Active energy ray curable silicone composition and cured product thereof

By curable silicone compositions without using solvents, the problem of the inability to flow at room temperature and the difficulty in controlling the thickness of the solvent-based composition in the prior art is solved, and the formation of excellent at room temperature is achieved Handiability and thermal melting properties are cured products suitable for optical semiconductor components in electrical/electronic devices.

CN119095916APending Publication Date: 2024-12-06DOW SILICONES CORP
View PDF 21 Cites 0 Cited by

Patent Information

Application Number
CN202380033972.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-26
Filing Date
2023-04-25
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing silicone hot melt composition cannot flow at room temperature, making it difficult to produce a hot melt film, and the thickness control of the solvent-based silicone composition in the coating process is difficult, and ineffective solvent drying makes it difficult to reach 200 μm- 500μm.

Method used

Using active ray curable silicone compositions without solvents, the pre-cured product is formed by hydrosilylation reaction, and given excellent melt viscosity under heating and pressure, followed by further curing by active rays to form non-existent The curing product with hot melt characteristics.

Benefits of technology

A silicone composition with excellent handling ability at room temperature is achieved, forming precured products that are less viscous or non-viscosity, and curing by active rays to form a solidified product that no longer has hot melt characteristics, suitable for electrical/electronics Optical semiconductor component sealant, adhesive or coating for the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005082456990000041
    Figure BDA0005082456990000041
  • Figure BDA0005082456990000051
    Figure BDA0005082456990000051
  • Figure BDA0005082456990000052
    Figure BDA0005082456990000052
Patent Text Reader

Abstract

An active energy ray-curable silicone composition comprising: (A) an organopolysiloxane resin having an alkenyl group in a molecule; (B) an organosiloxane oligomer having a viscosity at 25 DEG C of not more than 1,000 mPa.s, having in a molecule at least one silicon atom-bonded alkenyl group or a silicon atom-bonded hydrogen atom, and at least one silicon atom-bonded aryl group; (C) optionally, an organosilicon compound; the organosilicon compound is selected from the group consisting of (C1) organopolysiloxanes having at least one alkenyl group in the molecule and not having silicon atom-bonded aryl groups and SiO4 / 2 units, (C2) organopolysiloxanes having at least one silicon atom-bonded hydrogen atom in the molecule and not having silicon atom-bonded aryl groups, (C3) a disilylbenzene and mixtures thereof; (D) an organosilicon compound having, in a molecule, at least one silicon atom-bonded acryloyloxyalkyl group or silicon atom-bonded methacryloyloxyalkyl group, and at least one silicon atom-bonded hydrogen atom; and (E) a hydrosilylation reaction catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to and all advantages of U.S. Provisional Patent Application No. 63 / 334,824, filed on April 26, 2022, the contents of which are incorporated herein by reference. Technical Field

[0003] The invention relates to an active energy ray-curable organic silicon composition and a cured product thereof. Background Art

[0004] Since heat-curable, water-curable or active energy ray-curable silicone compositions are cured to form cured products having excellent heat resistance, cold resistance, electrical insulation, weather resistance, water resistance and transparency, these curable silicone compositions can be widely used in the industrial field. Specifically, compared with other organic materials, their cured products are difficult to fade, and the cured products rarely cause deterioration of physical properties. Therefore, the cured products are suitable as optical materials.

[0005] For example, Patent Document 1 proposes a liquid silicone resin composition for a photoelectric device, which contains: an alkenyl group-containing silicone resin, an organopolysiloxane containing silicon-bonded hydrogen atoms, and a hydrosilylation reaction catalyst.

[0006] Meanwhile, in recent years, materials that are solid or semi-solid at room temperature have been proposed for use in the production process of optoelectronic devices. For example, an organosilicon hot melt composition has been reported. This organosilicon hot melt composition mainly comprises an organic modified polysilicate resin, which is a non-flowable solid at room temperature and is essentially composed of an organosilicate (T) unit (i.e., RSiO 3 / 2 units, wherein R represents a monovalent organic group, such as methyl or phenyl) and / or silicate (Q) units (i.e., SiO 4 / 2 units), and further comprises a linear organopolysiloxane and a crosslinking agent.

[0007] For example, Patent Document 2 proposes an active energy ray-curable hot-melt silicone composition, which contains: a high amount (about 80% by weight) of an organic modified polysilicate resin (MQ resin), as well as a linear organic polysiloxane, a mercapto-functional crosslinking agent and a photo-radical initiator, which is solid or semi-solid at room temperature and melts at a high temperature; Patent Document 3 proposes an addition-curable adhesive silicone composition, which contains an organic polysilicate resin (MT resin) containing a vinyl (Vi) group and a hydrosilyl (SiH) group, which is solid or semi-solid in an uncured state at room temperature; Patent Documents 4 and 5 propose a solvent-based hot-melt composition, which is a metal-catalyzed pre-reaction of a vinyl-containing organic modified polysilicate resin and a hydrosilyl-modified linear polysiloxane in a solvent (such as toluene), and their melting and further crosslinking with an additional multifunctional hydrosilyl crosslinking agent are carried out at an elevated temperature.

[0008] However, such silicone hot melt compositions or solvent-based flowable hot melt compositions that are not flowable at room temperature are not suitable for manufacturing hot melt films (or layers or sheets) because precise temperature control is required to melt and reduce the viscosity of the silicone hot melt composition to obtain a uniform silicone hot melt film via a hot melt coating process, and to avoid premature curing (further hydrosilylation crosslinking) at elevated temperatures during the coating process. In addition, in the case of a solvent-based silicone composition, it is suitable for a coating process, however, due to ineffective solvent drying, it is difficult to control the thickness and it is difficult to obtain a thick (200 μm-500 μm) hot melt film.

[0009] Prior art literature

[0010] Patent Literature

[0011] Patent document 1: U.S. Patent Application Publication No. US2004 / 0116640 A1

[0012] Patent Document 2: U.S. Patent Application Publication No. US2018 / 0305547 A1

[0013] Patent document 3: U.S. Patent Application Publication No. US2008 / 0308828 A1

[0014] Patent Document 4: U.S. Patent Application Publication No. US2018 / 0208816 A1

[0015] Patent Document 5: U.S. Patent Application Publication No. US2017 / 0355804 A1 Summary of the invention

[0016] Technical issues

[0017] An object of the present invention is to provide an active energy ray-curable silicone composition which has excellent processability without using a solvent, is cured by heating to form a less viscous or non-viscous pre-cured product having excellent melt viscosity by heating at room temperature, and is further cured by active energy rays to form a cured product which no longer has hot-melt properties.

[0018] Solution to the problem

[0019] The active energy ray-curable silicone composition of the present invention comprises:

[0020] (A) an organopolysiloxane resin represented by the following average unit formula:

[0021] (R 1 3 SiO 1 / 2 ) a (R 2 R 1 2 SiO 1 / 2 ) b (SiO 4 / 2 ) c (HO 1 / 2 ) d

[0022] Each R 1 are independently alkyl groups; R 2 is an alkenyl group; and the subscripts a, b, c and d are numbers satisfying the following conditions: a≥0, b>0, 0.3≤c≤0.7, 0≤d

[0023] ≤0.05, and a+b+c=1;

[0024] (B) an organosiloxane oligomer having a viscosity of not more than 1,000 mPa·s at 25° C. and selected from the group consisting of: (B 1 ) an organosiloxane oligomer having at least one silicon-bonded alkenyl group and at least one silicon-bonded aryl group in the molecule, (B 2 ) an organosiloxane oligomer having at least one silicon-bonded hydrogen atom and at least one silicon-bonded aryl group in the molecule and component (B 1 ) and (B 2 )

[0025] (C) optionally, an organosilicon compound selected from the group consisting of: (C 1 ) has at least one alkenyl group in the molecule and has no silicon-bonded aryl group and SiO 4 / 2Unit organopolysiloxane, (C 2 ) an organopolysiloxane having at least one silicon-bonded hydrogen atom and no silicon-bonded aryl group in the molecule, (C 3 ) is a dimethylsilylbenzene represented by the following general formula:

[0026] HR 1 2 Si-C 6 H 4 -SiR 1 2 H

[0027] Each R 1 as above, and mixtures thereof;

[0028] (D) an organosilicon compound having at least one silicon-atom-bonded acryloyloxyalkyl group or silicon-atom-bonded methacryloyloxyalkyl group and at least one silicon-atom-bonded hydrogen atom in a molecule; and

[0029] (E) a catalytic amount of a hydrosilylation reaction catalyst;

[0030] wherein the amount of component (A) is in the range of 50% by mass to 80% by mass, the amount of component (B) is in the range of 5% by mass to 40% by mass, the amount of component (C) is in the range of 0% by mass to 30% by mass, each based on the total mass of components (A) to (C), and the amount of component (D) is in the range of 2 parts by mass to 20 parts by mass relative to 100 parts by mass of the total mass of components (A) to (C), provided that the molar ratio of all silicon atom-bonded hydrogen atoms to all silicon atom-bonded alkenyl groups in components (A) to (D) is 0.5 or more and less than 1.0.

