Transparent substrate provided with functional stack of thin layers
By adopting a thin layer stack structure of transparent substrate containing titanium nitride and doped tungsten oxide layers in the functional stack, the problem of insufficient emissivity and durability in the prior art is solved, and high selectivity and low emission are achieved and improve chemical and mechanical durability.
Patent Information
- Application Number
- CN202380036599.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-28
- Filing Date
- 2023-04-26
- Publication Date
- 2024-12-06
AI Technical Summary
When the existing functional stacks meet the requirements of high light transmittance, low solar factor and low emissivity, there is a problem of high emissivity, and lack a functional metal layer that reflects infrared radiation, especially a silver-based layer, and has durability. Insufficient, especially when in contact with the external environment.
A thin layer stack structure using a transparent substrate, including one or more dielectric modules, a titanium nitride layer and a tungsten oxide layer, the tungsten oxide layer contains Group 1 chemical element doping elements of the IUPAC nomenclature, through magnetron control The tungsten oxide layer is deposited by a sputtering method and the tungsten oxide layer is encapsulated in a dielectric module to improve durability.
Significantly improve selectivity, maintain high light transmittance and low emissivity, and enhance mechanical and chemical durability, especially in single-layer assembly glass applications, selectivity is increased by more than 10% and emissivity is below 5W/m2. K.
Smart Images

Figure CN119095809A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a transparent substrate provided with a functional stack of thin layers. Technical Background
[0002] Functional stacks of thin layers are often used to provide insulation and / or sun protection functions for glazing in buildings. They are particularly intended to reduce air conditioning work and / or reduce excessive overheating (so-called "solar control" glazing) and / or reduce the amount of energy dissipated to the outside (so-called "low-emission" glazing).
[0003] For glazing that is exposed to high levels of sunlight, a solar control function is desired. The ability of a glazing to limit the amount of transmitted light energy is defined by the solar factor g, which is the ratio of the total energy transmitted through the glass surface or interior glazing to the incident solar energy. The lower the value of the solar factor g, the better the protection against solar radiation.
[0004] EP 0 239 280 A2 [GORDON ROY GERALD] 09.30.1987 describes a transparent glass substrate provided with a thin-film stack, starting from the substrate, comprising a first fluorine-doped tin oxide layer, a titanium nitride layer and a tin oxide layer. The stack provides solar control properties with reduced light reflection and coloration.
[0005] WO 2018 / 129135 A1 [GUARDIAN GLASS LLC [US]] 07.12.2018 describes a transparent glass substrate provided with a thin layer stack comprising three silicon nitride films sandwiched between two infrared radiation reflecting titanium nitride films. The stack imparts solar control properties that reduce the red color in the reflection, maintains chemical and mechanical durability and low emissivity.
[0006] WO 2020 / 128327 A1 [SAINT GOBAIN [FR]] 06.25.2020 also describes a transparent glass substrate having a thin-film stack comprising three silicon nitride films between which two infrared radiation-reflecting titanium nitride films are sandwiched. The stack imparts solar control and external invisibility properties, making the building almost or completely invisible from the outside to the occupants. The stack also has a reflection coefficient a* of 10 to -10 in the La*b* system.
[0007] WO 2021 / 170959 A1 [SAINT GOBAIN [FR]] 09.02.2021 describes a transparent glass substrate provided with a multilayer comprising a two-layer dielectric module between which is inserted a thin layer based on titanium nitride reflecting infrared radiation and a metallic intermediate layer based on silicon, aluminum, titanium or a mixture thereof. The multilayer provides solar control properties with a light transmittance of more than 30% and an emissivity of less than 50%. The multilayer also has a certain chemical and mechanical durability when directly exposed.
[0008] JP 2010180449 A [SUMITOMO METAL MINING CO [JP]] 08 / 19 / 2010 describes a tungsten oxide-based layer deposited by sputtering using a tungsten oxide target containing a chemical element selected from hydrogen, alkali metals, alkaline earth metals and rare earth metals. The layer has a "sunlight control" function due to its high absorption of near-infrared radiation.
[0009] EP 3686312 A1 [SUMITOMO METAL MINING CO [JP]] 07 / 29 / 2020 describes a layer based on tungsten oxide doped with cesium, and a method for depositing such a layer by sputtering. The layer has a "sunlight control" function, in particular due to its high absorption of infrared radiation. SUMMARY OF THE INVENTION
[0011] Technical issues
[0012] A functional stack is said to be suitable for such applications when it meets the triple requirement of high light transmittance, low solar factor value and low emissivity value. Thus, a functional stack is suitable when it has a high selectivity value s (defined as the ratio of light transmittance to high solar factor) and low emissivity.
