Method for producing sulfide-based solid electrolyte, lithium halide-containing composition, and lithium sulfide-containing composition

By heating and melting and using lithium halide and lithium sulfide compositions under a sulfur element atmosphere, the problems of high purity and impurities in the recovery of lithium elements in lithium-ion secondary batteries are solved, and efficient manufacturing and cost reduction of sulfide-based solid electrolytes are achieved. .

CN119096310APending Publication Date: 2024-12-06AGC INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380036202.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-27
Filing Date
2023-04-24
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the prior art, when lithium elements are recovered from lithium ion secondary batteries that have been used, it is difficult to directly obtain a high-purity lithium source for the manufacture of sulfide-based solid electrolytes, and due to the influence of impurities, the characteristics of sulfide-based solid electrolytes are insufficient. Higher productivity and cost.

Method used

The aqueous solution containing lithium and impurities is heated and melted under an atmosphere containing sulfur elements, and the impurities are removed through reactions, and a sulfide-based solid electrolyte is directly produced using a lithium source, and a composition containing lithium halide and lithium sulfide is used as raw materials.

Benefits of technology

It is possible to efficiently reuse lithium elements without performing high purity treatment, suppress the influence of impurities, improve the characteristics and productivity of the sulfide-based solid electrolyte, and reduce costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119096310A_ABST
    Figure CN119096310A_ABST
Patent Text Reader

Abstract

The present invention relates to a method for producing a sulfide-based solid electrolyte, the method comprising a step for heating and melting a starting material in an atmosphere containing elemental sulfur, the starting material containing a lithium source obtained using an aqueous solution containing Li and SO4, the ratio of the SO4 to the Li in the aqueous solution being 0.1 mol% or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a sulfide-based solid electrolyte and also to a composition containing lithium halide and a composition containing lithium sulfide used in the production of the sulfide-based solid electrolyte. Background Art

[0002] Lithium-ion secondary batteries are widely used in portable electronic devices such as mobile phones and laptop computers.

[0003] In the past, liquid electrolytes have been used in lithium-ion secondary batteries, but there are concerns about leakage and fire, and the housing needs to be enlarged for safety design. In addition, improvements are also expected in terms of short battery life and narrow operating temperature range.

[0004] In view of this, all-solid-state lithium ion secondary batteries using a solid electrolyte as the electrolyte of the lithium ion secondary battery are attracting attention from the perspectives of improved safety, high-speed charging and discharging, and miniaturization of the housing.

[0005] Solid electrolytes are roughly divided into sulfide-based solid electrolytes and oxide-based solid electrolytes. The sulfide ions constituting the sulfide-based solid electrolyte have a larger polarizability than the oxide ions constituting the oxide-based solid electrolyte, and show high ion conductivity. As sulfide-based solid electrolytes, for example, sulfide-based solid electrolytes containing lithium, sulfur and phosphorus can be cited. As a raw material for a sulfide-based solid electrolyte, for example, a raw material is obtained by mixing components that are element sources of each element contained in a sulfide-based solid electrolyte.

[0006] In addition, research is underway to recover lithium from used lithium-ion secondary batteries and reuse it as battery materials. For example, when the positive electrode material of a lithium-ion secondary battery using a liquid electrolyte is calcined, lithium becomes lithium oxide (Li 2 O), and if it is immersed in water, lithium oxide becomes lithium hydroxide (LiOH) and lithium ions are dissolved in water. According to this method, lithium can be separated and extracted from non-aqueous metal elements such as Co, Mn, and Ni.

[0007] On the other hand, water-soluble Al(OH) 4 - 、F - 、SO 4 2- ,PO 4 3- Therefore, methods of removing impurities from such lithium element extracts by membrane separation or concentrating lithium elements to purify them have been studied (for example, Patent Documents 1 to 3).