[0031] In various embodiments, component (B 1 ) is at least one selected from the following: (B 11 ) An organosiloxane oligomer represented by the following general formula:

[0032] R 2 R 3 2 SiO(R 3 2 SiO) m S i 3 2 R 2

[0033] Each R 2 is independently an alkenyl group; each R 3 are independently an alkyl group or an aryl group, provided that at least one R 3is an aryl group; and the subscript m is an integer from 0 to 10.

[0034] In various embodiments, component (B 11 ) is at least one selected from the group consisting of organosiloxane oligomers represented by the following formula:

[0035] (CH 2 =CH)(CH 3 ) 2 SiO(C 6 H 5 ) 2 SiOSi(CH 3 ) 2 (CH=CH 2 );

[0036] (CH 2 =CH)(CH 3 ) 2 SiO(C 6 H 5 )(CH 3 )SiOSi(CH 3 ) 2 (CH=CH 2 );and

[0037] (CH 2 =CH)(CH 3 )(C 6 H 5 )SiOSi(CH 3 )(C 6 H 5 )(CH=CH 2 ).

[0038] In various embodiments, component (B 2 ) is at least one selected from the following: (B 21 ) An organosiloxane oligomer represented by the following general formula:

[0039] HR 3 2 SiO(R 3 2 SiO) m S i 3 2 H

[0040] Each R 3 are independently an alkyl group or an aryl group, provided that at least one R 3 is an aryl group; and the subscript m is an integer from 0 to 10.

[0041] In various embodiments, component (B21 ) is at least one selected from the group consisting of organosiloxane oligomers represented by the following formula:

[0042] H(CH 3 ) 2 SiO(C 6 H 5 ) 2 SiOSi(CH 3 ) 2 H; and

[0043] H(CH 3 ) 2 SiO(C 6 H 5 )(CH 3 )SiOSi(CH 3 ) 2 H.

[0044] In various embodiments, component (D) has an acryloyloxyalkyl group or a methacryloyloxyalkyl group represented by the following general formula:

[0045]

[0046] Where R 4 is a methyl group or a hydrogen atom; and R 5 is an alkylene group having 2 to 6 carbon atoms.

[0047] In various embodiments, component (D) is at least one organosilicon compound selected from compounds represented by the following general formula:

[0048]

[0049] Each R 6 are independently an alkyl group or an aryl group; and X is a group represented by the following general formula:

[0050]

[0051] Where R 4 is a methyl group or a hydrogen atom, and R 5 is an alkylene group having 2 to 6 carbon atoms; and subscript n is an integer from 1 to 10, subscript n′ is an integer from 1 to 10, and subscript n″ is an integer from 0 to 10.

[0052] In various embodiments, component (D) is used in an amount such that the content of acryloyloxyalkyl groups or methacryloyloxyalkyl groups is 4 mmol / 100 g relative to the total mass of components (A) to (E), optional components (A) to (G) (wherein components (F) and (G) are described below).

[0053] In various embodiments, the curable silicone composition further comprises: (F) a hydrosilylation reaction inhibitor in an amount that regulates the cure of the composition.

[0054] In various embodiments, the curable silicone composition further comprises: (G) a photo radical initiator in an amount to accelerate curing of the composition by active energy rays.

[0055] The precured product of the present invention is obtained by subjecting the above-mentioned curable silicone composition to a hydrosilylation reaction.

[0056] The cured product of the present invention is obtained by exposing the above-mentioned pre-cured product to active energy rays.

[0057] The method for producing the cured product of the present invention comprises the following steps:

[0058] 1) curing the curable silicone composition of the present invention through a hydrosilylation reaction to form a precured product;

[0059] 2) placing the precured product on a target substrate, and applying heat and / or pressure to the precured product placed on the target substrate; and

[0060] 3) The precured product is exposed to active energy rays.

[0061] Effects of the Invention

[0062] The active energy ray-curable silicone composition of the present invention has excellent processability at room temperature without using a solvent, and is cured by heating to form a less viscous or non-viscous pre-cured product having excellent melt viscosity at room temperature by heating, and is further cured by active energy rays to form a cured product that no longer has hot-melt properties.

[0063] definition

[0064] The term "comprising" or "containing" is used in its broadest sense herein, meaning and encompassing the concepts of "including", "consisting essentially of" and "consisting of". The use of "for example", "for example", "such as" and "including" to list illustrative examples is not meant to be limited to the listed examples. Therefore, "for example" or "such as" means "for example, but not limited to" or "such as, but not limited to" and encompasses other similar or equivalent examples. As used herein, the term "about" is used to reasonably encompass or describe minor variations of numerical values ​​measured by instrumental analysis or as a result of sample processing. Such minor variations can be approximately ±0-25, ±0-10, ±0-5 or ±0-2.5% of a numerical value. In addition, the term "about" is applicable to two numerical values ​​when associated with a range of values. In addition, the term "about" is applicable to numerical values ​​even when not explicitly stated.

[0065] It should be understood that the appended claims are not limited to the specific and particular compounds, compositions or methods described in the detailed description, which may vary between specific embodiments falling within the scope of the appended claims. With respect to any Markush group relied upon herein to describe specific features or aspects of various embodiments, it should be understood that different, special and / or unexpected results may be obtained from each member of the corresponding Markush group independent of all other Markush members. Each member of the Markush group may be relied upon individually and / or in combination and provides adequate support for specific embodiments within the scope of the appended claims.

[0066] It should also be understood that any ranges and sub-ranges relied upon in describing various embodiments of the present invention fall within the scope of the appended claims independently and collectively, and should be understood to describe and contemplate all ranges including integer values ​​and / or fractional values ​​therein, even if such values ​​are not explicitly written herein. It will be readily appreciated by those skilled in the art that the enumerated ranges and sub-ranges fully describe and enable various embodiments of the present invention, and such ranges and sub-ranges may be further delineated as related halves, thirds, quarters, fifths, etc. As just one example, the range of "0.1 to 0.9" may be further delineated as the lower third (i.e., 0.1 to 0.3), the middle third (i.e., 0.4 to 0.6), and the upper third (i.e., 0.7 to 0.9), which are individually and collectively within the scope of the appended claims, and may be individually and / or collectively relied upon and provide sufficient support for specific embodiments within the scope of the appended claims. In addition, with respect to language such as "at least," "greater than," "less than," "not exceeding," etc., which limits or modifies a range, it should be understood that such language includes sub-ranges and / or upper or lower limits. As another example, a range of "at least 10" essentially includes a subrange of at least 10 to 35, a subrange of at least 10 to 25, a subrange of 25 to 35, etc., and each subrange can be relied upon individually and / or collectively and provide sufficient support for specific embodiments within the scope of the appended claims. Finally, independent numerical values ​​within the disclosed ranges can be relied upon and provide sufficient support for specific embodiments within the scope of the appended claims. For example, a range of "1 to 9" includes individual integers such as 3, and individual numbers including decimal points (or fractions) such as 4.1, which can be relied upon and provide sufficient support for specific embodiments within the scope of the appended claims.

[0067] The term "active energy ray" is used herein as ultraviolet rays, electron beams, radiation rays, etc. Examples of devices that emit ultraviolet rays include a high-pressure mercury lamp, a medium-pressure mercury lamp, and ultraviolet LEDs. DETAILED DESCRIPTION

[0068] The active energy ray-curable silicone composition of the present invention will be explained in detail.

[0069] Component (A) is an organopolysiloxane resin represented by the following average unit formula:

[0070] (R 1 3 SiO 1 / 2 ) a (R 2 R 1 2 SiO 1 / 2 ) b (SiO4 / 2 ) c (HO 1 / 2 ) d .

