Hard carbon composite material and preparation method and application thereof
By forming a porous structure on the hard carbon negative electrode material and covering the metal oxide, the problem of low ICE of the hard carbon negative electrode material is solved, and its performance in sodium ion batteries is significantly improved, achieving high ICE and good cycling performance.
Patent Information
- Application Number
- CN202411216175.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
AI Technical Summary
The first Coulombic efficiency (ICE) of hard carbon anode materials is low, much lower than that of graphite anodes in lithium-ion batteries, limiting their commercial applications.
Using hard carbon composite materials, by forming a porous channel structure on the hard carbon matrix and covering metal oxides, the electrolyte interface reaction kinetics and charge-to-movement mechanics are improved, and the reversible capacity and cycling efficiency are increased.
The ICE and cycling performance of hard carbon anode material is significantly improved, and its charging and discharging performance and stability in sodium ion batteries are enhanced.
Smart Images

Figure CN119092682A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of energy storage materials, and in particular relates to a hard carbon composite material and a preparation method and application thereof. Background Art
[0002] Sodium-ion batteries are more cost-effective and sustainable than lithium-ion batteries because of their abundant reserves of sodium salt raw materials, the ability to use low-cost positive electrode materials (iron-manganese-nickel-based positive electrode materials), current collectors (aluminum foil) and low-concentration electrolytes, and are expected to become a substitute for lithium-ion batteries.
[0003] Among the potential anode materials for sodium-ion batteries, hard carbon has attracted much attention due to its competitive advantages in capacity and operation potential. However, the commercialization of hard carbon anode materials faces several obstacles, mainly the low first coulombic efficiency (ICE), which is much lower than that of graphite anode in lithium-ion batteries. Summary of the invention
[0004] The purpose of the present application is to provide a hard carbon composite material and a preparation method and application thereof, aiming to solve the problem of low ICE of hard carbon negative electrode materials.
[0005] In order to achieve the above application purpose, the technical solution adopted in this application is as follows:
[0006] In a first aspect, the present application provides a hard carbon composite material, comprising a hard carbon matrix and a metal oxide, wherein the hard carbon matrix has multiple pores, and the metal oxide is distributed on the outer surface of the hard carbon matrix and the inner wall surface of the pores.
[0007] Hard carbon composites have both a multi-porous structure and metal oxides. The multi-porous structure can construct continuous connecting channels to accelerate the transport of electrolytes. Electrolytes are an important factor in the formation of electrolyte interface (SEI) films, so they are beneficial to the reaction kinetics of SEI films. The multi-porous structure gives the material a high specific surface area, so there is a large contact area between the electrolyte and the material, which is beneficial to the formation of good contact between the electrolyte and the material, thereby shortening the active ions in the battery, such as Na + The diffusion path promotes the charge transfer kinetics of the material. The reaction kinetics of the SEI film and the charge largely determines the ICE of the material. Therefore, the multi-porous structure of the embodiment of the present application improves the ICE of the material by improving the reaction kinetics of the SEI film and the charge.
[0008] The outer surface of the hard carbon matrix and the inner wall of the pores are covered with metal oxides, which can serve as an artificial SEI film on the electrode surface. They can effectively inhibit the decomposition of the electrolyte both on the outer surface and in the pores of the material (usually the formation of the SEI film includes the decomposition and deposition of the electrolyte and other substances. Therefore, using metal oxides as artificial SEI films can inhibit the decomposition of the electrolyte and reduce the consumption of the electrolyte), reduce the interface resistance and electrode overpotential, thereby increasing the reversible capacity and making the material have high ICE and cycle efficiency.
[0009] Therefore, under the combined effect of the porous structure and metal oxides, the ICE of the material can be greatly improved, and the cycle performance of the material can also be improved.
[0010] In some embodiments, the metal oxide is coated on the outer surface of the hard carbon matrix and the inner wall of the pore. The metal oxide is coated on the outer surface of the hard carbon matrix and the inner wall of the pore to form a coating layer, which can form a partial coating or a complete coating on the outer surface of the hard carbon matrix and the inner wall of the pore independently. The metal oxide forms a coating layer, which acts as an artificial SEI film to isolate the inside of the material from the electrolyte, effectively inhibit the decomposition of the electrolyte, reduce the interface resistance and electrode overpotential, thereby increasing the reversible capacity and making the material have high ICE and cycle efficiency.
[0011] In some embodiments, the pore volume or porosity of the hard carbon composite material gradually decreases from the inside of the hard carbon matrix to its outer surface. In this direction, the pore volume or porosity gradually decreases, which is conducive to the coverage of the metal oxide on the inner wall surface of the hard carbon matrix pore channel, reducing the loss of the metal oxide, and then giving full play to the role of the metal oxide as an artificial SEI film to isolate the inside of the material from the electrolyte and effectively inhibit the decomposition of the electrolyte.
[0012] In some embodiments, the average pore size of the hard carbon composite material is in the range of 1.2 to 4 nm. + The storage model divides the discharge curve into two regions: the slope region and the platform region. The platform region is related to the pore structure. Generally, the larger the pore size, the more conducive it is to the insertion and extraction of sodium ions. A larger pore size can provide more channels, reduce the diffusion resistance of sodium ions, and thus improve the cycle performance of the material. Therefore, by providing a multi-pore channel with the above pore size, it is beneficial to improve the discharge capacity and cycle performance of the platform region.
[0013] In some embodiments, the pore volume of the hard carbon composite material is 0.01 to 0.15 cm 3 / g. The hard carbon composite material has a large pore volume, can provide a large sodium ion storage space, and has a good sodium storage capacity, which is beneficial to improve the charge and discharge capacity.
[0014] In some embodiments, the BET specific surface area of the hard carbon composite material is 4 to 100 m 2 / g. The hard carbon composite material has a moderate specific surface area and has more active sites, which can increase the embedding amount of sodium ions and thus improve the first charge capacity.
[0015] In some embodiments, the mass percentage of the metal oxide in the hard carbon composite material is 0.5wt% to 5wt%. Distributing a certain amount of metal oxide in the hard carbon composite material can effectively inhibit the direct contact between the electrolyte and the active material, reduce side reactions, and thus improve ICE and cycle stability. At the same time, at this mass content, the metal oxide can not occupy too much of the hard carbon matrix used to provide capacity, so that the hard carbon composite material has a high capacity.
[0016] In some embodiments, the metal oxide includes one or more of aluminum oxide, zinc oxide, zirconium dioxide, and titanium dioxide. After these metal oxides cover the outer surface and the inner wall of the pores of the hard carbon composite material, they can inhibit the direct contact between the electrolyte and the active material, reduce side reactions, and thus improve ICE and cycle stability.
[0017] In some embodiments, the hard carbon composite material further includes graphite dispersed in the hard carbon matrix.
[0018] The graphite is dispersed in the hard carbon matrix, and the graphite can be embedded in the skeleton of the hard carbon matrix or distributed on the skeleton surface of the hard carbon matrix, forming an inseparable whole with the hard carbon matrix. + The storage model divides the discharge curve into two regions: the slope region and the platform region. The slope region is the graphite domain, which is formed by the random stacking of a few layers of graphene (graphene plane, the microscopic basic unit of carbon materials), usually composed of Na + Inserting stacked graphene or adsorbing on defective surfaces forms a slope capacity. The hard carbon composite material of the present application contains graphite, which is conducive to the formation and extension of the slope area, thereby improving the slope capacity. The slope capacity is an important component of the discharge capacity, so improving the slope capacity is conducive to improving the discharge capacity, which in turn is conducive to improving the ICE of the material.
