Melamine foam electromagnetic shielding composite material coated with conducting layer and preparation method and application thereof
By using PEDOT:PSS reflective layer and melamine foam composite absorbing layer in melamine foam electromagnetic shielding material, combined with conductive nanocarbon material and PDMS treatment, the problem of degradation of existing materials in harsh environments is solved, and high efficiency is achieved The electromagnetic shielding and mechanical properties are improved, suitable for industrial applications.
Patent Information
- Application Number
- CN202411137860.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-12-06
AI Technical Summary
In harsh environments such as when soaking in water for a long time, the loss of conductive filler seriously damages its electromagnetic interference shielding performance, and it is difficult to take into account excellent EMI shielding performance, flexibility, water resistance and damping resistance.
The melamine foam electromagnetic shielding composite material coated with a conductive layer is composed of PEDOT:PSS reflective layer and melamine foam composite absorbing layer. The magnetic iron tetroxide is anchored on the melamine foam skeleton by hydrothermal reaction to fill the conductive Nanocarbon material and PDMS is applied to the surface to obtain hydrophobicity, combined with conductive polymer PEDOT:PSS to achieve hydrophilic and hydrophobic properties on one side.
It has achieved the improvement of the electromagnetic shielding performance and mechanical properties of the material, and at the same time it has electromagnetic shielding performance with the main absorption and reflection on the other side. It is suitable for industrial production and maintains good performance in harsh environments.
Smart Images

Figure CN119095354A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electromagnetic shielding materials, and in particular to a melamine foam electromagnetic shielding composite material coated with a conductive layer, and a preparation method and application thereof. Background Art
[0002] With the rapid development of fifth-generation (5G) information technology, electromagnetic (EM) functional materials and devices have promoted the development of social productivity and the improvement of quality of life. However, the resulting electromagnetic radiation pollution not only affects human health and the normal operation of electronic instruments, but also poses a hidden danger to national defense security. Therefore, the study of low-density, flexible, and efficient electromagnetic interference shielding materials is extremely important for preventing or eliminating electromagnetic pollution. In addition, in practical applications, materials with excellent EMI shielding performance should also have other properties such as flexibility, water resistance, and damping resistance to cope with harsh environmental conditions. For example, the loss of conductive fillers due to long-term immersion of the material in water will seriously damage the electromagnetic interference shielding performance of the material. Therefore, in order to improve the electromagnetic shielding performance of polymer materials and reduce secondary pollution, electromagnetic shielding composite materials with one side absorbing as the main side, one side reflecting as the main side, one side hydrophobic, and one side hydrophilic have important market application value. Summary of the invention
[0003] The purpose of the present invention is to provide a melamine foam electromagnetic shielding composite material coated with a conductive layer, and a preparation method and application thereof. The melamine foam electromagnetic shielding composite material of the present invention has good electromagnetic shielding performance and mechanical properties, and is mainly absorbing on one side, mainly reflecting on the other side, and is hydrophilic on one side and hydrophobic on the other side.
[0004] The technical solution of the present invention is a melamine foam electromagnetic shielding composite material coated with a conductive layer, which consists of a PEDOT:PSS reflective layer and a melamine foam composite material absorption layer.
