Reducing stress agent and resin composition

By using organosiloxane-based rubber and graft copolymers containing epoxy-containing units in the sealing material, a low-stressing agent is formed, and the dispersion and line of the low-stressing agent in the matrix resin in the prior art is solved. The problem of insufficient expansion coefficient achieves low elastic modulus and good linear expansion coefficient of the sealing material, improving the heat and impact resistance of the material.

CN119095915APending Publication Date: 2024-12-06KANEKA CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202380030441.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-29
Filing Date
2023-03-24
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

There is room for improvement in the dispersion of existing low-stressing agents in matrix resins and the linear expansion coefficient of cured substances. Especially when reducing the elastic modulus of the sealing material, it is difficult to take into account both the low elastic modulus and the good linear expansion coefficient.

Method used

The graft copolymer containing organosiloxane-based rubber and epoxy-containing units is used as polymer particles to form a low-stressing agent to ensure excellent dispersion of polymer particles in the matrix resin and low elastic mode of cured substances. quantity and good linear expansion coefficient.

Benefits of technology

Excellent dispersion in the matrix resin, low elastic modulus and good linear expansion coefficient of the cured substance are achieved, and the heat resistance and impact resistance of the sealing material are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005059820650000451
    Figure BDA0005059820650000451
Patent Text Reader

Abstract

Provided is a low-stress agent which (i) has excellent dispersibility in a matrix resin and (ii) can provide a cured product having a good linear expansion coefficient. The problem is solved by a low stress agent containing polymer microparticles (A), the polymer microparticles (A) containing a rubber-containing graft copolymer having an elastomer and a graft part that is graft-bonded to the elastomer, the elastomer containing an organosiloxane rubber, and the amount of the rubber-containing graft copolymer being less than or equal to 100% by weight of the polymer microparticles (A), and the amount of the rubber-containing graft copolymer being less than or equal to 100% by weight of the polymer microparticles (A). The content of the elastomer is more than 70% by weight and 97% by weight or less, the graft part contains an epoxy group-containing constituent unit, the content of the epoxy group-containing constituent unit in the graft part is 0.5-4.0% by weight with respect to 100% by weight of the rubber-containing graft copolymer, and the low stress agent is a powder particle.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a stress reducing agent and a resin composition. Background Art

[0002] As a sealing material mainly used in semiconductor materials, a sealing material containing epoxy resin and silicon dioxide is used. When the sealing material is exposed to heat and light for a long time, cracks may be generated inside the sealing material. Therefore, in order to ensure the long-term reliability of the sealing material, a method of adding a stress reducing agent to the sealing material is widely used.

[0003] As such a stress reducing agent, a graft copolymer may be used.

[0004] For example, Patent Document 1 discloses a graft copolymer developed to reduce the elastic modulus of a curable resin composition and a molded body and to improve stress relaxation capability. The graft copolymer is obtained by polymerizing a grafting vinyl monomer with a rubber containing a polyorganosiloxane and a poly(meth)acrylic acid alkyl ester, wherein the poly(meth)acrylic acid alkyl ester in the rubber contains a (meth)acrylic acid alkyl ester unit having an alkyl group with 5 to 13 carbon atoms.

[0005] Patent Document 2 discloses a sealing liquid epoxy resin composition using a graft copolymer having a relatively low rubber content region.

[0006] Although not a technology related to a stress reducing agent, the polymer fine particles disclosed in Patent Document 3 are also graft copolymers.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Publication No. 2015-172185

[0010] Patent Document 2: International Publication No. 2017 / 188286 Pamphlet

[0011] Patent Document 3: Japanese Patent Publication No. 2018-035210 Summary of the invention

[0012] However, the above-mentioned conventional stress reducing agents still have room for further improvement from the viewpoints of (i) dispersibility in the matrix resin and (ii) linear expansion coefficient of a cured product of a resin composition containing the stress reducing agent and the matrix resin.

[0013] An object of one embodiment of the present invention is to provide a stress reducing agent that (i) has excellent dispersibility in a matrix resin and (ii) can provide a cured product having a good linear expansion coefficient when a resin composition containing the stress reducing agent and a matrix resin is cured.

[0014] The present inventors have conducted intensive studies to solve the above-mentioned problems and have completed the present invention as a result.

[0015] That is, one embodiment of the present invention includes the following configurations.

[0016] A stress reducing agent according to one embodiment of the present invention comprises polymer particles (A), wherein the polymer particles (A) comprise a rubber-containing graft copolymer, wherein the rubber-containing graft copolymer comprises an elastomer and a graft portion graft-bonded to the elastomer, wherein the proportion of the elastomer in the polymer particles (A) is greater than 70% by weight and less than 97% by weight relative to 100% by weight of the polymer particles (A), the elastomer comprises an organosilicone-based rubber, the graft portion comprises an epoxy-containing constituent unit, and the content of the epoxy-containing constituent unit in the graft portion is 0.5% by weight to 4.0% by weight relative to 100% by weight of the rubber-containing graft copolymer, and the stress reducing agent is a powder or granular material.

[0017] In another embodiment of the present invention, a stress reducing agent comprises polymer particles (A), wherein the polymer particles (A) comprise a rubber-containing graft copolymer, wherein the rubber-containing graft copolymer comprises an elastomer and a graft portion graft-bonded to the elastomer, wherein the proportion of the elastomer in the polymer particles (A) is greater than 70% by weight and less than 97% by weight relative to 100% by weight of the polymer particles (A), the elastomer comprises an organosilicone-based rubber, the graft portion comprises an epoxy-containing constituent unit, and the content of the epoxy-containing constituent unit in the graft portion is 3.3% by weight to 26.7% by weight relative to 100% by weight of the graft portion in the rubber-containing graft copolymer, and the stress reducing agent is a powder or granular material.

[0018] According to one embodiment of the present invention, there is provided an effect of being able to provide a stress reducing agent which (i) has excellent dispersibility in a matrix resin and (ii) can provide a cured product having a good linear expansion coefficient when a resin composition containing the stress reducing agent and a matrix resin is cured. DETAILED DESCRIPTION

[0019] Hereinafter, an embodiment of the present invention will be described, but the present invention is not limited thereto. The present invention is not limited to the various configurations described below, and various changes can be made within the scope indicated by the scope of the claims. In addition, embodiments or embodiments obtained by appropriately combining the technical means respectively disclosed in different embodiments or embodiments are also included in the technical scope of the present invention. In addition, by combining the technical means respectively disclosed in each embodiment, new technical features can be formed. It should be noted that all the academic literature and patent documents recorded in this specification are cited in this specification as references. In addition, in this specification, as long as there is no special explanation, "A to B" indicating a numerical range means "above A (including A and greater than A) and below B (including B and less than B)".

[0020] [1. Technical concept of one embodiment of the present invention]

[0021] The low stress agent added to the sealing material (resin composition) in order to ensure long-term reliability may need to reduce the function of the elastic modulus of the sealing material. On the other hand, the reduction of the elastic modulus of the sealing material caused by the low stress agent often leads to the deterioration of the linear expansion coefficient of the sealing material. That is, in the past, the reduction of the elastic modulus of the sealing material caused by the low stress agent and the maintenance of the linear expansion coefficient of the sealing material (reducing the deterioration of the linear expansion coefficient) had a divergent relationship, which was difficult to take into account. It should be noted that here, the deterioration of the linear expansion coefficient refers to the expansion of the sealing material due to the rise in temperature, in other words, the linear expansion coefficient becomes larger.

[0022] Under such circumstances, the present inventors have conducted intensive studies to provide a stress reducing agent capable of obtaining a cured product having a low elastic modulus and reduced deterioration in the linear expansion coefficient (in other words, having a good linear expansion coefficient).

[0023] During the in-depth research, the inventors independently discovered the following new insights:

[0024] (1) A stress reducing agent comprising polymer particles containing a rubber-containing graft copolymer having an elastomer containing an organosiloxane-based rubber and a graft portion graft-bonded to the elastomer can surprisingly provide a cured product having a low elastic modulus and reduced deterioration in the linear expansion coefficient, i.e., a good linear expansion coefficient; and

[0025] (2) It has surprisingly been found that the polymer fine particles described above can provide a cured product having a low elastic modulus and further reduced deterioration in the linear expansion coefficient, that is, a cured product having a better linear expansion coefficient, by including an epoxy group-containing structural unit in the graft portion.

[0026] Conventionally, diene rubber has been used as an elastomer of a rubber-containing graft copolymer contained in a stress reducing agent. In a stress reducing agent containing a rubber-containing graft copolymer containing an elastomer containing a diene rubber, the effect of reducing the deterioration of the linear expansion coefficient of a cured product brought about by the epoxy-containing constituent unit in the graft portion is small. That is, the effect of reducing the deterioration of the linear expansion coefficient of a cured product brought about by the epoxy-containing constituent unit in the graft portion is an effect that the inventors discovered for the first time in the process of intensive research using an elastomer containing an organosiloxane rubber, and is a heterogeneous effect that cannot be easily imagined based on conventional technical common sense.

[0027] In addition, the present inventors have independently obtained the following new insights during the process of in-depth research: when the amount of epoxy-containing constituent units contained in the grafted portion exceeds a certain amount, it is surprisingly found that the dispersibility of the stress reducing agent in the matrix resin decreases. The stress reducing agent is also required to have good dispersibility in the matrix resin. Therefore, the present inventors have further conducted in-depth research to provide a stress reducing agent that can obtain a cured product with excellent dispersibility in the matrix resin, low elastic modulus, and good linear expansion coefficient.

[0028] As a result, the inventors independently found the following new knowledge, thereby completing the present invention: It has surprisingly been found that a stress reducing agent containing the following polymer microparticles can provide a resin composition that can provide a cured product that (i) has excellent dispersibility in a matrix resin and (ii) has a low elastic modulus and a good linear expansion coefficient, wherein the polymer microparticles contain a rubber-containing graft copolymer having an elastomer containing an organosiloxane-based rubber and a graft portion containing a specific amount of epoxy-containing structural units graft-bonded to the elastomer.

[0029] 〔2. Stress Reduction Agent〕

[0030] The stress reducing agent involved in one embodiment of the present invention is a powder and contains polymer particles (A). The polymer particles (A) contain a rubber-containing graft copolymer having an elastomer and a graft portion graft-bonded to the elastomer. The proportion of the elastomer in the polymer particles (A) is greater than 70% by weight and less than 97% by weight relative to 100% by weight of the polymer particles (A), the elastomer contains an organosilicone rubber, and the graft portion contains an epoxy-containing constituent unit. The epoxy-containing constituent unit in the graft portion is contained in an amount of 0.5% to 4.0% by weight relative to 100% by weight of the rubber-containing graft copolymer.

[0031] Alternatively, in one embodiment of the present invention, the polymer particles (A) comprise a rubber-containing graft copolymer having an elastomer and a graft portion graft-bonded to the elastomer, wherein the proportion of the elastomer in the polymer particles (A) is greater than 70% by weight and less than 97% by weight relative to 100% by weight of the polymer particles (A), the elastomer comprises an organosilicone rubber, the graft portion comprises an epoxy-containing constituent unit, and the content of the epoxy-containing constituent unit in the graft portion is 3.3% by weight to 26.7% by weight relative to 100% by weight of the graft portion in the rubber-containing graft copolymer.

[0032] Hereinafter, "the low stress agent of one embodiment of the present invention" may also be referred to as "the present low stress agent". Since the present low stress agent has the above-mentioned structure, it has the advantage that the polymer particles (A) are excellently dispersed in the matrix resin. In other words, since the present low stress agent has the above-mentioned structure, it has the following advantages: by mixing the low stress agent with the matrix resin, a resin composition in which the polymer particles (A) are uniformly dispersed in the matrix resin can be provided. In addition, the present low stress agent has the following advantages: by curing the resin composition containing the low stress agent and the matrix resin, a cured product with a low elastic modulus and a good linear expansion coefficient can be provided. In this specification, "reducing the deterioration of the linear expansion coefficient of the cured product" is sometimes expressed as "the linear expansion coefficient of the cured product is good".

[0033] (2-1. Polymer microparticles (A))

[0034] The polymer fine particles (A) contain a rubber-containing graft copolymer having an elastomer and a graft portion graft-bonded to the elastomer.

[0035] (2-1-1. Elastic body)

[0036] The elastomer contains an organosiloxane rubber. The stress reducing agent can provide a cured product with a low elastic modulus and a good linear expansion coefficient by virtue of the elastomer containing the organosiloxane rubber. In addition, the resin composition can provide a cured product with sufficient heat resistance and excellent impact resistance at low temperatures by virtue of the elastomer containing the organosiloxane rubber. The elastomer can also be referred to as an elastic portion or rubber particles.

[0037] Examples of the organosiloxane rubber include (a) organosiloxane polymers composed of alkyl or aryl disubstituted siloxy units such as dimethylsiloxy, diethylsiloxy, methylphenylsiloxy, diphenylsiloxy, and dimethylsiloxy-diphenylsiloxy, and (b) organosiloxane polymers composed of alkyl or aryl monosubstituted siloxy units such as organohydrosiloxy in which a part of the alkyl group in the side chain is substituted with a hydrogen atom. These organosiloxane polymers may be used alone or in combination of two or more.

[0038] Cyclic siloxanes composed of a plurality of dimethylsiloxy units may also be used as a raw material for the organosiloxane rubber. Examples of the cyclic siloxanes include octamethylcyclotetrasiloxane (also known as "D4") having four dimethylsiloxy units, decamethylcyclopentasiloxane (also known as "D5") having five dimethylsiloxy units, and dodecamethylcyclohexasiloxane (also known as "D6") having six dimethylsiloxy units.

[0039] In this specification, for example, a polymer composed of dimethylsiloxy units is referred to as dimethylsiloxy rubber, a polymer composed of methylphenylsiloxy units is referred to as methylphenylsiloxy rubber, and a polymer composed of dimethylsiloxy units and diphenylsiloxy units is referred to as dimethylsiloxy-diphenylsiloxy rubber. As the organosiloxane rubber, (a) the linear expansion coefficient of the cured product is better, and the obtained resin composition can provide a cured product with excellent heat resistance, so it is more preferably selected from dimethylsiloxy rubber, methylphenylsiloxy rubber and dimethylsiloxy-diphenylsiloxy rubber. (b) Since it is easily available and economical, it is more preferably dimethylsiloxy rubber.

[0040] When preparing the organosiloxane rubber, as a raw material, a monomer containing (a) one or more hydrolyzable silyl groups and (b) one or more ethylenically unsaturated groups and / or mercapto groups in the molecule (hereinafter also referred to as "monomer M") can be used. In other words, the organosiloxane rubber can contain a constituent unit derived from the monomer M (hereinafter also referred to as "constituent unit M").

[0041] As the hydrolyzable silyl group contained in the monomer M, there is no particular limitation. As the hydrolyzable silyl group, for example, a halosilyl group, an acyloxysilyl group, an amide silyl group, an aminosilyl group, an alkenyloxysilyl group, an aminooxysilyl group, an oxime silyl group, an alkoxysilyl group, a thioalkoxysilyl group, a silanol group, etc. can be cited. Because it is rich in polymerization reactivity and easy to handle, an alkoxysilyl group is more preferably used as the hydrolyzable silyl group. When the monomer M contains more than two hydrolyzable silyl groups in the molecule, the multiple hydrolyzable silyl groups may be the same or different from each other.