[0019] In some embodiments, the carbon interlayer spacing of the hard carbon composite material is 0.365-0.385 nm. Too low a carbon interlayer spacing is not conducive to Na + If the carbon interlayer spacing is too high, the material cycle performance will be seriously degraded. Appropriate carbon interlayer spacing is conducive to the storage of Na + The insertion and storage of hard carbon composites make them exhibit high rate performance.
[0020] In some embodiments, the degree of graphitization of the hard carbon composite material is 2% to 20%. Generally, the higher the degree of graphitization, the better the conductivity of the material, thereby increasing the active ions such as Na + The migration speed is beneficial to enhance the ICE and cycle performance of the material. At the same time, the material with a moderate degree of graphitization can provide a large sodium ion embedding capacity, which can improve the first charge capacity of the material.
[0021] In some embodiments, the mass percentage of graphite in the hard carbon composite material is 2 wt % to 5 wt %.
[0022] In some embodiments, oxygen-containing functional groups are distributed in the hard carbon composite material, and the oxygen content of the hard carbon composite material is 3wt% to 5wt%. The oxygen-containing functional groups can serve as important active sites of the hard carbon composite material and can react with Na + Binds, helps store and release Na + , charge, which is beneficial to improving the capacity and ICE of the material.
[0023] In a second aspect, the present application provides a method for preparing a hard carbon composite material, comprising:
[0024] Providing a carbon precursor and etching the carbon precursor; the carbon precursor includes a hard carbon precursor and a pore former, the pore former is distributed in the hard carbon precursor, and the pore former contains a metal element;
[0025] The calcination treatment is carried out under a protective atmosphere.
[0026] In the preparation method of the embodiment of the present application, the carbon precursor is etched to form corrosion from the outside to the inside, forming a loose multi-porous structure; and the pore-forming agent decomposes under high-temperature calcination to produce gas, which etches from the inside to the outside to form open pores and a large number of closed pores. Under the combined action of the inside and outside, a multi-porous structure, especially a sponge-like multi-porous structure, can be finally obtained, which greatly enriches the pores of the hard carbon composite material.
[0027] This multi-porous channel can construct a continuous connection channel to accelerate the transport of electrolytes. Electrolytes are an important factor in the formation of SEI membranes, so they are beneficial to the reaction kinetics of SEI membranes. The multi-porous structure gives the material a high specific surface area, so there is a large contact area between the electrolyte and the material, which is beneficial to the formation of good contact between the electrolyte and the material, thereby shortening the active ions in the battery, such as Na + The diffusion path promotes the charge transfer kinetics of the material. The reaction kinetics of the SEI film and the charge largely determines the ICE of the material. Therefore, the multi-porous structure of the embodiment of the present application improves the ICE of the material by improving the reaction kinetics of the SEI film and the charge.
[0028] At the same time, part of the pore former flows out of the outer surface of the carbon precursor through the pores formed above, and the distribution range of the pore former includes: in the pores and on the outer surface of the carbon precursor. Then, during the calcination process, the metal oxides formed by the decomposition of the metal elements in these pore formers can cover the inner wall of the pores of the hard carbon matrix formed by carbonization and the outer surface of the hard carbon. The formed metal oxide covering layer can serve as an artificial SEI, effectively inhibiting the decomposition of the electrolyte during the battery charging and discharging process, and showing high ICE and cycle stability.
[0029] Therefore, through the preparation method of the embodiment of the present application, a hard carbon matrix with a multi-porous structure can be obtained, and metal oxides are distributed on the inner wall and outer surface of the pores of the hard carbon matrix. Under the action of the multi-porous structure and metal oxides, the ICE of the material can be greatly improved, and the cycle performance of the material can also be improved.
[0030] In some embodiments, the melting point of the pore former is 800-1400° C. The pore former has a lower melting point, so during the calcination process, before or during the decomposition of the pore former, the pore former can melt and flow, so that the metal oxide formed after its decomposition can be distributed on the outer surface of the hard carbon matrix and the inner wall of the pores at the same time.
[0031] In some embodiments, the pore former includes one or more of metal carbonates, metal bicarbonates, and metal chlorides. The metal element in the pore former includes one or more of Al, Zn, Zr, and Ti. For example, the pore former may specifically include one or more of Al2(CO3)3, ZnCO3, NH4Al(OH)CO3, ZnCl2, and Zr(OH)2CO3·ZrO2.
[0032] These pore formers have multiple functions during the calcination process:
[0033] 1) Decomposition produces gas, which etches the material from the inside out and enriches the pore structure of the material;
[0034] 2) It can melt and flow at high temperature and decompose to form metal oxides, which are distributed on the inner wall and outer surface of the hard carbon pores to form a covering layer. This covering layer can serve as an artificial SEI, effectively inhibiting the decomposition of the electrolyte during the battery charge and discharge process, and exhibiting high ICE and cycle stability;
[0035] 3) It can catalyze the carbonization of nearby hard carbon precursors and cause graphitization reaction to form a local graphitized structure. The interlayer spacing of graphite is larger than that of hard carbon, so it can expand the overall carbon interlayer spacing of hard carbon composite materials; at the same time, the pore-forming agent containing metal elements can also inhibit the excessive growth of graphite layers, so that the material has a suitable carbon interlayer spacing, and a reasonable carbon interlayer spacing can improve the rate performance of the material; and the presence of graphite is conducive to the formation and extension of the slope zone, thereby increasing the slope capacity and improving ICE.
[0036] 4) For pore-forming agents containing carbonate or bicarbonate, they can decompose to produce CO2, and CO2 reacts with the carbon formed by calcination to form CO. Part of the CO remains in the pore structure of the material and chemically combines to form oxygen-containing functional groups, thereby increasing the oxygen-containing functional groups of the hard carbon composite material. These oxygen-containing functional groups are one of the important performance providers of the hard carbon material, and therefore are beneficial to improving the physical and chemical properties of the hard carbon material.
[0037] In some embodiments, the hard carbon precursor includes one or more of a biomass-based precursor, an organic polymer-based precursor, and a fossil fuel-based precursor.
[0038] In some embodiments, the mass ratio of the pore former to the hard carbon precursor is 1:(0.1-10).
[0039] In some embodiments, the method for preparing the carbon precursor includes: mixing a pore former with a hard carbon precursor; or, mixing the pore former with a reaction material of the hard carbon precursor, and reacting the reaction material of the hard carbon precursor to generate the hard carbon precursor.
[0040] In some embodiments, the etching treatment method includes one or more of acid etching, alkaline etching, and gas phase etching. These methods can produce an outside-to-inside corrosion effect on the carbon precursor to form a loose multi-porous structure.
[0041] In some embodiments, the calcination temperature is 1100-1600° C., optionally 1200-1400° C. At high temperatures, the hard carbon precursor can be carbonized to form a hard carbon matrix. At the same time, the pore-forming agent can melt and flow from the inside of the carbon precursor through the pores and partially reach the surface of the carbon precursor, and decompose into metal oxides, thereby being distributed on the inner and outer surfaces of the pores of the hard carbon matrix.
[0042] In some embodiments, the calcination treatment time is 2 to 6 hours, optionally 2 to 4 hours.