[0005] The preparation method of the above-mentioned melamine foam electromagnetic shielding composite material coated with a conductive layer is carried out according to the following steps:
[0006] (1) Dissolve 0.1-1.9 g of tris(hydroxymethyl)aminomethane (Tris) in 1000 mL of deionized water, add 0.1-3.0 g of dopamine hydrochloride (DA) to dissolve, and then add 20-30 pieces of melamine foam cut into 2 cm*3 cm*1 cm blocks to obtain MF@PDA foam
[0007] (2) Add 1-10 g of ferric chloride hexahydrate (FeCl3·6H2O) to 96 mL of deionized water and stir to dissolve, add MF@PDA foam to immerse it, heat to 50-70°C, then add 2-8 g of ferrous sulfate heptahydrate (FeSO4·7H2O) and 5-30 mL of ammonia water (NH3·H2O) and continue stirring until dissolved, keep the reaction at 50-70°C for 25-35 minutes, and obtain MF@Fe3O4 composite material;
[0008] (3) adding the conductive nanocarbon material (NC) to a cellulose nanofiber dispersion (CNF) having a concentration of 1-10 mg / mL to make the concentration of the conductive nanocarbon material (NC) reach 0.2-5 mg / mL, stirring, and ultrasonically treating the mixture with a cell disruptor to obtain a CNF@NC dispersion;
[0009] (4) immersing 2-4 pieces of MF@Fe3O4 composite materials in 50 mL of CNF@NC dispersion under vacuum conditions for 2-6 hours, and then drying at 80°C for 4 hours. Repeating the immersion and drying process 2-8 times to obtain MF@Fe3O4 / CNF@NC composite materials;
[0010] (5) adding 0.1-5 mL of ethyl acetate to 0.1-5 g of PDMS liquid and mixing, and then dropping the mixture onto the MF@FeFe3O4 / CNF@NC composite material, completely soaking the composite material, and drying the mixture at 80°C for 4 hours to obtain the MF@Fe3O4 / CNF@NC / PDMS composite material, i.e., the melamine foam composite material;
[0011] (6) 0.01-5 mL PEDOT:PSS is coated on the upper surface of the MF@Fe3O4 / CNF@NC / PDMS composite material to obtain the MF@Fe3O4 / CNF@NC / PDMS / PEDOT:PSS composite material, i.e., the melamine foam electromagnetic shielding composite material.
[0012] In the above step (1), 0.5-0.7 g of tris(hydroxymethyl)aminomethane (Tris) is dissolved in 1000 mL of deionized water, 0.2-0.4 g of dopamine hydrochloride (DA) is added and dissolved, and then 25 pieces of melamine foam cut into 2 cm*3 cm*1 cm blocks are added to obtain MF@PDA foam.
[0013] In the above step (2), 5-7 g of ferric chloride hexahydrate (FeCl3·6H2O) is added to 96 mL of deionized water and stirred to dissolve, MF@PDA foam is added to immerse it, heated to 60°C, and then 4-7 g of ferrous sulfate heptahydrate (FeSO4·7H2O) and 20-30 mL of ammonia water (NH3·H2O) are added and stirred until dissolved, and the reaction is maintained at 60°C for 30 minutes to obtain a MF@Fe3O4 composite material.
[0014] In the above step (3), the conductive nanocarbon material (NC) is added to the cellulose nanofiber dispersion (CNF) with a concentration of 1-5 mg / mL to make the concentration of the conductive nanocarbon material (NC) reach 0.2-0.3 mg / mL, stirred, and ultrasonically treated for 2 min by a cell disruptor at 500-1200 W to obtain a CNF@NC dispersion;
[0015] The aforementioned conductive nanocarbon material (NC) includes carbon nanotubes (CNT), reduced graphene oxide (rGO), conductive carbon black or MXene.
[0016] In the above step (4), three pieces of MF@Fe3O4 composite materials are immersed in CNF@NC dispersion under vacuum conditions, immersed for 2 hours and then dried at 80°C for 4 hours. The above immersion and drying process is repeated 3-5 times to obtain MF@Fe3O4 / CNF@NC composite materials.
[0017] In the above step (5), 2-3 mL of ethyl acetate is added to 0.2-0.3 g of PDMS liquid and mixed, and then dropped onto the MF@FeFe3O4 / CNF@NC composite material, after which it is completely soaked, and dried at 80°C for 4 hours to obtain the MF@Fe3O4 / CNF@NC / PDMS composite material, i.e., the melamine foam composite material.
[0018] In the above step (6), 0.8-2.4 mL PEDOT:PSS is coated on the upper surface of the MF@Fe3O4 / CNF@NC / PDMS composite material to obtain MF@Fe3O4 / CNF@NC
[0019] / PDMS / PEDOT:PSS composite material, that is, melamine foam electromagnetic shielding composite material.
[0020] The above-mentioned melamine foam electromagnetic shielding composite material coated with a conductive layer is used in the preparation of an electromagnetic shielding composite material with one side mainly absorbing and the other side mainly reflecting.