[0071] In this formula, each R 1 The alkyl group is independently an alkyl group. The alkyl group is exemplified by an alkyl group having 1 to 12 carbon atoms, such as a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a tert-butyl group, a pentyl group, a neopentyl group, a hexyl group, a cyclohexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, an undecyl group, and a dodecyl group. Among them, a methyl group is preferred.

[0072] In the formula, R 2 The alkenyl group is exemplified by an alkenyl group having 2 to 12 carbon atoms, such as a vinyl group, an allyl group, a butenyl group, a pentenyl group, a hexenyl group, a heptenyl group, an octenyl group, a nonenyl group, a decenyl group, an undecenyl group and a dodecenyl group. Among them, a vinyl group is preferred.

[0073] In the formula, subscripts a, b, c and d are numbers satisfying the following conditions: a≥0, b>0, 0.3≤c≤0.7, 0≤d≤0.05, and a+b+c=1, optionally 0.1≤a≤0.5, 0.01≤b≤0.2, 0.4≤c≤0.7, 0≤d≤0.05, and a+b+c=1, or optionally 0.2≤a≤0.5, 0.01≤b≤0.2, 0.4≤c≤0.7, 0≤d≤0.05, and a+b+c=1. This is because if subscripts a, b, c and d are numbers within the above range, the cured product obtained by curing the composition of the present invention will have appropriate hardness and mechanical strength.

[0074] The molecular weight of the organopolysiloxane resin used for component (A) is not limited, however, its number average molecular weight (Mn) measured by gel permeation chromatography (GPC) according to standard polystyrene is preferably at least 1,500 g / mol, alternatively at least 2,000 g / mol, or alternatively at least 3,000 g / mol; at the same time, Mn is preferably not more than 6,000 g / mol; alternatively not more than 5,500 g / mol. The Mn of component (A) can be any range combining the above upper and lower limits. It should be noted that if component (A) is solid at 25°C and it is difficult to uniformly mix other components in the composition of the present invention, this can be solved by preparing an organic solution of component (A) in advance and mixing it with part or all of components (B) and (C), and then the used organic solvent can be removed from this mixture. It should be noted that an organic solvent that can be used to prepare an organic solution of component (A) can be used as long as it can dissolve component (A) and be easily removed. Specific examples thereof include, but are not limited to: aromatic hydrocarbons such as toluene and xylene; and aliphatic hydrocarbons such as hexane and heptane.

[0075] Component (A) is used in an amount of 50% to 80% by mass, alternatively 55% to 80% by mass, or alternatively 55% to 75% by mass, each based on the total mass of components (A) to (C). This is because if the amount is equal to or higher than the lower limit of the above range, the cured product obtained by curing the composition of the present invention will have a less sticky or non-sticky surface and appropriate hardness and mechanical strength, while if the amount is equal to or lower than the upper limit of the above range, the composition has a suitable viscosity at 25°C.

[0076] Component (B) is an organosiloxane oligomer that imparts flowability to the curable silicone composition and imparts hot melt properties to the cured product obtained by curing the composition. The molecular structure of the organosiloxane oligomer of component (B) is not limited, however, a linear structure or a partially branched linear structure is exemplified. Component (B) may be one type of organosiloxane oligomer having these molecular structures, or may be a mixture of two or more types of organosilicon compounds having these molecular structures. The molecular weight of the organosiloxane oligomer of component (B) is not limited, however, it is preferably not more than 2,000 g / mol, alternatively not more than 1,500 g / mol. The viscosity of the organosiloxane oligomer at 25°C is generally not more than 1,000 mPa·s, alternatively not more than 500 mPa·s, or alternatively not more than 100 mPa·s. Please note that in this specification, the viscosity is a value measured at 23°C±2°C using a B-type viscometer according to ASTM D 1084.

[0077] The organosiloxane oligomer of component (B) also acts as a chain extender or crosslinker of the composition and is selected from (B 1 ) an organosiloxane oligomer having at least one silicon-bonded alkenyl group and at least one silicon-bonded aryl group in the molecule, (B 2 ) an organosiloxane oligomer having at least one silicon-bonded hydrogen atom and at least one silicon-bonded aryl group in the molecule and component (B 1 ) and (B 2 ).

[0078] Component (B 1 The organosiloxane oligomer of ) is generally an organosiloxane oligomer represented by the following general formula:

[0079] R 2 R 3 2 SiO(R 3 2 SiO) m S i 3 2 R 2 .

[0080] In this formula, each R 2 is independently an alkenyl group, and examples thereof include the same groups as those described above. Among them, a vinyl group is preferred.

[0081] In this formula, each R 3 R is independently an alkyl group or an aryl group. 3 Examples of the alkyl group include 1 The same alkyl group. 3 Examples of the aryl group of include aryl groups having 6 to 12 carbon atoms, such as a phenyl group, a tolyl group, a xylyl group, and a naphthyl group. However, at least one R 3 is an aryl group, typically a phenyl group.

[0082] In the formula, the subscript m is an integer from 0 to 10, alternatively an integer from 0 to 5, alternatively an integer from 0 to 3, or alternatively an integer of 0 or 1.

[0083] Component (B 1 ) is usually at least one selected from the group consisting of organosiloxane oligomers represented by the following formula:

[0084] (CH 2 =CH)(CH 3 ) 2 SiO(C 6 H 5 ) 2 SiOSi(CH3 ) 2 (CH=CH 2 );

[0085] (CH 2 =CH)(CH 3 ) 2 SiO(C 6 H 5 )(CH 3 )SiOSi(CH 3 ) 2 (CH=CH 2 );and

[0086] (CH 2 =CH)(CH 3 )(C 6 H 5 )SiOSi(CH 3 )(C 6 H 5 ) 2 (CH=CH 2 ).

[0087] Component (B 2 The organosiloxane oligomer of ) is generally an organosiloxane oligomer represented by the following general formula:

[0088] HR 3 2 SiO(R 3 2 SiO) m S i 3 2 H.

[0089] In this formula, each R 3 is an alkyl group or an aryl group, and examples thereof include the same groups as those described above. However, at least one R 3 is an aryl group, typically a phenyl group.

[0090] In the formula, the subscript m is an integer from 0 to 10, alternatively an integer from 0 to 5, alternatively an integer from 0 to 3, or alternatively an integer of 0 or 1.

[0091] Component (B 2 ) is usually at least one selected from the group consisting of organosiloxane oligomers represented by the following formula:

[0092] H(CH 3 ) 2 SiO(C 6 H 5 ) 2 SiOSi(CH 3 )2 H; and

[0093] H(CH 3 ) 2 SiO(C 6 H 5 )(CH 3 )SiOSi(CH 3 ) 2 H.

[0094] Component (B) is used in an amount of 5% to 40% by mass, alternatively in an amount of 10% to 35% by mass or alternatively in an amount of 20% to 35% by mass, each based on the total mass of components (A) to (C). This is because if the amount is equal to or higher than the lower limit of the above range, the composition has good processability, and the cured product obtained by curing the composition of the present invention will have a less sticky or non-sticky surface, and if the amount is equal to or lower than the upper limit of the above range, the cured product obtained has good transparency. The organosiloxane oligomer of component (B) can be component (B 1 ) and (B 2 ) mixture. And component (B 1 ) and (B 2 ) is not limited, and the amount of component (B) should be such that the molar ratio of all silicon-bonded hydrogen atoms to all silicon-bonded alkenyl groups in components (A) to (D) is 0.5 or more and less than 1.0.

[0095] Component (C) is an optional component and is an organosilicon compound selected from (C 1 ) has at least one alkenyl group in the molecule and has no silicon-bonded aryl group and SiO 4 / 2 Unit organopolysiloxane, (C 2 ) an organopolysiloxane having at least one silicon-bonded hydrogen atom and no silicon-bonded aryl group in the molecule, (C 3 ) is a dimethylsilylbenzene represented by the following general formula:

[0096] HR 1 2 Si-C 6 H 4 -SiR 1 2 H

[0097] And mixtures thereof. 1 As mentioned above.

[0098] If the mixture of components (A) and (B) can be fully cured, the addition of component (C) is optional. However, if the mixture cannot be cured due to the lack of silicon-bonded alkenyl groups, component (C) should be added. 1 ), and if the mixture cannot be cured due to lack of hydrogen atoms bonded to silicon atoms, component (C 2 ) and / or (C 3 ). In addition, if the cured product obtained by curing the composition of the present invention is hard, component (C) as a chain extender should be added, and if the cured product obtained by curing the composition of the present invention is soft, component (C) as a crosslinking agent should be added.

