping element selected from dysprosium, molybdenum, nickel, manganese, zinc and cobalt.
[0008] In an optional embodiment, the chemical formula of the precursor of the nickel cobalt aluminum oxide positive electrode material is Ni x Co y Al z (OH) 2 , where x+y+z=1, 0.8≤x<1;
[0009] Optionally, the chemical formula of the precursor is Ni 0.90 Co 0.06 Al 0.04 (OH)2 ;
[0010] And / or, the chemical formula of the coating material is Ti 0.98 Nb 1.96 Dy 0.06 O 7 、Ti 0.98 Nb 1.96 Mo 0.06 O 7 、Ti 0.98 Nb 1.96 Ni 0.06 O 7 、Ti 0.98 Nb 1.96 Mn 0.06 O 7 、Ti 0.98 Nb 1.96 Zn 0.06 O 7 or Ti 0.98 Nb 1.96 Co 0.06 O 7 Any one of .
[0011] In a second aspect, the present application provides a method for preparing the modified titanium niobate-coated ternary positive electrode material.
[0012] In an optional embodiment, the preparation method comprises:
[0013] (1) mixing a lithium source with a precursor of a nickel cobalt aluminum oxide positive electrode material and sintering the mixture to obtain a nickel cobalt aluminum oxide positive electrode material;
[0014] (2) dissolving a titanium source, a niobium source and a metal salt of a doping element in a solvent to form a metal salt solution, adding a complexing agent to the metal salt solution and performing a gelation treatment to obtain a coating material;
[0015] (3) The nickel cobalt aluminum lithium positive electrode material is mixed with the coating material and calcined to obtain a modified titanium niobate coated ternary positive electrode material.
[0016] In an optional embodiment, in step (1), the ratio of the total molar number of the lithium element in the lithium source to the total molar number of the metal element in the precursor of the lithium nickel cobalt aluminum oxide positive electrode material is (1.0-1.05):1;
[0017] And / or, the lithium source includes lithium hydroxide.
[0018] In an optional embodiment, in the step (1), the sintering process satisfies at least one of the following conditions A to D:
[0019] A: The sintering temperature is 600-900°C;
[0020] B: The sintering time is 6-12h;
[0021] C: The sintering atmosphere is an oxygen atmosphere;
[0022] D: After the sintering process, the material is further crushed and sieved.
[0023] In an optional embodiment, step (2) satisfies at least one of the following i-v:
[0024] i: the titanium source comprises at least one of titanium tetrachloride, tetrabutyl titanate and titanium isopropoxide;
[0025] ii: the niobium source includes ammonium niobium oxalate;
[0026] iii: the metal salt of the doping element includes at least one of dysprosium nitrate, molybdate, nickel nitrate, manganese sulfate, zinc nitrate and cobalt nitrate;
[0027] iv: the complexing agent comprises at least one of citric acid, tartaric acid and gluconic acid;
[0028] v: The molar ratio of the titanium source to the complexing agent is 1:(4-7).
[0029] In an optional embodiment, in step (2), the concentration of titanium in the metal salt solution is 0.1-0.5M;
[0030] And / or, the solvent is water and / or ethanol.
[0031] In an optional embodiment, in the step (2), the temperature of the gelation treatment is 50-130° C., and optionally, the duration of the gelation treatment is 5-40 hours;
[0032] And / or, the gelation treatment is carried out under a vacuum degree ≤-0.08 MPa; optionally, the vacuum degree is -0.1 MPa to -0.08 MPa.
[0033] In an optional embodiment, in the step (3), the mass ratio of the lithium nickel cobalt aluminum oxide positive electrode material to the coating material is 100: (0.002-0.008);
[0034] And / or, the temperature of the calcination treatment is 600-800° C., and optionally, the duration of the calcination treatment is 6-15 hours;
[0035] And / or, the calcination treatment is carried out in an atmosphere of air.
[0036] In a third aspect, the present application provides a use of the modified titanium niobate-coated ternary positive electrode material or the modified titanium niobate-coated ternary positive electrode material obtained according to the preparation method in a lithium battery.
[0037] A positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer arranged on at least one side of the positive electrode current collector, wherein the positive electrode active material layer comprises the modified titanium niobate coated ternary positive electrode material or the modified titanium niobate coated ternary positive electrode material obtained according to the preparation method.
[0038] In a fourth aspect, the present application provides a secondary battery, comprising the above-mentioned positive electrode plate.
[0039] In a fifth aspect, the present application provides an electrical device, comprising the secondary battery.