[0021] In the aforementioned application, one layer of the electromagnetic shielding composite material is a PEDOT:PSS reflective layer, and the other layer is a melamine foam composite material absorption layer.
[0022] Beneficial Effects
[0023] The invention provides a method for preparing a melamine foam electromagnetic shielding composite material coated with a conductive layer. Magnetic ferroferric oxide is anchored on a melamine foam skeleton by hydrothermal reaction to form a magnetic foam skeleton, and on this basis, conductive nanocarbon materials (NC) including carbon nanotubes (CNT), reduced graphene oxide (rGO), conductive carbon black, and MXene are filled in by soaking, and then PDMS is coated to make the composite material hydrophobic, and finally a conductive polymer PEDOT:PSS is coated on the upper surface to make the composite material hydrophilic on one side and hydrophobic on the other side, and to achieve electromagnetic shielding performance of mainly absorbing on one side and mainly reflecting on the other side, and has good market application value.
[0024] The present invention also provides a method for preparing a melamine foam electromagnetic shielding composite material coated with a conductive layer. The method is simple and easy to implement and is suitable for industrial production. The prepared electromagnetic shielding composite material has electromagnetic shielding properties in which one side is hydrophilic and the other side is hydrophobic, and one side is mainly absorbing and the other side is mainly reflecting, thereby ensuring the material's resilience. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 :SEM images of MF@Fe3O4 / CNF@rGO / PDMS / PETDOT:PSS composite materials (ac: MF@Fe3O4; df: MR2; gi: MR2PP-2.4);
[0026] Figure 2 :SE of MF@Fe3O4 / CNF@rGO / PDMS / PETDOT:PSS composites T value;
[0027] Figure 3 :SE of MF@Fe3O4 / CNF@rGO / PDMS / PETDOT:PSS composites R ,SE A ,SE T and comparative analysis;
[0028] Figure 4 : AR value of MF@Fe3O4 / CNF@rGO / PDMS / PETDOT:PSS composite material (PEDOT:PSS surface incidence);
[0029] Figure 5 : Contact angle of MF composites. DETAILED DESCRIPTION
[0030] The present invention will be further described below in conjunction with the embodiments, but they are not intended to limit the present invention.
[0031] The reagents used in the following examples are:
[0032] PDMS liquid was purchased from Dow Corning 184PDMS, before use, mix the polydimethylsiloxane base (Part A) and the curing agent (Part B) in a mass ratio of 10:1 according to the instructions to obtain PDMS liquid.
[0033] PEDOT:PSS was purchased from Xi'an Yuri Solar Energy Technology Co., Ltd. with the brand name Clevios PH1000.
[0034] Example 1
[0035] This embodiment provides a melamine foam electromagnetic shielding composite material coated with a conductive layer. The preparation method is as follows based on the effective addition amount:
[0036] (1) 0.5 g of tris(hydroxymethyl)aminomethane (Tris) was dissolved in 1000 mL of deionized water, 0.2 g of dopamine hydrochloride was added to dissolve, and then 25 pieces of melamine foam cut into 2 cm*3 cm*1 cm blocks were added to obtain MF@PDA foam;
[0037] (2) Take another 5 g of FeCl3·6H2O and dissolve it in 96 mL of deionized water, add MF@PDA foam to immerse it, heat it to 60°C, then add 4 g of FeSO4·7H2O and 20 mL of NH3·H2O and continue stirring until dissolved, keep the reaction at 60°C for 30 minutes, and obtain MF@Fe3O4 composite material;
[0038] (3) The CNF@CNT solution (containing CNT concentration of 0.2 mg / mL) was ultrasonicated in a cell disruptor for 2 minutes (ultrasonic power 1000 W) to obtain a well-dispersed CNF@CNT solution;
[0039] (4) Three pieces of MF@Fe3O4 composite materials were vacuum immersed in 50 mL of CNF@CNT solution. After 2 hours, they were dried at 80°C for 4 hours. The immersion and drying were repeated three times to obtain MF@Fe3O4 / CNF@NC composite materials.