[0099] Component (C 1 ) is an aryl group having at least one alkenyl group in the molecule and having no silicon atom-bonded aryl group and SiO 4 / 2 The organopolysiloxane of the unit. Examples of alkenyl groups include alkenyl groups having 2 to 12 carbon atoms, such as vinyl groups, allyl groups, butenyl groups, pentenyl groups, hexenyl groups, heptenyl groups, octenyl groups, nonenyl groups, decenyl groups, undecenyl groups and dodecenyl groups. Among them, vinyl groups are preferred. In addition, in addition to alkenyl groups, component (C 1 ) include alkyl groups having 1 to 12 carbon atoms, such as methyl group, ethyl group, propyl group, isopropyl group, butyl group, isobutyl group, tert-butyl group, pentyl group, neopentyl group, hexyl group, cyclohexyl group, heptyl group, octyl group, nonyl group, decyl group, undecyl group and dodecyl group.

[0100] Component (C 1 The molecular structure of component (C) is not limited, but is generally a linear structure, a partially branched linear structure, a branched structure or a cyclic structure. 1 ) may be one type of organopolysiloxane having these molecular structures, or may be a mixture of two or more types of organopolysiloxane having these molecular structures.

[0101] Such components (C 1 ) include dimethylpolysiloxane terminated with dimethylvinylsiloxy groups at both molecular chain ends; copolymers of dimethylsiloxane and methylvinylsiloxane terminated with dimethylvinylsiloxy groups at both molecular chain ends; copolymers of dimethylsiloxane and methylvinylsiloxane terminated with trimethylsiloxy groups at both molecular chain ends; and mixtures of two or more types thereof.

[0102] Component (C2 ) is an organopolysiloxane having at least one silicon-bonded hydrogen atom in the molecule and having no silicon-bonded aryl groups. Component (C 2 ) include alkyl groups having 1 to 12 carbon atoms, such as a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a tert-butyl group, a pentyl group, a neopentyl group, a hexyl group, a cyclohexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, an undecyl group, and a dodecyl group.

[0103] Component (C 2 The molecular structure of component (C) is not limited, but is generally a linear structure, a partially branched linear structure, a branched structure, a ring structure or a three-dimensional network structure. 2 ) may be one type of organopolysiloxane having these molecular structures, or may be a mixture of two or more types of organopolysiloxane having these molecular structures.

[0104] Such components (C 2 Examples of ) include methylhydrogenpolysiloxane terminated at both molecular chain ends with trimethylsiloxy groups; copolymers of dimethylsiloxane and methylhydrogensiloxane terminated at both molecular chain ends with trimethylsiloxy groups; dimethylpolysiloxane terminated at both molecular chain ends with dimethylhydrogensiloxy groups; copolymers of dimethylsiloxane and methylhydrogensiloxane terminated at both molecular chain ends with dimethylhydrogensiloxy groups; 3 ) 2 HSiO 1 / 2 Unit and SiO 4 / 2 A copolymer composed of (CH 3 ) 2 HSiO 1 / 2 Unit, (CH 3 ) 3 HSiO 1 / 2 Unit and SiO 4 / 2 unit composition; and mixtures of two or more types thereof.

[0105] Component (C 3 ) is a disilylbenzene represented by the following general formula:

[0106] HR 1 2 Si-C 6 H 4 -SiR 1 2 H

[0107] Each R 1As mentioned above.

[0108] Such components (C 3 ) include the following disilylbenzenes:

[0109] H(CH 3 ) 2 Si-C 6 H 4 -Si(CH 3 ) 2 H; and

[0110] H(CH 3 )(C 2 H 5 )Si-C 6 H 4 -Si(CH 3 )(C 2 H 5 )H.

[0111] The organosilicon compound of component (C) may be 1 ) and (C 2 ). However, component (C) generally has a viscosity of not more than 1,000 mPa·s at 25°C, alternatively not more than 500 mPa·s, or alternatively not more than 100 mPa·s. Note that in this specification, the viscosity is a value measured at 23°C±2°C using a B-type viscometer according to ASTM D 1084.

[0112] Component (C) is used in an amount of 0% to 30% by mass, alternatively in an amount of 0% to 20% by mass, or alternatively in an amount of 0% to 10% by mass, each based on the total mass of components (A) to (C). This is because if the amount is equal to or higher than the lower limit of the above range, the composition has good processability, and if the amount is equal to or lower than the upper limit of the above range, the composition has good transparency. The organosilicon compound of component (C) may be component (C 1 ) to (C 3 ) mixture. And component (C 1 ) to (C 3 ) is not limited, and the amount of component (C) should be such that the molar ratio of all silicon-bonded hydrogen atoms to all silicon-bonded alkenyl groups in components (A) to (D) is 0.5 or more and less than 1.0.

[0113] The molar ratio of all silicon atom-bonded hydrogen atoms relative to all silicon atom-bonded alkenyl groups in components (A) to (D) ("SiH / Vi ratio") is 0.5 or more and less than 1.0, alternatively in the range of 0.5 to 0.95, or alternatively in the range of 0.6 to 0.9. This is because if the molar ratio is equal to or higher than the lower limit of the above range, the composition can be sufficiently cured, and the cured product obtained by curing the composition of the present invention will have appropriate hardness and a less sticky or non-sticky surface, and if the molar ratio is equal to or lower than the upper limit of the above range, the cured product has good hot melt properties.

[0114] Component (D) is an organic silicon compound having at least one silicon-atom-bonded acryloyloxyalkyl group or silicon-atom-bonded methacryloyloxyalkyl group and at least one silicon-atom-bonded hydrogen atom in the molecule, which is added to the composition described herein, for example, in order to provide a complete crosslinking reaction of the cured product obtained by the hydrosilylation reaction, conform it to a substrate by active energy rays, etc.

[0115] The acryloyloxyalkyl group or methacryloyloxyalkyl group in component (D) is not limited, but it is usually an acryloyloxyalkyl group or methacryloyloxyalkyl group represented by the following general formula:

[0116]

[0117] In this formula, R 4 is a methyl group or a hydrogen atom.

[0118] In this formula, R 5 is an alkylene group having 2 to 6 carbon atoms. Examples of the alkylene group include an ethylene group, a propylene group, a methylethylene group, a butylene group, a pentylene group and a hexylene group. Among them, the propylene group is preferred.

[0119] The silicon atom-bonded organic groups other than the acryloyloxyalkyl group and the methacryloyloxyalkyl group in component (D) are not limited, but they are exemplified by alkyl groups having 1 to 12 carbon atoms, such as methyl groups, ethyl groups, propyl groups, isopropyl groups, butyl groups, isobutyl groups, tert-butyl groups, pentyl groups, neopentyl groups, hexyl groups, cyclohexyl groups, heptyl groups, octyl groups, nonyl groups, decyl groups, undecyl groups, and dodecyl groups; aryl groups having 6 to 12 carbon atoms, such as phenyl groups, tolyl groups, xylyl groups, and naphthyl groups; and aralkyl groups having 7 to 12 carbon atoms, such as benzyl groups and phenethyl groups. Among them, the methyl group is preferred.

[0120] The molecular structure of component (D) is not limited, but is generally a linear structure, a partially branched linear structure, a branched structure, a cyclic structure, or a three-dimensional network structure. Component (D) may be one type of organosilicon compound having these molecular structures, or may be a mixture of two or more types of organopolysiloxanes having these molecular structures.

[0121] Examples of component (D) include organic silicon compounds represented by the following formula:

[0122]

[0123] In this formula, each R 6 is independently an alkyl group or an aryl group, and examples thereof include the same groups as those described above.

[0124] In the formula, each X is an acryloyloxyalkyl group or a methacryloyloxyalkyl group, and examples thereof include the same groups as those described above.

[0125] In the formula, subscript n is an integer from 1 to 10, subscript n′ is an integer from 1 to 10, and subscript n″ is an integer from 0 to 10.

[0126] Examples of component (D) include organic silicon compounds represented by the following formula:

[0127]

[0128]

[0129]

[0130] Methods for preparing component (D) are well known in the art, as exemplified in U.S. Pat. Nos. 4,554,339, 5,256,754, 5,334,796, and 9,018,332, and U.S. Patent Application Publication Nos. 2021 / 0122769 and 2014 / 0203323.