[0013] Prior art solutions consisting of using only infrared radiation absorbing layers as functional layers in a functional stack are unsuitable since they have a higher emissivity which is incompatible with applications in the residential market, for example.
[0014] On the other hand, for applications in the residential market, in particular as single-glazing, the functional stack must have a certain chemical and mechanical durability, especially when it comes into contact with the external environment.
[0015] There is still a need to improve the energy performance of thin-layer stacks that do not contain any functional metal layers reflecting infrared radiation, in particular do not contain functional metal layers based on silver.
[0016] More specifically, there remains a need for multilayers having at least one titanium nitride-based layer reflecting infrared radiation with high selectivity and suitable overall energetic properties, in particular in terms of emissivity.
[0017] Solutions to technical problems
[0018] A first aspect of the invention relates to a transparent substrate as disclosed in claim 1, the dependent claims being advantageous embodiments. The transparent substrate is provided on one of its main surfaces with a stack of thin layers, said stack consisting, starting from the substrate, of the following layers:
[0019] - a first dielectric module of one or more thin layers;
[0020] - a layer based on titanium nitride;
[0021] - one or more thin layers of a second dielectric module;
[0022] The first dielectric module and / or the second dielectric module comprises, starting from the substrate:
[0023] - a first thin layer based on nitride;
[0024] - an absorber layer based on tungsten oxide;
[0025] - a second thin layer based on nitride;
[0026] - the tungsten oxide comprises at least one doping element selected from the chemical elements of group 1 according to the IUPAC nomenclature.
[0027] Advantageous embodiments are described in the detailed description.
[0028] According to a second aspect of the present invention, there is provided a single glazing and a laminated glazing comprising a transparent substrate according to the first aspect of the present invention.
[0029] According to a third aspect of the present invention, there is provided a method for producing a transparent substrate according to the first aspect of the present invention.
[0030] Advantages of the invention
[0031] The significant advantages of glazing comprising the transparent substrate according to the invention are gains of up to 10% or more in selectivity while maintaining sufficient light transmittance levels (greater than 65% in single-glazing applications) and 5 W / m 2 .K or even lower emissivity.
[0032] Another advantage of the present invention is that the functional stack has better mechanical and chemical durability, in particular by encapsulating the tungsten oxide layer with a nitride-based layer, as detailed in some embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] [ Figure 1 ] is a schematic diagram of an embodiment of the first aspect of the present invention.
[0035] [ Figure 2 ] is a schematic diagram of a second embodiment of the first aspect of the present invention.
[0036] Implementation Detail
[0037] The following definitions and conventions apply.
[0038] The terms "above" and "below", which respectively describe the position of a layer or a layer assembly and are defined relative to the position of another layer or another assembly, mean that the layer or the layer assembly is closer to the substrate or farther away from the substrate, respectively. The two terms "above" and "below" in no way mean that the layer or layer assembly they describe is in contact with the other layer or another assembly defined relative to it. They do not exclude the presence of other intermediate layers between the two layers. The expression "in contact" is explicitly used to indicate that no other layers are arranged between them.
[0039] In the absence of any more complete information or qualifiers, the term "thickness" used for a layer corresponds to the physical thickness, actual thickness or geometric thickness e of said layer. It is expressed in nanometers.
[0040] The expression "dielectric module" means one or more layers in contact with one another, which form a layer assembly which is dielectric as a whole, that is to say which does not have the function of a functional metallic layer. If the dielectric module comprises a plurality of layers, these themselves may be dielectric. The physical thickness, actual thickness or geometric thickness of a dielectric module of a plurality of layers corresponds to the sum of the physical thickness, actual thickness or geometric thickness of each of the layers constituting it.
[0041] In the present description, the expressions "layer of" or "layer based on" used to describe a material or a material contained in a layer are used equally. They mean that the mass fraction of the components contained therein is at least 50%, in particular at least 70%, preferably at least 90%. In particular, the presence of minority or doping elements is not excluded.
[0042] The term "transparent" as used to describe the substrate means that the substrate is preferably colorless, non-opaque and non-translucent to minimize light absorption and thereby maintain maximum light transmittance in the visible electromagnetic spectrum.
[0043] In the case of architectural glazing, in particular single-glazing, "light transmittance" is understood to mean the light transmittance as defined and measured in section 4.2 of standard EN 410, denoted TL.