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: Japanese Patent Application Publication No. 2011-154811

[0011] Patent Document 2: Japanese Patent Application Publication No. 2019-81953

[0012] Patent Document 3: Japanese Patent Application Publication No. 2012-200666 Summary of the invention

[0013] In the past, when lithium was extracted from a used lithium ion secondary battery into an aqueous solution to recover lithium, it was considered difficult to directly obtain a lithium source from the extract and use it as a material for a lithium ion secondary battery. That is, as described in Patent Documents 1 to 3, it is a prerequisite to first remove impurities from the extract by membrane separation or concentrate the lithium element to obtain a high purity.

[0014] In addition, the inventors of the present invention found that this is the same as the case where the recovered lithium is used as a raw material for a sulfide-based solid electrolyte. That is, when a lithium source is directly obtained from an extract and used to synthesize a sulfide-based solid electrolyte using a general solid phase reaction method, the synthesis does not proceed because impurities hinder the reaction, the reaction takes time, or homogeneous synthesis cannot be performed, and therefore the properties of the obtained sulfide-based solid electrolyte are sometimes insufficient.

[0015] However, since a lot of time and energy are required for highly purified treatment of the extract, or the membrane used for separation is expensive, the cost tends to increase, and the productivity is poor.

[0016] Therefore, an object of the present invention is to provide a method for producing a sulfide-based solid electrolyte, which can suppress the influence of impurities and efficiently reuse lithium even when a lithium source obtained from an aqueous solution containing lithium and impurities is directly used as a raw material. Another object is to provide a composition containing lithium halide and a composition containing lithium sulfide suitable for use in the production of the above-mentioned sulfide-based solid electrolyte.

[0017] The present inventors have repeatedly conducted intensive studies and have found that, according to a method of heating and melting a raw material in an atmosphere containing sulfur element, even when the raw material contains a predetermined amount of the above-mentioned impurities, the influence of the impurities can be suppressed and a sulfide-based solid electrolyte can be appropriately produced, thereby completing the present invention.

[0018] That is, the present invention relates to the following 1 to 12.

[0019] 1. A method for producing a sulfide-based solid electrolyte,

[0020] The method comprises the steps of heating and melting the raw materials in an atmosphere containing sulfur.

[0021] The above raw materials include Li and SO 4 The lithium source is obtained by aqueous solution,

[0022] The above SO in the above aqueous solution 4 The ratio to the above-mentioned Li is 0.1 mol% or more.

[0023] 2. The method for producing a sulfide-based solid electrolyte according to 1 above, wherein:

[0024] The aqueous solution further contains at least one of Al and F,

[0025] In the aqueous solution, at least one of a ratio of the Al to the Li and a ratio of the F to the Li is 0.01 mol % or more.

[0026] 3. The method for producing a sulfide-based solid electrolyte according to 1 or 2 above, wherein the aqueous solution comprises an extract obtained by immersing a treated material of a used lithium-ion secondary battery in water.

[0027] 4. The method for producing a sulfide-based solid electrolyte according to 3 above, wherein the aqueous solution is selected from SO 4 , Al and F and the content ratio of one or more components and Li.

[0028] 5. A method for producing a sulfide-based solid electrolyte,

[0029] Including the use of Li and SO 4 a step of obtaining a lithium source from an aqueous solution and a step of heating and melting a raw material containing the lithium source in an atmosphere containing sulfur,

[0030] In the above aqueous solution, the above SO 4 The ratio to the above-mentioned Li is 0.1 mol% or more.

[0031] 6. The method for producing a sulfide-based solid electrolyte according to 5 above, wherein:

[0032] The aqueous solution further contains at least one of Al and F,

[0033] In the aqueous solution, at least one of a ratio of the Al to the Li and a ratio of the F to the Li is 0.01 mol % or more.

[0034] 7. The method for producing a sulfide-based solid electrolyte according to 5 or 6 above, wherein the aqueous solution comprises an extract obtained by immersing a treated material of a used lithium-ion secondary battery in water.