[0040] Compared with the prior art, the beneficial effects of this application are:
[0041] The modified titanium niobate coated ternary positive electrode material of the present application comprises a nickel cobalt aluminum lithium positive electrode material and a coating material coated on the surface of the nickel cobalt aluminum lithium positive electrode material; the chemical formula of the coating material is Ti x Nb y M z O 7 , where y=2x, z=0.02-0.08, x+y+z=3, and M includes at least one doping element selected from dysprosium, molybdenum, nickel, manganese, zinc, and cobalt. Titanium niobate is modified by doping elements and coated on the surface of the nickel-cobalt-aluminum lithium positive electrode material, thereby improving the structural stability of the high-nickel-low-cobalt positive electrode material and the capacity, cycle performance, and rate performance of the ternary lithium battery.
[0042] The preparation method of the modified titanium niobate coated ternary positive electrode material of the present application includes mixing a lithium source with a precursor of a nickel cobalt aluminum oxide positive electrode material and sintering to obtain a nickel cobalt aluminum oxide positive electrode material; dissolving a titanium source, a niobium source and a metal salt of a doping element in a solvent to form a metal salt solution, adding a complexing agent to the metal salt solution and performing a gelation treatment to obtain a coating material; mixing the nickel cobalt aluminum oxide positive electrode material with the coating material and performing a calcination treatment to obtain a modified titanium niobate coated ternary positive electrode material. The coating material obtained by adding a complexing agent to the metal salt solution and performing a gelation treatment can further improve the structural stability of the high-nickel and low-cobalt positive electrode material, and the assembled battery has a first-cycle discharge specific capacity of more than 210.5 mAh / g, a 1C specific capacity of more than 200.5 mAh / g, and a cycle retention rate of more than 95.2%. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0044] Figure 1 This is a SEM image of the high nickel NCA positive electrode material of Example 1 of the present application;
[0045] Figure 2 This is a SEM image of the modified titanium niobate-coated ternary positive electrode material of Example 1 of the present application. DETAILED DESCRIPTION
[0046] The following examples are provided for a better understanding of the present application, but are not limited to the best implementation mode described, and do not limit the content and protection scope of the present application. Any product identical or similar to the present application obtained by anyone under the inspiration of the present application or by combining the features of the present application with other prior arts shall fall within the protection scope of the present application.
[0047] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:
[0048] In this application, the selection scope of "and / or" includes any one of two or more related listed items, and also includes any and all combinations of related listed items, and the said any and all combinations include any combination of two related listed items, any more related listed items, or all related listed items. For example, "A and / or B" includes three parallel solutions of A, B and A+B.
[0049] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0050] In the present application, the percentage content, unless otherwise specified, refers to mass percentage for solid-liquid mixing and solid-solid mixing, and refers to volume percentage for liquid-liquid mixing.
[0051] In this application, percentage concentrations, unless otherwise specified, refer to final concentrations. Final concentration refers to the percentage of an added component in a system after the addition of the component; M is the molar concentration (i.e., the amount of substance), expressed as mol / L.
[0052] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.
[0053] Traditional polycrystalline ternary materials are composed of micron-sized secondary particles (about 1-30μm) agglomerated from densely arranged submicron-sized primary particles (about 50-300nm). However, the capacity and cycle life of polycrystalline ternary cathode materials are challenged by the instability of the layered structure caused by reactions and phase changes during charge and discharge, mechanical instability between and within the primary particle crystals, and structural damage caused by oxygen precipitation. High-nickel, low-cobalt ternary cathode materials are more affected due to the lack of cobalt stabilization. By coating a layer of oxide or other salt substances on the surface of the cathode material, its specific capacity, cycle performance, and rate performance can be improved.
[0054] Fast ion conductors have broad application prospects in high-energy and high-density batteries, electrochemical energy storage and other fields. Titanium niobate binary metal oxides should be able to produce batteries with high-rate and high-capacity electrochemical properties due to their suitable lithium insertion potential, large specific capacity (theoretical capacity is about 387.6 mAh / g), and kinetically favorable shear layered structure. They are considered to be a new type of lithium-ion battery negative electrode material with great potential. However, the low intrinsic conductivity of titanium niobate hinders the high-rate performance of ternary lithium-ion batteries.
[0055] In order to solve the problems existing in the above-mentioned related technologies, according to the first aspect of the present application, a modified titanium niobate-coated ternary positive electrode material is provided.