[0042] Specific examples of the monomer M include vinyl silanes such as vinylmethyldimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, and tetramethyltetravinylcyclotetrasiloxane; β-methacryloxyethyldimethoxymethylsilane, 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyldimethoxymethylsilane, 3-(meth)acryloxypropylmethoxydimethylsilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropyldiethoxymethylsilane, 3- (Meth)acryloxyalkylsilanes such as (meth)acryloxypropyldiethoxyethylsilane, 3-(meth)acryloxypropylethoxydimethylsilane, 3-(meth)acryloxypropylethoxydiethylsilane, and δ-(meth)acryloxybutyldiethoxymethylsilane; and mercaptoalkylsilanes such as 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyldimethoxymethylsilane, 3-mercaptopropylmethoxymethylsilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropyldiethoxymethylsilane, and 3-mercaptopropyldiethoxyethylsilane. Specific examples of the monomer M include p-vinylphenylmethyldimethoxysilane, 2-(m-vinylphenyl)ethylmethyldimethoxysilane, 1-(m-vinylphenyl)methyldimethylisopropoxysilane, 2-(p-vinylphenyl)ethylmethyldimethoxysilane, 3-(p-vinylphenoxy)propylmethyldiethoxysilane, 3-(p-vinylbenzoyloxy)propylmethyldimethoxysilane, 1-(o-vinylphenyl)-1,1,2-trimethyl-2,2-dimethoxydisilane, 1-(p-vinylphenyl)-1,1-diphenyl-3-ethyl-3,3-diethoxydisiloxane, m-vinylphenyl-[3-(triethoxysilyl)propyl]diphenylsilane, and [3-(p-isopropenylbenzoylamino)propyl]phenyldipropoxysilane. These monomers M may be used alone or in combination of two or more.

[0043] Among them, as the monomer M, the compounds mentioned above as specific examples of (meth)acryloxyalkylsilanes are more preferred, and 3-(meth)acryloxypropyltrimethoxysilane and 3-(meth)acryloxypropyldimethoxymethylsilane are further preferred. According to this configuration, there is an advantage that the polymerization of the monomer mixture for forming the graft portion in the presence of the organosiloxane rubber can be effectively carried out.

[0044] The organosiloxane rubber preferably contains 0.001 to 10.0% by weight of the structural unit M, more preferably 0.001 to 5.0% by weight of the structural unit M, further preferably 0.01 to 5.0% by weight of the structural unit M, and particularly preferably 1.0 to 5.0% by weight of the structural unit M, based on 100% by weight of the organosiloxane rubber. This constitution has the advantage that polymerization of the graft portion-forming monomer mixture can be efficiently carried out in the presence of the organosiloxane rubber.

[0045] The organosiloxane rubber contained in the elastomer may be composed of only one type of polyorganosiloxane rubber having the same composition of constituent units, or may be composed of two or more types of polyorganosiloxane rubber having different compositions (types and content ratios) of constituent units.

[0046] The polymer particles (A) preferably contain 60% to 100% by weight of an organosiloxane rubber relative to 100% by weight of the elastomer contained in the polymer particles (A), more preferably 70% to 100% by weight of an organosiloxane rubber, more preferably 80% to 100% by weight of an organosiloxane rubber, further preferably 90% to 100% by weight of an organosiloxane rubber, and particularly preferably 95% to 100% by weight of an organosiloxane rubber. According to this structure, the present stress reducing agent can provide a cured product having a better linear expansion coefficient. The polymer particles (A) can contain 100% by weight of an organosiloxane rubber in the elastomer contained in the polymer particles (A), that is, the above-mentioned elastomer can be composed only of the organosiloxane rubber.

[0047] The above-mentioned elastomer may contain one or more other rubbers in addition to the above-mentioned organosiloxane rubber within the range that does not impair the effect of one embodiment of the present invention. As the above-mentioned other rubbers, for example, diene rubber, (meth) acrylate rubber and natural rubber can be cited. With respect to 100 weight % of the elastomer contained in the polymer particles (A), the total content of the above-mentioned other rubbers is less than 40 weight %, more preferably less than 30 weight %, more preferably less than 20 weight %, further preferably less than 10 weight %, and particularly preferably less than 5 weight %.

[0048] Examples of the diene rubber include butadiene rubber (also referred to as polybutadiene rubber) composed of structural units derived from 1,3-butadiene, butadiene-styrene rubber (also referred to as polystyrene-butadiene) which is a copolymer of 1,3-butadiene and styrene, and the like.

[0049] Examples of the (meth)acrylate rubber include ethyl (meth)acrylate rubber, butyl (meth)acrylate rubber, and 2-ethylhexyl (meth)acrylate rubber.

[0050] (Cross-linked structure of elastomer)

[0051] Since the dispersion stability of the polymer particles (A) in the matrix resin can be maintained, it is more preferable to introduce a cross-linked structure into the above-mentioned elastomer. By using a multifunctional alkoxysilane compound and / or a multifunctional monomer during the preparation (polymerization) of the organosiloxane rubber, a cross-linked structure can be introduced into the organosiloxane rubber. Therefore, the multifunctional alkoxysilane compound and the multifunctional monomer used in the preparation of the organosiloxane rubber can also be referred to as a cross-linking agent in the organosiloxane rubber.

[0052] Examples of the polyfunctional alkoxysilane compound include tetramethoxysilane, tetraethoxysilane (TEOS), tetraisopropoxysilane, tetrabutoxysilane, tetraoctylsilane, methyltrimethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, methyltriisopropoxysilane, vinyltrimethoxysilane, phenyltrimethoxysilane, and dimethyldimethoxysilane.

[0053] The multifunctional monomer can be said to be a monomer having two or more free radical polymerizable reaction groups in the same molecule. The above-mentioned free radical polymerizable reaction group is preferably a carbon-carbon double bond. As a multifunctional monomer, excluding butadiene, (meth)acrylates with ethylenically unsaturated double bonds such as (meth)acrylate allyl alkyl esters and (meth)acrylate allyloxyalkyl esters can be exemplified. As a monomer having two (meth)acrylate groups, for example, ethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, butanediol di(meth)acrylate, hexanediol di(meth)acrylate, cyclohexanedimethanol di(meth)acrylate and polyethylene glycol di(meth)acrylate can be cited. As the above-mentioned polyethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol (600) di(meth)acrylate, etc. can be exemplified. In addition, as a monomer having three (meth) acrylic groups, alkoxylated trimethylolpropane tri(meth)acrylates, glycerol propoxy tri(meth)acrylate, pentaerythritol tri(meth)acrylate, tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate, etc. can be exemplified. As alkoxylated trimethylolpropane tri(meth)acrylates, for example, trimethylolpropane tri(meth)acrylate, trimethylolpropane triethoxy tri(meth)acrylate, etc. can be cited. In addition, as a monomer having four (meth) acrylic groups, pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, etc. can be exemplified. In addition, as a monomer having five (meth) acrylic groups, dipentaerythritol penta(meth)acrylate, etc. can be exemplified. In addition, as a monomer having six (meth) acrylic groups, ditrimethylolpropane hexa(meth)acrylate, etc. can be exemplified. Examples of the polyfunctional monomer also include diallyl phthalate, triallyl cyanurate, triallyl isocyanurate, and divinylbenzene.

[0054] (Glass transition temperature of elastomer)

[0055] The glass transition temperature of the elastomer is preferably 80°C or less, more preferably 70°C or less, more preferably 60°C or less, more preferably 50°C or less, more preferably 40°C or less, more preferably 30°C or less, more preferably 20°C or less, more preferably 10°C or less, more preferably 0°C or less, more preferably -20°C or less, more preferably -40°C or less, more preferably -45°C or less, more preferably -50°C or less, more preferably -55°C or less, more preferably -60°C or less, more preferably -65°C or less, more preferably -70°C or less, more preferably -75°C or less, more preferably -80°C or less, more preferably -85°C or less, more preferably -90°C or less, more preferably -95°C or less, more preferably -100°C or less, more preferably -105°C or less, more preferably -110°C or less, more preferably -115°C or less, further preferably -120°C or less, particularly preferably -125°C or less. In this specification, "glass transition temperature" may be referred to as "Tg" in some cases. According to this structure, polymer particles (A) having a low Tg and a low stress agent having a low Tg can be obtained. As a result, the resin composition containing the obtained low stress agent can provide a cured product having excellent toughness. In addition, according to this structure, the viscosity of the resin composition containing the obtained low stress agent can be further reduced. The Tg of the elastomer can be obtained by measuring the viscoelasticity using a flat plate composed of polymer particles (A). Specifically, Tg can be measured as follows, that is, (1) for a flat plate composed of polymer particles (A), a dynamic viscoelasticity measurement is performed under tensile conditions using a dynamic viscoelasticity measurement device (for example, DVA-200 manufactured by IT Measurement and Control Co., Ltd.) to obtain a tanδ curve graph; (2) for the obtained tanδ curve graph, the peak temperature of tanδ is used as the glass transition temperature. Here, in the case where multiple peaks are obtained in the tanδ curve graph, the lowest peak temperature is used as the glass transition temperature of the elastomer.

[0056] On the other hand, since it is possible to reduce the decrease in the elastic modulus (rigidity) of the resulting cured product, that is, to obtain a cured product having a sufficient elastic modulus (rigidity), the Tg of the elastomer is preferably greater than 0°C, more preferably above 20°C, further preferably above 50°C, particularly preferably above 80°C, and most preferably above 120°C.

[0057] The Tg of the elastomer can be determined by the composition of the structural units contained in the elastomer, etc. In other words, the Tg of the obtained elastomer can be adjusted by changing the composition of the monomers used when producing (polymerizing) the elastomer.

[0058] Here, when a homopolymer is formed by polymerizing only one monomer, the group of monomers that provide a homopolymer having a Tg greater than 0°C is referred to as monomer group a. In addition, when a homopolymer is formed by polymerizing only one monomer, the group of monomers that provide a homopolymer having a Tg less than 0°C is referred to as monomer group b. An elastomer containing 50 to 100% by weight (more preferably 65 to 99% by weight) of constituent units derived from at least one monomer selected from monomer group a and 0 to 50% by weight (more preferably 1 to 35% by weight) of constituent units derived from at least one monomer selected from monomer group b is referred to as elastomer X. The Tg of elastomer X is greater than 0°C. In addition, when the elastomer contains elastomer X, the resin composition containing the obtained stress reducing agent can provide a cured product having sufficient rigidity.

[0059] It is also preferable to introduce a cross-linked structure into the elastomer when the Tg of the elastomer is higher than 0° C. Examples of the method for introducing the cross-linked structure include the above-mentioned methods.

[0060] The monomers that can be included in the monomer group a are not limited to the following, and examples thereof include unsubstituted vinyl aromatic compounds such as styrene and 2-vinylnaphthalene; vinyl substituted aromatic compounds such as α-methylstyrene; cycloalkylated vinyl aromatic compounds such as 3-methylstyrene, 4-methylstyrene, 2,4-dimethylstyrene, 2,5-dimethylstyrene, 3,5-dimethylstyrene, and 2,4,6-trimethylstyrene; cycloalkoxylated vinyl aromatic compounds such as 4-methoxystyrene and 4-ethoxystyrene; cyclohalogenated vinyl aromatic compounds such as 2-chlorostyrene and 3-chlorostyrene; cycloester substituted vinyl aromatic compounds such as 4-acetoxystyrene The invention also includes the following: aromatic compounds; vinyl aromatic compounds with ring hydroxylation, such as 4-hydroxystyrene; vinyl esters, such as vinyl benzoate and vinyl cyclohexanoate; vinyl halides, such as vinyl chloride; aromatic monomers, such as dihydroacenaphthene and indene; alkyl methacrylates, such as methyl methacrylate, ethyl methacrylate and isopropyl methacrylate; aromatic methacrylates, such as phenyl methacrylate; methacrylates, such as isobornyl methacrylate and trimethylsilyl methacrylate; methacrylic acid esters, such as methacrylic acid derivatives, such as methacrylonitrile; certain acrylic acid esters, such as isobornyl acrylate and tert-butyl acrylate; acrylic acid monomers, such as acrylic acid derivatives, such as acrylonitrile, etc. In addition, examples of monomers that may be included in the monomer group a include monomers that can provide a homopolymer having a Tg of 120° C. or higher when forming a homopolymer, such as acrylic acid amide, isopropyl acrylic acid amide, N-vinyl pyrrolidone, isobornyl methacrylate, dicyclopentyl methacrylate, 2-methyl-2-adamantyl methacrylate, 1-adamantyl acrylate, and 1-adamantyl methacrylate. These monomers a may be used alone or in combination of two or more.

[0061] As the above-mentioned monomer b, for example, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, octyl (meth)acrylate, dodecyl (meth)acrylate, 2-hydroxyethyl acrylate, 4-hydroxybutyl acrylate, etc. can be cited. These monomers b can be used alone or in combination of two or more. Among these monomers b, ethyl acrylate, butyl acrylate and 2-ethylhexyl acrylate are particularly preferred.

[0062] (Volume average particle size of elastomer)

[0063] The volume average particle size of the elastomer is preferably 0.03 μm to 50.00 μm, more preferably 0.05 μm to 10.00 μm, more preferably 0.08 μm to 2.00 μm, further preferably 0.10 μm to 1.00 μm, further preferably 0.10 μm to 0.80 μm, and particularly preferably 0.10 μm to 0.50 μm. When the volume average particle size of the elastomer is (a) 0.03 μm or more, an elastomer having a desired volume average particle size can be stably obtained, and when (b) is 50.00 μm or less, the heat resistance and impact resistance of the obtained cured product become good. The volume average particle size of the elastomer can be measured by using an aqueous latex containing the elastomer as a sample and a dynamic light scattering particle size distribution measuring device. The method for measuring the volume average particle size of the elastomer is described in detail in the following examples.

[0064] (Ratio of elastic body)

[0065] The proportion of the above-mentioned elastomer in the polymer particles (A) is set to 100 weight % as a whole, preferably greater than 70 weight % and less than 97 weight %, more preferably greater than 70 weight % and less than 95 weight %, and further preferably greater than 70 weight % and less than 93 weight %. When the above-mentioned proportion of the elastomer is greater than 70 weight %, the resin composition containing the obtained low stress agent can provide a cured product with excellent toughness and impact resistance. When the above-mentioned proportion of the above-mentioned elastomer is less than 97 weight %, the polymer particles (A) are not easy to condense (not easy to condense), so the resin composition containing the obtained low stress agent will not be high viscosity. As a result, the resin composition will be easy to handle. In the past, when the proportion of the above-mentioned elastomer in the polymer particles (A) was greater than 70 weight %, due to the large proportion of the elastomer, the elastic modulus of the cured product can be effectively reduced. On the other hand, due to the small proportion of the grafted portion, there is a tendency that the dispersibility of the powder in the matrix resin is easily deteriorated. However, according to one embodiment of the present invention, even when the proportion of the above-mentioned elastomer in the polymer particles (A) is greater than 70 weight %, it is possible to achieve low stress of a cured product of a resin composition having good dispersibility in a matrix resin and containing a stress reducing agent and a matrix resin.

[0066] (Gel content of elastomer)

[0067] The above-mentioned elastomer can swell in a suitable solvent, but is preferably substantially insoluble. The elastomer is preferably insoluble in the matrix resin used.

[0068] The gel content of the elastomer is preferably 60% by weight or more, more preferably 80% by weight or more, further preferably 90% by weight or more, and particularly preferably 95% by weight or more. When the gel content of the elastomer is within the above range, the resin composition containing the obtained stress reducing agent can provide a cured product with excellent toughness.

[0069] The method for calculating the gel content in this specification is as follows. First, an aqueous latex containing polymer particles (A) is obtained, and then a powder of the polymer particles (A) is obtained from the aqueous latex. There is no particular limitation on the method for obtaining the powder of the polymer particles (A) from the aqueous latex. For example, there can be cited a method of obtaining the powder of the polymer particles (A) by (i) agglomerating the polymer particles (A) in the aqueous latex, (ii) dehydrating the obtained agglomerates, and (iii) further drying the agglomerates. Next, 2.0 g of the powder of the polymer particles (A) is dissolved in 50 mL of methyl ethyl ketone (MEK). Then, the obtained MEK dissolved material is separated into components soluble in MEK (MEK soluble fraction) and components insoluble in MEK (MEK insoluble fraction). Specifically, the obtained MEK solution was centrifuged at 30,000 rpm for 1 hour using a centrifuge (manufactured by Hitachi Koki Co., Ltd., CP60E) to separate the solution into a MEK soluble fraction and a MEK insoluble fraction. Here, a total of 3 sets of centrifugal separation operations were performed. The weights of the obtained MEK soluble fraction and MEK insoluble fraction were measured, and the gel content was calculated by the following formula.

