Two-dimensional ferroelectric photoelectric memristor and preparation method and application thereof

By forming two-dimensional ferroelectric photomemristors with SnSey and Bi2Te3-xSex functional layers and Pd top electrode layers on SiO2/Si substrates, the problem of difficulty in storing and processing information efficiently is solved by a single device, and multiple devices are realized Functional integration and demonstrate application potential in neuromorphic computing and biological applications.

CN119095473APending Publication Date: 2024-12-06HEBEI UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411076893.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The prior art is difficult to achieve multifunctional integration of efficient storage and processing of information in a single device, especially in neuromorphic computing and biological applications, and the research on two-dimensional ferroelectric materials has not yet fully utilized its potential.

Method used

Two-dimensional ferroelectric photomemristors using SnSey functional layer, Bi2Te3-xSex functional layer and Pd top electrode layer are formed on SiO2/Si substrate in turn. Through specific preparation processes and structural design, efficient storage and information of the device are achieved. Processing function.

Benefits of technology

The device demonstrates efficient storage performance and can simulate two types of optical/electroelectric synapses. It has broad application prospects in the fields of information processing and neuromorphic computing, realizing efficient storage and processing of information.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119095473A_ABST
    Figure CN119095473A_ABST
Patent Text Reader

Abstract

The invention provides a two-dimensional ferroelectric photoelectric memristor and a preparation method and application thereof. The structure of the memristor provided by the invention can be represented as Pd / Bi2Te3-xSex / SnSey / SiO2 / Si, x is more than 0 and less than 3, and y is more than 0.6 and less than 2. The preparation method of the memristor comprises the following steps: cleaning and drying a Si wafer; putting the treated Si wafer into a thermal oxidation furnace for high-temperature annealing, and growing a SiO2 thin film; growing a SnSey functional layer on the SiO2 / Si substrate layer through a PLD (Pulsed Laser Deposition) technology; growing a Bi2Te < 3-x > Se < x > functional layer on the SnSe < y > functional layer; and finally, growing a Pd top electrode layer on the Bi2Te3-xSex functional layer through a magnetron sputtering method. The memristor has optical and electric synaptic characteristics, a single device can realize multifunctional integration of efficient storage and information processing, an I-V curve has good stability and good performance, and the memory is a nonvolatile memory with good storage performance and wider application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of memory technology, in particular to a two-dimensional ferroelectric photoelectric memristor based on bismuth tellurium selenide / tin selenide, and a preparation method and application thereof. Background Art

[0002] The concept of neuromorphic computing was first proposed by Mead in 1990 and experimented in resistive switching devices. It is considered a promising direction to overcome the bottleneck of the von Neumann architecture. The goal of neuromorphic computing is to achieve artificial intelligence by simulating the mechanisms of neurons and synapses in the human brain. For a long time, people have been trying to simulate brain-like behaviors through hardware. Studies have shown that memristors can be used in electronic circuits to achieve more efficient neuromorphic computing.

[0003] Memristor is a circuit device that represents the relationship between magnetic flux and charge. Its full name is memory resistor. Memristor has the dimension of resistance, but unlike resistor, the resistance value of memristor is determined by the charge flowing through it. Therefore, by measuring the resistance value of memristor, we can know the amount of charge flowing through it, so it has the function of memorizing charge. Memristor was first proposed by Professor Shaotang Cai of University of California, Berkeley in 1971. Simply put, memristor is a nonlinear resistor with memory function. Its resistance value can be changed by controlling the change of current. If high resistance value is defined as "1" and low resistance value is defined as "0", then this resistor can realize the function of storing data. In fact, it is a nonlinear resistor with memory function. As the fourth basic circuit element, memristor is widely used in many fields such as information storage, logical operation, neural network, machine learning, etc., and has become a research hotspot today.