[0040] (5) 2 mL of ethyl acetate was added to 0.2 g of PDMS liquid and mixed, and then dropped onto the MF@FeFe3O4 / CNF@NC composite material to completely soak it, and then dried at 80 °C for 4 hours to obtain the MF@Fe3O4 / CNF@NC / PDMS composite material, i.e., the melamine foam composite material;
[0041] (6) 0.8 mL of PEDOT:PSS was coated on the upper surface of the MF@Fe3O4 / CNF@CNT / PDMS composite material to obtain the MF@Fe3O4 / CNF@CNT / PDMS / PEDOT:PSS composite material.
[0042] Example 2
[0043] This embodiment provides a melamine foam electromagnetic shielding composite material coated with a conductive layer. The preparation method is as follows based on the effective addition amount:
[0044] (1) 0.6 g of tris(hydroxymethyl)aminomethane (Tris) was dissolved in 1000 mL of deionized water, 0.3 g of dopamine hydrochloride was added to dissolve, and then 25 pieces of melamine foam cut into 2 cm*3 cm*1 cm blocks were added to obtain MF@PDA foam;
[0045] (2) Take another 6 g of FeCl3·6H2O and dissolve it in 96 mL of deionized water, add MF@PDA foam to immerse it, heat it to 60°C, then add 6 g of FeSO4·7H2O and 25 mL of NH3·H2O and continue stirring until dissolved, keep the reaction at 60°C for 30 minutes, and obtain MF@Fe3O4 composite material;
[0046] (3) The CNF@CNT solution (containing CNT concentration of 0.3 mg / mL) was ultrasonicated in a cell disruptor for 2 minutes (ultrasonic power 500 W) to obtain a well-dispersed CNF@CNT solution;
[0047] (4) immersing three pieces of MF@Fe3O4 composite materials in 50 mL of CNF@CNT solution under vacuum, drying after 2 hours, repeatedly immersing, and drying at 80 °C for 4 hours to obtain MF@Fe3O4 / CNF@NC composite materials;
[0048] (5) 3 mL of ethyl acetate was added to 0.3 g of PDMS liquid and mixed, and then dropped onto the MF@FeFe3O4 / CNF@NC composite material to completely soak it, and then dried at 80 °C for 4 hours to obtain the MF@Fe3O4 / CNF@NC / PDMS composite material, i.e., the melamine foam composite material;
[0049] (6) 1.2 mL of PEDOT:PSS was coated on the upper surface of the MF@Fe3O4 / CNF@CNT / PDMS composite material to obtain the MF@Fe3O4 / CNF@CNT / PDMS / PEDOT:PSS composite material.
[0050] Example 3
[0051] This embodiment provides a melamine foam electromagnetic shielding composite material coated with a conductive layer. The preparation method is as follows based on the effective addition amount:
[0052] (1) 0.7 g of tris(hydroxymethyl)aminomethane (Tris) was dissolved in 1000 mL of deionized water, 0.4 g of dopamine hydrochloride was added to dissolve, and then 25 pieces of melamine foam cut into 2 cm*3 cm*1 cm blocks were added to obtain MF@PDA foam;
[0053] (2) Take another 7g of FeCl3·6H2O and dissolve it in 96mL of deionized water, add MF@PDA foam to immerse it, heat it to 60°C, then add 7g of FeSO4·7H2O and 30mL of NH3·H2O and continue stirring until dissolved, keep the reaction at 60°C for 30 minutes, and obtain MF@Fe3O4 composite material;
[0054] (3) The CNF@CNT solution (containing CNT concentration of 0.3 mg / mL) was ultrasonicated in a cell disruptor for 2 minutes (ultrasonic power 1200 W) to obtain a well-dispersed CNF@CNT solution;
[0055] (4) Three pieces of MF@Fe3O4 composite materials were vacuum immersed in 50 mL of CNF@CNT solution. After 2 hours, they were dried at 80°C for 4 hours. The immersion and drying were repeated 5 times to obtain MF@Fe3O4 / CNF@NC composite materials.