[0131] Component (D) is used in an amount of 2 to 20 parts by mass, alternatively 4 to 20 parts by mass, each relative to 100 parts by mass of the total mass of components (A) to (C). This is because if the amount is equal to or higher than the lower limit of the above range, the composition has good active energy ray curability, and if the amount is equal to or lower than the upper limit of the above range, the composition has good stability.

[0132] Since the content of acryloyloxyalkyl groups or methacryloyloxyalkyl groups (hereinafter referred to as "(meth)acryloyl content") varies depending on the molecular structure of component (D), it is recommended that the (meth)acryloyl content is contained in an amount of 4 mmol / 100 g or more, alternatively 8 mmol / 100 g or more, or alternatively 10 mmol / 100 g or more, relative to the total mass of components (A) to (E), and optionally components (A) to (F) or components (A) to (G) (i.e., in an embodiment where component (F) and / or component (G) are used together with components (A) to (E)). This is because if the amount is equal to or higher than the lower limit of the above range, the composition has good active energy ray curability and high temperature stability. The upper limit thereof is not limited because a higher (meth)acryloyl content preferably has better UV curability. However, it is usually 60 mmol / 100 g or less.

[0133] Component (E) is a hydrosilylation catalyst for promoting the curing of the composition of the present invention. The hydrosilylation catalyst of component (E) is well known in the art and commercially available. Suitable hydrosilylation catalysts include, but are not limited to, platinum group metals or their organometallic compounds including platinum, rhodium, ruthenium, palladium, osmium or iridium metals and any combination of two or more thereof. Component (E) is generally a platinum-based catalyst so that the curing of the composition of the present invention can be significantly accelerated. Examples of platinum-based catalysts include platinum fine powder, chloroplatinic acid, alcohol solutions of chloroplatinic acid, platinum-alkenyl siloxane complexes, platinum-olefin complexes and platinum-carbonyl complexes, wherein platinum-alkenyl siloxane complexes are the most typical.

[0134] In various embodiments, component (E) is a hydrosilylation catalyst comprising a complex of platinum and a low molecular weight organopolysiloxane, the low molecular weight organopolysiloxane comprising a complex of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane and platinum. These complexes may be microencapsulated in a resin matrix. In a specific embodiment, the catalyst comprises a 1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex with platinum.

[0135] Examples of suitable hydrosilylation catalysts for component (E) are described, for example, in U.S. Pat. Nos. 3,159,601, 3,220,972, 3,296,291, 3,419,593, 3,516,946, 3,814,730, 3,989,668, 4,784,879, 5,036,117, and 5,175,325 and in EP 0 347895 B. Microencapsulated hydrosilylation catalysts and methods for their preparation are exemplified in U.S. Pat. Nos. 4,766,176 and 5,017,654.

[0136] The amount of component (E) in the composition of the present invention is an effective amount for promoting the curing of the composition of the present invention. Specifically, in order to satisfactorily cure the composition of the present invention, the content of component (E) is generally an amount such that the catalytic metal in component (E) is about 0.01 ppm to about 500 ppm, alternatively about 0.01 ppm to about 100 ppm, alternatively about 0.01 ppm to about 50 ppm, alternatively about 0.1 ppm to about 10 ppm, relative to the content of the composition of the present invention in mass units.

[0137] In various embodiments, the active energy ray-curable silicone composition contains (F) a hydrosilylation reaction inhibitor in order to adjust the curing rate of the curable silicone composition. In certain embodiments, component (F) includes, but is not limited to, alkynols such as 2-methyl-3-butyn-2-ol, 3,5-dimethyl-1-hexyn-3-ol, 2-phenyl-3-butyn-2-ol, or 1-ethynylcyclohexane-1-ol; enyne compounds such as 3-methyl-3-pentene-1-yne or 3,5-dimethyl-3-hexene-1-yne; or 1,3,5,7-tetramethyl-1,3,5,7-tetravinylcyclotetrasiloxane, 1,3,5,7-tetramethyl-1,3,5,7-tetrahexenylcyclotetrasiloxane, tris[(1,1-dimethyl-2-propynyl)oxy]methylsilane, diallyl maleate, or benzotriazole as an optional component incorporated into the composition of the present invention.

[0138] The amount of component (F) in the composition of the present invention is not particularly limited, but if included, the amount is generally about 1 ppm to about 10,000 ppm in this component, and alternatively about 10 ppm to about 5,000 ppm, based on the mass unit relative to the composition of the present invention. This is because when the amount of component (F) is greater than or equal to the lower limit of the above range, the storage stability of the composition is good, and when the amount of component (F) is less than or equal to the upper limit of the above range, the curability of the composition at low temperatures is good.

[0139] In various embodiments, the active energy ray-curable silicone composition includes (G) a photoradical initiator to accelerate the curing of the composition by active energy rays. Examples of the photoradical initiator include acetophenone, propiophenone, benzophenone, 2-hydroxy-2-methylpropiophenone, 2,2-dimethoxy-1,2-diphenylethane-1-one, 1-hydroxycyclohexylphenylketone, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one, 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropane-1-one, 2-benzyl-2-dimethylamino-(4-morpholinophenyl)-butanone-1,2-(dimethylamino)-2-[(4-methylphenyl)methyl] -1-[4-(4-morpholinyl)phenyl]-1-butanone, 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 1,2-octanedione, 1-[4-(phenylthio)-2-(o-benzoyl oxime)]ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-1-(o-acetyl oxime), ethyl 4-dimethylaminobenzoate, 2-ethylhexyl-4-dimethylaminobenzoate, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethyl-pentylphosphine oxide, benzoyl peroxide, cumene peroxide, and mixtures of two or more thereof.

[0140] The amount of component (G) in the composition of the present invention is an effective amount for curing the composition of the present invention by irradiating it with active energy rays, and is preferably in the range of 0.1 to 15 parts by mass, alternatively in the range of 0.1 to 10 parts by mass, relative to 100 parts by mass of the total amount of components (A) to (C). This is because when the content of component (G) is greater than or equal to the lower limit of the above range, the obtained composition can be sufficiently cured, while, when the content is less than or equal to the upper limit of the above range, the heat resistance and light resistance of the obtained composition are enhanced.

[0141] In various embodiments, the active energy ray curable silicone composition includes a free radical scavenger (scavenger), which can be optionally used to control or inhibit the free radical reaction of the active energy ray curable silicone composition. Because the active energy ray curable silicone composition includes component (D), there may be a feasible free radical scavenger to prevent premature reactions during storage and use of the active energy ray reactive hot melt film prepared using the composition of the present invention. Scavengers containing phenolic compounds are a class of such substances that can be used in the present invention, and these substances include, for example, 4-methoxyphenol (MEHQ, methyl ether of hydroquinone), hydroquinone, 2-methylhydroquinone, 2-tert-butylhydroquinone, tert-butylcatechol, butylated hydroxytoluene and butylated hydroxyanisole, and combinations of two or more thereof. Other scavengers that can be used include phenothiazines and anaerobic inhibitors, such as NPAL type inhibitors (tris-(N-nitroso-N-phenylhydroxylamine) aluminum salts) from Albemarle Corporation (Baton Rouge, La.). Alternatively, the free radical scavenger may be selected from phenolic compounds, phenothiazines and anaerobic inhibitors. Free radical scavengers are known, for example, from US Pat. No. 9,475,968 and are commercially available.

[0142] The amount of the scavenger in the active energy ray-curable silicone composition will depend on various factors, including the type and amount of component (D), but the scavenger may be present in an amount of 1 ppm to 5,000 ppm by mass, alternatively in an amount of 10 ppm to 1,000 ppm by mass, or alternatively in an amount of 50 ppm to 500 ppm by mass, each relative to 100 mass of the composition of the present invention.

[0143] The viscosity of the composition of the present invention at 25° C. is not limited, but it is usually in the range of 100 mPa·s to 100,000 mPa·s.

[0144] Next, the precured and cured products of the present invention will be explained in detail.