[0004] Ferroelectric memristors are memristors that use ferroelectric materials as functional layers. The polarization reversal of ferroelectric thin films determines the change in their resistance. They have the characteristics of stable performance, low power consumption, and flexible plasticity. Compared with traditional memristors, they overcome the disadvantages of unstable displacement of internal materials. In tunnel junctions with ferroelectric barriers, the polarization reversal of ferroelectric thin films will cause changes in the resistance of ferroelectric tunnel junctions. Compared with ordinary ferroelectric materials, two-dimensional ferroelectric materials are more conducive to the preparation of small-sized devices, making them easier to integrate on a large scale. Therefore, research on the application of ferroelectric materials in memristor devices, especially research on small-sized and easy-to-integrate two-dimensional ferroelectric materials, will play an important role in promoting the field of resistive memory. The research and application of two-dimensional ferroelectric materials in biology is even more important. Memristors based on two-dimensional materials have unique electrical properties, that is, their resistance can change and maintain under external stimulation, which is similar to the characteristics of neural synapses. Memristors based on two-dimensional materials can simulate some simple functions of neural synapses. They have also become a strong candidate for future data storage and computing. Summary of the invention

[0005] The purpose of the present invention is to provide a two-dimensional ferroelectric photoelectric memristor, a preparation method and application thereof, so as to solve the problem of multifunctional integration of a single device to achieve efficient storage and processing of information at the same time.

[0006] The present invention is achieved in that:

[0007] The two-dimensional ferroelectric photoelectric memristor provided by the present invention has a structure in which SnSe is sequentially formed on a SiO2 / Si substrate. y Functional layer, Bi2Te 3-x Se x Functional layer and Pd top electrode layer, wherein the value range of x is 0-3, and the value range of y is 0.6-2.

[0008] Preferably, SnSe y The thickness of the functional layer is 3 to 90 nm, Bi2Te 3-x Se x The thickness of the functional layer is 3 to 120 nm, and the thickness of the Pd top electrode layer is 30 to 200 nm.

[0009] More preferably, SnSe y The thickness of the functional layer is 10-12 nm, Bi2Te 3-x Se x The thickness of the functional layer is 3-5 nm, and the thickness of the Pd top electrode layer is 30-40 nm.

[0010] The preparation method of the above two-dimensional ferroelectric photoelectric memristor comprises the following steps:

[0011] (a) Granular Sn (99.999%) and Se (99.999%) were mixed in a set ratio and calcined in a muffle furnace (KSL-1600X) at 800-950°C for 24 hours. After cooling for 24 hours, the ball-milled tin selenide powder was calcined again in a plasma sintering furnace (SPS-30) at 40-50 MPa and 450-550°C. Using the above preparation process, a SnSe y Target material.

[0012] (b) Bi (99.999%), Te (99.999%) and Se (99.999%) were mixed in a set ratio and calcined in a muffle furnace (KSL-1600X) at 800-950°C for 24 hours. After cooling for 24 hours, the ball-milled bismuth tellurium selenide powder was calcined again in a plasma sintering furnace (SPS-30) at 40-50 MPa and 450-550°C. Using the above preparation process, a Bi2Te 3-x Se x Target material.

[0013] (c) The Si substrate is ultrasonically cleaned with acetone, alcohol and deionized water for 2 to 3 minutes in sequence to remove the ions adsorbed on the substrate surface. The treated substrate is then immersed in HF solution (H2O:HF=3:1) for 1 to 2 minutes to remove the naturally grown SiO2 film layer on the substrate surface. The treated Si substrate is then placed in a thermal oxidation furnace and dry O2 with a flow rate of 0.1 to 1 sccm is introduced for medium-high temperature annealing at 300 to 600°C for 1 to 3 minutes to grow a 2 to 4 nm thick SiO2 film.

[0014] (d) The SiO2 / Si substrate is fixed to the substrate sample stage of the growth chamber of the pulsed laser deposition equipment. y Target and Bi2Te 3-x Se x The target is fixed on the target holder, the target spacing is adjusted appropriately, and the back of the chamber is evacuated to a vacuum of 2×10 -4 Pa, heat the sample stage to 250-300°C, introduce argon into the cavity, adjust the gate valve to maintain the pressure in the cavity at 0.1-0.2 Pa, turn on the excimer laser, and adjust the laser energy density to 1.3-1.5 J / cm 2 The laser frequency is 3 to 5 Hz, so that the laser passes through the lens and hits the SnSe y The target center is pre-sputtered for 1 to 2 minutes, followed by formal sputtering for 20 to 30 minutes to form SnSe on the SiO2 / Si substrate. y Functional layer, where the value range of x is 0 to 3, and the value range of y is 0.6 to 2.