[0056] (5) adding 2.5 mL of ethyl acetate to 0.3 g of PDMS liquid and mixing, and then dropping it onto the MF@FeFe3O4 / CNF@NC composite material, completely soaking it, and drying it at 80 °C for 4 hours to obtain the MF@Fe3O4 / CNF@NC / PDMS composite material, i.e., the melamine foam composite material;
[0057] (6) 2.4 mL of PEDOT:PSS was coated on the upper surface of the MF@Fe3O4 / CNF@CNT / PDMS composite material to obtain the MF@Fe3O4 / CNF@CNT / PDMS / PEDOT:PSS composite material.
[0058] Example 4
[0059] This embodiment provides a melamine foam electromagnetic shielding composite material coated with a conductive layer, which is prepared according to the preparation method of Example 3, except that: in Example 4, the carbon nanotubes (CNTs) are replaced with reduced graphene oxide (rGO) to obtain a MF@Fe3O4 / CNF@rGO / PDMS / PEDOT:PSS composite material.
[0060] Example 5
[0061] This embodiment provides a melamine foam electromagnetic shielding composite material coated with a conductive layer, which is prepared according to the preparation method of Example 3, except that: in Example 5, carbon nanotubes (CNTs) are replaced with conductive carbon black to obtain MF@Fe3O4 / CNF@conductive carbon black / PDMS / PEDOT:PSS composite material.
[0062] Example 6
[0063] This embodiment provides a melamine foam electromagnetic shielding composite material coated with a conductive layer, which is prepared according to the preparation method of Example 3, except that: in Example 5, the carbon nanotubes (CNTs) are replaced with MXene to obtain a MF@Fe3O4 / CNF@MXene / PDMS / PEDOT:PSS composite material.
[0064] Test Example 1
[0065] The electromagnetic shielding performance and hydrophilicity and hydrophobicity of the materials prepared in Examples 1-6 were tested, and the results are shown in Table 1. Test method: The electromagnetic shielding performance was tested using a vector network analyzer, and the hydrophobicity was tested using a water contact angle meter.
[0066] Table 1 Test results of electromagnetic shielding performance and hydrophilicity and hydrophobicity
[0067]
[0068] According to Table 1, the melamine foam electromagnetic shielding composite material coated with a conductive layer provided by the embodiment of the present invention, and its preparation method and application, have good electromagnetic shielding performance and mechanical properties, and are a melamine foam electromagnetic shielding composite material with one side mainly absorbing, one side mainly reflecting, one side hydrophilic, and one side hydrophobic. The embodiments described above are part of the embodiments of the present invention, but not all of them. The detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
Claims
1. A melamine foam electromagnetic shielding composite material coated with a conductive layer, Features: It consists of a PEDOT:PSS reflective layer and a melamine foam composite absorption layer.
2. The method for preparing the melamine foam electromagnetic shielding composite material coated with a conductive layer according to claim 1, Features: Follow these steps: (1) Dissolve 0.1-1.9 g of tris(hydroxymethyl)aminomethane in 1000 mL of deionized water, add 0.1-3.0 g of dopamine hydrochloride to dissolve, and then add 20-30 pieces of melamine foam cut into 2 cm*3 cm*1 cm blocks to obtain MF@PDA foam; (2) Add 1-10 g of ferric chloride hexahydrate to 96 mL of deionized water and stir to dissolve, add MF@PDA foam to immerse it, heat to 50-70 ° C, then add 2-8 g of ferrous sulfate heptahydrate and 5-30 mL of ammonia water and continue stirring until dissolved, keep the reaction at 50-70 ° C for 25-35 minutes, and obtain MF@Fe 3 O 4 Composite materials; (3) adding the conductive nanocarbon material to a cellulose nanofiber dispersion having a concentration of 1-10 mg / mL to make the concentration of the conductive nanocarbon material reach 0.2-5 mg / mL, stirring, and ultrasonically treating with a cell disruptor to obtain a CNF@NC dispersion; (4) 2-4 pieces of MF@Fe 3 O 4 The composite material was immersed in 50 mL of CNF@NC dispersion under vacuum conditions for 2-6 hours, and then dried at 80 °C for 4 hours. The above immersion and drying process was repeated 2-8 times to obtain MF@Fe 3 O 4 / CNF@NC composites; (5) Add 0.1-5 mL of ethyl acetate to 0.1-5 g of PDMS liquid and mix well, then add dropwise to the MF@FeFe 3 O 4 / CNF@NC composite material, and then dried at 80℃ for 4 hours to obtain MF@Fe 3 O 4 / CNF@NC / PDMS composite material, i.e., melamine foam composite material; (6) 0.01-5 mL PEDOT:PSS was coated on the upper surface of MF@Fe3O4 / CNF@NC / PDMS composite material to obtain MF@Fe 3 O 4 / CNF@NC / PDMS / PEDOT:PSS composite material, that is, melamine foam electromagnetic shielding composite material.