[0145] The precured product of the present invention is obtained by hydrosilylation reaction of the above-mentioned curable silicone composition. The term "precured" means that there is a crosslinked, but not completely crosslinked network state (a state having intermediate physical properties between an uncured product and a completely cured product). The precured product may have a less sticky or non-sticky surface. In particular, the storage modulus G' of the cured product at 20°C is not limited, but under the conditions of frequency = 1 Hz, strain = 1%, the storage modulus is generally in the range of 0.05 MPa to 15 MPa, alternatively in the range of 0.07 MPa to 10 MPa, or alternatively in the range of 0.1 MPa to 5 MPa. The melt viscosity of the precured product at 100°C is not limited, but it is generally in the range of 1 Pa·s to 5000 Pa·s.

[0146] Then, the cured product of the present invention is obtained by irradiating the above-mentioned precured product with active energy rays. Examples of active energy rays used to cure the precured product include ultraviolet light and visible light; however, preferably, light with a wavelength in the range of 250nm to 500nm is preferred. This is because excellent curability is achieved and the cured product is not decomposed by the active energy rays.

[0147] The cured product is usually optically transparent. This is because when the cured product is preferably used for optical devices or image displays, in order to obtain high performance, optical transparency is required. The form of the cured product is not limited, and can be in the form of a sheet, film, lens or block. The cured product can be combined with various substrates. The cured product is usually laminated between the same or different substrates, especially between the same or different substrates in optical devices.

[0148] The state of the cured product is not limited, but is preferably an elastomer. In particular, the storage modulus G' of the cured product at 20°C is not limited, but under the conditions of frequency = 1 Hz, strain = 1%, the storage modulus is generally in the range of 0.05 MPa to 20 MPa, alternatively in the range of 0.07 MPa to 15 MPa, or alternatively in the range of 0.1 MPa to 10 MPa. This is because when the cured product is within the above range, good cohesive strength against deformation and good flexibility against material rupture are obtained. Generally, the cured product no longer has hot melt properties.

[0149] The method for preparing the cured product is not limited, but an example thereof is a method comprising the following steps:

[0150] 1) curing the curable silicone composition of the present invention through a hydrosilylation reaction to form a precured product;

[0151] 2) placing the precured product on a target substrate, and applying heat and / or pressure to the precured product placed on the target substrate; and

[0152] 3) The precured product is exposed to active energy rays.

[0153] In step 1), the curable silicone composition is heated to form a pre-cured product of a desired shape by a hydrosilylation reaction. Generally, the curing rate can be controlled by the amount and ratio of components (E) and (F), and the temperature can be from room temperature to 180°C, preferably from 80°C to 150°C. The shape of the pre-cured product is not limited, but it is preferably in the form of a sheet, a film, a lens or a block. The pre-cured product contains free (meth) acryloyl groups, which can be analyzed by Fourier transform-infrared (FT-IR) spectroscopy, as described in the following documents: "UV coatings: basics, recent developments and new applications", page 33 (Elsevier; December 21, 2006) and Schwalm, Polymer Chemistry., 2013; Vol. 4 No. 8: pp. 2449-2456, Espeel.

[0154] In step 2), since the pre-cured product has thermoplastic and hot-melt properties, the pre-cured product is deformed or melted by heating and / or pressure to conform to the target substrate. Typically, the temperature can be as high as 150°C, preferably, up to 100°C. When pressure is applied to the pre-cured product to conform to the target substrate, the applied pressure can typically be 0.05 MPa or greater, alternatively 0.1 MPa or greater, and 2 MPa or less, alternatively 1 MPa or less. In order to completely remove voids (to obtain a bubble-free laminate), a vacuum of typically 25 Torr or less, alternatively 5 Torr or less, can be applied to the complex structure of the three-dimensional features of the target surface during lamination.

[0155] In step 3), the pre-cured product is exposed to active energy rays (e.g., by a UV LED lamp) to form a cured product without changing the shape. UV curing is performed by ultraviolet irradiation, however, if the lamp used for irradiation emits rays close to ultraviolet rays, the ultraviolet source is generally not important. Typically, in order to accurately control the curing rate, a UV LED lamp is generally used. Typical wavelengths of UV LED lamps are 365nm, 385nm, 395nm and 405nm. Preferably, 365nm and 395nm are generally used. The irradiation dose is preferably 0.1J / cm 2 Up to 200J / cm 2 In the range of or optionally in the range of 1 J / cm 2 Up to 100J / cm 2The irradiation of ultraviolet rays is usually in the air. Optionally, in order to prevent surface oxygen inhibition, the precured product can be irradiated with ultraviolet rays in a laminated state with a transparent or translucent substrate (e.g., polyethylene terephthalate film and glass). Alternatively, the precured product can be irradiated with ultraviolet rays in an environment of a gas that does not cause curing inhibition, such as nitrogen and carbon dioxide.

[0156] The precured product can be used as a laminate on various target substrates with flat surfaces and uneven surfaces in electronic devices, optical devices or image displays, and is used to obtain a laminated cured product by ultraviolet irradiation. Electronic devices are, for example, semiconductor devices. Examples of semiconductor devices include semiconductor packages such as ball grid array (BGA) packages, pin grid array (PGA) packages, and grid array (LGA). Optical devices are, for example, optical semiconductor devices. Examples of optical semiconductor devices include light emitting diodes (LEDs), optical couplers, and charge coupled devices (CCDs). In addition, light emitting diode (LED) elements and solid-state image sensors are exemplified as optical semiconductor elements. In particular, even in the case of a so-called micro-LED (mini LED) having a structure in which a large number of small LED elements are arranged on a substrate in a common seal, the curable silicone composition of the present invention can be appropriately used. In addition, since the curable silicone composition of the present invention has excellent heat resistance and moisture resistance, it rarely causes a decrease in transparency and hardly causes turbidity. Therefore, the advantage is that the light extraction efficiency of the optical semiconductor device containing micro-LEDs can be well maintained.

[0157] Example

[0158] Hereinafter, the active energy ray-curable silicone composition and the cured product of the present invention will be described in detail using Examples and Comparative Examples. However, the present invention is not limited by the description of the Examples listed below.

[0159] [Gel Permeation Chromatography (GPC)]

[0160] The GPC data of component (a1) was collected using a Waters 2695 separation module and a Waters 2414 refractive index detector (RID) from Waters Corporation. Three (7.8 mm × 300 mm) Styragel HR columns (molecular weight separation range of 100 to 4,000,000) and a Styragel guard column (4.6 mm × 30 mm) with toluene were used as columns. The sample was prepared as a 0.5 mass % toluene solution and filtered through a 0.45 micron PTFE injection filter. A flow rate of one milliliter per minute was used, the temperature of the detector and column was 45 ° C, the injection volume was 100 microliters, and the run time was 60 minutes. The number average molecular weight (Mn) was calculated relative to a linear polystyrene standard covering a molecular weight range of 580 to 2,610,000.

[0161] [Viscosity]

[0162] The viscosity of each organosiloxane oligomer at 25°C was measured by a DV1 viscometer (Brookfield) using a spindle #CPA-40Z. The active energy ray-curable silicone composition was measured by a HADVIII viscometer (Brookfield) using a spindle #CP-25. The viscosity was measured for 2 minutes, and the torque was controlled within a range of 20% to 80%. The latest data was collected after the measurement was completed.

[0163] [Degree of stickiness]

[0164] The samples of the active energy ray-curable silicone composition were cured and the degree of stickiness was evaluated as follows: Each sample prepared as described above was poured into an aluminum pan and cured by heating the sample at 120° C. for 30 minutes and then cooled to room temperature. If the sample did not stick to the finger, it was considered "non-sticky". If the sample stuck to the finger, it was considered "sticky".

[0165] [Melt viscosity]

[0166] The melting behavior of the resulting silicone hot melt obtained by curing the active energy ray-curable silicone composition at 120°C for 30 minutes can be observed by exposing the solid sample to 100°C. "Melt" means that the shape of the sample collapses and spreads on the substrate. "Not melted" means that the shape of the sample is maintained. If the sample does not melt at an elevated temperature, the melt viscosity cannot be measured due to its complete crosslinking. In order to measure the melt viscosity, a hot melt sample is prepared in the same manner as described above, and the sample is mounted on a parallel plate geometry (25 mm) of a rheometer (ARES-G2, TA Instruments). Then, the melt viscosity is collected at 100°C at a fixed shear rate of 1 1 / s and a gap of 300 μm.