[0015] (e) Re-evacuate the bottom of the cavity to 2×10 -4 Pa, introduce argon into the chamber, adjust the gate valve to maintain the pressure in the chamber at 35-40 Pa, and replace Bi2Te 3-x Se x Target, turn on the excimer laser, and adjust the laser energy density to 1-1.2 J / cm 2 The laser frequency is 3 to 5 Hz, so that the laser passes through the lens and hits Bi2Te 3-x Se x The target center, pre-sputtering 1 ~ 2min; then formal sputtering 5 ~ 10min, in SnSe y Bi2Te is formed on the functional layer 3-x Se x Functional layer.

[0016] (f) Using a DC magnetron sputtering device, the mask is placed on the Bi2Te 3-x Se x / SnSe yThe functional layer substrate is fixed on the substrate stand of the chamber, the chamber is evacuated, argon is introduced into the chamber, the DC source for controlling the ignition of the palladium target is turned on, the DC source is adjusted to ignite the palladium target, the DC power is 8-10W, pre-sputtering for 1-2 minutes, and then formal sputtering for 10-15 minutes, in Bi2Te 3-x Se x / SnSe y A Pd top electrode layer is formed on the functional layer.

[0017] In the above preparation method, the SnSe formed in step (d) y The thickness of the functional layer is 10 to 12 nm.

[0018] In the above preparation method, the Bi2Te formed in step (e) 3-x Se x The thickness of the functional layer is 3 to 5 nm.

[0019] In the above preparation method, the mask described in step (f) is uniformly distributed with circular holes with a diameter of 100 μm.

[0020] In the above preparation method, the Pd top electrode layer in step (f) includes a plurality of uniformly distributed 3-x Se x / SnSe y Circular electrodes with a diameter of 100 μm on the functional layer.

[0021] In the above preparation method, Si, Sn, Se, Bi, Te, and Pd materials are commercially available products.

[0022] The two-dimensional ferroelectric photoelectric memristor provided by the present invention uses SiO2 / Si as a substrate and two-dimensional ferroelectric material bismuth tellurium selenide / tin selenide as a functional layer. The finally formed memristor has demonstrated efficient storage performance through a series of electrical and optical performance tests, and can simultaneously simulate both optical / electrical synapses, and has broad application prospects in information processing and storage, and neuromorphic computing. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a schematic structural diagram of the two-dimensional ferroelectric photoelectric memristor provided by the present invention.

[0024] Figure 2 This is the HRTEM test result of the two-dimensional ferroelectric SnSe film prepared by the present invention.

[0025] Figure 3 1. The ferroelectric phase reversal curve (upper) and amplitude butterfly curve (lower) of the two-dimensional ferroelectric photoelectric memristor prepared in Example 2 of the present invention.

[0026] Figure 4is 10 of the two-dimensional ferroelectric photoelectric memristor prepared in Example 2 of the present invention 4 Looped logarithmic I–V curve.

[0027] Figure 5 The long-term plasticity behaviors of the electrical synapses of the two-dimensional ferroelectric photoelectric memristor prepared in Example 2 of the present invention are: long-term potentiation (LTP) and long-term depression (LTD).

[0028] Figure 6 This is a current response diagram of the two-dimensional ferroelectric photoelectric memristor prepared in Example 2 of the present invention under light with a wavelength of 405 nm.

[0029] Figure 7 It is the short-term synaptic plasticity behavior of the two-dimensional ferroelectric photoelectric memristor prepared in Example 2 of the present invention under 405nm wavelength light: the transformation from paired pulse facilitation (PPF) to paired pulse depression (PPD).

[0030] Figure 8 The two-dimensional ferroelectric photoelectric memristor prepared in Example 2 of the present invention simulates the "learning-forgetting-relearning-reforgetting" behavior of the human brain under 405nm wavelength light. DETAILED DESCRIPTION

[0031] The following examples are used to further illustrate the present invention, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art and do not limit the present invention in any form.

[0032] Example 1

[0033] like Figure 1 As shown, the two-dimensional ferroelectric photoelectric memristor provided by the present invention comprises a SiO2 / Si substrate layer, a SnSe y Functional layer, Bi2Te 3-x Se x Functional layer and Pd top electrode layer, wherein the value range of x is 0-3, and the value range of y is 0.6-2.

[0034] Example 2

[0035] The structure of the two-dimensional ferroelectric photoelectric memristor in this embodiment includes a SiO2 / Si substrate layer, a SnSe 1.2 Functional layer, Bi2Te 2.7 Se 0.3 Functional layer and Pd top electrode layer. SnSe 1.2 The thickness of the functional layer is 11.7nm, Bi2Te 2.7 Se 0.3The thickness of the functional layer is 4.4 nm, and the thickness of the Pd top electrode layer is 30 nm.