[0044] In the case of architectural glazing, the light transmittance TL in the visible spectrum, the solar factor g and the selectivity s, the internal reflectance Rint in the visible spectrum and the external reflectance Rext are defined in accordance with the standards EN 410, ISO 9050 and ISO 10292 in the case of glazing, measured and calculated accordingly.
[0045] In the case of laminated glazing, the “heat transmission coefficient” Ug is understood to mean the heat transmission coefficient as defined in accordance with standard EN 673.
[0046] According to the IUPAC nomenclature, Group 1 chemical elements contain hydrogen and the alkaline elements, namely lithium, sodium, potassium, rubidium, cesium, and francium.
[0047] The expressions "optical refractive index" and "optical extinction coefficient" are understood as the optical refractive index n and the optical extinction coefficient k as defined in the technical field, in particular according to Forouhi & Bloomer as described in Forouhi & Bloomer, Handbook of Optical Constants of Solids II, Palik, ED (ed.), Academic Press, 1991, Chapter 7.
[0048] According to a first aspect of the present invention, referring to Figure 1 , a transparent substrate 1000 is provided with a stack 1001 of thin layers on one of its main surfaces, the stack 1001 consisting, starting from the substrate, of the following layers:
[0049] - a first dielectric module 1002 of one or more thin layers;
[0050] - a layer 1003 based on titanium nitride;
[0051] - one or more thin layers of a second dielectric module 1004;
[0052] The first dielectric module 1002 and / or the second dielectric module 1003 include, starting from the substrate 1001:
[0053] - a first thin layer 1002a, 1004a based on nitride;
[0054] - Absorption layers 1002b, 1004b based on tungsten oxide;
[0055] - a second thin layer 1002c, 1004c based on nitride;
[0056] - the tungsten oxide comprises at least one doping element selected from the chemical elements of group 1 according to the IUPAC nomenclature.
[0057] According to the first aspect of the present invention, the first dielectric module 1002 and / or the second dielectric module 1004 comprises a layer 1002b, 1004b of tungsten oxide. Thus, in a first embodiment, only the first dielectric module 1002 comprises a layer 1002b of tungsten oxide. In a second embodiment, only the second dielectric module 1004 comprises a layer 1004b of tungsten oxide. In a third embodiment, the dielectric modules 1002, 1004 each comprise a layer 1002b, 1004b of tungsten oxide.
[0058] When the first dielectric module and the second dielectric module each include a tungsten oxide layer, the tungsten oxides in the two tungsten oxide layers may have different compositions.
[0059] The transparent substrate 1000 may preferably be planar. It may be organic or inorganic, rigid or flexible. In particular, it may be an inorganic glass, such as soda-lime-silica glass.
[0060] Examples of organic substrates that can be advantageously used in the implementation of the present invention may be polymeric materials such as polyethylene, polyester, polyacrylate, polycarbonate, polyurethane or polyamide. These polymers may be fluorine-containing polymers.
[0061] Examples of inorganic substrates that can be advantageously used in the present invention can be sheets of inorganic glass or glass ceramics. The glass can preferably be a glass of soda-lime-silica, borosilicate, aluminosilicate or aluminoborosilicate type. According to a preferred embodiment of the present invention, the transparent substrate 1000 is a sheet of soda-lime-silica inorganic glass.
[0062] According to the invention, stack 1001 of thin layers does not contain any functional metal layers reflecting infrared radiation, in particular does not contain any functional metal layers based on silver.
[0063] Preferably, the optical refractive index of the tungsten oxide layers 1002b, 1004b decreases monotonically with wavelength from a maximum value greater than 2.4 at 350nm to a minimum value between 600nm and 1400nm, so that the difference between the maximum and minimum values is greater than 0.8, preferably greater than 1.0, or even greater than 1.4.
[0064] In other words, the value of the optical refractive index decreases monotonically by at least 0.8, preferably at least 1.0, or even at least 1.4 between a maximum value of greater than 2.4 at 350 nm and a minimum value of 600 nm to 1400 nm. For example, the optical refractive index value may decrease monotonically by at least 0.8, preferably at least 1.0, or even at least 1.4 between a maximum value of greater than 2.4 at 350 nm and a minimum value of less than 2.3 at 600 nm to 1400 nm, especially at 800 nm to 1100 nm.
[0065] While not particularly required to achieve the effects of the present invention, these optical refractive index values may still be beneficial in improving color neutrality in transmission and reflection.