[0070] Gel content (%)=(weight of methyl ethyl ketone insoluble matter) / {(weight of methyl ethyl ketone insoluble matter)+(weight of methyl ethyl ketone soluble matter)}×100.

[0071] (Deformation example of elastic body)

[0072] In one embodiment of the present invention, the "elastomer" of the polymer microparticles (A) may be composed of only one type of elastomer having the same composition of constituent units. In this case, the "elastomer" of the polymer microparticles (A) is one type selected from organosiloxane rubbers.

[0073] In one embodiment of the present invention, the "elastomer" of the polymer microparticles (A) may be composed of a plurality of elastomers having different compositions of constituent units. In this case, the "elastomer" of the polymer microparticles (A) may be two or more selected from organosiloxane rubbers, or may be a mixture of one selected from organosiloxane rubbers and one or more selected from the above-mentioned other rubbers such as diene rubbers and (meth)acrylate rubbers.

[0074] In one embodiment of the present invention, the "elastic body" of the polymer microparticle (A) is composed of a plurality of elastomers having different compositions of constituent units. In this case, the plurality of elastomers are respectively referred to as elastomer 1, elastomer 2, ..., and elastomer n Here, n is an integer greater than or equal to 2. The "elastic body" of the polymer microparticles (A) may include elastomer 1, elastomer 2, ..., and elastomer 3, which are each polymerized separately. nThe "elastomer" of the polymer microparticle (A) may include elastomer 1, elastomer 2, ... and elastomer n An elastomer obtained by sequentially polymerizing each of the elastomers. In this way, sequentially polymerizing multiple elastomers (polymers) is also called multi-stage polymerization. An elastomer obtained by multi-stage polymerization of multiple elastomers is also called a multi-stage polymerized elastomer. The method for producing a multi-stage polymerized elastomer will be described in detail later.

[0075] For elastic body 1, elastic body 2, ... and elastic body n The multi-stage polymerized elastomer is described below. n Can be coated with elastomer n-1 At least a portion of the elastic body, or the entire elastic body may be covered n-1 In the multi-stage polymerized elastomer, there is also an elastomer n Part of the elastomer n-1 The inside situation.

[0076] In a multi-stage polymerized elastomer, a plurality of elastomers may form a layer structure. For example, in the case where the multi-stage polymerized elastomer is composed of elastomer 1, elastomer 2, and elastomer 3, elastomer 1 forms the innermost layer, a layer of elastomer 2 is formed on the outside of elastomer 1, and a layer of elastomer 3 is formed on the outside of the layer of elastomer 2 as the outermost layer of the elastomer, which is also one embodiment of the present invention. In this way, a multi-stage polymerized elastomer in which a plurality of elastomers form a layer structure may also be referred to as a multilayer elastomer. That is, in one embodiment of the present invention, the "elastomer" of the polymer microparticle (A) may include (a) a composite of a plurality of elastomers, (b) a multi-stage polymerized elastomer, and / or (c) a multilayer elastomer.

[0077] (2-1-2. Grafting section)

[0078] In this specification, the polymer graft-bonded to the above-mentioned elastomer is referred to as a graft portion. The polymer microparticles (A) contain the above-mentioned rubber-containing graft copolymer having an elastomer and a graft portion graft-bonded to the elastomer. The above-mentioned graft portion can play various roles. "Various roles" refers to, for example, (a) improving the compatibility between the matrix resin and the polymer microparticles (A), (b) improving the dispersibility of the polymer microparticles (A) in the matrix resin, and (c) enabling the polymer microparticles (A) to be dispersed in the form of primary particles in a resin composition containing the obtained stress reducing agent or a cured product.

[0079] The graft portion contains an epoxy-containing constituent unit, i.e., a constituent unit having an epoxy group as a constituent unit. When the graft portion contains a constituent unit derived from a monomer containing an epoxy group, such as glycidyl methacrylate, the stress reducing agent has the advantage of being able to provide a cured product having a better linear expansion coefficient. In the preparation of the graft portion, a graft portion containing an epoxy-containing constituent unit can be obtained by using (polymerizing) a mixture containing a monomer having an epoxy group (a monomer mixture for forming the graft portion).

[0080] Specific examples of monomers having epoxy groups include vinyl monomers containing glycidyl groups such as (meth) acrylate glycidyl, (meth) acrylate 4-hydroxybutyl glycidyl ether, and allyl glycidyl ether. These can be used alone or in combination of two or more. Glycidyl methacrylate is more preferred as the monomer having epoxy groups because it is easily available and economical.

[0081] The grafted portion preferably contains 0.5 to 4.0% by weight of epoxy-containing constituent units, more preferably 0.6 to 3.8% by weight of epoxy-containing constituent units, more preferably 0.7 to 3.5% by weight of epoxy-containing constituent units, more preferably 0.8 to 3.3% by weight of epoxy-containing constituent units, more preferably 0.8 to 3.2% by weight of epoxy-containing constituent units, further preferably 0.9 to 3.0% by weight of epoxy-containing constituent units, and particularly preferably 1.0 to 3.0% by weight of epoxy-containing constituent units. The grafted portion contains 0.5% by weight or more of epoxy-containing constituent units, relative to 100% by weight of the rubber-containing grafted copolymer, thereby having the following advantages: the linear expansion coefficient of the cured product of the resin composition obtained by adding the stress reducing agent to the base resin is significantly reduced, that is, a cured product with a better linear expansion coefficient of the stress reducing agent can be provided. When the epoxy group-containing structural unit in the graft portion is 4.0 wt % or less based on 100 wt % of the rubber-containing graft copolymer, the stressing agent has an advantage of being excellent in dispersibility in the matrix resin.

[0082] In addition, for the above-mentioned graft part, as a constituent unit, it is preferred to contain 3.3% to 26.7% by weight of epoxy-containing constituent units relative to 100% by weight of all constituent units of the graft part in the rubber-containing graft copolymer, more preferably 4.0% to 25.0% by weight of epoxy-containing constituent units, further preferably 5.0% to 22.0% by weight of epoxy-containing constituent units, and particularly preferably 6.0% to 20.0% by weight of epoxy-containing constituent units. By containing 3.3% or more of epoxy-containing constituent units relative to 100% by weight of all constituent units of the graft part, the above-mentioned graft part has the following advantages: the linear expansion coefficient of the cured product of the resin composition obtained by adding the low stress agent to the base resin is significantly reduced, that is, the low stress agent can provide a cured product with a better linear expansion coefficient. In addition, if the epoxy-containing constituent units in the above-mentioned graft part are 26.7% or less by weight relative to 100% by weight of all constituent units of the graft part, the stress agent has the advantage of excellent dispersibility in the base resin.

[0083] Among them, it is more preferred that the graft portion contains epoxy-containing constituent units within the above range based on 100 wt % of the rubber-containing graft copolymer and contains epoxy-containing constituent units within the above range based on 100 wt % of all constituent units of the graft portion in the rubber-containing graft copolymer.

[0084] The graft portion may contain, as constituent units not containing an epoxy group, constituent units derived from one or more monomers selected from aromatic vinyl monomers not containing an epoxy group, vinyl cyan monomers not containing an epoxy group, and (meth)acrylate monomers not containing an epoxy group.

[0085] One or more monomers selected from the group consisting of the aromatic vinyl monomers, vinyl cyan monomers and (meth)acrylate monomers may be used alone or in combination of two or more.

[0086] In the grafted portion, the total content of the constituent units derived from the aromatic vinyl monomer not containing an epoxy group, the constituent units derived from the vinyl cyanide monomer not containing an epoxy group, and the constituent units derived from the (meth)acrylate monomer not containing an epoxy group is preferably 10 to 97% by weight, more preferably 30 to 96% by weight, further preferably 50 to 95% by weight, particularly preferably 60 to 94% by weight, and most preferably 70 to 94% by weight in 100% by weight of all the constituent units in the grafted portion.

[0087] The grafted portion may contain, as a constituent unit, a constituent unit derived from a monomer having a reactive group other than an epoxy group. Examples of monomers having a reactive group other than an epoxy group include monomers having an oxetane group, a hydroxyl group, an amino group, an imide group, a carboxylic acid group, a carboxylic anhydride group, a cyclic ester group, a cyclic amide group, a benzoic acid group, and the like. Monomers containing oxazine and cyanate groups.

[0088] The grafted portion may contain a constituent unit derived from a multifunctional monomer as a constituent unit. When the grafted portion contains a constituent unit derived from a multifunctional monomer, the following advantages are achieved: (a) the polymer particles (A) can be prevented from swelling in the resin composition containing the obtained stress reducing agent, (b) the viscosity of the resin composition containing the obtained stress reducing agent is reduced, so there is a tendency that the handling property of the resin composition becomes better, and (c) the dispersibility of the polymer particles (A) in the above-mentioned resin composition in the matrix resin is improved.

[0089] When the graft portion does not contain a structural unit derived from a polyfunctional monomer, the resin composition containing the obtained stress reducing agent can provide a cured product having better toughness and impact resistance than when the graft portion contains a structural unit derived from a polyfunctional monomer.

[0090] Specific examples of the multifunctional monomer are the same as those described in the above section (crosslinked structure of elastomer), and thus the description is cited and the description is omitted here.

[0091] The graft portion may contain, as a constituent unit, constituent units derived from other monomers in addition to the constituent units derived from the above-mentioned monomers.

[0092] (Glass transition temperature of grafted portion)

[0093] The glass transition temperature of the grafted portion is preferably 190°C or less, more preferably 160°C or less, more preferably 140°C or less, more preferably 120°C or less, preferably 80°C or less, more preferably 70°C or less, more preferably 60°C or less, more preferably 50°C or less, more preferably 40°C or less, more preferably 30°C or less, more preferably 20°C or less, more preferably 10°C or less, more preferably 0°C or less, more preferably -20°C or less, more preferably -40°C or less, more preferably -45°C or less, more preferably -50°C or less, more preferably -55°C or less, more preferably -60°C or less, more preferably -65°C or less, more preferably -70°C or less, more preferably -75°C or less, more preferably -80°C or less, more preferably -85°C or less, more preferably -90°C or less, more preferably -95°C or less, more preferably -100°C or less, more preferably -105°C or less, more preferably -110°C or less, more preferably -115°C or less, further preferably -120°C or less, particularly preferably -125°C or less.

[0094] The glass transition temperature of the grafted portion is preferably 0°C or higher, more preferably 30°C or higher, more preferably 50°C or higher, more preferably 70°C or higher, further preferably 90°C or higher, and particularly preferably 110°C or lower.

[0095] The Tg of the grafted portion can be determined by the composition of the structural units contained in the grafted portion, etc. In other words, the Tg of the obtained grafted portion can be adjusted by changing the composition of the monomers used when producing (polymerizing) the grafted portion.

[0096] The Tg of the grafted portion was measured in the same manner as the Tg of the elastomer, and a tan δ graph was obtained. When a plurality of peaks were obtained in the obtained tan δ graph, the highest peak temperature was taken as the glass transition temperature of the grafted portion.

[0097] (Grafting rate of grafted part)

[0098] In one embodiment of the present invention, the polymer microparticles (A) are polymers having the same structure as the grafted portion, and may have polymers that are not graft-bonded to the elastomer. In this specification, polymers having the same structure as the grafted portion and being graft-bonded to the elastomer are also referred to as non-grafted polymers. The above-mentioned non-grafted polymers may also be referred to as polymers that are not graft-bonded to the elastomer in the polymers produced by polymerization of the grafted portion.

[0099] In this specification, the ratio of the polymer grafted to the elastomer in the polymer produced in the preparation step of the grafted portion, i.e., the grafted portion, is referred to as the grafting ratio. The grafting ratio can also be said to be a value represented by (weight of the grafted portion) / {(weight of the grafted portion)+(weight of the non-grafted polymer)}×100.

[0100] In the preparation step of the grafted part, in addition to the grafted part and the non-grafted polymer, a soluble component may exist. The soluble component refers to unpolymerized monomers and secondary raw materials such as an initiator.

[0101] As a method for determining whether it is a graft copolymer (A), a non-grafted polymer, or a soluble component, for example, a method of determining by soluble / insoluble in a solvent can be cited. For example, the following method can be cited: (i) when it is insoluble in MEK, it is determined to be a graft copolymer (A); (ii) when it is soluble in MEK and insoluble in methanol, it is determined to be a non-grafted polymer; (iii) when it is soluble in MEK and soluble in methanol, it is determined to be a soluble component.

[0102] The grafting rate of the grafted portion is preferably 70% or more, more preferably 80% or more, and further preferably 90% or more. When the grafting rate is 70% or more, there is an advantage that the viscosity of the resin composition containing the obtained stress reducing agent does not become too high.

[0103] As described above, the polymer microparticles (A) and the non-grafted polymer can be separated using a solvent, and in this specification, the non-grafted polymer also constitutes a part of the polymer microparticles (A) of one embodiment of the present invention. For example, in one embodiment of the present invention, when the weight of the polymer microparticles (A) is mentioned, the "weight of the polymer microparticles (A)" refers to the total weight of the polymer microparticles (A) that are MEK-insoluble and the non-grafted polymer that is MEK-soluble and methanol-insoluble.

[0104] The weight of the polymer in the grafted portion is the feed amount of the monomer constituting the polymer in the grafted portion. In addition, in the calculation of the grafting rate, the method for coagulating the polymer microparticles (A) is not particularly limited, and a method using a solvent, a method using a coagulant, a method of spraying an aqueous latex, etc. can be used.

[0105] (Modification of the graft portion)

[0106] In one embodiment of the present invention, the graft portion may be composed of only one type of graft portion having constituent units of the same composition. In one embodiment of the present invention, the graft portion may be composed of a plurality of types of graft portions having constituent units of different compositions.

[0107] In one embodiment of the present invention, a case where the graft portion is composed of a plurality of graft portions will be described. In this case, the plurality of graft portions are respectively designated as graft portion 1, graft portion 2, ..., and graft portion n (n is an integer greater than or equal to 2). The graft portion may include a graft portion 1, a graft portion 2, ..., and a graft portion 3, which are each polymerized separately. nThe grafted portion may include a grafted portion 1, a grafted portion 2, ... and a grafted portion n A polymer obtained by multi-stage polymerization. A polymer obtained by multi-stage polymerization of a plurality of grafted parts is also referred to as a multi-stage polymerized grafted part. The method for producing the multi-stage polymerized grafted part will be described in detail later.

[0108] In the case where the grafted portion is composed of multiple grafted portions, not all of these multiple grafted portions may be graft-bonded to the elastomer. As long as at least a portion of at least one grafted portion is graft-bonded to the elastomer, other types (other multiple types) of grafted portions may be graft-bonded to the grafted portion graft-bonded to the elastomer. In addition, in the case where the grafted portion is composed of multiple grafted portions, it is a polymer having the same structure as the multiple grafted portions, and may have multiple polymers (multiple non-grafted polymers) that are not graft-bonded to the elastomer.

[0109] The grafted part 1, the grafted part 2, ... and the grafted part n The multi-stage polymer grafting section is described below. n Can be covered with grafted part n-1 At least a portion of the graft portion may be covered, or the entire graft portion may be covered n-1 In the multi-stage polymer grafting section, there is also a grafting section n Part of the grafting n-1 The inside situation.