[0056] In some embodiments, the modified titanium niobate coated ternary positive electrode material includes a nickel cobalt aluminum oxide lithium positive electrode material and a coating material coated on the surface of the nickel cobalt aluminum oxide lithium positive electrode material;
[0057] The chemical formula of the coating material is Ti x Nb y M z O 7 , wherein y=2x, z=0.02-0.08, x+y+z=3, and M includes at least one doping element selected from dysprosium, molybdenum, nickel, manganese, zinc and cobalt.
[0058] By modifying titanium niobate with doping elements and coating it on the surface of nickel-cobalt-aluminum-lithium cathode material, the structural stability of high-nickel-low-cobalt cathode material is improved, and the capacity, cycle performance and rate performance of ternary lithium battery are improved. Ti doping can effectively inhibit the generation of cracks through grain boundary strengthening and bulk phase stabilization, thereby improving the cycle stability of the material and reducing the occurrence of side reactions, but excessive doping will occupy the channels originally used for lithium ion transmission, reduce the diffusion rate of lithium ions, and thus affect the charge and discharge performance of the material.
[0059] In some embodiments, the chemical formula of the precursor of the nickel cobalt aluminum oxide positive electrode material is Ni x Co y Al z (OH) 2 , where x+y+z=1, 0.8≤x<1;
[0060] Optionally, the chemical formula of the precursor is Ni 0.90 Co 0.06 Al 0.04 (OH) 2 ;
[0061] And / or, the chemical formula of the coating material is Ti 0.98 Nb 1.96 Dy 0.06 O 7 、Ti 0.98 Nb 1.96 Mo 0.06 O 7 、Ti 0.98 Nb 1.96 Ni 0.06 O 7 、Ti 0.98 Nb 1.96 Mn 0.06 O 7 、Ti 0.98 Nb 1.96 Zn 0.06 O 7 or Ti 0.98 Nb 1.96 Co 0.06 O 7 Any one of .
[0062] In a second aspect, the present application provides a method for preparing the modified titanium niobate-coated ternary positive electrode material.
[0063] In some embodiments, the preparation method comprises:
[0064] (1) mixing a lithium source with a precursor of a nickel cobalt aluminum oxide positive electrode material and sintering the mixture to obtain a nickel cobalt aluminum oxide positive electrode material;
[0065] (2) dissolving a titanium source, a niobium source and a metal salt of a doping element in a solvent according to a ratio to form a metal salt solution, adding a complexing agent to the metal salt solution and performing a gelation treatment to obtain a coating material;
[0066] (3) The nickel cobalt aluminum lithium positive electrode material is mixed with the coating material and calcined to obtain a modified titanium niobate coated ternary positive electrode material.
[0067] By coating the nickel cobalt aluminum oxide positive electrode material with the coating material obtained by the sol-gel method, doped titanium niobate can be produced in situ on the surface of the high-nickel ternary positive electrode material, which can further improve the structural stability of the nickel cobalt aluminum oxide positive electrode material and further improve the first-cycle discharge capacity, rate performance and cycle performance of the battery.
[0068] In some embodiments, in step (1), the ratio of the total molar number of the lithium element in the lithium source to the total molar number of the metal element in the precursor of the lithium nickel cobalt aluminum oxide positive electrode material is (1.0-1.05):1;
[0069] And / or, the lithium source includes lithium hydroxide.
[0070] In some embodiments, in step (1), the sintering process satisfies at least one of the following AD:
[0071] A: The sintering temperature is 600-900°C;
[0072] B: The sintering time is 6-12h;
[0073] C: The sintering atmosphere is an oxygen atmosphere;
[0074] D: After the sintering process, the material is further crushed and sieved.
[0075] In some embodiments, step (2) satisfies at least one of the following i-v:
[0076] i: the titanium source comprises at least one of titanium tetrachloride, tetrabutyl titanate and titanium isopropoxide;
[0077] ii: the niobium source includes ammonium niobium oxalate;
[0078] iii: the metal salt of the doping element includes at least one of dysprosium nitrate, molybdate, nickel nitrate, manganese sulfate, zinc nitrate and cobalt nitrate;
[0079] iv: the complexing agent comprises at least one of citric acid, tartaric acid and gluconic acid;
[0080] v: The molar ratio of the titanium source to the complexing agent is 1:(4-7).
[0081] In some embodiments, in step (2), the concentration of titanium in the metal salt solution is 0.1-0.5M;
[0082] And / or, the solvent is water and / or ethanol.
[0083] In some embodiments, in step (2), the temperature of the gelation treatment is 50-130° C., and optionally, the duration of the gelation treatment is 5-40 hours;
[0084] And / or, the gelation treatment is carried out under a vacuum degree ≤-0.08 MPa; optionally, the vacuum degree is -0.1 MPa to -0.08 MPa.