[0066] Preferably, the optical extinction coefficient of the tungsten oxide layers 1002b, 1004b may be less than 0.2 or even 0.1 at 500 nm, and may be less than 2 or even less than 1.5 at 1200 nm, thereby further improving the selectivity.
[0067] The optical extinction coefficient and the optical diffraction index can vary depending on the nature and amount of the doping element selected from the elements of group 1 according to the IUPAC nomenclature. However, it is currently difficult to establish a general law of behavior of the optical extinction coefficient and the refractive index depending on the nature and / or amount of the doping element.
[0068] According to certain specific embodiments, the tungsten oxide layers 1002b, 1004b contain a doping element X or multiple doping elements X1, X2... in a ratio such that the molar ratio X / W of the element to tungsten W or the sum of the molar ratios of each element to tungsten (X1+X2+...) / W is 0.01 to 0.6, preferably 0.02 to 0.3.
[0069] It is observed that these molar ratio values can advantageously make it possible to obtain the values of the optical extinction coefficient and the refractive index described in the previous embodiments, while limiting the amount of doping elements. In addition, this may lead to a saving in the mining of mineral resources of the doping elements, as well as a reduction in costs.
[0070] According to some embodiments, the tungsten oxide layers 1002b, 1004b contain at least one doping element selected from hydrogen, lithium, sodium, potassium and cesium. Among the elements of group 1, these specific elements make it possible to obtain the values of the optical extinction coefficient and the refractive index that are optimal for the desired technical effect.
[0071] According to particularly preferred embodiments, the tungsten oxide layers 1002b, 1004b contain cesium as a doping element, and the molar ratio of cesium to tungsten is 0.01 to 0.4, preferably 0.01 to 0.2. These embodiments allow for optimal performance to improve selectivity, maintain neutral color and cost savings.
[0072] According to some advantageous embodiments, the physical thickness of the tungsten oxide layers 1002b, 1004b may be 6nm to 350nm, in particular 20nm to 250nm, preferably 40nm to 200nm. These thickness intervals are sufficient to obtain the significant advantages of the first aspect of the present invention.
[0073] According to some embodiments, the first nitride-based film 1002a, 1004a and the second nitride-based film 1002c, 1004c of the first dielectric module 1002 and / or the second dielectric module 1004 may be selected from aluminum nitride, silicon zirconium nitride, or silicon nitride optionally doped with aluminum, zirconium and / or boron.
[0074] In a preferred embodiment, the first nitride layers 1002a, 1004a and the second nitride layers 1002c, 1004c of the first dielectric module 1002 and the second dielectric module 1004 are based on aluminum nitride or silicon nitride.
[0075] The first nitride-based layers 1002a, 1004a and the second nitride-based layers 1002c, 1004c of the first dielectric module 1002 and / or the second dielectric module 1004 are located on either side of the tungsten oxide-based layers 1002b, 1004b. The tungsten oxide-based layers 1002b, 1004b are then encapsulated.
[0076] This encapsulation allows a double protection of the absorbing layers 1002b, 1004b based on tungsten oxide. On the one hand, it prevents any contamination by elements capable of diffusing from the substrate into the stack, such as alkali metals or oxygen ions in particular in the case of inorganic glass substrates. On the other hand, it makes it possible to limit, in particular during the annealing heat treatment step, the diffusion of oxygen from the atmosphere and / or the substrate towards the absorbing layers based on tungsten oxide into the stack.
[0077] Due to the encapsulation, the chemical composition and the degree of oxidation of the absorptive tungsten oxide layer hardly change over time, or if they do, this change is favorable to the selectivity. In addition, the encapsulation ensures an appropriate level of selectivity when the stack is subjected to an annealing heat treatment. In use, the substrate according to the first aspect of the invention is more durable, in particular its properties are retained for a long time.
[0078] The first dielectric module 1002 and the second dielectric module 1004 may contain additional thin layers. In particular, these additional layers may have a chemical composition that allows to impart specific optical properties to the substrate (for example in terms of color or filtering of specific wavelengths of the electromagnetic spectrum). They may also impart certain mechanical and / or chemical properties, such as resistance to wear, delamination and / or chemical attack. These layers are generally based on oxides or oxynitrides of metals or metal alloys.
[0079] Depending on their composition and their arrangement in the stack, these additional layers can be sources of contamination of the tungsten oxide-based absorber layer. These sources of contamination can be diffusion of certain metal or dopant ions or oxygen diffusion. They can occur during the deposition of the additional layers, during the optional heat treatment of the stack, or in use.