[0035] 8. The method for producing a sulfide-based solid electrolyte according to item 7 above, further comprising the step of preparing the aqueous solution, wherein the step of preparing the aqueous solution comprises adjusting the extract to be selected from SO 4 , a step of determining the content ratio of one or more components among Al and F and Li.

[0036] 9. A composition containing lithium halide, containing less than 10% by mass of SO 4 , used to manufacture sulfide-based solid electrolytes.

[0037] 10. The composition containing lithium halide according to 9 above, wherein the halogen element constituting the lithium halide is a halogen element other than F, and further contains at least one of Al and F.

[0038] 11. A composition containing lithium sulfide, containing more than 0.5 mass % and less than 10 mass % of SO 4 , used to manufacture sulfide-based solid electrolytes.

[0039] 12. The lithium sulfide-containing composition according to 11 above, which contains at least one of Al and F.

[0040] According to the present invention, even when the raw material contains a predetermined amount of the above-mentioned impurities, the influence of the impurities can be suppressed, and the sulfide-based solid electrolyte can be appropriately manufactured. As a result, the lithium source obtained from the aqueous solution containing lithium and impurities can be directly used as a raw material to manufacture the sulfide-based solid electrolyte, and since high-purification treatment based on membrane separation or the like is not required for the aqueous solution, lithium can be efficiently reused. In addition, a composition containing lithium halide and a composition containing lithium sulfide as a raw material suitable for the manufacture of the above-mentioned sulfide-based solid electrolyte can also be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 This is a flowchart illustrating a manufacturing method according to an embodiment of the present invention.

[0042] Figure 2 This is a flowchart illustrating a manufacturing method according to an embodiment of the present invention.

[0043] Figure 3 This is a flowchart illustrating a manufacturing method according to an embodiment of the present invention.

[0044] Figure 4 is the SO in the lithium bromide obtained in Examples 1 to 64 A graph showing the relationship between the concentration and the lithium ion conductivity of a sulfide-based solid electrolyte produced using the same.

[0045] Figure 5 is the SO in the lithium bromide obtained in Examples 1 and 7 to 10 4 A graph showing the relationship between the concentration and the lithium ion conductivity of a sulfide-based solid electrolyte produced using the same.

[0046] Figure 6 is the SO in the lithium bromide obtained in Example 1 and the lithium sulfide obtained in Examples 12 to 15. 4 A graph showing the relationship between the concentration and the lithium ion conductivity of a sulfide-based solid electrolyte produced using the same. DETAILED DESCRIPTION

[0047] Hereinafter, the present invention will be described in detail, but the present invention is not limited to the following embodiments, and can be arbitrarily deformed and implemented without departing from the scope of the gist of the present invention. In addition, the " to " representing a numerical range is used to include the numerical value recorded before and after it as the meaning of the lower limit and the upper limit.

[0048] The manufacturing method of the present invention is a manufacturing method of a sulfide-based solid electrolyte, comprising the step of heating and melting a raw material in an atmosphere containing sulfur, wherein the raw material contains Li and SO 4 The lithium source is obtained by mixing the aqueous solution of SO 4 The ratio to the above-mentioned Li is 0.1 mol% or more.

[0049] (Sulfide-based solid electrolyte)

[0050] In the method for manufacturing a sulfide-based solid electrolyte according to an embodiment of the present invention (hereinafter also referred to as the present manufacturing method), the type and composition of the manufactured sulfide-based solid electrolyte are not particularly limited and can be appropriately selected according to the application, desired physical properties, etc. The sulfide-based solid electrolyte manufactured by the present manufacturing method contains at least lithium and sulfur. As a sulfide-based solid electrolyte, more specifically, for example, a sulfide-based solid electrolyte containing Li, P and S, a sulfide-based solid electrolyte containing Li, P, S and Ha, etc. can be cited. Here, Ha represents at least one element selected from the halogen elements. Specifically, Ha is, for example, at least one element selected from F, Cl, Br and I. In order to obtain a thiourea-type crystal structure, as Ha, it is more preferred to contain at least one of Cl and Br, further preferably to contain Cl, and further preferably a Cl single substance or a mixture of Cl and Br.