[0043] In a third aspect, the present application provides a negative electrode, comprising the hard carbon composite material, or comprising a hard carbon composite material prepared according to the above preparation method.
[0044] In a fourth aspect, the present application provides a sodium battery, comprising the above-mentioned negative electrode or the above-mentioned hard carbon composite material, or comprising the hard carbon composite material prepared according to the above-mentioned preparation method.
[0045] The hard carbon composite material of the present application exhibits high ICE and good cycle performance, so applying it to negative electrodes and batteries is beneficial to improving their charge-discharge performance and cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0047] Figure 1 is a scanning electron microscope image (SEM image) of the hard carbon composite material provided in Example 1 of the present application;
[0048] Figure 2 It is the transmission electron microscopy scanning spectrum (TEM mapping spectrum) of the hard carbon composite material provided in Example 1 of the present application;
[0049] Figure 3 This is a scanning electron microscope image (SEM image) of the hard carbon composite material provided in Comparative Example 4 of the present application. DETAILED DESCRIPTION
[0050] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0051] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.
[0052] In this application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b and c", can all mean: a, b, c, ab (i.e. a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.
[0053] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.
[0054] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0055] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass described in the embodiment description of the present application can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.
[0056] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. For example, without departing from the scope of the embodiments of the present application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features.
[0057] A first aspect of an embodiment of the present application provides a hard carbon composite material, including a hard carbon matrix and a metal oxide, wherein the hard carbon matrix has multiple pores, and the metal oxide is distributed on the outer surface of the hard carbon matrix and the inner wall surface of the pores.
[0058] Among them, a multi-porous channel is a structure with multiple interconnected channels, which form a network inside the material to provide a multi-dimensional transmission channel. The multi-porous channel of the embodiment of the present application can be a sponge-like multi-porous channel (a material structure with a sponge-like morphology, which has many interconnected holes and channels, and these holes and channels form a complex network inside the material).
[0059] The hard carbon composite material of the embodiment of the present application has both a multi-porous structure and a metal oxide. The multi-porous structure can construct a continuous connection channel to accelerate the transport of electrolytes. The electrolyte is an important factor in the formation of the electrolyte interface (SEI) film, so it is beneficial to the reaction kinetics of the SEI film; and the multi-porous structure makes the material have a high specific surface area, so there is a large contact area between the electrolyte and the material, which is beneficial to the formation of good contact between the electrolyte and the material, thereby shortening the active ions such as Na in the battery. +The diffusion path promotes the charge transfer kinetics of the material. The reaction kinetics of the SEI film and the charge largely determines the ICE of the material. Therefore, the multi-porous structure of the embodiment of the present application improves the ICE of the material by improving the reaction kinetics of the SEI film and the charge.
[0060] The outer surface of the hard carbon matrix and the inner wall of the pores are covered with metal oxides, which can serve as an artificial SEI film on the electrode surface. They can effectively inhibit the decomposition of the electrolyte both on the outer surface and in the pores of the material (usually the formation of the SEI film includes the decomposition and deposition of the electrolyte and other substances. Therefore, using metal oxides as artificial SEI films can inhibit the decomposition of the electrolyte and reduce the consumption of the electrolyte), reduce the interface resistance and electrode overpotential, thereby increasing the reversible capacity and making the material have high ICE and cycle efficiency.
[0061] Therefore, under the combined effect of the porous structure and metal oxides, the ICE of the material can be greatly improved, and the cycle performance of the material can also be improved.
[0062] In some embodiments, the metal oxide is coated on the outer surface of the hard carbon matrix and the inner wall of the pore. The metal oxide is coated on the outer surface of the hard carbon matrix and the inner wall of the pore to form a coating layer, which can form a partial coating or a complete coating on the outer surface of the hard carbon matrix and the inner wall of the pore independently. The metal oxide forms a coating layer, which acts as an artificial SEI film to isolate the inside of the material from the electrolyte, effectively inhibit the decomposition of the electrolyte, reduce the interface resistance and electrode overpotential, thereby increasing the reversible capacity and making the material have high ICE and cycle efficiency.
[0063] In some embodiments, the pore volume or porosity of the hard carbon composite material gradually decreases from the inside of the hard carbon matrix to its outer surface. In this direction, the pore volume or porosity gradually decreases, which is conducive to the coverage of the metal oxide on the inner wall surface of the hard carbon matrix pore channel, reducing the loss of the metal oxide, and then giving full play to the role of the metal oxide as an artificial SEI film to isolate the inside of the material from the electrolyte and effectively inhibit the decomposition of the electrolyte.
[0064] In some embodiments, the average pore size of the hard carbon composite material is in the range of 1.2 to 4 nm, and optionally in the range of 1.2 to 2.5 nm, for example, any one of 1.2 nm, 1.5 nm, 2 nm, 2.5 nm, 3 nm, 3.5 nm, 4 nm, or any two thereof. +The storage model divides the discharge curve into two regions: the slope region and the platform region. The platform region is related to the pore structure. Generally, the larger the pore size, the more conducive it is to the insertion and extraction of sodium ions. A larger pore size can provide more channels, reduce the diffusion resistance of sodium ions, and thus improve the cycle performance of the material. Therefore, by providing a multi-pore channel with the above pore size, it is beneficial to improve the discharge capacity and cycle performance of the platform region.
[0065] In some embodiments, the pore volume of the hard carbon composite material is 0.01 to 0.15 cm 3 / g, optionally 0.05 to 0.15 cm 3 / g, for example 0.01cm 3 / g,0.05cm 3 / g,0.1cm 3 / g, 0.15cm 3 / g or any two thereof. The hard carbon composite material has a large pore volume, can provide a large sodium ion storage space, and has a good sodium storage capacity, which is beneficial to improve the charge and discharge capacity.
[0066] In some embodiments, the BET specific surface area of the hard carbon composite material is 4 to 100 m 2 / g, optionally 25~100m 2 / g, for example 4m 2 / g,10m 2 / g,20m 2 / g,25m 2 / g,30m 2 / g,4m 2 / g,50m 2 / g,60m 2 / g,70m 2 / g,80m 2 / g,90m 2 / g,100m 2 The hard carbon composite material has a moderate specific surface area and more active sites, which can increase the amount of sodium ions inserted, thereby increasing the first charge capacity.
[0067] In some embodiments, the mass percentage of the metal oxide in the hard carbon composite material is 0.5wt% to 5wt%, such as 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt%, 5wt% or any range between two of them. Distributing a certain amount of metal oxide in the hard carbon composite material can effectively inhibit the direct contact between the electrolyte and the active material, reduce side reactions, and thus improve ICE and cycle stability. At the same time, at this mass content, the metal oxide can not occupy too much of the hard carbon matrix used to provide capacity, so that the hard carbon composite material has a high capacity.
[0068] In some embodiments, the metal oxide includes one or more of aluminum oxide, zinc oxide, zirconium dioxide, and titanium dioxide. After these metal oxides cover the outer surface and the inner wall of the pores of the hard carbon composite material, they can inhibit the direct contact between the electrolyte and the active material, reduce side reactions, and thus improve the ICE rate and cycle stability.
[0069] In some embodiments, the hard carbon composite material further includes graphite dispersed in the hard carbon matrix.