[0080] Such contamination may alter the tungsten oxide based absorbing layer and be detrimental to the performance of the substrate according to the first aspect of the invention.
[0081] In a preferred embodiment, the first nitride-based layers 1002a, 1004a and the second nitride-based layers 1002c, 1004c of the first dielectric module 1002 and the second dielectric module 1004 are in contact with the tungsten oxide layers 1002b, 1004b.
[0082] According to certain embodiments, the first dielectric module 1002 and / or the second dielectric module 1004 are formed starting from the substrate 1000 by:
[0083] - a first thin layer 1002a, 1004a based on nitride;
[0084] - an absorption layer 1002b, 1004b based on tungsten oxide; and
[0085] - A second thin layer 1002c, 1004c based on nitride.
[0086] When the first dielectric module 1002 and / or the second dielectric module 1004 are constructed in this way, i.e. only contain the above-mentioned nitride-based layers, the risk of the tungsten oxide-based absorption layer being altered by possible oxygen diffusion is limited or even eliminated. The durability of the substrate according to the first aspect of the invention can then be maximum in the required "solar control".
[0087] According to an embodiment, the thickness of the titanium nitride layer 1003 is 5 nm to 25 nm, preferably 10 nm to 20 nm, the thickness of the tungsten oxide-based absorption layer is 5 to 100 nm, preferably 10 to 50 nm, and the thickness of the nitride-based layers 1002a, 1004a, 1002c, 1004c of the first dielectric module 1002 and the second dielectric module 1004 is 5 nm to 100 nm, preferably 5 nm to 50 nm.
[0088] According to a second aspect of the present invention, there is provided a single-layer glazing comprising a substrate according to the first aspect of the present invention. Figure 2 , also provided is a laminated assembly glass 2000, which includes a first transparent substrate 1000 according to the first aspect of the present invention, a laminated interlayer 2001 and a second transparent substrate 2002, so that the first transparent substrate 1000 and the second transparent substrate 2002 are bonded and contacted with the laminated interlayer 2001, and a stack 1001 of thin layers of the first transparent substrate 1000 is in contact with the laminated interlayer 2001.
[0089] The lamination interlayer 2001 may consist of one or more layers of thermoplastic material. Examples of thermoplastic materials are polyurethane, polycarbonate, polyvinyl butyral (PVB), polymethyl methacrylate (PMMA), ethylene vinyl acetate (EA) or ionomer resins.
[0090] The laminate interlayer 2001 may be in the form of a multilayer film. It may also have specific functions, such as acoustic or anti-UV properties.
[0091] Typically, the laminate interlayer 2001 comprises at least one PVB layer. Its thickness ranges from 50 μm to 4 mm. Typically, it is less than 1 mm.
[0092] According to certain preferred embodiments, the laminated glazing 2000, when used as a glazing for a motor vehicle, for example as a windshield, is such that the substrate 1000 according to the first aspect of the invention is located inside the vehicle. In other words, the stack is placed starting with the substrate 1000 facing the interior of the vehicle on face 2 of the glazing, face 1 being the face facing the interior, or starting with the substrate 1000 facing the exterior of the vehicle on face 3 of the glazing, face 1 being the face facing the exterior.
[0093] According to certain embodiments, the second substrate 2002 can be an inorganic glass that is dyed in the mass. Dyeing or coloring in an inorganic glass mass is known and is described in great detail in the technical literature. The coloring can generally be obtained by adding a colored oxide to the glass chemical composition. Examples of colored oxides can be iron II oxide, copper oxide, chromium oxide, nickel oxide, gold oxide, manganese oxide, cobalt oxide, uranium oxide, neodymium oxide, and erbium oxide. Mixtures of oxides can also be used, such as copper tin oxide, or ionic complexes, such as iron-sulfur or cadmium-sulfur complexes.
[0094] Laminated glass manufacturing methods are well known in the glass industry. For example, a method for manufacturing laminated glazing may be a method of laminating a laminated interlayer between two glass sheets. The glass sheets may be preformed, for example in a curved shape using a bending process. They may also be coated with one or more thin layer coatings using any suitable thin layer deposition process.
[0095] Methods for depositing thin layers on substrates, particularly glass sheets, are well known in the industry. For example, depositing a stack of thin layers on a glass substrate is performed by successively depositing each thin layer of the stack by passing the glass substrate through a series of deposition chambers suitable for depositing a given thin layer.