[0051] The sulfide-based solid electrolyte may be an amorphous sulfide-based solid electrolyte, a sulfide-based solid electrolyte having a specific crystal structure, or a sulfide-based solid electrolyte including a crystalline phase and an amorphous phase, depending on its purpose.

[0052] From the viewpoint of improving lithium ion conductivity, the sulfide-based solid electrolyte preferably contains a crystal structure. When the sulfide-based solid electrolyte contains a crystal structure, the crystal contained in the sulfide-based solid electrolyte is preferably an ion-conducting crystal. Specifically, the ion-conducting crystal refers to a crystal having a lithium ion conductivity preferably greater than 10 -4 S / cm, more preferably greater than 10 -3 S / cm crystals.

[0053] As the sulfide-based solid electrolyte, more specifically, Li 10 G 2 S 12 The sulfide-based solid electrolyte of LGPS type crystals, including Li 6 PS 5 Cl 1 Sulfide solid electrolytes of Argentite type crystals, Li-P-S-Ha type glass-ceramics, and Li 7 P 3 S 11 The sulfide-based solid electrolyte may also be an electrolyte composed of these, or an electrolyte containing crystals of various compositions and different crystal structures. From the viewpoint of excellent lithium ion conductivity, the sulfide-based solid electrolyte is preferably a sulfide-based solid electrolyte containing argyrodite-type crystals.

[0054] When the sulfide-based solid electrolyte includes crystals, the crystal structure preferably includes argyrodite from the viewpoint of the symmetry of the crystal structure. Crystals with high symmetry have lithium ion conduction paths that easily expand three-dimensionally and are preferred when molding powders.

[0055] In order to obtain an argyrodite-type crystal structure, the crystal phase contains Ha in addition to Li, P and S. Ha more preferably contains at least one of Cl and Br, further preferably contains Cl, and further preferably contains a single substance of Cl or a mixture of Cl and Br.

[0056] Argentum-type crystals are defined as follows: containing Li, P, S and Ha, and having peaks at 2θ=15.7±0.5° and 30.2±0.5° in an X-ray powder diffraction (XRD) pattern. In addition to the above, the XRD pattern preferably also has a peak at 2θ=18.0±0.5°, and more preferably has a peak at 2θ=25.7±0.5°.

[0057] The sulfide-based solid electrolyte obtained by the present production method may contain impurities derived from a lithium source described later. Examples of such impurities include Li 2 SO 4 , Li 2 PO 4 、Al 2 O 3 、LiF、AlF 3 In addition, various elements derived from impurities in the lithium source may be mixed into the sulfide solid electrolyte crystal or exist in an amorphous state. For example, these may be contained in a total of 0 to 10% by mass, preferably 0 to 5% by mass, in the sulfide-based solid electrolyte.

[0058] It should be noted that by including F in the sulfide-based solid electrolyte, the oxidation resistance of the sulfide-based solid electrolyte may be improved. From this viewpoint, the sulfide-based solid electrolyte may contain 0.01 mol% to 10 mol% of F element relative to the Li element, preferably 0.1 mol% to 5 mol%. Here, the content of the F element relative to the Li element may be 0.01 mol% or more, preferably 0.1 mol% or more, and may be 10 mol% or less, preferably 5 mol% or less.

[0059] In addition, in Al 2 O 3 In the case where Al is contained in the form of Li, the lithium ion conductivity may be improved by promoting the crystallization of the sulfide solid electrolyte. From this viewpoint, the sulfide solid electrolyte may contain 0.01 mol% to 10 mol% of Al element relative to the Li element, and preferably contains 0.1 mol% to 5 mol%. Here, the content of the Al element relative to the Li element may be 0.01 mol% or more, preferably 0.1 mol% or more, and may be 10 mol% or less, preferably 5 mol% or less.