[0085] The gelation treatment is carried out under the condition of vacuum degree ≤-0.08MPa, so that the coating material layer is more compact, no impurities are generated in the positive electrode material, the coating layer is evenly distributed, and the morphology of the ternary positive electrode material after coating is regular.
[0086] In some embodiments, in step (3), the mass ratio of the lithium nickel cobalt aluminum oxide positive electrode material to the coating material is 100: (0.002-0.008);
[0087] And / or, the temperature of the calcination treatment is 600-800° C., and optionally, the duration of the calcination treatment is 6-15 hours;
[0088] And / or, the calcination treatment is carried out in an air atmosphere;
[0089] And / or, before the calcination treatment, the mixture of the high-nickel NCA positive electrode material and the coating material is dried for 6-10 hours.
[0090] The appropriate ratio of nickel cobalt aluminum oxide positive electrode material and coating material can further improve the structural stability of high nickel and low cobalt positive electrode materials. The assembled battery has a high first-cycle discharge capacity, good rate performance and excellent cycle performance.
[0091] In a third aspect, the present application provides a use of the modified titanium niobate-coated ternary positive electrode material or the modified titanium niobate-coated ternary positive electrode material obtained according to the preparation method in a lithium battery.
[0092] A positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer arranged on at least one side of the positive electrode current collector, wherein the positive electrode active material layer comprises the modified titanium niobate coated ternary positive electrode material or the modified titanium niobate coated ternary positive electrode material obtained according to the preparation method.
[0093] In a fourth aspect, the present application provides a secondary battery, comprising the positive electrode plate.
[0094] In a fifth aspect, the present application provides an electrical device, comprising the secondary battery.
[0095] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.
[0096] If no specific experimental steps or conditions are specified in the following experiments, the conventional experimental steps or conditions described in the literature in this field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be purchased commercially.
[0097] Example 1
[0098] This embodiment provides a modified titanium niobate coated ternary positive electrode material, and the preparation method thereof is as follows:
[0099] 1) 275.87 g of lithium hydroxide monohydrate (41.9636 g / mol), 600 g of Ni 0.90 Co 0.06 Al 0.04 (OH) 2 After the ternary precursor is mixed in a high-speed mixer, it is placed in a box furnace and sintered at 720°C in an oxygen atmosphere for 10 hours. After that, it is crushed and sieved to obtain a high-nickel NCA positive electrode material with a particle size of 8-15 μm. The SEM image (scanning electron microscope image) of the high-nickel NCA positive electrode material is shown in the figure. Figure 1 ;
[0100] (2) According to the coating material Ti 0.98 Nb 1.96 Dy 0.06 O 7 Titanium isopropoxide, ammonium niobium oxalate and dysprosium nitrate are weighed in a stoichiometric ratio and dissolved in ethanol to form a metal salt solution, and then citric acid is added as a complexing agent, and the solution is placed in a vacuum environment of -0.08 MPa, and gelled at 100°C for 24 hours to obtain a coating material, wherein the concentration of titanium isopropoxide in the metal salt solution is 0.33 M, and the molar ratio of titanium isopropoxide to citric acid is 1:5;
[0101] (3) According to the mass ratio of high nickel NCA positive electrode material to coating material of 100:0.002, the high nickel NCA positive electrode material prepared in step (1) and the coating material prepared in step (2) were mixed, and then placed in a vacuum drying oven for drying for 8 hours, and finally calcined at a temperature of 650° C. for 6 hours in an air atmosphere to obtain a ternary positive electrode material coated with dysprosium (Dy), denoted as Dy-TNO@NCA. The SEM image (scanning electron microscope image) of the Dy-doped titanium niobate coated ternary positive electrode material is shown in FIG. Figure 2 .
[0102] Example 2
[0103] This embodiment provides a modified titanium niobate coated ternary positive electrode material, and the preparation method thereof is as follows:
[0104] 1) 275.87 g of lithium hydroxide monohydrate and 600 g of Ni 0.90 Co 0.06 Al 0.04 (OH) 2 The ternary precursors were mixed in a high-speed mixer, placed in a box furnace, and sintered at 600°C in an oxygen atmosphere for 12 hours, and then crushed and sieved to obtain a high-nickel NCA positive electrode material with a particle size of 8-15 μm;
[0105] (2) According to the coating material Ti 0.98 Nb 1.96 Mo 0.06 O 7 Titanium tetrachloride, ammonium niobium oxalate and ammonium molybdate were weighed and dissolved in ethanol in a stoichiometric ratio to form a metal salt solution, and tartaric acid was added as a complexing agent. The solution was placed in a vacuum environment of -0.08 MPa and subjected to gelation treatment at 130°C for 5 h to obtain a coating material, wherein the concentration of titanium tetrachloride in the metal salt solution was 0.33 M, and the molar ratio of titanium tetrachloride to citric acid was 1:4;
[0106] (3) The high nickel ternary positive electrode material prepared in step (1) and the coating material prepared in step (2) were mixed in a mass ratio of 100:0.002, and then placed in a vacuum drying oven for drying for 8 hours. Finally, they were calcined at 650° C. for 6 hours in an air atmosphere to obtain a molybdenum (Mo)-doped titanium niobate-coated ternary positive electrode material, which was recorded as Mo-TNO@NCA.