[0096] The deposition chamber may use deposition methods such as magnetic field assisted sputtering, ion beam assisted deposition (IBAD), evaporation, chemical vapor deposition (CVD), plasma enhanced chemical vapor deposition (PECVD), low pressure chemical vapor deposition (LPCVD), and the like.
[0097] In particular, a magnetic field enhanced sputtering deposition method is used. The conditions for depositing the layers are widely described in the literature, for example in patent applications WO 2012 / 093238 A1 and WO 2017 / 00602 A1.
[0098] According to a third aspect of the present invention, a method for manufacturing a substrate 1000 according to the first aspect of the present invention is provided, wherein one or more absorptive tungsten oxide layers 1002b, 1004c are deposited by magnetron sputtering using a tungsten oxide target, and the tungsten oxide target is doped with a chemical element selected from the chemical elements of Group 1 according to the IUPAC nomenclature.
[0099] The tungsten oxide target may contain one or more doping elements in particular in the ratios as described for the doped tungsten oxide layer in some embodiments of the first aspect of the present invention.
[0100] The tungsten oxide layers 1002b, 1004b can be deposited by sputtering using the above-mentioned target in a deposition atmosphere consisting of 60% to 100% argon and 0% to 40% molecular oxygen, preferably 70% to 85% argon and 15% to 30% molecular oxygen.
[0101] The tungsten oxide layers 1002b, 1004b may be deposited at a pressure of 1 to 15 mTorr, preferably 3 to 10 mTorr.
[0102] Preferably, for this substrate, the deposition can be carried out under cold conditions, ie at a temperature of less than 100°C, in particular from 20°C to 60°C.
[0103] The deposition can also be carried out under thermal conditions, in particular at a temperature between 100°C and 400°C.
[0104] According to a specific embodiment, after depositing the stack 1001, the substrate 1000 may be subjected to an annealing heat treatment. The annealing temperature may be 450° C. to 800° C., in particular 550° C. to 750° C., or even 600° C. to 700° C. The annealing time may be 5 minutes to 30 minutes, in particular 5 minutes to 20 minutes, or even 5 minutes to 10 minutes.
[0105] All embodiments described, whether they relate to the first or second aspect of the invention, can be combined with one another without modification or special adaptation. If technical incompatibilities arise during the implementation of one of these combinations, it is within the scope of the skilled person to be able to resolve these incompatibilities with the help of their knowledge without undue effort, in particular by implementing research solutions. Example
[0106] The features and advantages of the present invention are demonstrated by the non-limiting examples disclosed hereinafter.
[0107] Two examples E1 to E2 according to the invention and two comparative examples CE1 and CE2 not according to the invention are described in Table 1, indicating the composition and thickness in nanometers of the various layers. The numbers in the first two columns correspond to the reference numbers in the drawings.
[0108] The cesium-doped tungsten oxide layer, denoted as CWO, has a molar ratio of cesium to tungsten of about 0.05-0.06.
[0109]
[0110] Comparative Example CE1 differs from the other examples in that no tungsten oxide layer is present.
[0111] The thin-layer stack 1004 of the functional coating of Examples E1 to E3 and Comparative Examples CE1 and CE2 was deposited by magnetic field-assisted cathode sputtering (magnetron method), the properties of which are widely described in the literature, for example in patent applications WO2012 / 093238 and WO2017 / 00602.
[0112] The properties of the targets used and the deposition conditions of Examples E1 to E2 and Comparative Example CE1 are described in Table 2.
[0113] The functional coating 1001 is deposited directly on a glass sheet 1000. The glass sheet 1000 is a 6 mm thick sheet of soda-lime-silica inorganic glass. Immediately after deposition, the functional coating is subjected to a heat treatment at 650°C for 10 minutes.
[0114]
[0115] The solar factor g, the selectivity s, the light transmittance TL, the light reflectance Rint on the inner face and the light reflectance Rext on the outer face, and the color in transmission on the inner face and on the outer face were measured for each of Examples E1 to E2 and Comparative Example CE1.
[0116] The light transmittance TL in the visible spectrum, the solar factor g, the selectivity s, as well as the internal reflectance Rint and the external reflectance Rext in the visible spectrum are defined, measured and calculated in accordance with standards EN 410, ISO 9050 and / or ISO 10292.
[0117] Emissivity Ug is defined, measured and calculated in accordance with EN 410 and EN 12898.