[0070] The graphite is dispersed in the hard carbon matrix, and the graphite can be embedded in the skeleton of the hard carbon matrix or distributed on the skeleton surface of the hard carbon matrix, forming an inseparable whole with the hard carbon matrix. + The storage model divides the discharge curve into two regions: the slope region and the platform region. The slope region is the graphite domain, which is formed by the random stacking of a few layers of graphene (graphene plane, the microscopic basic unit of carbon materials), usually composed of Na + Inserting stacked graphene or adsorbing on the defect surface forms a slope capacity. The hard carbon composite material of the embodiment of the present application contains graphite, which is conducive to the formation and extension of the slope area, thereby improving the slope capacity. The slope capacity is an important component of the discharge capacity, so improving the slope capacity is conducive to improving the discharge capacity, which in turn is conducive to improving the ICE of the material.
[0071] At the same time, graphite has excellent electrical conductivity, so graphite dispersed in the hard carbon matrix is also beneficial to improve the conductivity of the material, thereby increasing the active ions such as Na + The migration speed is beneficial to enhance the ICE and cycle performance of the material.
[0072] In some embodiments, the carbon interlayer spacing of the hard carbon composite material is 0.365-0.385 nm, for example, any one of 0.365 nm, 0.370 nm, 0.375 nm, 0.380 nm, 0.385 nm or any two thereof. A low carbon interlayer spacing is not conducive to Na +If the carbon interlayer spacing is too high, the material cycle performance will be seriously degraded. Appropriate carbon interlayer spacing is conducive to the storage of Na + The insertion and storage of hard carbon composites make them exhibit high rate performance.
[0073] In some embodiments, the degree of graphitization of the hard carbon composite material is 2% to 20%, for example, 2%, 4%, 6%, 8%, 10%, 12%, 14%, 16%, 18%, 20% or any two thereof. Generally, the higher the degree of graphitization, the better the conductivity of the material, thereby increasing the active ions such as Na + The migration speed is beneficial to enhance the ICE and cycle performance of the material. At the same time, the material with a moderate degree of graphitization can provide a large sodium ion embedding capacity, which can improve the first charge capacity of the material.
[0074] In some embodiments, the mass percentage of graphite in the hard carbon composite material is 2 wt % to 5 wt %, for example, any one of 2 wt %, 3 wt %, 4 wt %, 5 wt % or any two thereof.
[0075] In some embodiments, oxygen-containing functional groups are distributed in the hard carbon composite material, and the oxygen mass content of the hard carbon composite material is 3wt% to 5wt%, such as any one of 3wt%, 3.5wt%, 4wt%, 4.5wt%, 5wt% or any two thereof. The oxygen-containing functional groups can serve as important active sites of the hard carbon composite material, and can react with Na + Binds, helps store and release Na + , charge, which is beneficial to improving the capacity and ICE of the material.
[0076] A second aspect of the embodiment of the present application provides a method for preparing a hard carbon composite material, comprising:
[0077] Providing a carbon precursor and etching the carbon precursor; the carbon precursor includes a hard carbon precursor and a pore former, the pore former is distributed in the hard carbon precursor, and the pore former contains a metal element;
[0078] The calcination treatment is carried out under a protective atmosphere.
[0079] In the embodiments of the present application, the hard carbon precursor refers to a substance that can generate hard carbon after high temperature or other effects. The pore former refers to a substance that can decompose and generate gas. The pore former is distributed in the hard carbon precursor, which may include the situation where the pore former is encapsulated in the hard carbon precursor.
[0080] In the preparation method of the embodiment of the present application, the carbon precursor is etched to form corrosion from the outside to the inside, forming a loose multi-porous structure; and the pore-forming agent decomposes under high-temperature calcination to produce gas, which etches from the inside to the outside to form open pores and a large number of closed pores. Under the combined action of the inside and outside, a multi-porous structure, especially a sponge-like multi-porous structure, can be finally obtained, which greatly enriches the pores of the hard carbon composite material.
[0081] This multi-porous structure can construct continuous connection channels and accelerate the transport of electrolytes. Electrolytes are an important factor in the formation of SEI membranes, so they are beneficial to the reaction kinetics of SEI membranes. In addition, the multi-porous structure gives the material a high specific surface area, so there is a large contact area between the electrolyte and the material, which is beneficial to the formation of good contact between the electrolyte and the material, thereby shortening the active ions in the battery, such as Na + The diffusion path promotes the charge transfer kinetics of the material. The reaction kinetics of the SEI film and the charge largely determines the ICE of the material. Therefore, the multi-porous structure of the embodiment of the present application improves the ICE of the material by improving the reaction kinetics of the SEI film and the charge.
[0082] At the same time, part of the pore former flows out of the outer surface of the carbon precursor through the pores formed above, and the distribution range of the pore former includes: in the pores and on the outer surface of the carbon precursor. Then, during the calcination process, the metal oxides formed by the decomposition of the metal elements in these pore formers can cover the inner wall of the pores of the hard carbon matrix formed by carbonization and the outer surface of the hard carbon matrix. The formed metal oxide covering layer can serve as an artificial SEI, effectively inhibiting the decomposition of the electrolyte during the battery charging and discharging process, and showing high ICE and cycle stability.
[0083] Therefore, through the preparation method of the embodiment of the present application, a hard carbon matrix with multiple channels can be obtained, and metal oxides are distributed on the inner wall and outer surface of the channels of the hard carbon matrix. Under the action of the multi-porous structure and metal oxides, the ICE of the material can be greatly improved, and the cycle performance of the material can also be improved.
[0084] In some embodiments, the melting point of the pore former is 800-1400° C., for example, any one of 800° C., 900° C., 1000° C., 1100° C., 1200° C., 1300° C., 1400° C. or any two thereof. The pore former has a lower melting point, so that during the calcination process, before or during the decomposition of the pore former, the pore former can melt and flow, so that the metal oxide formed after its decomposition can be distributed simultaneously on the outer surface of the hard carbon matrix and the inner wall surface of the pores.
[0085] In some embodiments, the pore former includes one or more of metal carbonates, metal bicarbonates, and metal chlorides. The metal element in the pore former includes one or more of Al, Zn, Zr, and Ti. For example, the pore former may specifically include one or more of Al2(CO3)3 (melting point of about 1300°C), ZnCO3, NH4Al(OH)CO3, ZnCl2, and Zr(OH)2CO3·ZrO2.
[0086] These pore formers have multiple functions during the calcination process:
[0087] 1) Decomposition produces gas, which etches the material from the inside out and enriches the pore structure of the material;
[0088] 2) It can melt and flow at high temperature and decompose to form metal oxides, which are distributed on the inner wall and outer surface of the hard carbon pores to form a covering layer. This covering layer can serve as an artificial SEI, effectively inhibiting the decomposition of the electrolyte during the battery charge and discharge process, and exhibiting high ICE and cycle stability;
[0089] 3) It can catalyze the carbonization of nearby hard carbon precursors and cause graphitization reaction to form a local graphitized structure. The interlayer spacing of graphite is larger than that of hard carbon, so it can expand the overall carbon interlayer spacing of hard carbon composite materials; at the same time, the pore-forming agent containing metal elements can also inhibit the excessive growth of graphite layers, so that the material has a suitable carbon interlayer spacing, and a reasonable carbon interlayer spacing can improve the rate performance of the material; and the presence of graphite is conducive to the formation and extension of the slope zone, thereby increasing the slope capacity and improving ICE.