[0107] Example 3
[0108] This embodiment provides a modified titanium niobate coated ternary positive electrode material, and the preparation method thereof is as follows:
[0109] 1) 275.87 g of lithium hydroxide monohydrate and 600 g of Ni 0.90 Co 0.06 Al 0.04 (OH) 2 After the ternary precursor is mixed in a high-speed mixer, it is placed in a box furnace and sintered at 900°C in an oxygen atmosphere for 6 hours. After that, it is crushed and sieved to obtain a high-nickel NCA positive electrode material with a particle size of 8-15μm.
[0110] (2) According to the coating material Ti 0.98 Nb 1.96 Ni 0.06 O 7Tetrabutyl titanate, ammonium niobium oxalate and nickel nitrate were weighed and dissolved in water in a stoichiometric ratio to form a metal salt solution, and gluconic acid was added as a complexing agent. The solution was placed in a vacuum environment of -0.08 MPa and subjected to gelation treatment at 50°C for 40 hours to obtain a coating material, wherein the concentration of tetrabutyl titanate in the metal salt solution was 0.33 M, and the molar ratio of tetrabutyl titanate to citric acid was 1:7;
[0111] (3) The high nickel ternary positive electrode material prepared in step (1) and the coating material prepared in step (2) were mixed in a mass ratio of 100:0.008, and then placed in a vacuum drying oven for drying for 8 hours. Finally, they were calcined at 600° C. for 15 hours in an air atmosphere to obtain a nickel (Ni)-doped titanium niobate-coated ternary positive electrode material, which was recorded as Ni-TNO@NCA.
[0112] Example 4
[0113] This embodiment provides a modified titanium niobate coated ternary positive electrode material, and the preparation method thereof is as follows:
[0114] 1) 275.87 g of lithium hydroxide monohydrate (41.9636 g / mol), 600 g of Ni 0.90 Co 0.06 Al 0.04 (OH) 2 The ternary precursors were mixed in a high-speed mixer, placed in a box furnace, and sintered at 720°C in an oxygen atmosphere for 10 hours, and then crushed and sieved to obtain a high-nickel NCA positive electrode material with a particle size of 8-15 μm;
[0115] (2) According to the coating material Ti 0.98 Nb 1.96 Mn 0.06 O 7 Titanium isopropoxide, ammonium niobium oxalate and manganese sulfate are weighed in a stoichiometric ratio and dissolved in ethanol to form a metal salt solution, and then citric acid is added as a complexing agent, and the solution is placed in a vacuum environment of -0.08 MPa, and gelled at 100°C for 24 hours to obtain a coating material, wherein the concentration of titanium isopropoxide in the metal salt solution is 0.33 M, and the molar ratio of titanium isopropoxide to citric acid is 1:5;
[0116] (3) According to the mass ratio of high-nickel NCA positive electrode material to coating material of 100:0.005, the high-nickel NCA positive electrode material prepared in step (1) and the coating material prepared in step (2) were mixed, and then placed in a vacuum drying oven for 8 hours, and finally calcined at 650° C. for 6 hours in an air atmosphere to obtain a manganese (Mn)-doped titanium niobate coated ternary positive electrode material, recorded as Mn-TNO@NCA.