[0118] The expression "color" used to describe a transparent substrate provided with a multilayer is understood to mean the color as defined in the L*a*b*CIE 1976 color space according to standard ISO 11664, in particular with a D65 illuminant and a field of view of 2° or 10° for a reference observer. It is measured according to said standard.
[0119] The measured values of emissivity, solar factor, selectivity, transmittance, internal reflectivity, external reflectivity, color parameters a* and b* in transmission (a*T, b*T), external reflection (a*Rext, b*Rext) and internal reflection (a*Rint, b*Rint) are summarized in Table 3.
[0120]
[0121]
[0122] Compared to comparative example CE1, examples E1 and E2 have a lower solar factor for the same light transmittance. Their selectivity is therefore higher. The heat transfer coefficients of examples E1 and E2 are similar to the comparative example, or even slightly lower for example E1. The parameters a* and b* are close to zero both in transmission and reflection, indicating that examples E1 and E2 have a relatively neutral color in transmission and / or reflection.
[0123] Examples E1 and E2 also exhibit lower, if not comparable, levels of internal and external reflection as compared to Comparative Example CE1.
[0124] The stacks 1001 of Examples E1 to E2 and Comparative Example CE1 have also been used to form laminated glazings, respectively labeled VFE1, VFE2 and VFCE1.
[0125] The functional coating 1001 was deposited on a 4 mm thick sheet of soda-lime-silica inorganic glass 1000 under the same conditions as above. Just after deposition, the functional coating was subjected to a heat treatment at 650° C. for 10 minutes.
[0126] Once the deposition and heat treatment are complete, each glass sheet 1000 with the functional coating 1001 is laminated with a laminating interlayer 2001 of 0.38 mm thick PVB and a second glass sheet 2002 of 4 mm thick soda-lime-silica inorganic glass to form a laminate such as Figure 2 Laminated glazing shown in .
[0127] The solar factor g, the selectivity s, the light transmittance TL, the light reflectance Rint on the inner face and Rext on the outer face, and the color in transmission on the inner face and on the outer face were measured for each of the examples VFE1 to VFE2 and the comparative example VFCE1.
[0128] The light transmittance TL in the visible spectrum, the solar factor TTS, the selectivity s as well as the internal reflectance Rint and the external reflectance Rext in the visible spectrum are defined, measured and calculated in accordance with standard ISO 13837:2021.-convention A.
[0129] The heat transfer coefficient Ug is defined, measured and calculated according to standard EN 673.
[0130] The expression "color" used to describe a transparent substrate provided with a multilayer is understood to mean the color as defined in the L*a*b*CIE 1976 color space according to standard ISO 11664, in particular with a D65 illuminant and a field of view of 2° or 10° for a reference observer. It is measured according to said standard.
[0131] The measured values of emissivity, solar factor, selectivity, transmittance, internal reflectivity, external reflectivity, color parameters a* and b* in transmission (a*T, b*T), external reflection (a*Rext, b*Rext) and internal reflection (a*Rint, b*Rint) are summarized in Table 4.
[0132] Table 4 VFE1 VFE2 VFCE1 g 58.8 56.1 57.9 s 1.16 1.19 1.14 TL 68.3 66.5 66 a*T -4.0 -4.0 -3.4 b*T 0.0 0.0 0.0 Rext 8.1 12.7 8.0 a*Rext 0.9 -3.6 0.5 b*Rext -2.3 -0.1 0.0 Rint 7.2 7.2 8.1 a*Rint 1.4 1.9 0.3 b*Rint -5.0 -6.4 0.5 Ug 5.6 5.6 5.6
[0133] Compared to comparative example VFCE1, examples VFE1 and VFE2 provide higher selectivity. The emissivity of examples E1 and E2 is similar to that of the comparative example. The parameters a* and b* are close to zero in both transmission and reflection, indicating that examples E1 and E2 have relatively neutral colors in transmission and / or reflection.
[0134] These examples show very clearly the advantages of the substrates and glazings according to the invention, namely their higher selectivity and neutral color.
Claims
1. A transparent substrate (1000) provided on one of its main surfaces with a stack of thin layers (1001), said stack (1001) consisting, starting from the substrate, of the following layers: - a first dielectric module (1002) of one or more thin layers; - a layer (1003) based on titanium nitride; - a second dielectric module (1004) of one or more thin layers; The first dielectric module (1002) and / or the second dielectric module (1004) comprises, starting from the substrate (1001): - a first thin layer (1002a, 1004a) based on nitride; - an absorption layer (1002b, 1004b) based on tungsten oxide; - a second thin layer based on nitride (1002c, 1004c); - the tungsten oxide comprises at least one doping element selected from the chemical elements of group 1 according to the IUPAC nomenclature.