[0110] In a multi-stage polymer grafted portion, a plurality of grafted portions may form a layer structure respectively. For example, in a case where a multi-stage polymer grafted portion is composed of a grafted portion 1, a grafted portion 2, and a grafted portion 3, the grafted portion 1 forms the innermost layer of the grafted portion, a layer of the grafted portion 2 is formed on the outside of the grafted portion 1, and a layer of the grafted portion 3 is formed on the outside of the layer of the grafted portion 2 as the outermost layer, which is also one embodiment of the present invention. In this way, a multi-stage polymer grafted portion in which a plurality of grafted portions form a layer structure respectively can also be said to be a multi-layer grafted portion. That is, in one embodiment of the present invention, the grafted portion may include (a) a mixture of a plurality of grafted portions, (b) a multi-stage polymer grafted portion, and / or (c) a multi-layer grafted portion.

[0111] When the elastomer and the grafted portion are polymerized sequentially in the production of the polymer microparticles (A), at least a portion of the grafted portion may be covered with at least a portion of the elastomer in the obtained polymer microparticles (A). Sequential polymerization of the elastomer and the grafted portion can also be said to be multi-stage polymerization of the elastomer and the grafted portion. The polymer microparticles (A) obtained by multi-stage polymerization of the elastomer and the grafted portion can also be called multi-stage polymers.

[0112] When the polymer microparticles (A) are multistage polymers, the grafted portion may cover at least a portion of the elastomer or the entire elastomer. When the polymer microparticles (A) are multistage polymers, a portion of the grafted portion may enter the inside of the elastomer.

[0113] When the polymer particles (A) are multi-stage polymers, the elastomer and the grafted portion may form a layer structure. For example, a method in which the elastomer forms the innermost layer (also referred to as the core layer) and the layer of the grafted portion is formed on the outside of the elastomer as the outermost layer (also referred to as the shell layer) is also one method of the present invention. The structure in which the elastomer is the core layer and the grafted portion is the shell layer may also be referred to as a core-shell structure. In this way, the polymer particles (A) in which the elastomer and the grafted portion form a layer structure (core-shell structure) may also be referred to as a multilayer polymer or a core-shell polymer. That is, in one embodiment of the present invention, the polymer particles (A) may be a multi-stage polymer and / or a multilayer polymer or a core-shell polymer. However, as long as the grafted portion is graft-bonded to the elastomer, the polymer particles (A) are not necessarily limited to the above-mentioned structure.

[0114] It is preferred that at least a part of the grafted portion covers at least a part of the elastomer. In other words, it is preferred that at least a part of the grafted portion is present on the outermost side of the polymer fine particle (A).

[0115] (2-1-3. Surface cross-linked polymer)

[0116] In addition to the elastomer and the grafted portion graft-bonded to the elastomer, the rubber-containing graft copolymer may further have a surface cross-linked polymer. When the rubber-containing graft copolymer further has a surface cross-linked polymer, it has the following advantages: (a) the anti-blocking property can be improved in the production of the polymer particles (A), and (b) the dispersibility of the polymer particles (A) in the matrix resin in the resin composition containing the obtained low stress agent becomes better. When the rubber-containing graft copolymer further has a surface cross-linked polymer, it may further have the following effects: (a) the effect of reducing the viscosity of the resin composition containing the obtained low stress agent, (b) the effect of increasing the cross-linking density of the elastomer, and (c) the effect of increasing the grafting efficiency of the grafted portion. The cross-linking density of the elastomer refers to the degree of the number of cross-linked structures of the elastomer as a whole.

[0117] The surface crosslinked polymer is composed of a polymer containing, as constituent units, 30 to 100% by weight of constituent units derived from a polyfunctional monomer and 0 to 70% by weight of constituent units derived from other vinyl monomers, totaling 100% by weight.

[0118] Specific examples of the multifunctional monomer are the same as those described in the above section (crosslinked structure of elastomer), and thus the description is cited and the description is omitted here.

[0119] (2-1-4. Physical properties of polymer microparticles (A))

[0120] The physical properties of the polymer fine particles (A) are described below.

[0121] (Volume Average Particle Size (Mv) of Polymer Microparticles (A))

[0122] Since a resin composition having a desired viscosity and being highly stable can be obtained, the volume average particle size (Mv) of the polymer microparticles (A) is preferably 0.03 μm to 50.00 μm, more preferably 0.05 μm to 10.00 μm, more preferably 0.08 μm to 2.00 μm, further preferably 0.10 μm to 1.00 μm, further preferably 0.10 μm to 0.80 μm, and particularly preferably 0.10 μm to 0.50 μm. When the volume average particle size (Mv) of the polymer microparticles (A) is within the above range, there is also an advantage that the dispersibility of the polymer microparticles (A) in the matrix resin is good. It should be noted that in this specification, "the volume average particle size (Mv) of the polymer microparticles (A)" refers to the volume average particle size of the primary particles of the polymer microparticles (A) unless otherwise specified. The volume average particle size of the polymer particles (A) can be measured by using an aqueous latex containing the polymer particles (A) as a sample and using a dynamic light scattering particle size distribution measuring device. The volume average particle size of the polymer particles (A) is described in detail in the following examples. The volume average particle size of the polymer particles (A) can also be measured by cutting a cured product of the resin composition, photographing the cut surface using an electron microscope, etc., and using the obtained photographed data (photographed image).

[0123] In order to obtain a resin composition having a low viscosity and being easy to handle, the number distribution of the volume average particle size of the polymer fine particles (A) in the matrix resin preferably has a half value width of 0.5 to 1 times the volume average particle size.

[0124] (2-1-5. Method for producing polymer microparticles (A))

[0125] The polymer fine particles (A) can be produced by polymerizing an elastomer and then graft-polymerizing a polymer constituting a graft portion onto the elastomer in the presence of the elastomer.

[0126] The polymer particles (A) can be manufactured by known methods, such as emulsion polymerization, suspension polymerization, microsuspension polymerization and the like. Specifically, the polymerization of the elastomer in the polymer particles (A), the polymerization of the grafted portion (graft polymerization) and the polymerization of the surface cross-linked polymer can be implemented by known methods, such as emulsion polymerization, suspension polymerization, microsuspension polymerization and the like. Among them, as a method for manufacturing polymer particles (A), emulsion polymerization is particularly preferred. According to the emulsion polymerization method, there are the following advantages: (a) the composition design of the polymer particles (A) is easy, (b) the industrial production of the polymer particles (A) is easy, and (c) it is easy to obtain an aqueous latex of the polymer particles (A) that can be preferably used in the manufacture of the present resin composition described later. Below, the method for manufacturing the elastomer, grafted portion and any surface cross-linked polymer that can be contained in the polymer particles (A) is described.

[0127] (Method for producing elastomer)

[0128] The method for preparing the organosiloxane rubber is not particularly limited, and a known emulsion polymerization method may be used. Specifically, the method for preparing the organosiloxane rubber includes emulsion polymerization of an organosiloxane and the above-mentioned monomer M in the presence of an acidic emulsifier.

[0129] Since the organosiloxane rubber is readily available and can be easily prepared, the organosiloxane used as a raw material for preparing the organosiloxane rubber is preferably various organosiloxane cyclic bodies having three or more membered rings, such as hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, dodecamethylcyclohexasiloxane, trimethyltriphenylcyclotrisiloxane, tetradecamethylcycloheptasiloxane, and dimethylcyclosiloxane (a mixture of 3 to 7 dimethylsiloxane cyclic oligomers).

[0130] The acidic emulsifier is not particularly limited. When an organosiloxane cyclic body is used, an acidic emulsifier that can open the ring of the organosiloxane cyclic body is preferred. As an acidic emulsifier, for example, dodecylbenzenesulfonic acid can be appropriately cited. The amount of the acidic emulsifier used is not particularly limited, as long as it is appropriately set according to (a) the desired volume average particle size of the organosiloxane rubber and the polymer particles (A), (b) the solid content (monomer mixture) concentration in the reaction solution, (c) the polymerization conditions such as the polymerization temperature, and (d) the use of additives such as surfactants and the amount of use.

[0131] The volume average particle size of the obtained organosiloxane rubber can be controlled by (a) the degree of preliminary dispersion of the raw materials, (b) the amount of the emulsifier used, (c) the polymerization temperature, and (d) the method of supplying the raw materials.

[0132] When the organosiloxane rubber is obtained by emulsion polymerization in the presence of an acidic emulsifier, the obtained aqueous latex is strongly acidic, so it is preferably neutralized after the polymerization reaction. There are no particular restrictions on the alkaline compound used for neutralization, and examples thereof include sodium hydroxide, potassium hydroxide, ammonia, triethylamine, etc. The aqueous latex can be neutralized by adding these alkaline compounds directly or in the form of an aqueous solution to the aqueous latex containing the organosiloxane rubber.

[0133] As a method for preparing the organosiloxane rubber, for example, the method described in WO2006 / 070664 can also be used.

[0134] When the above-mentioned elastomer contains at least one selected from diene rubber and (meth)acrylate rubber, these elastomers can be produced, for example, by emulsion polymerization, suspension polymerization, microsuspension polymerization and the like. As a production method thereof, for example, the method described in WO2005 / 028546 can be used.

[0135] (Method for producing grafted portion)

[0136] The grafted portion can be formed, for example, by polymerizing the monomers used in the formation of the grafted portion using known free radical polymerization. When a polymer particle precursor containing (a) an elastomer or (b) an elastomer and a surface cross-linked polymer is obtained in the form of an aqueous latex, the grafted portion is preferably polymerized by emulsion polymerization. The grafted portion can be manufactured, for example, by the method described in WO2005 / 028546.

[0137] When the grafted portion is composed of multiple grafted portions, the grafted portions having multiple grafted portions can be polymerized and then grafted onto an elastomer to produce polymer microparticles (A). Alternatively, multiple polymers constituting the grafted portion can be grafted onto an elastomer in sequence in the presence of an elastomer to produce polymer microparticles (A).

[0138] When an emulsion polymerization method is adopted as a method for preparing the diene rubber and the (meth)acrylate rubber and / or a method for preparing the graft portion, a known emulsifier (dispersant) can be used.

[0139] As emulsifiers, for example, anionic emulsifiers, nonionic emulsifiers, polyvinyl alcohol, alkyl-substituted cellulose, polyvinyl pyrrolidone, polyacrylic acid derivatives, etc. can be cited. As anionic emulsifiers, for example, sulfur emulsifiers, phosphorus emulsifiers, sarcosine emulsifiers, carboxylic acid emulsifiers, etc. can be cited. As sulfur emulsifiers, for example, sodium dodecylbenzene sulfonate (abbreviation: SDBS) can be cited. As phosphorus emulsifiers, for example, sodium polyoxyethylene lauryl ether phosphate can be cited.

[0140] When an emulsion polymerization method is used as a method for preparing diene rubber and (meth)acrylate rubber and / or a method for preparing a grafted portion, a thermal decomposition type initiator can be used. As the above-mentioned thermal decomposition type initiator, for example, known initiators such as (a) 2,2'-azobisisobutyronitrile and (b) peroxides such as organic peroxides and inorganic peroxides can be mentioned. As the above-mentioned organic peroxide, tert-butyl peroxyisopropyl carbonate, p-menthane hydroperoxide, cumene hydroperoxide, diisopropylbenzene peroxide, tert-butyl hydroperoxide, di-tert-butyl peroxide and di-tert-hexyl peroxide can be mentioned. As the above-mentioned inorganic peroxide, hydrogen peroxide, potassium persulfate, ammonium persulfate, etc. can be mentioned.

[0141] When an emulsion polymerization method is used as a method for preparing diene rubber and (meth)acrylate rubber and / or a method for preparing a grafted portion, a redox initiator may also be used. The redox initiator is an initiator that uses (a) a peroxide such as an organic peroxide or an inorganic peroxide and (b) a reducing agent such as a transition metal salt such as iron (II) sulfate, sodium formaldehyde sulfoxylate, or glucose. A chelating agent such as disodium ethylenediaminetetraacetate and a phosphorus-containing compound such as sodium pyrophosphate may also be used in combination as required.

[0142] When a redox initiator is used, polymerization can be carried out even at a relatively low temperature at which the above-mentioned peroxide does not substantially thermally decompose, and the polymerization temperature can be set within a wide range. Therefore, it is preferred to use a redox initiator. Among the redox initiators, it is also preferred to use organic peroxides such as cumene hydroperoxide, diisopropylbenzene peroxide, p-menthane hydroperoxide and tert-butyl hydroperoxide as a redox initiator of peroxide. The amount of the above-mentioned initiator used, and the amount of the above-mentioned reducing agent, transition metal salt and chelating agent used when a redox initiator is used can be used within a known range.

[0143] When a multifunctional monomer is used in the preparation of an elastomer and / or a grafted portion, a known chain transfer agent can be used within a known usage amount. By using a chain transfer agent, the molecular weight and / or the degree of crosslinking of the resulting elastomer, grafted portion or surface crosslinked polymer can be easily adjusted.

[0144] In the production of polymer microparticles (A), a surfactant may be used in addition to the above-mentioned components. The type and amount of the surfactant used are within known ranges.

[0145] In the production of the polymer microparticles (A), conditions within known numerical ranges can be appropriately applied as to the polymerization temperature, pressure, deoxygenation and other conditions during polymerization.

[0146] (2-2. Resin (B))

[0147] The present stress reducing agent may further contain a resin (B) in addition to the polymer fine particles (A). The present stress reducing agent containing the resin (B) has the advantage that the polymer fine particles (A) have better dispersibility in the matrix resin.

[0148] The resin (B) may be, for example, a thermosetting resin, a thermoplastic resin, or any combination of a thermosetting resin and a thermoplastic resin.

[0149] (2-2-1. Thermosetting resin)

[0150] The thermosetting resin in the resin (B) is not particularly limited, but preferably contains at least one selected from a resin containing a polymer formed by polymerizing an ethylenically unsaturated monomer, an epoxy resin, a phenolic resin, a polyol resin, and an amino-formaldehyde resin. The thermosetting resin in the resin (B) may also be a resin containing a polymer formed by polymerizing an aromatic polyester raw material. In the resin (B), only one thermosetting resin may be used, or two or more thermosetting resins may be used in combination.

[0151] (Epoxy resin)

[0152] The epoxy resin is not particularly limited as long as it has at least one epoxy group in the molecule.

[0153] Specific examples of epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol AD ​​type epoxy resins, bisphenol S type epoxy resins, glycidyl ester type epoxy resins, glycidyl amine type epoxy resins, novolac type epoxy resins, glycidyl ether type epoxy resins of bisphenol A propylene oxide adducts, hydrogenated bisphenol A (or F) type epoxy resins, fluorinated epoxy resins, rubber-modified epoxy resins containing polybutadiene or NBR, flame-retardant epoxy resins such as glycidyl ether of tetrabromobisphenol A, p-hydroxybenzoic acid glycidyl ether ester type epoxy resins, meta-aminophenol type epoxy resins, diaminodiphenylmethane type epoxy resins, polyurethane-modified epoxy resins having urethane bonds, various alicyclic epoxy resins, glycidyl ethers of polyols, hydantoin type epoxy resins, epoxides of unsaturated polymers such as petroleum resins, and amino group-containing glycidyl ether resins. As the above-mentioned polyol, for example, N,N-diglycidyl aniline, N,N-diglycidyl o-toluidine, triglycidyl isocyanurate, polyalkylene glycol diglycidyl ether and glycerol can be cited. As the epoxy resin, for example, epoxy compounds obtained by addition reaction of bisphenol A (or F) or polyacids with the above-mentioned epoxy resin can also be cited. The epoxy resin is not limited to this, and generally used epoxy resins can be used. These epoxy resins can be used alone or in combination of two or more.

[0154] Among the above epoxy resins, epoxy resins having at least two epoxy groups in one molecule are preferred because they have high reactivity during the curing of the resin composition and the obtained cured product easily forms a three-dimensional mesh. In addition, as the epoxy resin, epoxy resins having at least two epoxy groups in one molecule are preferred because they are economical and easy to obtain.

[0155] (2-2-2. Thermoplastic resin)

[0156] Examples of the thermoplastic resin in the resin (B) include acrylic polymers, vinyl copolymers, polycarbonates, polyamides, polyesters, polyphenylene ethers, polyurethanes, and polyvinyl acetates, etc. These may be used alone or in combination of two or more.