[0117] Example 5
[0118] This embodiment provides a modified titanium niobate coated ternary positive electrode material, and the preparation method thereof is as follows:
[0119] 1) 275.87 g of lithium hydroxide monohydrate (41.9636 g / mol), 600 g of Ni 0.90 Co 0.06 Al 0.04 (OH) 2 The ternary precursors were mixed in a high-speed mixer, placed in a box furnace, and sintered at 720°C in an oxygen atmosphere for 10 hours, and then crushed and sieved to obtain a high-nickel NCA positive electrode material with a particle size of 8-15 μm;
[0120] (2) According to the coating material Ti 0.98 Nb 1.96 Zn 0.06 O 7 Titanium isopropoxide, ammonium niobium oxalate and zinc nitrate are weighed in a stoichiometric ratio and dissolved in ethanol to form a metal salt solution, and then citric acid is added as a complexing agent, and the solution is placed in a vacuum environment of -0.08 MPa, and gelled at 100°C for 24 hours to obtain a coating material, wherein the concentration of titanium isopropoxide in the metal salt solution is 0.1 M, and the molar ratio of titanium isopropoxide to citric acid is 1:5;
[0121] (3) According to the mass ratio of high nickel NCA positive electrode material to coating material of 100:0.005, the high nickel NCA positive electrode material prepared in step (1) and the coating material prepared in step (2) were mixed, and then placed in a vacuum drying oven for 8 hours, and finally calcined at 650° C. for 6 hours in an air atmosphere to obtain a zinc (Zn)-doped titanium niobate coated ternary positive electrode material, recorded as Zn-TNO@NCA.
[0122] Example 6
[0123] This embodiment provides a modified titanium niobate coated ternary positive electrode material, and the preparation method thereof is as follows:
[0124] 1) 275.87 g of lithium hydroxide monohydrate (41.9636 g / mol), 600 g of Ni 0.90 Co 0.06 Al 0.04 (OH) 2 The ternary precursors were mixed in a high-speed mixer, placed in a box furnace, and sintered at 720°C in an oxygen atmosphere for 10 hours, and then crushed and sieved to obtain a high-nickel NCA positive electrode material with a particle size of 8-15 μm;
[0125] (2) According to the coating material Ti0.98 Nb 1.96 Co 0.06 O 7 Titanium isopropoxide, ammonium niobium oxalate and cobalt nitrate are weighed in a stoichiometric ratio and dissolved in ethanol to form a metal salt solution, and then citric acid is added as a complexing agent, and the solution is placed in a vacuum environment of -0.08 MPa, and gelled at 100°C for 24 hours to obtain a coating material, wherein the concentration of titanium isopropoxide in the metal salt solution is 0.5 M, and the molar ratio of titanium isopropoxide to citric acid is 1:5;
[0126] (3) According to the mass ratio of high nickel NCA positive electrode material to coating material of 100:0.002, the high nickel NCA positive electrode material prepared in step (1) and the coating material prepared in step (2) were mixed, and then placed in a vacuum drying oven for 8 hours, and finally calcined at 650° C. for 6 hours in an air atmosphere to obtain a cobalt (Co)-doped titanium niobate-coated ternary positive electrode material, which was recorded as Co-TNO@NCA.
[0127] Example 7
[0128] This embodiment provides a modified titanium niobate coated ternary positive electrode material, and the preparation method thereof is as follows:
[0129] 1) 275.87 g of lithium hydroxide monohydrate (41.9636 g / mol), 600 g of Ni 0.90 Co 0.06 Al 0.04 (OH) 2 The ternary precursors were mixed in a high-speed mixer, placed in a box furnace, and sintered at 720°C in an oxygen atmosphere for 10 hours, and then crushed and sieved to obtain a high-nickel NCA positive electrode material with a particle size of 8-15 μm;
[0130] (2) According to the coating material Ti 0.98 Nb 1.96 Dy 0.06 O 7 Titanium isopropoxide, ammonium niobium oxalate and dysprosium nitrate are weighed and mixed in a stoichiometric ratio to obtain a coating material;
[0131] (3) According to the mass ratio of high-nickel NCA positive electrode material to coating material of 100:0.002, the high-nickel NCA positive electrode material obtained in step (1) and the coating material obtained in step (2) are mixed, and then placed in a vacuum drying oven for 8 hours, and finally calcined at 650° C. for 6 hours in an air atmosphere to obtain a ternary positive electrode material coated with dysprosium (Dy)-doped titanium niobate.
[0132] Comparative Example 1
[0133] This comparative example provides a TiNb-coated high-nickel ternary positive electrode material, and its preparation method is as follows:
[0134] (1) placing 275.87 g of lithium hydroxide monohydrate and 600 g of Ni0.90Co0.06Al0.04(OH)2 ternary precursor in a box furnace, sintering for 10 h at 720° C. in an oxygen atmosphere, and then crushing and sieving to obtain a high-nickel ternary positive electrode material to be coated;
[0135] (2) Weigh 100 g of the high-nickel ternary positive electrode material prepared in step (1), 0.084 g of titanium dioxide, and 0.143 g of niobium pentoxide, mix them in a high-speed mixer, and calcine them at 650° C. for 6 h to prepare a TiNb-coated high-nickel ternary positive electrode material, denoted as TiNb@NCA.