2. The substrate according to claim 1, wherein the tungsten oxide layer (1002b, 1004b) comprises a doping element X or multiple doping elements X1, X2, ... in a ratio such that the molar ratio X / W of the element to tungsten W or the sum of the molar ratios of each element to tungsten (X1+X2+...) / W is 0.01 to 0.6, preferably 0.02 to 0.
3.
3. The substrate according to any one of claims 1 to 2, wherein the tungsten oxide layer (1002b, 1004b) contains at least one doping element selected from the group consisting of hydrogen, lithium, sodium, potassium and cesium.
4. The substrate according to claim 3, wherein the tungsten oxide layer (1002b, 1004b) contains cesium as a doping element, and the molar ratio of cesium to tungsten is 0.01 to 0.4, preferably 0.01 to 0.
2.
5. The substrate according to any one of claims 1 to 4, wherein the physical thickness of the tungsten oxide layer (1002b, 1004b) can be 6nm to 350nm, in particular 20nm to 250nm, preferably 40nm to 200nm.
6. The substrate according to any one of claims 1 to 5, wherein the first nitride-based layer (1002a, 1004a) and the second nitride-based layer (1002c, 1004c) of the first dielectric module (1002) and the second dielectric module (1004) are based on aluminum nitride or silicon nitride.
7. The substrate according to any one of claims 1 to 6, wherein the first nitride-based layer (1002a, 1004a) and the second nitride-based layer (1002c, 1004c) of the first dielectric module (1002) and the second dielectric module (1004) are in contact with the tungsten oxide layer (1002b, 1004b).
8. The substrate according to any one of claims 1 to 7, wherein the first dielectric module (1002) and / or the second dielectric module (1004) is formed starting from the substrate (1000) by: - a first thin layer (1002a, 1004a) based on nitride; - an absorption layer based on tungsten oxide (1002b, 1004b); - a second thin layer based on nitride (1002c, 1004c).
9. The transparent substrate according to any one of claims 1 to 8, wherein the thickness of the titanium nitride layer (1003) is 5 nm to 100 nm, preferably 10 nm to 50 nm, the thickness of the tungsten oxide-based absorption layer is 5 to 100 nm, preferably 10 to 50 nm, and the thickness of the nitride-based layers (1002a, 1004a, 1002c, 1004c) of the first dielectric module (1002) and the second dielectric module (1004) is 5 nm to 100 nm, preferably 5 nm to 50 nm. 10 . A single-glazing comprising the substrate according to claim 1 .
11. A laminated glazing (2000), comprising a first transparent substrate (1000), a laminating interlayer (2001) and a second transparent substrate (2002) according to any one of claims 1 to 9, wherein the first transparent substrate (1000) and the second transparent substrate (2002) are in adhesive contact with the laminating interlayer (2001), and a stack (1001) of thin layers of the first transparent substrate (1000) is in contact with the laminating interlayer (2001).
12. A method for manufacturing a transparent substrate according to any one of claims 1 to 9, wherein the tungsten oxide layer (1002b, 1004c) is deposited by magnetron sputtering using a tungsten oxide target, and the tungsten oxide target is doped with a chemical element selected from the chemical elements of Group 1 according to the IUPAC nomenclature.
13. The manufacturing method according to claim 12, wherein the absorptive tungsten oxide layer is deposited at a substrate temperature of less than 100°C, preferably 20°C to 60°C.
14. The manufacturing method according to claim 12, wherein the absorptive tungsten oxide layer is deposited in a deposition atmosphere consisting of 60% to 100% argon and 0% to 40% molecular oxygen, preferably 70% to 85% argon and 15% to 30% molecular oxygen. 15 . The manufacturing method according to claim 12 , wherein the tungsten oxide layer is deposited at a pressure of 1 to 15 mTorr, preferably 3 to 10 mTorr.
Citation Information
Patent Citations
Target material of composite tungsten oxide, and method for manufacturing the same
JP2010180449A
Heat treatable coated article having titanium nitride based IR reflecting layer(s)
US20180186691A1
Glazing comprising a functional coating and an absorbing coating having a colorimetric adjustment
US20210347685A1
Conductive substrate for OLED device, as well as OLED device incorporating same
WO2014091137A1
Material provided with a stack having thermal properties
WO2017006029A1