[0157] The resin (B) may be the same resin as the matrix resin to be mixed later (a resin having the same composition), or may be a resin different from the matrix resin. In the resin composition, it is preferred that the matrix resin and the resin (B) are not phase-separated. The resin (B) is preferably a resin compatible with the matrix resin.

[0158] When the resin (B) is the same resin as the matrix resin to be mixed described below, there is an advantage that the resin (B) has no influence on various physical properties of the obtained resin composition containing the stress reducing agent or the cured product.

[0159] As an example, consider the case where resin (B) is a resin of the same type as the matrix resin. In this case, the matrix resin and the resin (B) cannot be distinguished in the resin composition containing the obtained low stress agent. Therefore, from the appearance, the resin composition containing the obtained low stress agent has only resin (B) or only matrix resin in addition to the polymer particles (A). Next, consider the case where resin (B) is a resin of a different type from the matrix resin. In this case, the matrix resin and the resin (B) can be identified in the resin composition containing the obtained low stress agent. In this case, the resin composition finally containing the obtained low stress agent may also contain resin (B) as a resin other than the matrix resin in addition to the polymer particles (A).

[0160] (2-2-3. Others)

[0161] In this specification, resin (B) also contains fats and fatty acid esters. As fats that can be used as resin (B), for example, epoxidized fats such as epoxidized soybean oil and epoxidized linseed oil can be cited. As epoxidized soybean oil, commercial products can also be used, for example, ADK CIZER O-130P manufactured by ADEKA can be cited. As fatty acid esters that can be suitable for use as resin (B), for example, epoxidized fatty acid butyl ester, epoxidized fatty acid 2-ethylhexyl ester, epoxidized fatty acid octyl ester, epoxidized fatty acid alkyl ester and the like can be cited.

[0162] Epoxidized fats and oils and epoxidized fatty acid esters are sometimes referred to as epoxy plasticizers. That is, in this specification, resin (B) also contains epoxy plasticizers separately. Examples of epoxy plasticizers other than epoxidized fats and oils and epoxidized fatty acid esters include diepoxystearyl epoxyhexahydrophthalate and di-2-ethylhexyl epoxyhexahydrophthalate.

[0163] The above-mentioned thermosetting resin, thermoplastic resin, mixture of thermosetting resin and thermoplastic resin, oil and fat and fatty acid ester can be mixed with antioxidant respectively. In this specification, antioxidant is regarded as a part of resin (B) as long as it is mixed with the above-mentioned other substances. When only antioxidant is used, antioxidant is not regarded as resin (B). The case of using only antioxidant to replace resin (B) is described. Since antioxidant is a component that does not help crosslinking, when the obtained low stress agent is mixed with the matrix resin, there is a tendency that the physical properties of the finally obtained substance (i.e., the final product. For example, when the matrix resin is a thermosetting resin, it is a cured product) deteriorate. For example, it is believed that the Tg of the final product is reduced and the impact resistance is deteriorated.

[0164] The antioxidant is not particularly limited and includes, for example, (a) primary antioxidants such as phenolic antioxidants, amine antioxidants, lactone antioxidants, and hydroxylamine antioxidants, and (b) secondary antioxidants such as sulfur antioxidants and phosphorus antioxidants.

[0165] As the above-mentioned antioxidant, other substances known in the past can also be used. As the antioxidant, for example, various substances recorded in the "Antioxidant Handbook" (first edition issued on October 25, 1975) issued by Dacheng Co., Ltd., the "Polymer Additive Handbook" (written by Haruna Tetsu, the first edition issued on November 7, 2010) issued by CMC Publishing, etc. can be used.

[0166] The resin (B) is preferably selected from thermosetting resins, mixtures of thermosetting resins and antioxidants, thermoplastic resins, mixtures of thermoplastic resins and antioxidants, oils, mixtures of oils and antioxidants, fatty acid esters, mixtures of fatty acid esters and antioxidants, epoxy curing agents, and mixtures of epoxy curing agents and antioxidants. It is more preferably selected from epoxy resins, acrylic polymers, mixtures of epoxy resins and antioxidants, mixtures of acrylic polymers and antioxidants, and mixtures of epoxy plasticizers and antioxidants. It is further preferably selected from mixtures of epoxy resins and antioxidants, mixtures of acrylic polymers and antioxidants, and mixtures of epoxy plasticizers and antioxidants. It is particularly preferably a mixture of epoxy plasticizers and antioxidants. According to this configuration, there are the following advantages: (a) the resin composition containing the obtained stress reducing agent can provide a cured product with excellent heat resistance, and (b) the dispersibility of the polymer particles (A) in the matrix resin can be improved.

[0167] (2-2-4. Physical properties of resin (B))

[0168] The resin (B) is not particularly limited in other properties as long as it is a liquid, semisolid, or solid having a viscosity of 100 mPa·s to 1,000,000 mPa·s at 25° C. It should be noted that in this specification, "the resin (B) has a viscosity of 100 mPa·s to 1,000,000 mPa·s at 25° C." means "the resin (B) at 25° C. has a viscosity of 100 mPa·s to 1,000,000 mPa·s."

[0169] When the resin (B) is liquid, the viscosity of the resin (B) is preferably 750,000 mPa·s or less at 25° C. According to the above configuration, there is an advantage that the stress reducing agent has excellent fluidity.

[0170] In addition, the viscosity of the resin (B) is more preferably 200 mPa·s or more, and more preferably 300 mPa·s or more at 25°C. According to this configuration, the resin (B) does not impregnate into the polymer microparticles (A), but enters between the particles of the plurality of polymer microparticles (A) and can be retained near the surface of the polymer microparticles (A). As a result, the resin (B) can prevent the polymer microparticles (A) from fusing with each other.

[0171] The viscosity of resin (B) at 25°C is more preferably 100 mPa·s to 750,000 mPa·s, more preferably 100 mPa·s to 700,000 mPa·s, more preferably 100 mPa·s to 350,000 mPa·s, more preferably 100 mPa·s to 300,000 mPa·s, more preferably 100 mPa·s to 50,000 mPa·s, further preferably 100 mPa·s to 30,000 mPa·s, and particularly preferably 100 mPa·s to 15,000 mPa·s.

[0172] When the resin (B) is semi-solid at 25°C, it can be said that the resin (B) is semi-liquid at 25°C, and it can be said that the resin (B) has a viscosity greater than 1,000,000 mPa·s at 25°C. When the resin (B) is semi-solid or solid at 25°C, the resin composition containing the obtained stress reducing agent has the advantage of less blocking and easy handling.

[0173] The content of the resin (B) in the stress reducing agent is 50 to 99% by weight, and the content of the resin (B) in the stress reducing agent is 100% by weight. The content of the resin (B) can be appropriately set within the above numerical range and within the range in which the stress reducing agent can be obtained, depending on the type of the resin (B) and the physical properties of the resin (B) (solid, solid, liquid or viscosity, etc.). When the resin (B) is liquid at 25°C and the content of the resin (B) in the stress reducing agent is large, the stress reducing agent may not be obtained. When the resin (B) is liquid at 25°C and the content of the resin (B) in the stress reducing agent is large, there is a concern that the fluidity (smoothness) of the stress reducing agent may deteriorate.

[0174] From the perspective of excellent anti-blocking properties, the content of the resin (B) in the stress reducing agent is described. When the total of the polymer microparticles (A) and the resin (B) is 100 wt%, it is more preferred that the polymer microparticles (A) are 55 to 99 wt% and the resin (B) is 1 to 45 wt%, more preferably the polymer microparticles (A) are 60 to 99 wt% and the resin (B) is 1 to 40 wt%, more preferably the polymer microparticles (A) are 65 to 99 wt% and the resin (B) is 1 to 35 wt%, more preferably the polymer microparticles (A) are 70 to 99 wt% and the resin (B) is 1 to 30 wt%, and more preferably the polymer microparticles (A) are 100 wt%. The polymer particles (A) are 75 to 99% by weight and the resin (B) is 1 to 25% by weight, more preferably the polymer particles (A) are 80 to 99% by weight and the resin (B) is 1 to 20% by weight, further preferably the polymer particles (A) are 85 to 99% by weight and the resin (B) is 1 to 15% by weight, further preferably the polymer particles (A) are 90 to 99% by weight and the resin (B) is 1 to 10% by weight, and particularly preferably the polymer particles (A) are 95 to 99% by weight and the resin (B) is 1 to 5% by weight.

[0175] From the perspective of good dispersibility of polymer particles (A) in the matrix resin, the content of resin (B) in the stress reducing agent is described. When the total of polymer particles (A) and resin (B) is set to 100% by weight, preferably the polymer particles (A) are 50 to 97% by weight and the resin (B) is 3 to 50% by weight, more preferably the polymer particles (A) are 50 to 95% by weight and the resin (B) is 5 to 50% by weight, more preferably the polymer particles (A) are 50 to 92% by weight and the resin (B) is 8 to 50% by weight, more preferably the polymer particles (A) are 50 to 90% by weight and the resin (B) is 10 to 50% by weight, and more preferably the polymer particles ( The amount of polymer microparticles (A) is 50 to 87 wt % and the amount of resin (B) is 13 to 50 wt %, more preferably the amount of polymer microparticles (A) is 50 to 85 wt % and the amount of resin (B) is 15 to 50 wt %, further preferably the amount of polymer microparticles (A) is 50 to 82 wt % and the amount of resin (B) is 18 to 50 wt %, further preferably the amount of polymer microparticles (A) is 50 to 80 wt % and the amount of resin (B) is 20 to 50 wt %, and particularly preferably the amount of polymer microparticles (A) is 60 to 80 wt % and the amount of resin (B) is 20 to 40 wt %.

[0176] (2-3. Anti-adhesion agent)

[0177] The stress reducing agent preferably further contains an anti-blocking agent. According to this configuration, the obtained stress reducing agent has (a) excellent anti-blocking property and (b) excellent dispersibility of the polymer fine particles (A) in the matrix resin.

[0178] As long as the anti-adhesive agent plays the effect of one embodiment of the present invention, there is no particular restriction. As the anti-adhesive agent, for example, anti-adhesive agents composed of inorganic particles such as silicon dioxide, titanium oxide, aluminum oxide, zirconium oxide, aluminum silicate, diatomaceous earth, zeolite, kaolin, talc, calcium carbonate, calcium phosphate, barium sulfate, magnesium hydroxide silicate, etc. can be cited; anti-adhesive agents composed of organic particles; grease-based anti-adhesive agents such as polyethylene wax, higher fatty acid amide groups, metal soaps, and silicone oils. Among them, the anti-adhesive agent composed of particles is preferred, and the anti-adhesive agent composed of organic particles is more preferred. As the anti-adhesive agent composed of organic particles, it is particularly preferred that the anti-adhesive agent is composed of organic particles of a polymer containing a constituent unit of one or more monomers selected from aromatic vinyl monomers, vinyl cyanide monomers, and (meth) acrylate monomers as a constituent unit.

[0179] The anti-blocking agent composed of microparticles is generally in the form of microparticles dispersed in a liquid or in a colloidal form. The volume average particle size (Mv) of the microparticles in the anti-blocking agent is usually less than 10 μm, preferably 0.05 μm to 10.00 μm. The content of the anti-blocking agent is preferably 0.01 wt% to 5.00 wt%, more preferably 0.50 wt% to 3.00 wt%, relative to the total weight (100 wt%) of the stress reducing agent.

[0180] (2-4. Other optional ingredients)

[0181] The stress reducing agent may contain other optional components in addition to the above components as necessary. Examples of other optional components include various components described in the section (4-4. Other optional components) described later.

[0182] The anti-blocking agent and other optional components can be appropriately added in any step of the method for producing the stress reducing agent. For example, the anti-blocking agent and other optional components can be added to the polymer microparticles (A) or the aqueous suspension (aqueous latex) of the polymer microparticles (A) and the resin (B) before or after coagulation. The anti-blocking agent and other optional components can be added separately to the polymer microparticles (A), the resin (B) or the stress reducing agent containing the polymer microparticles (A) and the resin (B).

[0183] [3. Method for producing a stress reducing agent]

[0184] In one embodiment of the present invention, the method for producing the stress reducing agent is not particularly limited. Hereinafter, an example of the method for producing the stress reducing agent is described by taking the case where the stress reducing agent contains polymer microparticles (A) and resin (B) as an example. It should be noted that when the resin (B) is not used in the following production method, a stress reducing agent containing polymer microparticles (A) and not containing resin (B) can be obtained.

[0185] In one embodiment of the present invention, the method for producing a stress reducing agent comprises: a resin (B) adding step of adding a resin (B) to an aqueous latex containing polymer microparticles (A), a coagulation step of preparing an agglomerate containing the polymer microparticles (A) and the resin (B) using the obtained aqueous latex, and a recovery step of recovering the agglomerate. In this specification, "coagulation", "condensation" and "solidification" have the same meanings and can be substituted for each other.

[0186] The resin (B) addition step is a step of obtaining an aqueous latex containing polymer particles (A) and resin (B). The resin (B) addition step can also be said to be a step of mixing polymer particles (A) and resin (B). There is no particular limitation on the specific method of adding resin (B) to the aqueous latex containing polymer particles (A), and examples thereof include a method of directly adding resin (B) to the aqueous latex containing polymer particles (A), a method of adding in the form of an aqueous emulsion, and a method of adding in the form of a solution. In the resin (B) addition step, it is preferred to add resin (B) to the aqueous latex containing polymer particles (A) in the form of an aqueous emulsion.

[0187] The coagulation step is a step for coagulating the polymer microparticles (A) and the resin (B) in the aqueous latex. In the coagulation step, a coagulate containing the polymer microparticles (A) and the above-mentioned resin (B) can be obtained. There is no particular limitation on the method for coagulating the polymer microparticles (A) and the resin (B). For example, a method using a solvent, a method using a coagulant (also called a coagulant and a coagulant), a method of spraying the aqueous latex containing the polymer microparticles (A) and the resin (B), etc. can be used.

[0188] As the aggregation step, it is preferred to have a step of preparing an aggregate containing polymer microparticles (A) and the resin (B) using a coagulant. According to this configuration, since there is no need to use a solvent, a thermosetting resin powder with a small environmental load can be used. In addition, according to this configuration, since no special facilities for spraying are required, a thermosetting resin powder can be easily obtained.

[0189] The recovery step is a step of removing water from the aqueous latex to obtain an agglomerate containing polymer particles (A) and a resin (B). The recovery step can also be described in another way as a step of separating the agglomerate containing polymer particles (A) and a resin (B) from the water component in the aqueous latex. It should be noted that the water component refers to a mixture containing water as a main component, an emulsifier, unagglomerated polymer particles (A), a resin (B), etc. There is no particular limitation on the method for recovering the agglomerate containing polymer particles (A) and a resin (B), and for example, methods such as filtration and centrifugation can be cited.

[0190] The aggregate obtained through the above-mentioned resin (B) adding step, aggregation step and recovery step can be used as a stress reducing agent.

[0191] In one embodiment of the present invention, the method for producing a stress reducing agent may further include a washing step.

[0192] The washing step is a step of washing the aggregates containing the polymer microparticles (A) and the resin (B) obtained in the above-mentioned recovery step. By washing the aggregates, a powder for thermosetting resin with a small content of inclusions, etc. is obtained. In the washing step, it is more preferred to wash the aggregates with water, and it is further preferred to wash with ion exchange water or pure water.

[0193] The washing process can be any process for washing the agglomerates, and the specific method is not particularly limited. For example, a method of mixing the agglomerates and water and stirring them with a stirrer, a method of kneading the agglomerates and water using a kneader, a method of mixing the agglomerates and water with a rotation and revolution stirrer, a method of spraying water on the agglomerates, a method of washing the filter cake using a pressure filter, etc. can be cited. As the kneader, various batch kneaders, continuous kneaders, extrusion kneaders, extruders, etc. can be used.