[0090] 4) For pore-forming agents containing carbonate or bicarbonate, they can decompose to produce CO2, and CO2 reacts with the carbon formed by calcination to form CO. Part of the CO remains in the pore structure of the material and chemically combines to form oxygen-containing functional groups, thereby increasing the oxygen-containing functional groups of the hard carbon composite material. These oxygen-containing functional groups are one of the important performance providers of the hard carbon composite material, and therefore are beneficial to improving the physical and chemical properties of the hard carbon composite material.
[0091] In some embodiments, the pore former has a nanometer particle size, for example, the particle size of the pore former is 30 to 400 nm, for example, any point value among 30 nm, 50 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm or a range between any two point values. The nanometer-sized pore former can be well dispersed in the hard carbon precursor and has good dispersibility in the hard carbon precursor.
[0092] In some embodiments, the hard carbon precursor includes one or more of a biomass precursor, an organic polymer precursor, and a fossil fuel precursor. The biomass precursor may include one or more of bamboo, coconut shell, starch, rice husk, and walnut shell; the organic polymer precursor includes one or more of phenolic resin, polyacrylonitrile, polyimide, and cellulose; the fossil fuel precursor includes one or more of coal, asphalt, and petroleum extracts.
[0093] In some embodiments, the mass ratio of the pore former to the hard carbon precursor is 1:(0.1-10), for example, any point value or a range between any two points in 1:0.1, 1:0.5, 1:1, 1:2, 1:4, 1:6, 1:8, 1:10. The pore former and the hard carbon precursor can be combined in a large mass ratio, which can not only make the pore former well distributed in the hard carbon precursor, but also have flexible operation convenience.
[0094] In some embodiments, the method for preparing the carbon precursor includes: mixing a pore former with a hard carbon precursor; or, mixing the pore former with a reaction material of the hard carbon precursor, and reacting the reaction material of the hard carbon precursor to generate the hard carbon precursor.
[0095] The reaction raw materials of the hard carbon precursor are substances that can generate the hard carbon precursor through reaction. For example, for an organic polymer precursor, the reaction raw materials can be various organic monomers.
[0096] More specifically, for example, for phenolic resin, its reaction raw materials include a first monomer and a second monomer, the first monomer includes a phenolic compound, and the second monomer includes an aldehyde compound.
[0097] The phenolic compounds include one or more of monohydric phenol, dihydric phenol and polyhydric phenol.
[0098] Monophenol is a compound formed by replacing a hydrogen atom on a benzene ring with a hydroxyl group, such as one or more of phenol, C1-C10 alkyl-substituted phenol, amino-substituted phenol, and halogen-substituted phenol. Among them, C1-C10 alkyl-substituted phenol may include phenols with one or more C1-C10 alkyl substituents, such as cresol, xylenol, ethylphenol, propylphenol, butylphenol, etc. In the case of having multiple substituents, the position between any substituent and the hydroxyl group includes any one or more of the ortho position, meta position, and para position. The benzene ring of amino-substituted phenol includes one or more amino groups, and the position between any amino group and the hydroxyl group includes any one or more of the ortho position, meta position, and para position, such as 3-aminophenol and 2-aminophenol. Halogen-substituted phenol includes one or more of bromine-substituted phenol and chlorine-substituted phenol, and the position between any halogen and the hydroxyl group includes any one or more of the ortho position, meta position, and para position.
[0099] Dihydric phenol is a compound formed by replacing two hydrogen atoms on a benzene ring with two hydroxyl groups, including one or more of catechol (ortho-diphenol, resorcinol, and hydroquinone), C1-C10 alkyl-substituted diphenol, amino-substituted diphenol, and halogen-substituted diphenol.
[0100] Polyphenols are compounds formed by replacing two or more hydrogen atoms on a benzene ring with two hydroxyl groups, including, for example, one or more of pyrogallol, C1-C10 alkyl-substituted pyrogallol, amino-substituted pyrogallol, and halogen-substituted pyrogallol.
[0101] The aldehyde compounds include one or more of C1-C10 alkyl aldehydes and furfural, and the C1-C10 alkyl aldehydes include one or more of formaldehyde, acetaldehyde, propionaldehyde, butyraldehyde, 2-methylbutyraldehyde, valeraldehyde, hexanal, heptaldehyde, nonanal and 2-ethylhexanal.
[0102] Phenolic compounds and aldehyde compounds can be polymerized to form phenolic resins.
[0103] More specifically, when the hard carbon precursor includes phenolic resin, the method for preparing the carbon precursor includes: mixing a pore former with a first monomer and then adding a second monomer for polymerization; or, mixing a pore former with a second monomer and then adding the first monomer for polymerization.
[0104] The pore-forming agent is first mixed evenly with one of the monomers, and then the other monomer is added, so that the pore-forming agent can be wrapped in the polymer during the polymerization process.
[0105] The polymerization reaction temperature is 50-120°C, optionally 60-100°C, for example, it can be any point value among 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, 110°C, 120°C or the range between any two points.
[0106] The polymerization reaction time is 1 to 8 hours, optionally 3 to 5 hours, for example, any point value among 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h or the range between any two points.
[0107] The polymerization reaction is carried out under stirring. Stirring can promote uniform mixing of various substances, accelerate the reaction, and form microspherical polymers (polymer microspheres).
[0108] The molar ratio of the pore-forming agent, the first monomer and the second monomer is 1:(3-20):(1-4), optionally 1:(6-20):(1-4), and further optionally 1:(8-12):(2-3), for example, any point value among 1:3:1, 1:6:1, 1:8:2, 1:10:2, 1:15:2, 1:16:4, 1:20:3, or a range between any two point values.
[0109] The polymerization reaction is carried out in an organic solvent, which includes one or more of acetone, methanol, and ethanol. Carrying out the polymerization reaction in an organic solvent can improve the solubility of the monomer, so that the polymerization reaction proceeds smoothly, and can also prevent the pore-forming agent from hydrolyzing.
[0110] In some embodiments, the etching treatment method includes one or more of acid etching, alkaline etching, and gas phase etching. These methods can produce an outside-to-inside corrosion effect on the carbon precursor to form a loose multi-porous structure.
[0111] In some embodiments, the acid used for acid etching includes one or more of sulfuric acid, nitric acid, and hydrochloric acid. Generally, the etching effect is better when concentrated acid is used, and the concentration of the acid is 2 to 6M, for example, any point value among 2M, 3M, 4M, 5M, and 6M or a range between any two points.
[0112] In some embodiments, the acid etching temperature is 50-80° C., optionally 50-70° C., for example, any point value or a range between any two points of 50° C., 55° C., 60° C., 65° C., 70° C., 75° C., and 80° C. The acid etching temperature can be controlled by a constant temperature water bath.
[0113] In some embodiments, the acid etching time is 2 to 18 hours, optionally 4 to 10 hours, for example, any point value among 2 hours, 4 hours, 6 hours, 8 hours, 10 hours, 12 hours, 14 hours, 16 hours, 18 hours or a range between any two points.
[0114] In some embodiments, the mass ratio of the carbon precursor to the acid is 1:(0.5-10), for example, any value among 1:0.5, 1:1, 1:2, 1:4, 1:6, 1:8, 1:10 or a range between any two values.
[0115] In some embodiments, the alkali used for alkaline etching includes one or more of sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, sodium bicarbonate, and potassium bicarbonate.
[0116] The temperature of alkali etching is 600-800°C, for example, any point value among 600°C, 650°C, 700°C, 750°C, 800°C or a range between any two points. The temperature can be controlled in a tube furnace or a muffle furnace; the time of alkali etching is 2-8h, for example, any point value among 2h, 4h, 6h, 8h or a range between any two points.