[0136] Comparative Example 2
[0137] This embodiment provides a modified titanium niobate coated ternary positive electrode material, and the preparation method thereof is as follows:
[0138] 1) 275.87 g of lithium hydroxide monohydrate (41.9636 g / mol), 600 g of Ni 0.90 Co 0.06 Al 0.04 (OH) 2 The ternary precursors were mixed in a high-speed mixer, placed in a box furnace, and sintered at 720°C in an oxygen atmosphere for 10 hours, and then crushed and sieved to obtain a high-nickel NCA positive electrode material with a particle size of 8-15 μm;
[0139] (2) according to the molar ratio of Ti element to Nb element of 0.98:1.96, titanium isopropoxide and ammonium niobium oxalate were weighed and dissolved in ethanol to form a metal salt solution, the concentration of titanium isopropoxide in the metal salt solution was 0.33M, and then citric acid was added as a complexing agent, the molar ratio of titanium isopropoxide to citric acid was 1:5, and the solution was placed in a vacuum environment of -0.08MPa, and gelation treatment was performed at 100°C for 24h to obtain a coating material;
[0140] (3) According to the mass ratio of high-nickel NCA positive electrode material to coating material of 100:0.002, the high-nickel NCA positive electrode material prepared in step (1) and the coating material prepared in step (2) were mixed, and then placed in a vacuum drying oven for 8 hours, and finally calcined at 650° C. for 6 hours in an air atmosphere to obtain a TiNb-coated high-nickel ternary positive electrode material, which was recorded as TN@NCA.
[0141] Test Example 1
[0142] The positive electrode materials prepared in Examples 1-7 and Comparative Examples 1-2 were used to prepare lithium-ion batteries (CR2032 type button half-cells), and the specific method was as follows:
[0143] The mass ratio of positive electrode material: carbon black: PVDF is 90:5:5, and N-methylpyrrolidone is used as a dispersant to prepare the positive electrode slurry, which is placed in a centrifuge and shaken for 30 minutes. The positive electrode slurry is evenly scraped on the carbon-coated aluminum foil and dried in an oven at 100°C for 2 hours to obtain a dried electrode sheet. The dried electrode sheet is rolled with a roller at 40kN, and then dried in an oven at 100°C for 2 hours. Finally, it is cut with a corresponding size mold to obtain a positive electrode sheet.
[0144] In the argon atmosphere of the glove box, Celgard 2500 diaphragm, lithium metal sheet as negative electrode, LBC3021C011 electrolyte were used. The battery was assembled in the order of negative electrode, electrolyte, diaphragm, electrolyte, and positive electrode.
[0145] Then at 25°C, charge to 4.25V at a rate of 0.2C, and then discharge to 2.8V at a rate of 0.2C. This is a cycle process. The charge and discharge capacity this time is the first charge and discharge specific capacity, and the charge and discharge ratio is the first efficiency. After 2 cycles, charge at 0.5C and discharge at 1C for 50 cycles. Record the charge and discharge capacity of the 3rd cycle and the charge and discharge capacity of the 52nd cycle. The retention rate is the ratio of the discharge capacity of the 52nd cycle to the 3rd cycle. See Table 1 for the test results.
[0146] Table 1 Test results
[0147]
[0148]
[0149] As can be seen from Table 1, no doping elements were added to Comparative Example 1, and the first-cycle discharge capacity of the battery composed of the obtained positive electrode material was 203.6Ah / g, the 1C capacity was 197.1mAh / g, and the cycle retention rate was 92.5%; the first-cycle discharge capacity of the battery composed of the positive electrode material of the present application was above 207.2mAh / g, the 1C capacity was above 197.6mAh / g, and the cycle retention rate was above 93.2%. It can be seen that by modifying titanium niobate with doping elements, the structural stability of the high-nickel and low-cobalt positive electrode material is improved, and the capacity, cycle performance and rate performance of the ternary lithium battery are improved. By coating the nickel cobalt aluminum oxide positive electrode material with the coating material obtained by the sol-gel method, doped titanium niobate can be produced in situ on the surface of the high-nickel ternary positive electrode material, which can further improve the structural stability of the nickel cobalt aluminum oxide positive electrode material and further improve the capacity and cycle stability of the battery.
[0150] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection created by this application.