[0194] The objects to be cleaned refer to all impurities contained in the aggregates, and are not particularly limited. For example, in addition to inclusions from emulsifiers (e.g., phosphorus emulsifiers, sulfonic acid emulsifiers), inclusions from coagulants when coagulants described below are used can also be cited.

[0195] Examples of the emulsifier include (a) anionic emulsifiers such as the acids exemplified below, alkali metal salts of the acids, or ammonium salts of the acids, (b) nonionic emulsifiers such as alkyl or aryl substituted polyethylene glycol, (c) polyvinyl alcohol, alkyl substituted cellulose, polyvinyl pyrrolidone, polyacrylic acid derivatives, etc. Examples of the acids include (a1) alkyl or aryl sulfonic acids represented by dioctylsulfosuccinic acid and dodecylbenzenesulfonic acid, or alkyl or aryl ether sulfonic acids, (a2) alkyl or aryl sulfuric acids represented by dodecylsulfuric acid, or alkyl or aryl ether sulfuric acids, (a3) ​​alkyl or aryl substituted phosphoric acids, or alkyl or aryl ether substituted phosphoric acids, (a4) N-alkyl or aryl sarcosine represented by dodecylsarcosine, (a5) alkyl or aryl carboxylic acids represented by oleic acid and stearic acid, or alkyl or aryl ether carboxylic acids, etc. Here, anionic emulsifiers formed from the acids described in (a1) and (a2) are referred to as sulfur-based emulsifiers, anionic emulsifiers formed from the acids described in (a3) ​​are referred to as phosphorus-based emulsifiers, anionic emulsifiers formed from the acids described in (a4) are referred to as sarcosine-based emulsifiers, and anionic emulsifiers formed from the acids described in (a5) are referred to as carboxylic acid-based emulsifiers. These emulsifiers may be used alone or in combination of two or more.

[0196] In one embodiment of the present invention, the method for producing a stress reducing agent may further include a drying step. By drying the stress reducing agent obtained by the above method, the stress reducing agent can be obtained as a powder or granular form.

[0197] The drying step is a step of drying the agglomerates containing the polymer microparticles (A) and the resin (B) obtained in the above-mentioned recovery step or the above-mentioned washing step to obtain a powder. The method of drying the agglomerates is not particularly limited, and examples thereof include a method of drying the agglomerates using a dryer, a method of placing the agglomerates in a container and heating and decompressing the container, a method of placing the agglomerates in a container and causing a dry gas to convectively contact the agglomerates in the container, and the like.

[0198] [4. Resin composition]

[0199] A resin composition containing the above-mentioned stress reducing agent and a base resin is also an embodiment of the present invention. Hereinafter, the "resin composition involved in one embodiment of the present invention" is sometimes referred to as the "present resin composition". According to the present stress reducing agent, by adding it to the base resin, the elastic modulus of the base resin can be reduced, and the deterioration of the linear expansion coefficient can be reduced.

[0200] (4-1. Matrix resin)

[0201] The matrix resin is not particularly limited, and examples thereof include a thermosetting resin, a thermoplastic resin, or any combination of a thermosetting resin and a thermoplastic resin.

[0202] Among them, from the viewpoint that the function of the present stress reducing agent can be properly exerted, as the above-mentioned base resin, thermosetting resins such as epoxy resins, phenolic resins, polyimide resins, and oxetane resins, and thermoplastic resins such as polycarbonate resins are more preferably used. Alternatively, the above-mentioned thermosetting resin and thermoplastic resin may be the same as the thermosetting resin and thermoplastic resin described in the item (2-2. Resin (B)) above.

[0203] The matrix resin is preferably an epoxy resin. The epoxy resin may be the same as the epoxy resin described in the item (2-2. Resin (B)). The epoxy resin may be used alone or in combination with one or more matrix resins other than the epoxy resin.

[0204] (4-2. Physical properties of matrix resin)

[0205] The properties of the matrix resin are not particularly limited. The matrix resin preferably has a viscosity of 100 mPa·s to 1,000,000 mPa·s at 25°C. The viscosity of the matrix resin is more preferably 50,000 mPa·s or less at 25°C, further preferably 30,000 mPa·s or less, and particularly preferably 15,000 mPa·s or less. According to the above-mentioned structure, the matrix resin has the advantage of excellent fluidity. A matrix resin having a viscosity of 100 mPa·s to 1,000,000 mPa·s at 25°C can also be said to be a liquid.

[0206] The greater the fluidity of the matrix resin, in other words, the smaller the viscosity, the more difficult it is to disperse the polymer microparticles (A) in the matrix resin in the form of primary particles. In the past, it was very difficult to disperse the polymer microparticles (A) in the form of primary particles in a matrix resin having a viscosity of 1000000 mPa·s or less at 25°C. However, the resin composition involved in one embodiment of the present invention has the following advantages: the polymer microparticles (A) having the above-mentioned structure are well dispersed in a matrix resin having a viscosity of 1000000 mPa·s or less at 25°C.

[0207] In addition, in order to prevent the fusion of polymer particles (A) by allowing the matrix resin to penetrate into the polymer particles (A), the viscosity of the matrix resin at 25°C is more preferably 100 mPa·s or more, further preferably 500 mPa·s or more, further preferably 1000 mPa·s or more, and particularly preferably 1500 mPa·s or more.

[0208] The viscosity of the matrix resin at 25°C is more preferably 100 mPa·s to 750,000 mPa·s, more preferably 100 mPa·s to 700,000 mPa·s, more preferably 100 mPa·s to 350,000 mPa·s, more preferably 100 mPa·s to 300,000 mPa·s, more preferably 100 mPa·s to 50,000 mPa·s, further preferably 100 mPa·s to 30,000 mPa·s, and particularly preferably 100 mPa·s to 15,000 mPa·s.

[0209] The matrix resin may have a viscosity greater than 1,000,000 mPa·s. The matrix resin may be semi-solid (semi-liquid) or solid. When the matrix resin has a viscosity greater than 1,000,000 mPa·s, the resin composition containing the obtained powder or granule has the advantage of less sticking and easier handling.

[0210] The matrix resin preferably has an endothermic peak at 25° C. or lower, and more preferably has an endothermic peak at 0° C. or lower in a thermogram of differential scanning calorimetry (DSC). According to the above configuration, the matrix resin has an advantage of excellent fluidity.

[0211] (4-3. Mixing ratio of stress reducing agent and base resin, etc.)

[0212] The mixing ratio of the stress reducing agent to the matrix resin is preferably 0.5 to 50 wt % of the stress reducing agent and 50 to 99.5 wt % of the matrix resin, when the total of the stress reducing agent and the matrix resin is 100 wt %, more preferably 1 to 40 wt % of the stress reducing agent and 60 to 99 wt % of the matrix resin, more preferably 1 to 25 wt % of the stress reducing agent and 75 to 99 wt % of the matrix resin, and particularly preferably 2.5 to 20 wt % of the stress reducing agent and 80 to 97.5 wt % of the matrix resin.

[0213] In order to make the ratio of the content of the polymer microparticles (A) and the matrix resin in the obtained resin composition to the desired value, the mixing ratio of the stress reducing agent and the matrix resin can be appropriately set based on (a) the content and water content of components other than the polymer microparticles (A) contained in the powder and granule and (b) the mixing method of the stress reducing agent and the matrix resin.

[0214] The ratio of the content of the polymer microparticles (A) and the matrix resin in the resin composition is generally preferably 0.5 to 50 wt % of the polymer microparticles (A) and 50 to 99.5 wt % of the matrix resin, when the total of the polymer microparticles (A) and the matrix resin is taken as 100 wt %, more preferably 1 to 40 wt % of the polymer microparticles (A) and 60 to 99 wt % of the matrix resin, more preferably 1 to 25 wt % of the polymer microparticles (A) and 75 to 99 wt % of the matrix resin, and particularly preferably 2.5 to 20 wt % of the polymer microparticles (A) and 80 to 97.5 wt % of the matrix resin.

[0215] When the matrix resin is an epoxy resin, the state of the matrix resin is not particularly limited as long as it flows when mixed with the stress reducing agent, and may be solid at room temperature, but is preferably liquid from the viewpoint of workability.

[0216] The temperature at which the stress reducing agent is mixed with the matrix resin is generally set to a temperature at which the matrix resin can flow. If the resin (B) in the powder and particles can flow at a temperature at which the matrix resin can flow, it is easy to uniformly mix the resin (B) and the matrix resin.

[0217] When this resin combination contains a thermosetting resin as a matrix resin, a cured product can be obtained by curing the resin combination. When this resin combination contains a thermoplastic resin as a matrix resin, a molded product can be obtained by molding the resin combination. The cured product formed by curing this resin combination and the molded product formed by molding this resin combination are also respectively an embodiment of the present invention.

[0218] The present resin composition may further contain a known thermosetting resin other than the matrix resin, and may further contain a known thermoplastic resin.

[0219] (4-4. Other optional ingredients)

[0220] The present resin composition can contain other arbitrary components except the above-mentioned components as required. The present resin composition preferably contains silicon dioxide as an inorganic filler. The above-mentioned silicon dioxide can use silicon dioxide alone, or can use silicon dioxide and one or more other arbitrary components except silicon dioxide. As other arbitrary components, for example, colorants such as curing agents, pigments and dyes, body pigments, pigment dispersants, ultraviolet absorbers, the above-mentioned antioxidants, heat stabilizers (anti-gelling agents), plasticizers, leveling agents, defoamers, silane coupling agents, antistatic agents, flame retardants, lubricants, viscosity reducers, viscosity modifiers, thixotropy imparting agents, low shrinkage agents, inorganic fillers, organic fillers, thermoplastic resins, desiccants, dispersants, thermal conductivity improvers, water binders, anti-sagging agents, anti-color separation agents, anti-settling agents, coating wear regulators, surface regulators, monobasic organic acids, camphor, castor oil, etc. can be cited.

[0221] (4-5. Method for producing resin composition)

[0222] The method for producing a resin composition according to one embodiment of the present invention comprises the step of mixing a stress reducing agent containing polymer microparticles (A), a thermosetting resin, and an inorganic filler. The stress reducing agent containing the polymer microparticles (A) can be produced by the production method described in the above-mentioned item [3. Production method of stress reducing agent].

[0223] The method for producing the resin composition is not particularly limited as long as it includes a step of mixing a stress reducing agent containing polymer particles (A), a thermosetting resin, and an inorganic filler. For example, a method of mixing a stress reducing agent and a thermosetting resin, and then adding an inorganic filler and the above-mentioned other optional components as required to the obtained mixture using a stirrer, etc. It should be noted that the order of adding the stress reducing agent, the thermosetting resin, the inorganic filler, and the other optional components is not limited to the above order, and can be any order.

[0224] The method for producing a resin composition according to one embodiment of the present invention is more preferably a method for producing a resin composition comprising a step of mixing a stress reducing agent containing polymer particles (A), an epoxy resin, and silica. In the method for producing a stress reducing agent containing polymer particles (A), an epoxy resin, and silica, the order of adding the stress reducing agent, the epoxy resin, the silica, and other arbitrary components can be any order, for example, a method of mixing the stress reducing agent and the epoxy resin, and then adding silica to the obtained mixture and mixing the above-mentioned other arbitrary components as needed using a stirrer or the like can be cited.

[0225] 〔5. Sealing materials〕

[0226] The sealing material according to one embodiment of the present invention is formed by using the above-mentioned stress reducing agent or resin composition. Since the sealing material according to one embodiment of the present invention has the above-mentioned structure, it has the advantages of excellent toughness and impact resistance.

[0227] The sealing material according to one embodiment of the present invention is also simply referred to as the present sealing material.

[0228] The use of the present sealing material is not particularly limited, and examples thereof include sealing materials for various electric devices such as semiconductors and power devices.

[0229] The present sealing material can be produced using a stress reducing agent or a resin composition. The method for producing the present sealing material is not particularly limited, and a known method can be used.

[0230] 〔Summarize〕

[0231] One embodiment of the present invention includes the following configurations.

[0232] [1] A stress reducing agent comprising polymer particles (A), wherein the polymer particles (A) contain a rubber-containing graft copolymer, wherein the rubber-containing graft copolymer has an elastomer and a graft portion graft-bonded to the elastomer, wherein the proportion of the elastomer in the polymer particles (A) is greater than 70% by weight and less than 97% by weight relative to 100% by weight of the polymer particles (A), the elastomer contains an organosilicone-based rubber, the graft portion contains an epoxy-containing constituent unit, and the content of the epoxy-containing constituent unit in the graft portion is 0.5% by weight to 4.0% by weight relative to 100% by weight of the rubber-containing graft copolymer, and the stress reducing agent is a powder or granular material.

[0233] [2] The stress reducing agent according to [1], wherein the content of the epoxy group-containing structural unit in the graft portion is 3.3% to 26.7% by weight relative to 100% by weight of the graft portion in the rubber-containing graft copolymer.

[0234] [3] A stress reducing agent comprising polymer particles (A), wherein the polymer particles (A) contain a rubber-containing graft copolymer, wherein the rubber-containing graft copolymer has an elastomer and a graft portion graft-bonded to the elastomer, wherein the proportion of the elastomer in the polymer particles (A) is greater than 70% by weight and less than 97% by weight relative to 100% by weight of the polymer particles (A), the elastomer contains an organosilicone rubber, the graft portion contains an epoxy-containing constituent unit, and the content of the epoxy-containing constituent unit in the graft portion is 3.3% by weight to 26.7% by weight relative to 100% by weight of the graft portion in the rubber-containing graft copolymer, and the stress reducing agent is a powder or granular material.

[0235] [4] The stress reducing agent according to any one of [1] to [3], wherein the epoxy group-containing structural unit in the graft portion is a glycidyl methacrylate unit.

[0236] [5] The stress reducing agent according to any one of [1] to [4], further comprising a resin (B).

[0237] [6] A resin composition comprising the stress reducing agent according to any one of [1] to [5], a thermosetting resin, and an inorganic filler.

[0238] [7] The resin composition according to any one of [1] to [6], wherein the thermosetting resin is an epoxy resin and the inorganic filler is silica.

[0239] [8] A sealing material comprising the resin composition described in [6].

[0240] [9] A sealing material comprising the resin composition described in [7].

[0241]

[10] A method for producing a resin composition, comprising the step of mixing a stress reducing agent containing polymer particles (A), a thermosetting resin and an inorganic filler, wherein the polymer particles (A) contain a rubber-containing graft copolymer, the rubber-containing graft copolymer has an elastomer and a graft portion graft-bonded to the elastomer, the proportion of the elastomer in the polymer particles (A) is greater than 70% by weight and less than 97% by weight relative to 100% by weight of the polymer particles (A), the elastomer contains an organosilicone rubber, the graft portion contains an epoxy-containing constituent unit, the content of the epoxy-containing constituent unit in the graft portion is 0.5% by weight to 4.0% by weight relative to 100% by weight of the rubber-containing graft copolymer, and the stress reducing agent is a powder or granular material.

[0242]

[11] The method for producing a resin composition according to

[10] , wherein the content of the epoxy group-containing structural unit in the graft portion is 3.3% to 26.7% by weight relative to 100% by weight of the graft portion in the rubber-containing graft copolymer.

[0243]

[12] A method for producing a resin composition, comprising the step of mixing a stress reducing agent containing polymer particles (A), a thermosetting resin and an inorganic filler, wherein the polymer particles (A) contain a rubber-containing graft copolymer, the rubber-containing graft copolymer has an elastomer and a graft portion graft-bonded to the elastomer, the proportion of the elastomer in the polymer particles (A) is greater than 70% by weight and less than 97% by weight relative to 100% by weight of the polymer particles (A), the elastomer contains an organic silicone rubber, the graft portion contains an epoxy-containing constituent unit, the content of the epoxy-containing constituent unit in the graft portion is 3.3% by weight to 26.7% by weight relative to 100% by weight of the graft portion in the rubber-containing graft copolymer, and the stress reducing agent is a powder or granular material.