[0167] [Storage modulus and loss modulus]

[0168] The samples of the active energy ray-curable silicone composition were cured, and the shear modulus of the resulting silicone hot melt was evaluated as follows: Each sample prepared as described above was poured into a mold (thickness = 1 mm) and sandwiched between release films. The assembled samples were cured by heating the samples at 120°C for 30 minutes. After cooling and removing the release film, the samples were mounted on the parallel plate geometry (25 mm) of a rheometer (ARES-G2, TA Instruments). The dynamic storage modulus (G') was then collected at 20°C and 100°C at a fixed frequency of 1 Hz, a strain of 0.5%, a gap of 300 μm, and a normal force of 0 N.

[0169] To measure the post-UV properties, the assembled samples were cured by heating them at 120°C for 30 minutes and then exposing them to UV light to promote the photo-radical crosslinking reaction. The UV irradiation conditions were 365 nm LED lamp (FireJet TM FJ100) irradiated with UV light at 10 J / cm from the top surface of the film 2 of ultraviolet light.

[0170] [Examples 1-8 and Comparative Examples 1-7]

[0171] The following components are mixed uniformly in the amount ratio shown in Table 1 to produce an active energy ray curable silicone composition. When component (A) is solid at 25°C, due to high viscosity, the component is added to other components by using solvents such as toluene and xylene. Then, in order to prepare a solvent-free composition, the solvent is evaporated and replaced with other components to promote mixing. For example, first, component (B) is added to a solution in which component (A) is dissolved in a solvent. Then, the solvent is removed under reduced pressure by heating under nitrogen bubbling. After cooling to room temperature, component (C) is added. The mixture is mixed at room temperature. In addition, other components are added to the mixture and mixed at room temperature. The resulting composition and the cured product are evaluated as described above. These results are given in Table 1. The "SiH / Vi ratio" in each of Table 1 represents the molar ratio of all silicon-bonded hydrogen atoms in components (A) to (D) relative to all silicon-bonded vinyl groups. In addition, the "(meth)acrylic acid content" in Table 1 represents the content of methacryloyloxypropyl groups relative to the total mass of components (A) to (G).

[0172] The following organopolysiloxane resin was used as component (A).

[0173] (a1): an organopolysiloxane resin represented by the following average unit formula:

[0174] [(CH3 ) 3 SiO 1 / 2 ] 0.40 [(CH 2 =CH)(CH 3 ) 2 SiO 1 / 2 ] 0.04 (SiO 4 / 2 ) 0.56

[0175] The vinyl group content was about 1.9 mass % and the number average molecular weight (Mn) was about 5,000, and it was solid at 25°C.

[0176] The following organosiloxane oligomers were used as component (B).

[0177] (b1): An organosiloxane oligomer represented by the following formula:

[0178] (CH 2 =CH)(CH 3 ) 2 SiO(C 6 H 5 ) 2 SiOSi(CH 3 ) 2 (CH=CH 2 )

[0179] And the viscosity was 8.7 mPa·s and the vinyl group content was about 14.06 mass %.

[0180] (b2): An organosiloxane oligomer represented by the following formula:

[0181] H(CH 3 ) 2 SiO(C 6 H 5 ) 2 SiOSi(CH 3 ) 2 H

[0182] And the viscosity was 4.4 mPa·s and the silicon atom-bonded hydrogen atom content was about 0.61 mass %.

[0183] The following organopolysiloxane or disilylbenzene was used as component (C).

[0184] (c1): an organopolysiloxane represented by the following formula:

[0185] (CH 2 =CH)(CH 3 ) 2 SiO[(CH 3) 2 SiO] 7 Si(CH 3 ) 2 (CH=CH 2 )

[0186] And the viscosity was 7 mPa·s and the vinyl group content was about 7.49 mass %.

[0187] (c2): 1,4-bis(dimethylsilyl)benzene

[0188] (c3): an organopolysiloxane represented by the following formula:

[0189] H(CH 3 ) 2 SiO[(CH 3 ) 2 SiO] 16 Si(CH 3 ) 2 H

[0190] And the viscosity is 15 mPa·s and the silicon atom-bonded hydrogen atom content is about 0.15 mass %.

[0191] The following organosilicon compounds were used as component (D).

[0192] (d1): an organotrisiloxane represented by the following formula:

[0193]

[0194] And the methacryloyl content was 313.0 mmol / 100 g, and the silicon atom-bonded hydrogen atom content was about 0.63 mass %.

[0195] (d2): an organodisiloxane represented by the following formula:

[0196]

[0197] And the methacryloyl content was 385.0 mmol / 100 g, and the silicon atom-bonded hydrogen atom content was about 0.38 mass %.

[0198] (d3): an organopolysiloxane represented by the following formula:

[0199]

[0200] And the methacryloyl content was 81.6 mmol / 100 g, and the silicon atom-bonded hydrogen atom content was about 0.086 mass %.

[0201] (d4): an organopolysiloxane represented by the following formula:

[0202]

[0203] And the methacryloyl content was 151.2 mmol / 100 g, and the silicon atom-bonded hydrogen atom content was about 0.076 mass %.

[0204] The following hydrosilylation reaction catalyst was used as component (E).

[0205] (e1): Platinum complex of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane and 1,3-divinyl-1,1,3,3-tetramethyldisiloxane in a 1,3-divinyl-1,1,3,3-tetramethyldisiloxane solution (platinum content = 4 mass%)

[0206] The following hydrosilylation reaction inhibitor was used as component (F).

[0207] (f1): 1-ethynyl-cyclohexane-1-ol

[0208] The following photoradical initiators were used as component (G).

[0209] (g1): 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1

[0210] (g2): 1-Hydroxycyclohexylphenylketone

[0211] [Table 1]

[0212]

[0213]

[0214] [Table 1] (Continued)

[0215]

[0216]

[0217] [Table 1] (Continued)

[0218]

[0219]

[0220] [Table 1] (Continued)

[0221]

[0222]

[0223] Examples 1-8 are representative examples of active energy ray-curable silicone compositions comprising components (A) to (G) that provide a flowable liquid in the range of 300 mPa·s to 30,000 mPa·s at 25°C. After thermal curing (hydrosilylation reaction), the curable silicone composition provides a solid or semisolid, non-tacky surface at room temperature having a viscosity greater than 9×10 4 Pa, and has a significant storage modulus reduction (melting) behavior at high temperatures such as 100°C. When exposed to high temperatures, the solid state of the heat-cured silicone composition is converted into a flowable liquid with a rotational viscosity in the range of 70 Pa·s to 1,300 Pa·s (at 100°C). UV irradiation after heat curing provides further crosslinking reaction through free radical reaction of free methacryloyl groups (from component (D)) initiated by the photoradical initiator (G), and this is fully consistent. Therefore, further crosslinking by UV promotes an increase in storage modulus of more than 1×10 at 100°C. 4 Pa, and finally showed high temperature stability without deformation. In addition, it showed good transparency in the visible light range.

[0224] In contrast, even though components (A)-(G) used in Examples 1-8 are included, Comparative Examples 1-7 exhibit unfavorable characteristics such as a sticky surface and no hot melt characteristics for use in industrial fields. Comparative Examples 1-2 and 7 show that the cured products have a sticky surface, and thus fail to prepare a high modulus hot melt base (after heat curing). Comparative Examples 3 and 6 show that the cured products have no hot melt behavior (not melted) (after heat curing), and thus fail to prepare a hot melt base. When comparing Comparative Example 1 with Examples 2-4, Comparative Example 1, which includes a relatively low amount of component (A) (51.9%), provides a high modulus hot melt base having a modulus of less than 2×10 4 When comparing Comparative Examples 2-3 with Examples 1-8, Comparative Example 2 (when the SiH / Vi ratio is 0.48) provides an adhesive surface having a lower storage modulus of less than 2×10 4 Pa. In addition, Comparative Example 3 (SiH / Vi=1.25) does not show melting behavior due to a higher crosslink density. Therefore, without wishing to be bound by theory, it is believed that when the SiH / Vi ratio is greater than 0.48 and less than 1.00, the curable silicone composition provides a less tacky or non-tacky surface and hot melt properties after thermal curing.