Claims
1. A modified titanium niobate coated ternary positive electrode material, It is characterized in that The modified titanium niobate coated ternary positive electrode material comprises a nickel cobalt aluminum oxide lithium positive electrode material and a coating material coated on the surface of the nickel cobalt aluminum oxide lithium positive electrode material; The chemical formula of the coating material is Ti x Nb y M z O 7 , wherein y=2x, z=0.02-0.08, x+y+z=3, and M includes at least one doping element selected from dysprosium, molybdenum, nickel, manganese, zinc and cobalt.
2. According to claim 1, the modified titanium niobate coated ternary positive electrode material, It is characterized in that The chemical formula of the precursor of the lithium nickel cobalt aluminum oxide positive electrode material is Ni x Co y Al z (OH) 2 , where x+y+z=1, 0.8≤x<1, 0.05≤y<0.12; Optionally, the chemical formula of the precursor is Ni 0.90 Co 0.06 Al 0.04 (OH) 2 ; And / or, the chemical formula of the coating material is Ti 0.98 Nb 1.96 Dy 0.06 O 7 、Ti 0.98 Nb 1.96 Mo 0.06 O 7 、Ti 0.98 Nb 1.96 Ni 0.06 O 7 、Ti 0.98 Nb 1.96 Mn 0.06 O 7 、Ti 0.98 Nb 1.96 Zn 0.06 O 7 or Ti 0.98 Nb 1.96 Co 0.06 O 7 Any one of .
3. A method for preparing the modified titanium niobate coated ternary positive electrode material according to claim 1 or 2, It is characterized in that The preparation method comprises the following steps: (1) mixing a lithium source with a precursor of a nickel cobalt aluminum oxide positive electrode material and sintering the mixture to obtain a nickel cobalt aluminum oxide positive electrode material; (2) dissolving a titanium source, a niobium source and a metal salt of a doping element in a solvent to form a metal salt solution, adding a complexing agent to the metal salt solution and performing a gelation treatment to obtain a coating material; (3) The nickel cobalt aluminum lithium positive electrode material is mixed with the coating material and calcined to obtain a modified titanium niobate coated ternary positive electrode material.
4. The preparation method according to claim 3, It is characterized in that In step (1), the ratio of the total molar number of the lithium element in the lithium source to the total molar number of the metal element in the precursor of the lithium nickel cobalt aluminum oxide positive electrode material is (1.0-1.05):1; And / or, the lithium source includes lithium hydroxide.
5. The preparation method according to claim 3, It is characterized in that In the step (1), the sintering process satisfies at least one of the following conditions A to D: A: The sintering temperature is 600-900°C; B: The sintering time is 6-12h; C: The sintering atmosphere is an oxygen atmosphere; D: After the sintering process, the material is further crushed and sieved.
6. The preparation method according to claim 3, It is characterized in that The step (2) satisfies at least one of the following i-v: i: the titanium source comprises at least one of titanium tetrachloride, tetrabutyl titanate and titanium isopropoxide; ii: the niobium source includes ammonium niobium oxalate; iii: the metal salt of the doping element includes at least one of dysprosium nitrate, molybdate, nickel nitrate, manganese sulfate, zinc nitrate and cobalt nitrate; iv: the complexing agent comprises at least one of citric acid, tartaric acid and gluconic acid; v: The molar ratio of the titanium source to the complexing agent is 1:(4-7).
7. The preparation method according to claim 6, Features In the step (2), the concentration of titanium in the metal salt solution is 0.1-0.5M; And / or, the solvent is water and / or ethanol.
8. The preparation method according to claim 3, It is characterized in that In the step (2), the temperature of the gelation treatment is 50-130° C., and optionally, the duration of the gelation treatment is 5-40 hours; And / or, the gelation treatment is carried out under a vacuum degree ≤-0.08 MPa; optionally, the vacuum degree is -0.1 MPa to -0.08 MPa.
9. The preparation method according to claim 3, It is characterized in that In the step (3), the mass ratio of the lithium nickel cobalt aluminum oxide positive electrode material to the coating material is 100: (0.002-0.008); And / or, the temperature of the calcination treatment is 600-800° C., and optionally, the duration of the calcination treatment is 6-15 hours; And / or, the calcination treatment is carried out in an atmosphere of air.
10. A positive electrode sheet, It is characterized in that It comprises a positive electrode current collector and a positive electrode active material layer arranged on at least one side of the positive electrode current collector, wherein the positive electrode active material layer comprises the modified titanium niobate coated ternary positive electrode material according to claim 1 or 2 or the modified titanium niobate coated ternary positive electrode material obtained by the preparation method according to claims 3-9.
Citation Information
Cited By
Positive plate for improving safety performance of lithium ion battery, preparation method of positive plate and lithium ion battery
CN122337995A