[0117] The mass ratio of the reagent used for alkali etching to the carbon precursor is 1:(0.2-2), for example, any value among 1:0.2, 1:0.5, 1:1, 1:1.5, 1:2 or a range between any two values.
[0118] In some embodiments, the etching raw materials used for gas phase etching include one or more of carbon dioxide and water vapor; the temperature of gas phase etching is 800-1100°C, for example, any point value among 800°C, 850°C, 900°C, 950°C, 1000°C, 1100°C or a range between any two point values; the time of gas phase etching is 2-8h, for example, any point value among 2h, 4h, 6h, 8h or a range between any two point values; the gas flow rate is 100-1000mL / min, for example, any point value among 100mL / min, 200mL / min, 400mL / min, 600mL / min, 800mL / min, 1000mL / min or a range between any two point values. Temperature and flow control can be performed in a tube furnace or a muffle furnace.
[0119] Before the etching step, the carbon precursor can be crushed into powder, so that the carbon precursor and the etchant can be evenly mixed, improving the efficiency and uniformity of etching. After the etching is completed, the sample can be processed by centrifugal filtration, water washing to neutrality, etc., so as to carry out the next calcination treatment.
[0120] In some embodiments, the temperature of the calcination treatment is 1100-1600°C, optionally 1200-1400°C, for example, any point value among 1100°C, 1200°C, 1300°C, 1400°C, 1500°C, 1600°C or a range between any two point values. At high temperatures, the hard carbon precursor can be carbonized to form a hard carbon matrix. At the same time, the pore-forming agent can melt and flow, flow through the pores from the inside of the carbon precursor and partially reach the surface of the carbon precursor, and decompose into metal oxides, thereby being distributed on the inner wall and outer surface of the pores of the hard carbon matrix.
[0121] In some embodiments, the calcination time is 2 to 6 hours, optionally 2 to 4 hours, such as any point value of 2 hours, 3 hours, 4 hours, 5 hours, 6 hours or a range between any two points. The calcination time refers to the holding time at the desired calcination temperature after the desired calcination temperature is reached.
[0122] In some embodiments, before the calcination treatment, a pre-calcination treatment is further included, and the temperature of the pre-calcination treatment is 700-1000° C., optionally 750-850° C., for example, any point value or a range between any two points of 700° C., 750° C., 800° C., 850° C., 900° C., 950° C., 1000° C. The pre-calcination treatment can better arrange and arrange the crystal structure in the material, thereby improving the structure and performance of the material.
[0123] The pre-calcination treatment time is 1 to 4 hours, and optionally 1 to 3 hours, such as any point value among 1 hour, 2 hours, 3 hours, and 4 hours, or a range between any two points. The pre-calcination treatment time refers to the holding time at the desired pre-calcination temperature after the desired pre-calcination temperature is reached.
[0124] In some embodiments, the protective atmosphere includes one or more of nitrogen, argon, neon, and helium. The calcination and pre-calcination are both performed under a protective atmosphere. When the calcination and pre-calcination are performed under a protective atmosphere, the carbon precursor will not be oxidized, and hard carbon can be obtained smoothly.
[0125] A third aspect of an embodiment of the present application provides a negative electrode, comprising the hard carbon composite material mentioned above, or comprising the hard carbon composite material prepared according to the above preparation method.
[0126] A fourth aspect of an embodiment of the present application provides a battery, comprising the above-mentioned negative electrode or the above-mentioned hard carbon composite material, or comprising a hard carbon composite material prepared according to the above-mentioned preparation method.
[0127] The battery may include one or more of a sodium ion battery and a lithium ion battery, and may optionally include a sodium ion battery.
[0128] The hard carbon composite material of the embodiment of the present application shows high ICE and good cycle performance, so its application in negative electrodes and batteries is beneficial to improving their charge-discharge performance and cycle performance.
[0129] The following describes the invention in conjunction with specific embodiments.
[0130] Example 1
[0131] This embodiment provides a hard carbon composite material, comprising a hard carbon matrix with a loose sponge-like multi-porous structure, wherein a portion of the outer surface of the hard carbon matrix and a portion of the inner wall surface of the pores are covered with an Al2O3 layer, and graphite is dispersed in the hard carbon matrix. A large number of oxygen-containing functional groups are also distributed in the hard carbon composite material.
[0132] The structural information of the hard carbon composite material is as follows:
[0133] (1) Multi-porous structure:
[0134] Average pore size: 2.2nm;
[0135] Pore volume: 0.09cm 3 / g; at the same time, it is observed that the porosity of the hard carbon composite material gradually decreases from the inside to the outer surface of the hard carbon matrix, that is, the pore volume gradually decreases;
[0136] Specific surface area: 50m 2 / g;
[0137] (2) Al2O3 layer
[0138] Al2O3 mass percentage: 2wt%;
[0139] (3) Graphite
[0140] Graphitization degree: 7%;
[0141] Carbon layer spacing: 0.37nm;
[0142] Graphite mass percentage: 2wt%;
[0143] (4) Oxygen mass content: 4%.
[0144] The preparation method of the hard carbon composite material of this embodiment comprises the following steps:
[0145] Step 1, dissolve 3-aminophenol and nano Al2(CO3)3 in ethanol and mix them evenly, then drop the formaldehyde solution into the previous mixture, and react for 4 hours under stirring at 75°C. Among them, the molar ratio of Al2(CO3)3, 3-aminophenol and formaldehyde is 1:8:2. Then centrifuge and wash, put it in an oven and dry it overnight to obtain a carbon precursor encapsulating Al2(CO3)3. In this process, 3-aminophenol and formaldehyde undergo a condensation reaction to form a phenolic resin, so the structure of the carbon precursor is specifically that Al2(CO3)3 is encapsulated in the phenolic resin, and according to the raw material ratio, it can be roughly calculated that the mass ratio of Al2(CO3)3 to the phenolic resin is about 1:4.
[0146] Step 2: ball-mill the carbon precursor to make it uniformly crushed and sieve to obtain powder. Then, mix the powder and concentrated sulfuric acid in a certain mass ratio (1:10) and mix them in a constant temperature water bath at 60°C for 6 hours for acid etching. After centrifuging and filtering the obtained sample, wash it with distilled water several times to make the pH neutral. After freeze-drying for 24 hours, heat the acid-etched carbon precursor to 800°C in an argon atmosphere for 2 hours, and then heat it to 1300°C and calcine it for 4 hours. The final hard carbon composite material is obtained.
[0147] Example 2
[0148] This embodiment provides a hard carbon composite material. The difference from the embodiment 1 is that the mass percentage of the Al2O3 layer in the hard carbon composite material is 1wt%, and the pore volume is 0.05cm 3 / g, specific surface area is 25m 2 / g.
[0149] The preparation method of the hard carbon composite material of this embodiment is different from that of Embodiment 1 in that the amount of Al2(CO3)3 added is less, and the molar ratio of Al2(CO3)3, 3-aminophenol and formaldehyde solution is 1:16:4.
[0150] Example 3
[0151] This embodiment provides a hard carbon composite material. The difference from the embodiment 1 is that the mass percentage of the Al2O3 layer in the hard carbon composite material is 5wt%, and the pore volume is 0.15cm 3 / g, specific surface area is 100m 2 / g.