[0225] Comparative Examples 4 and 5 show that the curable silicone compositions having a methacrylic acid content of 3.1 mmol / 100 g and 3.8 mmol / 100 g in the total composition show melting behavior even after UV irradiation, due to the lack of further crosslinking by UV free radical reaction. In contrast, Examples 1-8 show no melting behavior after complete curing (when the methacrylic acid content is 4 mmol / 100 g or more). Therefore, it is believed that the methacryloyl content imparts high temperature stability to the UV crosslinking reaction. Without wishing to be bound by theory, it is believed that when the methacryloyl content is 4 mmol / 100 g or more in the total mass of components (A) to (G), the curable silicone composition provides a fully compliant network after thermal curing followed by UV curing.

[0226] Comparative Examples 6 and 7 respectively show that the curable silicone composition without component (B) does not provide hot melt behavior when the SiH / Vi ratio is 0.86, and provides a tacky surface (less than 2×10 4 Pa). Therefore, in the absence of component (B), a solvent-free curable composition showing a non-tacky surface having hot-melt properties after thermal curing cannot be obtained.

[0227] Industrial Applicability

[0228] The active energy ray-curable silicone composition of the present invention has excellent processability at room temperature without using a solvent, is cured by heating to form a less viscous or non-viscous precured product having excellent melt viscosity by heating at room temperature, and is further cured by active energy rays to form a cured product that no longer has hot-melt properties. Therefore, the active energy ray-curable silicone composition can be used for a sealant, adhesive or coating of an optical semiconductor element in an electrical / electronic device.

Claims

1. An active energy ray-curable silicone composition, the active energy ray-curable silicone composition comprising: (A) an organopolysiloxane resin represented by the following average unit formula: (R 1 3SiO 1 / 2 ) a (R 2 R 1 2SiO 1 / 2 ) b (SiO 4 / 2 ) c (HO 1 / 2 ) d Each R 1 are independently alkyl groups; R 2 is an alkenyl group; and the subscripts a, b, c and d are numbers satisfying the following conditions: a≥0, b>0, 0.3≤c≤0.7, 0≤d≤0.05, and a+b+c=1; (B) an organosiloxane oligomer having a viscosity of not more than 1,000 mPa·s at 25° C. and selected from the group consisting of (B1) an organosiloxane oligomer having at least one silicon atom-bonded alkenyl group and at least one silicon atom-bonded aryl group in the molecule, (B2) an organosiloxane oligomer having at least one silicon atom-bonded hydrogen atom and at least one silicon atom-bonded aryl group in the molecule, and a mixture of components (B1) and (B2); (C) optionally, an organosilicon compound selected from the group consisting of: (C1) an organic silicon compound having at least one alkenyl group in the molecule and having no silicon atom-bonded aryl group and SiO 4 / 2 (C2) an organopolysiloxane having at least one silicon-bonded hydrogen atom and no silicon-bonded aryl group in the molecule, and (C3) a disilylbenzene represented by the following general formula: <h2 style=";text-align:left;direction:ltr">HR<h2 style=";text-align:left;direction:ltr"> 1 <h2 style=";text-align:left;direction:ltr"> 2Si-C6H4-SiR<h2 style=";text-align:left;direction:ltr"> 1 <h2 style=";text-align:left;direction:ltr"> 2H Each R 1 are independently alkyl groups, and mixtures thereof; (D) an organosilicon compound having at least one silicon atom-bonded acryloyloxyalkyl group or silicon atom-bonded methacryloyloxyalkyl group and at least one silicon atom-bonded hydrogen atom in a molecule; and (E) a catalytic amount of a hydrosilylation reaction catalyst; wherein the amount of component (A) is in the range of 50% by mass to 80% by mass, the amount of component (B) is in the range of 5% by mass to 40% by mass, the amount of component (C) is in the range of 0% by mass to 30% by mass, each based on the total mass of components (A) to (C), and the amount of component (D) is in the range of 2 parts by mass to 20 parts by mass relative to 100 parts by mass of the total mass of components (A) to (C), provided that the molar ratio of all silicon atom-bonded hydrogen atoms to all silicon atom-bonded alkenyl groups in components (A) to (D) is 0.5 or more and less than 1.

0.

2. The active energy ray-curable silicone composition according to claim 1, wherein component (B1) is present and is an organosiloxane oligomer represented by the following general formula: R 2 R 3 2SiO(R 3 2SiO) m SiR 3 2R 2 Each R 2 is independently an alkenyl group; each R 3 are independently an alkyl group or an aryl group, provided that at least one R 3 is an aryl group; and the subscript m is an integer from 0 to 10.

3. The active energy ray-curable silicone composition according to claim 2, wherein component (B1) is at least one selected from the group consisting of organosiloxane oligomers represented by the following formula: (CH2=CH)(CH3)2SiO(C6H5)2SiOSi(CH3)2(CH=CH2); (CH2=CH)(CH3)2SiO(C6H5)(CH3)SiOSi(CH3)2(CH=CH2); and (CH2=CH)(CH3)(C6H5)SiOSi(CH3)(C6H5)(CH=CH2).

4. The active energy ray-curable silicone composition according to claim 1, wherein component (B2) is present and is an organosiloxane oligomer represented by the following general formula: <h2 style=";text-align:left;direction:ltr">HR<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> 2SiO(R<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> 2SiO)<h2 style=";text-align:left;direction:ltr"> m <h2 style=";text-align:left;direction:ltr"> SiR<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> 2H Each R 3 are independently an alkyl group or an aryl group, provided that at least one R 3 is an aryl group; and the subscript m is an integer from 0 to 10.

5. The active energy ray-curable silicone composition according to claim 4, wherein component (B2) is at least one selected from the group consisting of organosiloxane oligomers represented by the following formula: H(CH3)2SiO(C6H5)2SiOSi(CH3)2H; and H(CH3)2SiO(C6H5)(CH3)SiOSi(CH3)2H.

6. The active energy ray-curable silicone composition according to claim 1, wherein the acryloxyalkyl group or methacryloyloxyalkyl group of component (D) is represented by the following general formula: Where R 4 is a methyl group or a hydrogen atom; and R 5 is an alkylene group having 2 to 6 carbon atoms.

7. The active energy ray-curable silicone composition according to claim 1, wherein component (D) is at least one silicone compound selected from the group consisting of compounds represented by the following general formula: Each R 6 are independently an alkyl group or an aryl group; and X is a group represented by the following general formula: Where R 4 is a methyl group or a hydrogen atom, and R 5 is an alkylene group having 2 to 6 carbon atoms; and subscript n is an integer from 1 to 10, subscript n′ is an integer from 1 to 10, and subscript n″ is an integer from 0 to 10.

8. The active energy ray-curable silicone composition according to claim 1, wherein component (D) is used in such an amount that the content of the acryloyloxyalkyl group or methacryloyloxyalkyl group is 4 mmol / 100 g or more relative to the total mass of components (A) to (E).

9. The active energy ray-curable silicone composition according to claim 1, further comprising: (F) a hydrosilylation reaction inhibitor, the amount of which regulates the cure of the composition.

10. The active energy ray-curable silicone composition according to claim 9, further comprising: (G) A photo radical initiator in an amount to accelerate the curing of the composition by active energy rays.

11. The active energy ray-curable silicone composition according to claim 10, wherein component (D) is used in such an amount that the content of the acryloyloxyalkyl group or methacryloyloxyalkyl group is 4 mmol / 100 g or more relative to the total mass of components (A) to (G).

12. The active energy ray-curable silicone composition according to claim 1, further comprising: (G) A photo radical initiator in an amount to accelerate the curing of the composition by active energy rays. 13 . A precured product obtained by subjecting the active energy ray-curable silicone composition according to claim 1 to a hydrosilylation reaction. 14 . A cured product obtained by exposing the precured product according to claim 13 to active energy rays.

15. A method for producing a cured product, the method comprising the steps of: 1) curing the curable silicone composition according to any one of claims 1 to 12 through a hydrosilylation reaction to form a precured product; 2) placing the precured product on a target substrate, and applying heat and / or pressure to the precured product placed on the target substrate; as well as 3) exposing the pre-cured product to active energy rays.

Citation Information

Patent Citations

  • Method for preparing a particulate material comprising a platinum-containing hydrosilylation catalyst and a silicone resin.

    EP0347895A2

  • Primer composition and optical semiconductor apparatus using same

    US20140203323A1

  • Curable organopolysiloxane composition, semiconductor sealant comprising same, and semiconductor device

    US20170355804A1

  • Siloxane compound and a method for preparing the same

    US20210122769A1

  • Platinum-olefin complex catalyzed addition of hydrogen- and alkenyl-substituted siloxanes

    US3159601A