[0060] The composition of the sulfide-based solid electrolyte can be determined by composition analysis using, for example, ICP emission spectrometry, atomic absorption spectrometry, ion chromatography, etc. In addition, the types of crystals contained in the sulfide-based solid electrolyte can be analyzed by X-ray powder diffraction (XRD).

[0061] (raw material)

[0062] The raw materials used in the present production method can use known raw materials as the raw materials of the above-mentioned various sulfide-based solid electrolytes. For example, in the case where the sulfide-based solid electrolyte contains Li, P and S, the raw materials contain lithium element (Li), sulfur element (S) and phosphorus element (P). As such raw materials, substances (components) containing Li such as Li simple substance and compounds containing Li; substances (components) containing S such as S simple substance and compounds containing S; substances (components) containing P such as P simple substance and compounds containing P can be used in appropriate combination. The compound containing Li, the compound containing S and the compound containing P can also be compounds containing two or more selected from Li, S and P at the same time. For example, as a compound serving as both a compound containing S and a compound containing P, phosphorus pentasulfide (P) can be cited. 2 S 5 )wait.

[0063] Examples of the substance containing Li include lithium sulfide (Li 2 S), lithium carbonate (Li 2 CO 3 ), lithium oxide (Li 2 O), lithium compounds such as lithium hydroxide (LiOH) and lithium halide (LiHa), metallic lithium, etc. From the viewpoint of easy handling, lithium sulfide is preferably used.

[0064] On the other hand, since lithium sulfide is expensive, from the viewpoint of reducing the manufacturing cost of sulfide-based solid electrolytes, it is preferred to use lithium compounds other than lithium sulfide, metallic lithium, etc. Specifically, in this case, the raw material preferably contains a lithium compound selected from metallic lithium, lithium carbonate (Li 2 CO 3 ), lithium oxide (Li 2 In the present manufacturing method, the raw material comprises a substance containing Li, and the substance containing Li comprises a lithium source obtained by a predetermined method described later.

[0065] Examples of the substance containing S include phosphorus trisulfide (P 2 S 3 ), phosphorus pentasulfide (P 2 S 5 ) and other phosphorus sulfides, other sulfur compounds containing phosphorus, elemental sulfur, and compounds containing sulfur. Examples of compounds containing sulfur include H 2 S.C.S. 2 , iron sulfide (FeS, Fe 2 S 3 , FeS 2 , Fe 1-xS, etc.), bismuth sulfide (Bi 2 S 3 ), copper sulfide (CuS, Cu 2 S, Cu 1-x From the viewpoint of suppressing the inclusion of elements other than the elements constituting the target sulfide-based solid electrolyte, the substance containing S is preferably phosphorus sulfide, and more preferably phosphorus pentasulfide (P 2 S 5 ). These substances may be used alone or in combination of two or more. It should be noted that phosphorus sulfide is considered to be a compound having both a substance containing S and a substance containing P.

[0066] Examples of substances containing P include phosphorus trisulfide (P 2 S 3 ), phosphorus pentasulfide (P 2 S 5 ) and other phosphorus sulfide, sodium phosphate (Na 3 PO 4 ) and phosphorus compounds and elemental phosphorus. From the viewpoint of suppressing the inclusion of elements other than the elements constituting the target sulfide-based solid electrolyte, the substance containing P is preferably phosphorus sulfide, and more preferably phosphorus pentasulfide (P 2 S 5 ). These substances may be used alone or in combination of two or more.

[0067] In the present production method, the raw material can be obtained by appropriately mixing the above substances according to the composition of the target sulfide-based solid electrolyte. The mixing ratio is not particularly limited. For example, the molar ratio Li / P of Li and P in the raw material is preferably 65 / 35 or more, more preferably 70 / 30 or more. In addition, the above molar ratio Li / P is preferably 88 / 12 or less.