[0152] The preparation method of the hard carbon composite material of this embodiment is different from that of Embodiment 1 in that a larger amount of Al2(CO3)3 is added, and the molar ratio of Al2(CO3)3, 3-aminophenol and formaldehyde solution is 1:3:1.
[0153] Example 4
[0154] This embodiment provides a hard carbon composite material. The difference from the embodiment 1 is that the Al2O3 layer is replaced by a ZrO2 layer. The mass percentage of ZrO2 in the hard carbon composite material is 3wt%, and the pore volume is 0.11cm 3 / g, specific surface area is 80m 2 / g.
[0155] The preparation method of the hard carbon composite material of this embodiment is different from that of Embodiment 1 in that Al2(CO3)3 is replaced by an equimolar amount of another pore former Zr(OH)2CO3·ZrO2.
[0156] Example 5
[0157] This embodiment provides a hard carbon composite material, which is different from the embodiment 1 in that the mass percentage of the Al2O3 layer in the hard carbon composite material is 2wt%, the pore volume is 0.02, and the specific surface area is 4m 2 / g, and the degree of graphitization is 20%.
[0158] The difference between the preparation method of the hard carbon composite material in this embodiment and that in Embodiment 1 is that the final sintering temperature is adjusted from 1300°C to 1600°C.
[0159] Comparative Example 1
[0160] This comparative example provides a hard carbon composite material, which is different from Example 1 in that the hard carbon composite material does not contain an Al2O3 layer, and the outer surface of the hard carbon matrix and the inner wall surface of the pores are also free of other covering layers.
[0161] The difference between the preparation method of the hard carbon composite material in this comparative example and that in Example 1 is that in step 1, Al2(CO3)3 is not added.
[0162] Comparative Example 2
[0163] This comparative example provides a hard carbon composite material, which is different from Example 1 in that the hard carbon composite material does not have sponge-like porous channels.
[0164] The difference between the preparation method of the hard carbon composite material of this comparative example and that of Example 1 is that in step one, Al2(CO3)3 is not added; meanwhile, in step two, the acid etching step is not performed.
[0165] Comparative Example 3
[0166] This comparative example provides a hard carbon composite material, which is different from Example 1 in that the Al2O3 layer is only coated on the outer surface of the hard carbon matrix and does not cover the inner wall surface of the pores.
[0167] The preparation method of the hard carbon composite material of this comparative example comprises the following steps: mixing nano alumina powder and commercial hard carbon in a mass ratio of 1:50, and stirring at 2000 rpm for 15 minutes using a self-rotating and revolving stirrer.
[0168] Comparative Example 4
[0169] This comparative example provides a hard carbon composite material, which is different from Example 1 in that the hard carbon composite material does not contain an Al2O3 layer, and the outer surface of the hard carbon matrix and the inner wall surface of the pores are also free of other covering layers.
[0170] The difference between the preparation method of the hard carbon composite material of this comparative example and that of Example 1 is that in step 1, no Al2(CO3)3 is added. In step 2, CO2 atmosphere is introduced during the calcination process.
[0171] The preparation process and structure-related parameters of the hard carbon composite materials of various embodiments and comparative examples are summarized in Tables 1 and 2.
[0172] [Table 1]
[0173]
[0174] [Table 2]
[0175]
[0176] Among them, the test method of each parameter is:
[0177] (1) Pore diameter and pore volume: Use a physical adsorption instrument to conduct relevant tests;
[0178] (2) Carbon layer spacing, graphitization degree, and graphite mass percentage: relevant tests are performed using an X-ray diffractometer;
[0179] (3) Mass percentage of Al2O3 (or ZrO2): Use ICP-MS mass spectrometer for relevant testing;
[0180] (4) Mass oxygen content (oxygen-containing functional group content): Use an elemental analyzer (O mode) for relevant tests.
[0181] The hard carbon composite materials provided in the above examples and comparative examples were used as negative electrode materials, and negative electrode sheets and sodium ion batteries were assembled according to the following methods to evaluate the electrochemical performance:
[0182] Preparation of negative electrode sheet: The negative electrode material is mixed with carboxymethyl cellulose (CMC), styrene butadiene rubber (SBR) and conductive carbon black (SP) in a mass ratio of 95.8:1.2:2:1, and the negative electrode slurry is obtained by ball milling and stirring. The negative electrode slurry is coated on the surface of aluminum foil, and vacuum dried at 110° C. overnight to obtain a negative electrode sheet;
[0183] Positive electrode: metal sodium sheet;
[0184] Electrolyte: Ethylene carbonate and ethyl methyl carbonate were mixed in a volume ratio of 3:7, and NaPF6 was added to form an electrolyte, and the concentration of NaPF6 was 1 mol / L;
[0185] Diaphragm: polypropylene microporous diaphragm;
[0186] Sodium ion battery assembly: Assemble button-type sodium ion batteries in an inert atmosphere glove box in the order of negative electrode sheet - separator - electrolyte - positive electrode sheet.
[0187] ICE test: During the first charge and discharge process (discharge at a constant current of about 0.1C to 0.01V, discharge at a constant voltage of 0.01V to 0.01C, and stand for 10 minutes; charge at a constant current of 0.1C to 1.5V), record the discharge capacity and charge capacity. ICE is equal to the ratio of discharge capacity to charge capacity.
[0188] Cycle performance test: The battery is fully discharged and then fully charged. Specifically, the battery is discharged at a constant current of about 0.1C to 0.01V, and then discharged at a constant voltage of 0.01V to 0.01C, and then left to stand for 10 minutes; the battery is charged at a constant current of 0.1C to 1.5V. This is considered one cycle. The cycle test is performed continuously for 100 times, and the reversible capacity retention rate of the battery is recorded.
[0189] The test results are shown in Table 3.
[0190] [Table 3]
[0191]
[0192] The electrochemical performance test results in Table 3 show that after the negative electrode plates are made of the hard carbon composite materials of Examples 1 to 5 and the sodium ion batteries are assembled, high ICE, high first charge capacity and high capacity retention rate can be obtained. In contrast, the ICE, first charge capacity and capacity retention rate of Comparative Examples 1 to 4 are significantly lower than those of Examples 1 to 5.
[0193] The excellent electrochemical performance of Examples 1 to 5 is mainly due to:
[0194] (1) In these hard carbon composite materials, metal oxides (such as Al2O3, ZrO2) are distributed in the hard carbon matrix with a multi-porous structure, including the outer surface of the hard carbon matrix and the inner wall of the pores, forming a covering layer. Figure 1 and Figure 2 As shown, they are the SEM image and TEM mapping of the hard carbon composite material of Example 1, Figure 1 No obvious multi-porous structure was observed on the surface of the material, indicating that the surface of the material was coated with Al2O3. Figure 2 It can be seen that Al2O3 is dispersed on the outer surface and pores of the hard carbon matrix with a high degree of dispersion. These metal oxide coatings can effectively inhibit the direct contact between the electrolyte and the active material, reduce side reactions, and thus improve ICE and cycle stability, so that the ICE of Examples 1 to 5 can be as high as 91% to 96%, and the capacity retention rate after 100 cycles is as high as 96% to 98%. The hard carbon composite materials of Comparative Examples 1 and 4 do not have metal oxide coatings (such as Figure 3 As shown, it can be seen that the multiple pores on the surface of the material are not covered), while Comparative Example 3 only wraps the metal oxide layer on the outer surface of the hard carbon matrix, while there is no metal oxide in the pores of the hard carbon matrix. As a result, their ICE and cycle stability are significantly reduced, with ICE only 56% to 80%, and the capacity retention rate after 100 cycles is only 74% to 82%.