[0244]

[13] The method for producing a resin composition according to any one of

[10] to

[12] , wherein the epoxy group-containing structural unit in the graft portion is a glycidyl methacrylate unit.

[0245]

[14] The method for producing a resin composition according to any one of

[10] to

[13] , wherein the stress reducing agent further contains a resin (B).

[0246]

[15] The method for producing a resin composition according to any one of

[10] to

[14] , wherein the thermosetting resin is an epoxy resin and the inorganic filler is silica.

[0247] Example

[0248] Hereinafter, one embodiment of the present invention will be described in more detail according to examples and comparative examples, but the present invention is not limited thereto. One embodiment of the present invention can be implemented by appropriately changing within the scope of the above or the following purport, and they are all included in the technical scope of the present invention. It should be noted that "parts" and "%" in the following examples and comparative examples refer to parts by weight or weight %.

[0249] <Ingredients>

[0250] The components used in each of the preparation examples, examples and comparative examples are as follows.

[0251] Polymer microparticles (A)

[0252] Each polymer microparticle (A) obtained in the following production example was used.

[0253] Resin (B)

[0254] (i) using epoxidized soybean oil (ADK CIZER O-130P manufactured by ADEKA CORPORATION) alone, or

[0255] (ii) A mixture of 90 parts by weight of the epoxidized soybean oil and 10 parts by weight of triethylene glycol bis[3-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate] (antioxidant) (IRGANOX 245, manufactured by BASF JAPAN Co., Ltd.) was used.

[0256] ·Base resin

[0257] A bisphenol A type epoxy resin (manufactured by Mitsubishi Chemical Corporation, JER828) was used.

[0258] <Evaluation Method>

[0259] First, the evaluation method of the resin composition produced in Examples and Comparative Examples will be described below.

[0260] (Measurement of volume average particle size)

[0261] The volume average particle size (Mv) of the elastomer (elastic core layer) and polymer microparticles (A) dispersed in the aqueous latex was measured using Nanotrac WaveII-EX150 (manufactured by Micro Track Bell Co., Ltd.). A solution prepared by diluting the aqueous latex with deionized water was used as the measurement sample. The measurement was performed by inputting the refractive index of water and each elastomer and polymer microparticle, measuring for 120 seconds, and adjusting the sample concentration in a manner to achieve a loading index within the range of 1 to 10.

[0262] (Dispersibility of powder in matrix resin)

[0263] Prepare 15 parts by weight (15 g) of the powders and granules obtained in the examples and comparative examples and 85 parts by weight (85 g) of bisphenol A epoxy resin as a base resin. Put the prepared powders and bisphenol A epoxy resin into a container with a capacity of 200 mL. The volume of the container is about twice the volume of the prepared powders and bisphenol A epoxy resin. The powders and bisphenol A epoxy resin are mixed at a speed of 3000 rpm using a disperser (manufactured by PRIMIX Co., Ltd.) having a stirring blade with a blade diameter of Φ32 mm to obtain a resin composition. The resin composition is placed on a grinder (fineness meter), and the resin composition on the fineness meter is scraped with a metal scraper, and the dispersion state is confirmed by visual inspection. Read the scale at 5 to 10 points in a band with a width of 3 mm produced by the movement of the scraper, and measure the time until the scale reaches 0 μm. The results are shown in Table 1.

[0264] (Determination of physical properties of epoxy + silica complex cured product)

[0265] To 24.6 parts by weight of "JER828" were added 47.1 parts by weight of "MH-700" (trade name, manufactured by Shin Nippon Rika Co., Ltd.) as a curing agent, 0.471 parts by weight of 2-ethyl-4-methylimidazole as a curing accelerator, 50 parts by weight of "CMC-12S" (trade name, manufactured by Ronson Co., Ltd.) as silica, 0.2 parts by weight of "BYK1790" (trade name, manufactured by BYK Co., Ltd.) as a defoaming agent, and 33.3 parts by weight of a resin composition (a resin composition obtained by subjecting the powders and particles obtained in the examples and comparative examples obtained in the above-mentioned item (dispersibility of powders and particles in matrix resin) to a dispersion test of the powders and particles in the matrix resin) and mixed at 2000 rpm for 60 minutes using a rotary and revolving stirrer to obtain an epoxy + silica complex (resin composition). The present compound was flowed into a mold frame, heated at 100°C for 1 hour and at 150°C for 3 hours to obtain a cured plate. The cured plate was cut and subjected to a bending test at a fulcrum distance of 80 mm and a test speed of 2 mm / min. In addition, the cured plate was cut and the coefficient of linear expansion (CTE) in the range of 100°C to 130°C was measured using TA7000 manufactured by Hitachi High-Technologies Corporation at a heating speed of 10°C / min.

[0266] <1. Preparation of aqueous latex containing polymer microparticles (A)>

[0267] (Production Example 1-1: Preparation of aqueous latex (L-1) containing polymer microparticles (A))

[0268] 110 parts by weight of deionized water, 0.5 parts by weight of SDS, 100 parts by weight of octamethylcyclotetrasiloxane (D4), 2 parts by weight of tetraethoxysilane and 2 parts by weight of γ-acryloxypropyldimethoxymethylsilane as monomer M were added to a pressure-resistant polymerizer and mixed. The obtained mixed solution was stirred at 10,000 rpm for 5 minutes using a homomixer to prepare an emulsion. The obtained emulsion was added together to a 5-mouth glass container. Here, the glass container has a thermometer, a stirrer, a reflux cooler, a nitrogen inlet, and a monomer and emulsifier addition port. While stirring the added raw materials, (i) a 10% dodecylbenzenesulfonic acid (DSA) aqueous solution in an amount equivalent to 1 part by weight of the solid content in the aqueous solution was added to the glass container, then (ii) the temperature in the glass container was raised to 80°C in about 40 minutes, and (iii) the mixture was reacted at 80°C for 6 hours. Then, the temperature in the glass container is cooled to 25°C. After the temperature in the glass container reaches 25°C, the mixture is placed in the glass container for 20 hours. Then, the pH of the reaction solution is adjusted to pH 6.8 using sodium hydroxide, thereby completing the polymerization. Through the above operation, an aqueous latex (R-1) containing an elastomer with an organic silicone rubber as the main component is obtained. The polymerization conversion rate of the monomer component is 99% or more. The volume average particle size of the elastomer with an organic silicone rubber as the main component contained in the obtained aqueous latex is 280nm.

[0269] 180 parts by weight of an aqueous latex (R-1) of an organosiloxane rubber (containing 85 parts by weight of an elastomer having polyorganosiloxane rubber as the main component) and 43 parts by weight of deionized water were added to a glass reactor. Here, the glass reactor has a thermometer, a stirrer, a reflux cooler, a nitrogen inlet, and a monomer addition device. The raw materials added at 60°C were stirred while replacing the gas in the glass reactor with nitrogen. Next, 0.004 parts by weight of EDTA, 0.001 parts by weight of ferrous sulfate heptahydrate, and 0.11 parts by weight of SFS were added to the glass reactor and stirred for 10 minutes. Then, 2.0 parts by weight of triallyl isocyanurate and 0.5 parts by weight of cumene hydroperoxide (QHP) were added to the glass reactor and stirred for 30 minutes. Then, 0.03 parts by weight of QHP was added to the glass reactor and further stirred for 60 minutes. By the above operation, an aqueous latex (R-2) containing an elastomer having a crosslinked organosiloxane rubber as a main component is obtained.

[0270] Next, a mixture of 14.25 parts by weight of methyl methacrylate (MMA), 0.75 parts by weight of butyl acrylate (BA) and 0.04 parts by weight of tert-butyl hydroperoxide (BHP) is continuously added to the above-mentioned glass reactor after manufacturing the aqueous latex (R-2) containing the obtained aqueous latex (R-2) for 30 minutes. Then, 0.013 parts by weight of BHP is added to the glass reactor, and the stirring of the mixture in the glass reactor is further continued for 1 hour to terminate the polymerization. The aqueous latex (L-1) containing polymer particles (A) is obtained by the above operation. The polymerization conversion rate of the monomer component is 99% or more. The volume average particle size of the polymer particles (A) contained in the obtained aqueous latex is 290nm.

[0271] (Production Example 1-2: Preparation of aqueous latex (L-2) containing polymer microparticles (A))

[0272] In Production Example 1-1, except that a mixture of 13.5 parts by weight of MMA, 0.75 parts by weight of BA, 0.75 parts by weight of glyceryl methacrylate (GMA) and 0.04 parts by weight of tert-butyl hydroperoxide (BHP) was used instead of a mixture of 14.25 parts by weight of MMA, 0.75 parts by weight of BA and 0.04 parts by weight of tert-butyl hydroperoxide (BHP), an aqueous latex (L-2) containing polymer microparticles (A) was obtained by the same method as in Production Example 1-1. The polymerization conversion rate of the monomer components was 99% or more. The volume average particle size of the polymer microparticles (A) contained in the obtained aqueous latex was 292 nm.

[0273] (Production Example 1-3: Preparation of Aqueous Latex (L-3) Containing Polymer Microparticles (A))

[0274] In Production Example 1-1, a mixture of 12.75 parts by weight of MMA, 0.75 parts by weight of BA, 1.5 parts by weight of GMA and 0.04 parts by weight of tert-butyl hydroperoxide (BHP) was used instead of a mixture of 14.25 parts by weight of MMA, 0.75 parts by weight of BA and 0.04 parts by weight of tert-butyl hydroperoxide (BHP). An aqueous latex (L-3) containing polymer microparticles (A) was obtained in the same manner as in Production Example 1-1. The polymerization conversion rate of the monomer components was 99% or more. The volume average particle size of the polymer microparticles (A) contained in the obtained aqueous latex was 290 nm.

[0275] (Production Example 1-4: Preparation of Aqueous Latex (L-4) Containing Polymer Microparticles (A))

[0276] In Production Example 1-1, a mixture of 10.75 parts by weight of MMA, 0.75 parts by weight of BA, 3.5 parts by weight of GMA and 0.04 parts by weight of tert-butyl hydroperoxide (BHP) was used instead of a mixture of 14.25 parts by weight of MMA, 0.75 parts by weight of BA and 0.04 parts by weight of tert-butyl hydroperoxide (BHP). An aqueous latex (L-4) containing polymer microparticles (A) was obtained by the same method as in Production Example 1-1. The polymerization conversion rate of the monomer components was 99% or more. The volume average particle size of the polymer microparticles (A) contained in the obtained aqueous latex was 291 nm.

[0277] (Production Example 1-5: Preparation of aqueous latex (L-5) containing polymer microparticles (A))

[0278] In Production Example 1-1, a mixture of 9.75 parts by weight of MMA, 0.75 parts by weight of BA, 4.5 parts by weight of GMA and 0.04 parts by weight of tert-butyl hydroperoxide (BHP) was used instead of a mixture of 14.25 parts by weight of MMA, 0.75 parts by weight of BA and 0.04 parts by weight of tert-butyl hydroperoxide (BHP). An aqueous latex (L-5) containing polymer microparticles (A) was obtained by the same method as in Production Example 1-1. The polymerization conversion rate of the monomer components was 99% or more. The volume average particle size of the polymer microparticles (A) contained in the obtained aqueous latex was 292 nm.

[0279] (Production Example 1-6: Preparation of Aqueous Latex (L-6) Containing Polymer Microparticles (A))

[0280] 200 parts by weight of deionized water, 0.03 parts by weight of tripotassium phosphate, 0.002 parts by weight of disodium ethylenediaminetetraacetate (EDTA), 0.001 parts by weight of ferrous sulfate heptahydrate, and 1.55 parts by weight of sodium dodecylbenzenesulfonate (SDBS) were added to the pressure polymerizer. Next, the gas inside the pressure polymerizer was replaced with nitrogen while stirring the added raw materials, thereby fully removing oxygen from the inside of the pressure polymerizer. Then, 100 parts by weight of butadiene (Bd) was added to the pressure polymerizer, and the temperature inside the pressure polymerizer was raised to 45°C. Then, 0.03 parts by weight of para-menthane hydroperoxide (PHP) was added to the pressure polymerizer, and then 0.10 parts by weight of sodium formaldehyde sulfoxylate (SFS) was added to the pressure polymerizer to initiate polymerization. At 15 hours from the initiation of polymerization, devolatilization was carried out under reduced pressure to remove the monomers remaining in the polymerization without being used, thereby terminating the polymerization. During the polymerization, PHP, EDTA and ferrous sulfate heptahydrate are added to the pressure-resistant polymerization vessel in any amount and at any time. Through the polymerization, an aqueous latex (R-2) containing an elastomer (core layer) with polybutadiene rubber as the main component is obtained. The volume average particle size of the elastomer (core layer) contained in the obtained aqueous latex is 90 nm.

[0281] Into a pressure polymerizer, 7 parts by weight of the above-obtained polybutadiene rubber latex (R-2), 200 parts by weight of deionized water, 0.03 parts by weight of tripotassium phosphate, 0.002 parts by weight of EDTA, and 0.001 parts by weight of ferrous sulfate heptahydrate were added. Next, while stirring the added raw materials, the gas inside the pressure polymerizer was replaced with nitrogen, thereby fully removing oxygen from the inside of the pressure polymerizer. Then, 93 parts by weight of Bd were added to the pressure polymerizer, and the temperature inside the pressure polymerizer was raised to 45°C. Then, 0.02 parts by weight of PHP was added to the pressure polymerizer, and then 0.10 parts by weight of SFS was added to the pressure polymerizer to initiate polymerization. At 30 hours from the initiation of polymerization, devolatilization was carried out under reduced pressure to devolatilize and remove the monomers that were not used and remained in the polymerization, thereby terminating the polymerization. During the polymerization, PHP, EDTA, and ferrous sulfate heptahydrate were added to the pressure polymerizer in any amount and at any time. By this polymerization, an aqueous latex (R-3) containing an elastomer (core layer) mainly composed of polybutadiene rubber was obtained. The volume average particle size of the elastomer (core layer) contained in the obtained aqueous latex was 195 nm.

[0282] 260 parts by weight of the polybutadiene rubber latex (R-3) (containing 85 parts by weight of an elastomer mainly composed of polybutadiene rubber) and 50 parts by weight of deionized water were added to a glass reactor. Here, the glass reactor has a thermometer, a stirrer, a reflux cooler, a nitrogen inlet, and a monomer addition device. The raw materials added at 60°C were stirred while replacing the gas in the glass reactor with nitrogen. Next, 1.8 parts by weight of 1,3-butylene dimethacrylate and 0.07 parts by weight of tert-butyl hydroperoxide (BHP) were added to the glass reactor and stirred for 10 minutes. Then, 0.004 parts by weight of EDTA, 0.001 parts by weight of ferrous sulfate heptahydrate, and 0.13 parts by weight of SFS were added to the glass reactor and stirred for 30 minutes. Then, 0.013 parts by weight of BHP was added to the glass reactor and stirred for a further 30 minutes. Then, a mixture of 14.25 parts by weight of MMA, 0.75 parts by weight of BA and 0.05 parts by weight of BHP was continuously added to the glass reactor over 60 minutes. Then, 0.013 parts by weight of BHP was added to the glass reactor, and the mixture in the glass reactor was further stirred for 1 hour to terminate the polymerization. The above operation obtained an aqueous latex (L-6) containing polymer particles (A). The polymerization conversion rate of the monomer component was 99% or more. The volume average particle size of the polymer particles (A) contained in the obtained aqueous latex was 200nm.