3. The method for preparing the melamine foam electromagnetic shielding composite material coated with a conductive layer according to claim 2, Features: In the step (1), 0.5-0.7 g of tris(hydroxymethyl)aminomethane is dissolved in 1000 mL of deionized water, 0.2-0.4 g of dopamine hydrochloride is added and dissolved, and then 25 pieces of melamine foam cut into 2 cm*3 cm*1 cm blocks are added to obtain MF@PDA foam.
4. The method for preparing the melamine foam electromagnetic shielding composite material coated with a conductive layer according to claim 2, Features: In the step (2), 5-7 g of ferric chloride hexahydrate is added to 96 mL of deionized water and stirred to dissolve, MF@PDA foam is added to immerse it, heated to 60°C, and then 4-7 g of ferrous sulfate heptahydrate and 20-30 mL of ammonia water are added and stirred until dissolved, and the reaction is maintained at 60°C for 30 minutes to obtain MF@Fe 3 O 4 Composite materials.
5. The method for preparing the melamine foam electromagnetic shielding composite material coated with a conductive layer according to claim 2, Features: In the step (3), the conductive nano-carbon material is added to the cellulose nanofiber dispersion having a concentration of 1-5 mg / mL to make the concentration of the conductive nano-carbon material reach 0.2-0.3 mg / mL, and the mixture is stirred and ultrasonically treated for 2 min at 500-1200 W by a cell disruptor to obtain a CNF@NC dispersion; The conductive nanocarbon material includes carbon nanotubes, reduced graphene oxide, conductive carbon black or MXene.
6. The method for preparing the melamine foam electromagnetic shielding composite material coated with a conductive layer according to claim 2, Features: In step (4), three pieces of MF@Fe 3 O 4 The composite material was immersed in CNF@NC dispersion under vacuum conditions for 2 hours, and then dried at 80 °C for 4 hours. The above immersion and drying process was repeated 3-5 times to obtain MF@Fe 3 O 4 / CNF@NC composites.
7. The method for preparing the melamine foam electromagnetic shielding composite material coated with a conductive layer according to claim 2, Features: In step (5), 2-3 mL of ethyl acetate is added to 0.2-0.3 g of PDMS liquid and mixed, and then added dropwise to the MF@FeFe 3 O 4 / CNF@NC composite material, and then dried at 80℃ for 4 hours to obtain MF@Fe 3 O 4 / CNF@NC / PDMS composite material, that is, melamine foam composite material.
8. The method for preparing the melamine foam electromagnetic shielding composite material coated with a conductive layer according to claim 2, Features: In the step (6), 0.8-2.4 mL PEDOT:PSS is coated on the MF@Fe 3 O 4 / CNF@NC / PDMS composite material to obtain MF@Fe3O4 / CNF@NC / PDMS / PEDOT:PSS composite material, that is, melamine foam electromagnetic shielding composite material.
9. Use of the melamine foam electromagnetic shielding composite material coated with a conductive layer according to claim 1 in preparing an electromagnetic shielding composite material with one side mainly absorbing and the other side mainly reflecting.
10. The use according to claim 9, Features: One layer of the electromagnetic shielding composite material is a PEDOT:PSS reflective layer, and the other layer is a melamine foam composite material absorption layer.
Citation Information
Cited By
Carbon nano composite conductive material and application thereof in cable shielding layer
CN119993602A