[0036] The method for preparing the two-dimensional ferroelectric photoelectric memristor in this embodiment comprises the following steps:

[0037] (1)SnSe 1.2 Preparation of target: Granular Sn (99.999%) and Se (99.999%) were mixed in a molar ratio of 1:1.2 and calcined in a muffle furnace (KSL-1600X) at 950°C for 24 hours. After cooling for 24 hours, the ball-milled tin selenide powder was calcined again in a spark plasma sintering furnace (SPS-30) at 50 MPa and 525°C. Using the above preparation process, a SnSe 1.2 Target material.

[0038] (2) Bi2Te 2.7 Se 0.3 Preparation of target material: Bi (99.999%), Te (99.999%) and Se (99.999%) were mixed in a molar ratio of 2:2.7:0.3 and calcined in a muffle furnace (KSL-1600X) at 950°C for 24 hours. After cooling for 24 hours, the ball-milled bismuth tellurium selenide powder was calcined again in a spark plasma sintering furnace (SPS-30) at 50 MPa and 525°C to obtain Bi2Te 2.7 Se 0.3 Target material.

[0039] (3) The Si substrate was ultrasonically cleaned with acetone, alcohol and deionized water for 3 minutes in sequence to remove the ions adsorbed on the substrate surface, and then the treated substrate was immersed in HF solution (H2O:HF=3:1) for 1.5 minutes to remove the naturally grown SiO2 film layer on the substrate surface. Then the treated Si substrate was placed in a thermal oxidation furnace, and dry O2 with a flow rate of 0.5 sccm was introduced for high-temperature annealing at 600°C for 3 minutes to grow a 2nm thick SiO2 film, thereby forming a SiO2 / Si substrate.

[0040] (4) Preparation of functional layer: First, grind the substrate sample stage in the pulse laser deposition equipment cavity with sandpaper, then clean the organic impurities on it with acetone, then clean the remaining acetone with anhydrous ethanol, and finally blow dry the surface of the sample stage with a nitrogen gun. Fix the SiO2 / Si substrate treated in step (3) to the sample stage with silver glue and place it on the heating table to prevent the substrate from falling off the sample stage during the experiment. Install the prepared sample stage into the pulse laser deposition equipment cavity, SnSe 1.2 Target and Bi2Te 2.7 Se 0.3The target is fixed on the target holder, the target spacing is adjusted appropriately, and the back of the chamber is evacuated to a vacuum of 2×10 -4 Pa, heat the sample stage to 300 °C and maintain for 10 min to ensure uniform heating, introduce O2 into the cavity, adjust the gate valve to maintain the pressure in the cavity at 0.1 Pa, turn on the excimer laser, and adjust the laser energy density to 1.5 J / cm 2 The laser frequency is 5Hz, and the laser is shot through the lens onto the SnSe 1.2 The center of the target material was pre-sputtered for 1 minute, followed by formal sputtering for 30 minutes, and deposition for 10 minutes after the sputtering to form SnSe on the SiO2 / Si substrate. 1.2 Functional layer. Re-evacuate the cavity to 2×10 -4 Pa, introduce argon into the chamber, adjust the gate valve to maintain the pressure in the chamber at 40Pa, and replace Bi2Te 2.7 Se 0.3 Target, turn on the excimer laser, and adjust the laser energy density to 1.2J / cm 2 The laser frequency is 5Hz, so that the laser passes through the lens and hits Bi2Te 2.7 Se 0.3 The target center was pre-sputtered for 1 minute, followed by formal sputtering for 5 minutes, and deposition for 10 minutes after sputtering. 1.2 Bi2Te is formed on the functional layer 2.7 Se 0.3 Functional layer.