[0195] In the hard carbon composite materials of Examples 1 to 5, the structure in which metal oxides are distributed in the hard carbon matrix with a multi-porous structure is mainly because during the preparation process, pore-forming agents such as Al2(CO3)3 and Zr(OH)2CO3·ZrO2 are pre-encapsulated in phenolic resin, and during the calcination process, these pore-forming agents decompose to generate gases, which achieve an etching effect on the material from the inside to the outside, forming a multi-porous structure, and the metal oxides formed by the decomposition of these pore-forming agents can be distributed on the outer surface of the hard carbon matrix and the inner wall of the pores.
[0196] (2) At the same time, a larger pore size and pore volume, specific surface area, and a moderate degree of graphitization have a great effect on improving the performance of the hard carbon composite material of the embodiment of the present application, and the specific effects are as follows:
[0197] 1) Pore diameter and pore volume
[0198] Generally, the larger the pore size, the more conducive it may be to the insertion and extraction of sodium ions. A larger pore size can provide more channels, reduce the diffusion resistance of sodium ions, and thus improve the cycle performance of the material. Materials with larger pore volumes generally have better sodium storage capacity because larger pore volumes can provide more sodium ion storage space. For example, the pore size of Example 3 is 4.0 nm and the pore volume is 0.15 cm 3 / g, with a larger pore size and pore volume, its first charge capacity reaches 336mAh / g, and the cycle capacity retention rate is 97%. The pore size of comparative example 3 is only 1.3nm, and the pore volume is only 0.005cm 3 / g, the pore size and pore volume are smaller than those in Example 3, the first charge capacity is only 254 mAh / g, and the cycle capacity retention rate is only 74%.
[0199] 2) Specific surface area
[0200] Materials with large specific surface areas usually have more active sites, which can increase the amount of sodium ions embedded, thereby increasing the initial charge capacity. For example, the specific surface areas of Examples 3 and 4 are 100 m 2 / g and 80m 2 / g, with a larger specific surface area, the first charge capacity of both is relatively high, 336mAh / g and 330mAh / g respectively. In contrast, the specific surface area of comparative example 3 is only 3m 2 / g, the specific surface area is very small and the first charge capacity is also significantly lower.
[0201] At the same time, a larger specific surface area may lead to more side reactions (such as electrolyte decomposition), thereby reducing ICE. However, a moderate specific surface area and optimized material design can improve the overall electrochemical performance of the material while ensuring a higher ICE. For example, Example 3 has a larger specific surface area (100 m 2 / g), but combined with the structural design of the hard carbon composite material (metal oxides are distributed on the outer surface of the hard carbon matrix and the inner wall of the pores to form a covering layer), its ICE is still relatively high (91%).
[0202] 3) Degree of graphitization
[0203] The higher the graphitization degree, the better the conductivity of the material, thereby increasing the migration speed of sodium ions and enhancing the ICE and cycle performance of the material. For example, the graphitization degree of Example 5 is 20%, its ICE is 96%, and the cycle capacity retention rate reaches 98%.
[0204] At the same time, materials with a moderate degree of graphitization can provide a large sodium ion embedding capacity, which can improve the initial charge capacity of the material, while an excessively high degree of graphitization may reduce the capacity of the material. The degree of graphitization of Example 2 is 5%, and the initial charge capacity is 325 mAh / g, which can better improve the initial charge capacity than Example 5 with a higher degree of graphitization (the degree of graphitization is 20%, and the initial charge capacity is 301 mAh / g), and Comparative Example 2 with a lower degree of graphitization (the degree of graphitization is only 4%, and the initial charge capacity is only 267 mAh / g).
[0205] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A hard carbon composite material, characterized in that: The invention comprises a hard carbon matrix and a metal oxide, wherein the hard carbon matrix has multiple pores, and the metal oxide is distributed on the outer surface of the hard carbon matrix and the inner wall surface of the pores.
2. The hard carbon composite material according to claim 1, characterized in that: The metal oxide is coated on the outer surface of the hard carbon matrix and the inner wall surface of the pore.
3. The hard carbon composite material according to claim 1, characterized in that: The pore volume or porosity of the hard carbon composite material gradually decreases from the interior of the hard carbon matrix to the outer surface thereof.
4. The hard carbon composite material according to claim 1, characterized in that: The average pore size of the hard carbon composite material is in the range of 1.2 to 4 nm; and / or, The pore volume of the hard carbon composite material is 0.01 to 0.15 cm 3 / g; and / or, The BET specific surface area of the hard carbon composite material is 4 to 100 m 2 / g.
5. The hard carbon composite material according to any one of claims 1 to 4, characterized in that: The mass percentage of the metal oxide in the hard carbon composite material is 0.5wt% to 5wt%; and / or, The metal oxide includes one or more of aluminum oxide, zinc oxide, zirconium dioxide, and titanium dioxide; and / or, The hard carbon composite material further includes graphite, which is dispersed in the hard carbon matrix.
6. The hard carbon composite material according to claim 5, characterized in that: The carbon interlayer spacing of the hard carbon composite material is 0.365 to 0.385 nm; and / or, The degree of graphitization of the hard carbon composite material is 2% to 20%; and / or, The mass percentage of the graphite in the hard carbon composite material is 2wt% to 5wt%; and / or, Oxygen-containing functional groups are distributed in the hard carbon composite material, and the oxygen mass content of the hard carbon composite material is 3wt% to 5wt%.
7. A method for preparing a hard carbon composite material, characterized in that: include: Providing a carbon precursor, and performing an etching treatment on the carbon precursor; the carbon precursor comprises a hard carbon precursor and a pore former, the pore former is distributed in the hard carbon precursor, and the pore former contains a metal element; The calcination treatment is carried out under a protective atmosphere.
8. The method for preparing the hard carbon composite material according to claim 7, characterized in that: The melting point of the pore-forming agent is 800-1400° C.; and / or, The pore-forming agent includes one or more of metal carbonates, metal bicarbonates, and metal chlorides; and / or, The metal elements contained in the pore-forming agent include one or more of Al, Zn, Zr, and Ti; and / or, The hard carbon precursor includes one or more of a biomass precursor, an organic polymer precursor, and a fossil fuel precursor; and / or, The mass ratio of the pore former to the hard carbon precursor is 1:(0.1-10); and / or, The method for preparing the carbon precursor comprises: mixing the pore former with the hard carbon precursor; or, mixing the pore former with the reaction raw materials of the hard carbon precursor, and allowing the reaction raw materials to react to generate the hard carbon precursor; and / or, The etching treatment method includes one or more of acid etching, alkaline etching, and vapor phase etching; and / or, The calcination temperature is 1100-1600°C; and / or, The calcination treatment time is 2 to 6 hours.
9. A negative electrode, characterized in that The hard carbon composite material comprises the hard carbon composite material according to any one of claims 1 to 6, or comprises the hard carbon composite material prepared according to the preparation method according to claim 7 or 8.
10. A battery, characterized in that: The invention comprises the negative electrode according to claim 9 or the hard carbon composite material according to any one of claims 1 to 6, or comprises the hard carbon composite material prepared according to the preparation method according to claim 7 or 8.