[0283] (Production Example 1-7: Preparation of an aqueous latex (L-7) containing polymer microparticles (A))

[0284] In Production Example 1-6, except that a mixture of 12.75 parts by weight of MMA, 0.75 parts by weight of BA, 1.5 parts by weight of GMA and 0.05 parts by weight of BHP was used instead of a mixture of 14.25 parts by weight of MMA, 0.75 parts by weight of BA and 0.05 parts by weight of BHP, an aqueous latex (L-7) containing polymer microparticles (A) was obtained by the same method as in Production Example 1-6. The polymerization conversion rate of the monomer component was 99% or more. The volume average particle size of the polymer microparticles (A) contained in the obtained aqueous latex was 200 nm.

[0285] (Production Example 1-8: Preparation of Aqueous Latex (L-8) Containing Polymer Microparticles (A))

[0286] In Production Example 1-6, except that a mixture of 9.75 parts by weight of MMA, 0.75 parts by weight of BA, 4.5 parts by weight of GMA and 0.05 parts by weight of BHP was used instead of a mixture of 14.25 parts by weight of MMA, 0.75 parts by weight of BA and 0.05 parts by weight of BHP, an aqueous latex (L-8) containing polymer microparticles (A) was obtained by the same method as in Production Example 1-6. The polymerization conversion rate of the monomer component was 99% or more. The volume average particle size of the polymer microparticles (A) contained in the obtained aqueous latex was 200 nm.

[0287] <2. Preparation of powder and granules>

[0288] (Example 1: Preparation of Powder (P-2))

[0289] Water, 100 parts by weight of epoxidized soybean oil as resin (B), and SDBS as an emulsifier were mixed together using a homogenizer to prepare an aqueous emulsion (S-1) (resin (B) content 50%) in which resin (B) was emulsified. In addition, 4 parts by weight of calcium acetate was dissolved to prepare 600 parts by weight of ion exchange water adjusted to 70°C. Next, 250 parts by weight of aqueous latex (L-2) equivalent to 100 parts by weight of polymer microparticles (A) and 22.2 parts by weight of the aqueous emulsion (S-1) (equivalent to 11.1 parts by weight of resin (B)) were added to the 600 parts by weight of ion exchange water to obtain a slurry containing a coagulated product of polymer microparticles (A) and resin (B). Next, the slurry was centrifugally dehydrated to obtain a wet powder as the coagulated product. Then, using the obtained wet powder, the operation of adding the wet powder to 500 parts by weight of ion exchange water and the operation of centrifugally dehydrating the obtained mixture were repeated for a total of 2 cycles to obtain a wet powder. Finally, the wet powder was dried in a dryer at 50°C for 48 hours to obtain a powder (P-2). The dispersibility of the obtained powder in the matrix resin was measured by the method described in the above section (Dispersibility of powder in matrix resin). The results are shown in Table 1.

[0290] The powder (P-2) was used to prepare a resin composition by the method described in the above (Measurement of physical properties of epoxy + silica complex cured product). Furthermore, the resin composition was used to prepare a cured product by the method described in the above (Measurement of physical properties of epoxy + silica complex cured product). The elastic modulus and linear expansion coefficient of the obtained cured product were measured by the above method. The results are shown in Table 1.

[0291] (Example 2: Preparation of Powder (P-3))

[0292] In Example 1, the powder (P-3) was obtained by the same method as in Example 1 except that the aqueous latex (L-3) was used instead of the aqueous latex (L-2). The dispersibility of the obtained powder in the matrix resin was measured by the method of the above-mentioned item (dispersibility of the powder in the matrix resin). The results are shown in Table 1.

[0293] The powder (P-3) was used to prepare a resin composition by the method described in the above (Measurement of physical properties of epoxy + silica complex cured product). Furthermore, the above resin composition was used to prepare a cured product by the method described in the above (Measurement of physical properties of epoxy + silica complex cured product). The elastic modulus and linear expansion coefficient of the obtained cured product were measured by the above method. The results are shown in Table 1.

[0294] (Example 3: Preparation of Powder (P-4))

[0295] In Production Example 2-1, a powder (P-4) was obtained by the same method as in Example 1 except that an aqueous latex (L-4) was used instead of the aqueous latex (L-2). The dispersibility of the obtained powder in the matrix resin was measured by the method described in the above-mentioned item (dispersibility of the powder in the matrix resin). The results are shown in Table 1.

[0296] The powder (P-4) was used to prepare a resin composition by the method described in the above (Measurement of physical properties of epoxy + silica complex cured product). Furthermore, the above resin composition was used to prepare a cured product by the method described in the above (Measurement of physical properties of epoxy + silica complex cured product). The elastic modulus and linear expansion coefficient of the obtained cured product were measured by the above method. The results are shown in Table 1.

[0297] (Comparative Example 1: Preparation of Powder (P-1))

[0298] In Example 1, the powder (P-1) was obtained by the same method as in Example 1 except that the aqueous latex (L-1) was used instead of the aqueous latex (L-2). The dispersibility of the obtained powder in the matrix resin was measured by the method of the above-mentioned item (dispersibility of the powder in the matrix resin). The results are shown in Table 1.

[0299] The powder (P-1) was used to prepare a resin composition by the method described in the above (Measurement of Physical Properties of Epoxy + Silica Complex Cured Material). Furthermore, the above resin composition was used to prepare a cured product by the method described in the above (Measurement of Physical Properties of Epoxy + Silica Complex Cured Material). The elastic modulus and linear expansion coefficient of the obtained cured product were measured by the above method. The results are shown in Table 1.

[0300] (Comparative Example 2: Preparation of Powder (P-5))

[0301] In Example 1, a powder (P-5) was obtained by the same method as in Example 1 except that an aqueous latex (L-5) was used instead of the aqueous latex (L-2). The dispersibility of the obtained powder in the matrix resin was measured by the method of the above-mentioned item (dispersibility of powder in matrix resin). The results are shown in Table 1.

[0302] The powder (P-5) was used to prepare a resin composition by the method described in the above (Measurement of physical properties of epoxy + silica complex cured product). Furthermore, the above resin composition was used to prepare a cured product by the method described in the above (Measurement of physical properties of epoxy + silica complex cured product). The elastic modulus and linear expansion coefficient of the obtained cured product were measured by the above method. The results are shown in Table 1.

[0303] (Comparative Example 3: Preparation of Powder (P-6))

[0304] (i) Water, (ii) a mixture of 90 parts by weight of epoxidized soybean oil as resin (B) and 10 parts by weight of triethylene glycol bis[3-(tert-butyl-4-hydroxy-5-methylphenyl) propionate], and (iii) SDBS as an emulsifier were mixed together using a homogenizer to prepare an aqueous emulsion (S-2) (resin (B) content 11.1%) in which the resin (B) was emulsified. In Example 1, a powder (P-6) was obtained by the same method as in Example 1, except that 22.2 parts by weight of the aqueous emulsion (S-2) was used instead of 22.2 parts by weight of the aqueous emulsion (S-1) and the aqueous latex (L-6) was used instead of the aqueous latex (L-2). The dispersibility of the obtained powder in the matrix resin was measured by the method of the above-mentioned item (dispersibility of the powder in the matrix resin). The results are shown in Table 1.

[0305] The powder (P-6) was used to prepare a resin composition by the method described in the above (Measurement of physical properties of epoxy + silica complex cured product). Furthermore, the above resin composition was used to prepare a cured product by the method described in the above (Measurement of physical properties of epoxy + silica complex cured product). The elastic modulus and linear expansion coefficient of the obtained cured product were measured by the above method. The results are shown in Table 1.

[0306] (Comparative Example 4: Preparation of Powder (P-7))

[0307] In Comparative Example 3, except that aqueous latex (L-7) was used instead of aqueous latex (L-6), a powder (P-7) was obtained by the same method as in Comparative Example 3. The dispersibility of the obtained powder in the matrix resin was measured by the method of the above-mentioned item (dispersibility of powder in matrix resin). The results are shown in Table 1.

[0308] The powder (P-7) was used to prepare a resin composition by the method described in the above (Measurement of physical properties of epoxy + silica complex cured product). Furthermore, the above resin composition was used to prepare a cured product by the method described in the above (Measurement of physical properties of epoxy + silica complex cured product). The elastic modulus and linear expansion coefficient of the obtained cured product were measured by the above method. The results are shown in Table 1.

[0309] (Comparative Example 5: Preparation of Powder (P-8))

[0310] In Comparative Example 3, except that aqueous latex (L-8) was used instead of aqueous latex (L-6), a powder (P-8) was obtained by the same method as in Comparative Example 3. The dispersibility of the obtained powder in the matrix resin was measured by the method of the above-mentioned item (dispersibility of powder in matrix resin). The results are shown in Table 1.

[0311] The powder (P-8) was used to prepare a resin composition by the method described in the above (Measurement of physical properties of epoxy + silica complex cured product). Furthermore, the above resin composition was used to prepare a cured product by the method described in the above (Measurement of physical properties of epoxy + silica complex cured product). The elastic modulus and linear expansion coefficient of the obtained cured product were measured by the above method. The results are shown in Table 1.

[0312] (Comparative Example 6)

[0313] In Comparative Example 6, a low stress agent (powder and granules) is not used. Powder and granules are not used, that is, 33.3 parts by weight of bisphenol A epoxy resin is used instead of 33.3 parts by weight of the resin composition containing powder and granules. In addition, the resin composition is prepared by the same method as the method of the above-mentioned item (measurement of physical properties of epoxy + silica complex cured product). Furthermore, using the above-mentioned resin composition, a cured product is prepared by the method of the above-mentioned item (measurement of physical properties of epoxy + silica complex cured product). The elastic modulus and linear expansion coefficient of the obtained cured product are measured by the above-mentioned method. The results are shown in Table 1.

[0314]

[0315] 〔result〕

[0316] According to Table 1, we can know the following facts:

[0317] (1) It can be seen that when the polymer particles (A) of Examples 1 to 3 containing a rubber-containing graft copolymer having an elastomer containing an organosiloxane rubber and a graft portion graft-bonded to the elastomer are used to prepare a stress reducing agent, the elastic modulus of the cured product is equivalent to or lower than that of Comparative Examples 3 to 5 using polymer particles not containing an organosiloxane rubber as an elastomer, and the linear expansion coefficient is significantly smaller, that is, the linear expansion coefficient is good.

[0318] (2) It can be seen that for the above-mentioned polymer particles, when the polymer particles (A) of Examples 1 to 3 containing epoxy-containing constituent units in the grafted portion are used to prepare the stress reducing agent, the elastic modulus of the cured product is lower and the linear expansion coefficient is better than that of Comparative Example 1 using polymer particles not containing epoxy-containing constituent units in the grafted portion.

[0319] (3) It is found that the polymer particles (A) of Examples 1 to 3, in which the content of epoxy-containing structural units in the grafted portion relative to the rubber-containing graft copolymer is 4.0 wt % or less, have better dispersibility in the matrix resin before curing than the polymer particles of Comparative Example 2, in which the content is 4.5 wt %.

[0320] Industrial Applicability

[0321] One embodiment of the present invention can provide a stress reducing agent, which (i) has excellent dispersibility in a matrix resin and (ii) can produce a cured product having a good linear expansion coefficient. Therefore, a resin composition containing the stress reducing agent of one embodiment of the present invention can be well used as a sealing material for electronic materials and the like.

Claims

1. A stress reducing agent comprising polymer microparticles (A), The polymer fine particles (A) contain a rubber-containing graft copolymer, wherein the rubber-containing graft copolymer has an elastomer and a graft portion graft-bonded to the elastomer. The ratio of the elastomer in the polymer fine particles (A) is greater than 70% by weight and less than 97% by weight relative to 100% by weight of the polymer fine particles (A), The elastomer contains an organic silicone rubber. The grafted portion contains an epoxy group-containing constituent unit, The content of the epoxy group-containing structural unit in the graft portion is 0.5 to 4.0% by weight relative to 100% by weight of the rubber-containing graft copolymer. Furthermore, the stress reducing agent is in the form of powder or granular material.

2. The stress reducing agent according to claim 1, wherein The content of the epoxy group-containing structural unit in the graft portion is 3.3% by weight to 26.7% by weight relative to 100% by weight of the graft portion in the rubber-containing graft copolymer.

3. A stress reducing agent comprising polymer microparticles (A), The polymer fine particles (A) contain a rubber-containing graft copolymer, wherein the rubber-containing graft copolymer has an elastomer and a graft portion graft-bonded to the elastomer. The ratio of the elastomer in the polymer fine particles (A) is greater than 70% by weight and less than 97% by weight relative to 100% by weight of the polymer fine particles (A), The elastomer contains an organic silicone rubber. The grafted portion contains an epoxy group-containing constituent unit, The content of the epoxy group-containing structural unit in the graft portion is 3.3% to 26.7% by weight relative to 100% by weight of the graft portion in the rubber-containing graft copolymer. Furthermore, the stress reducing agent is in the form of powder or granular material.

4. The stress reducing agent according to any one of claims 1 to 3, wherein The epoxy group-containing constituent unit in the graft portion is a glycidyl methacrylate unit.

5. The stress reducing agent according to any one of claims 1 to 3, wherein It further contains a resin (B). 6 . A resin composition comprising the stress reducing agent according to claim 1 , a thermosetting resin, and an inorganic filler.

7. The resin composition according to claim 6, wherein The thermosetting resin is an epoxy resin, and the inorganic filler is silicon dioxide.

8. A sealing material comprising the resin composition according to claim 6.

9. A sealing material comprising the resin composition according to claim 7.

10. A method for producing a resin composition, comprising the step of mixing a stress reducing agent containing polymer microparticles (A), a thermosetting resin and an inorganic filler, wherein: The polymer fine particles (A) contain a rubber-containing graft copolymer, wherein the rubber-containing graft copolymer has an elastomer and a graft portion graft-bonded to the elastomer. The ratio of the elastomer in the polymer fine particles (A) is greater than 70% by weight and less than 97% by weight relative to 100% by weight of the polymer fine particles (A), The elastomer contains an organic silicone rubber. The grafted portion contains an epoxy group-containing constituent unit, The content of the epoxy group-containing structural unit in the graft portion is 0.5 to 4.0% by weight relative to 100% by weight of the rubber-containing graft copolymer. Furthermore, the stress reducing agent is in the form of powder or granular material.

11. The method for producing a resin composition according to claim 10, wherein: The content of the epoxy group-containing structural unit in the graft portion is 3.3% by weight to 26.7% by weight relative to 100% by weight of the graft portion in the rubber-containing graft copolymer.

12. A method for producing a resin composition, comprising the step of mixing a stress reducing agent containing polymer microparticles (A), a thermosetting resin and an inorganic filler, wherein: The polymer fine particles (A) contain a rubber-containing graft copolymer, wherein the rubber-containing graft copolymer has an elastomer and a graft portion graft-bonded to the elastomer. The ratio of the elastomer in the polymer fine particles (A) is greater than 70% by weight and less than 97% by weight relative to 100% by weight of the polymer fine particles (A), The elastomer contains an organic silicone rubber. The grafted portion contains an epoxy group-containing constituent unit, The content of the epoxy group-containing structural unit in the graft portion is 3.3% to 26.7% by weight relative to 100% by weight of the graft portion in the rubber-containing graft copolymer. Furthermore, the stress reducing agent is in the form of powder or granular material.

13. The method for producing a resin composition according to any one of claims 10 to 12, wherein The epoxy group-containing constituent unit in the graft portion is a glycidyl methacrylate unit.

14. The method for producing a resin composition according to any one of claims 10 to 12, wherein The stress reducing agent further contains a resin (B).

15. The method for producing a resin composition according to any one of claims 10 to 12, wherein The thermosetting resin is an epoxy resin, and the inorganic filler is silicon dioxide.

Citation Information

Patent Citations

  • Graft copolymer, resin composition, and molding

    JP2015172185A

  • Epoxy resin composition for fiber-reinforced composite material

    JP2018035210A

  • Process for producing rubbery polymer particle and process for producing resin composition containing the same

    WO2005028546A1

  • Graft copolymer, method for producing same and resin composition containing such graft copolymer

    WO2006070664A1

  • Sealing liquid epoxy resin composition and electronic component device

    WO2017188286A1