[0041] (5) Use ultrasonic cleaning to clean the mask, use acetone to clean the organic matter attached to the surface of the mask, and finally wipe it clean with alcohol. 2.7 Se 0.3 / SnSe 1.2 A mask with a circular hole of 100 microns in diameter is attached to the functional layer. After the electrode layer is sputtered, the circular hole area is the size of the effective working area of ​​the memristor. Using a DC magnetron sputtering device, take the sample stage and the target stage target sleeve, use sandpaper to clean the impurities on the surface, wipe the organic matter attached to the surface with acetone, and finally wipe it clean with alcohol. Fix the palladium target on the DC sputtering target stage and install the target sleeve, and evacuate the cavity to 1.8×10 -4 Pa, argon gas was introduced into the chamber, the inlet valve was adjusted to maintain the pressure in the chamber at 1Pa, the DC source for controlling the ignition of the palladium target was turned on, the DC source power was adjusted to 10W, the palladium target was ignited, and the pre-sputtering was performed for 1min; then the formal sputtering was performed for 15min. 2.7 Se 0.3 / SnSe 1.2 A Pd top electrode layer with a thickness of 30 nm is generated on the functional layer. The Pd top electrode layer is the circular pattern not blocked by the mask.

[0042] Performance Testing

[0043] The Bi2Te prepared in Example 2 2.7 Se 0.3 / SnSe 1.2 The functional layer was characterized by high resolution transmission electron microscopy (HRTEM). The test results of the samples are as follows: Figure 2 As shown. Figure 2 It can be seen that the SnSe prepared in Example 2 1.2 The functional layer has good film quality.

[0044] The ferroelectricity of the two-dimensional ferroelectric photoelectric memristor prepared in Example 2 was tested using a piezoelectric force microscope. The results are as follows: Figure 3 As shown, when a voltage of ±6V is applied for testing, the ferroelectric chip exhibits a phase reversal of nearly 140 degrees and has a small coercive voltage.

[0045] The current-voltage characteristic curve of the two-dimensional ferroelectric photoelectric memristor prepared in Example 2 was measured by applying a scanning voltage to the two-dimensional ferroelectric photoelectric memristor prepared in Example 2. Figure 4 , the applied voltage is 0→9V→0→-9V→0. When the voltage is applied 0→9V→0, the resistance changes from high resistance state (HRS) to low resistance state (LRS); when the reverse voltage is applied 0→-9V→0, the resistance changes from low resistance state (LRS) to high resistance state (HRS). 10 4 The IV curve test results showed good repeatability.

[0046] The electrical synaptic behavior of the two-dimensional ferroelectric photoelectric memristor prepared in Example 2 was studied. When 70 consecutive positive electric pulses with an amplitude of 8V were applied to the device, the device conductivity value continued to increase, showing long-term potentiation (LTP); when 70 consecutive negative electric pulses with an amplitude of 8V were applied to the device, the device conductivity value continued to decrease, showing long-term depression (LTD), as shown in FIG. Figure 5 shown.

[0047] Figure 6 The stable characteristics of the current response of the two-dimensional ferroelectric photoelectric memristor prepared in Example 2 under light with a wavelength of 405nm and a power of 50mW. Figure 7 As shown, under the same lighting conditions, several light pulses of 1 Hz were applied first, followed by several light pulses of 0.18 Hz. The device exhibited short-term plasticity behavior of the optical synapse, which was transformed from paired pulse facilitation (PPF) to paired pulse depression (PPD). Figure 8Under the same lighting conditions, the device first applies 50 light pulses to make the current reach ΔI, then removes the light source for 93.623s, then applies 21 consecutive light pulses to make the current reach ΔI again, and then removes the light source. This simulates the "learning-forgetting-relearning-reforgetting" behavior of the human brain.

[0048] The structure of the two-dimensional ferroelectric photoelectric memristor prepared in Example 2 of the present invention can be expressed as Pd / Bi2Te 2.7 Se 0.3 / SnSe 1.2 / SiO2 / Si, which is a device with excellent storage performance, good stability under 405nm band light, and the ability to simulate both optical and electrical synapses at the same time. It is a non-volatile memory that can achieve efficient storage and processing of information and has broader application prospects.

[0049] Example 3

[0050] Compared with Example 2, the structure of the two-dimensional ferroelectric photoelectric memristor provided in this embodiment includes a SiO2 / Si substrate layer, a SnSe 1.4 Functional layer, Bi2Te 2.5 Se 0.5 Functional layer and Pd top electrode layer. Others are the same as in Example 2.

[0051] Example 4

[0052] Compared with Example 2, the structure of the two-dimensional ferroelectric photoelectric memristor provided in this embodiment includes a SiO2 / Si substrate layer, a SnSe functional layer, a Bi2Te 1.5 Se 1.5 Functional layer and Pd top electrode layer. Others are the same as in Example 2.

[0053] When voltage is applied to the devices in Examples 3 and 4, the polarization of the ferroelectric domain of the ferroelectric material in the functional layer is reversed, thereby changing the resistance of the device. However, the performance is not as comprehensive as that of the device in Example 2. The IV repeatability of the device in Example 3 is poor and the device response is slow. The device in Example 4 has a relatively weak response to light of 405 nm wavelength.

Claims

1. A two-dimensional ferroelectric photoelectric memristor, characterized in that The structure is formed on the SiO2 / Si substrate in sequence with SnSe y Functional layer, Bi2Te 3-x Se x Functional layer and Pd top electrode layer; wherein, 0<x<3, 0.6<y<2.

2. The two-dimensional ferroelectric photoelectric memristor according to claim 1, characterized in that Sn Se y The thickness of the functional layer is 3 to 90 nm, Bi2Te 3-x Se x The thickness of the functional layer is 3 to 120 nm, and the thickness of the Pd top electrode layer is 30 to 200 nm.

3. The two-dimensional ferroelectric photoelectric memristor according to claim 2, characterized in that Sn Se y The thickness of the functional layer is 10-12 nm, Bi2Te 3-x Se x The thickness of the functional layer is 3-5 nm, and the thickness of the Pd top electrode layer is 30-40 nm.

4. A method for preparing a two-dimensional ferroelectric photoelectric memristor, characterized in that: The steps include: (a) SnSe y Preparation of target material: Mix granular Sn and Se in a set ratio, calcine in a muffle furnace at 800-950°C for 20-24 hours, then cool for 20-24 hours, ball mill, and then calcine in a plasma sintering furnace at 40-50MPa and 450-525°C to obtain SnSe y Target material; 0.6<y<2; (b)Bi2Te 3-x Se x Preparation of target material: Bi2Te is prepared by mixing granular Bi, Te and Se in a set ratio, calcining them at 800-950°C for 20-24 hours in a muffle furnace, cooling them for 20-24 hours, ball milling them, and then calcining them in a plasma sintering furnace at 40-50 MPa and 450-525°C to obtain Bi2Te 3-x Se x Target material; 0<x<3; (c) ultrasonically cleaning the Si wafer with acetone, alcohol and deionized water in sequence, then soaking the Si wafer in HF solution for 1 to 2 minutes, then placing the Si wafer in a thermal oxidation furnace, passing dry O2 with a flow rate of 0.1 to 1 sccm, annealing at 300 to 600° C. for 1 to 3 minutes, and growing a SiO2 film with a thickness of 2 to 4 nm on the Si wafer to form a SiO2 / Si substrate; (d) SnSe was deposited on SiO2 / Si substrate using pulsed laser deposition technology y The conditions are: Ar pressure 0.1-0.2 Pa, laser energy density 1.3-1.5 J / cm 2 , laser frequency 3~5Hz, substrate temperature 250~300℃; (e) Pulsed laser deposition technology was used to continue the SnSe y Bi2Te film deposition 3-x Se x The conditions are: Ar pressure 35-40Pa, laser energy density 1-1.2J / cm 2 , laser frequency 3~5Hz, substrate temperature 250~300℃; (f) Using DC magnetron sputtering technology, the mask is placed on the Bi2Te 3-x Se x / SnSe y On the substrate of the functional layer, the chamber is evacuated, argon gas is introduced into the chamber, the pressure is 1-1.5 Pa, the DC source is turned on, and the DC source is adjusted to make the palladium target glow, pre-sputtering for 1-5 minutes, and then formal sputtering, on Bi2Te 3-x Se x / SnSe y A Pd top electrode layer is formed on the functional layer.

5. The method for preparing a two-dimensional ferroelectric photoelectric memristor according to claim 4, characterized in that: SnSe in step (a) y The target material is SnSe 1.2 Target material, Bi2Te in step (b) 3-x Se x The target material is Bi2Te 2.7 Se 0.3 Target material.

6. The method for preparing a two-dimensional ferroelectric photoelectric memristor according to claim 4, characterized in that: In step (f), the Pd top electrode layer includes a plurality of uniformly distributed 3-x Se x / SnSe y Circular electrodes with a diameter of 100 μm on the functional layer.

7. Application of the two-dimensional ferroelectric photoelectric memristor according to any one of claims 1 to 3 and the two-dimensional ferroelectric photoelectric memristor prepared by the method according to any one of claims 4 to 6 in neuromorphic computing.