[0068] As an example of a preferred combination of the above compounds, Li 2 S and P 2 S 5 The combination of Li 2 S and P 2 S 5 When Li and P are combined, the molar ratio Li / P is preferably 65 / 35 to 88 / 12, and more preferably 70 / 30 to 88 / 12. 2 S 5 Relative to Li 2 S is less, so it is easy to suppress the 2 S 5 The boiling point is lower than Li 2 The melting point of S causes the separation of sulfur and phosphorus during heat treatment.

[0069] The raw material of the present production method may further contain substances (compounds, etc.) other than the above substances, depending on the composition of the target sulfide-based solid electrolyte or as additives.

[0070] For example, in the case of manufacturing a sulfide-based solid electrolyte containing a halogen element such as F, Cl, Br or I, the raw material preferably contains a halogen element (Ha). In this case, the raw material preferably contains a compound of a halogen element. As a compound containing a halogen element, lithium halides such as lithium fluoride (LiF), lithium chloride (LiCl), lithium bromide (LiBr), lithium iodide (LiI), phosphorus halides, phosphoryl halides, sulfur halides, sodium halides, boron halides, etc. can be cited. As a compound containing a halogen element, from the viewpoint of suppressing the presence of elements other than the elements constituting the target sulfide-based solid electrolyte, lithium halides are preferred, and LiCl, LiBr, and LiI are more preferred. These compounds can be used alone or in combination of two or more.

[0071] It should be noted that the lithium halide may be a compound containing Li. When the raw material contains the lithium halide, a part or all of the Li in the raw material may be derived from the lithium halide.

[0072] When the raw material contains a halogen element, the molar equivalent of Ha relative to P in the raw material is preferably 0.2 to 4 molar equivalents, and more preferably 0.5 to 3 molar equivalents. Here, from the viewpoint of lowering the melting point when the raw material is heated and melted, the molar equivalent of Ha is preferably 0.2 molar equivalents or more, and more preferably 0.5 molar equivalents or more. In addition, from the viewpoint of improving the stability of the obtained sulfide-based solid electrolyte, the molar equivalent of Ha is preferably 4 molar equivalents or less, and more preferably 3 molar equivalents or less.

[0073] From the viewpoint of improving the glass formation state of the obtained sulfide-based solid electrolyte, the raw material preferably further contains SiS 2 , B 2 S 3 ,GeS 2 、Al 2 S 3 By making glass formation easier, when glass is obtained by rapid cooling, glass can be obtained even if the cooling rate is reduced, and the equipment load can be reduced. In addition, from the viewpoint of imparting moisture resistance to the sulfide-based solid electrolyte, it is also preferred to include SiO 2 , B 2 O 3 ,GeO 2 、Al 2 O 3 , P 2 O 5 These compounds may be used alone or in combination of two or more.

[0074] The addition amount of these compounds is preferably 0.1 to 50% by weight, more preferably 0.5 to 40% by weight relative to the total amount of the raw materials. Here, the above-mentioned addition amount is preferably 0.1% by weight or more, more preferably 0.5% by weight or more relative to the total amount of the raw materials. In addition, the addition amount is preferably 50% by weight or less, more preferably 40% by weight or less.

[0075] As raw materials, the above-mentioned various substances can be used in combination. As raw materials, when a plurality of substances are combined, for example, a known mixer or the like can be used to mix the raw materials. As mixers, for example, a V-type mixer, a W-type mixer, a ribbon mixer or the like can be used.

[0076] In the present manufacturing method, a sulfide-based solid electrolyte can be obtained by heating and melting the raw materials, but the raw materials can also be heat-treated in advance before heating and melting. Since the composition of the raw materials can be heated and melted from a state closer to the target composition after heat treatment, it is easy to control the composition. It should be noted that part of the raw materials can also be heat-treated and then mixed with the remaining raw materials for use. The heat-treated raw materials can contain, for example, Li 4 P 2 S 6 , Li 3 PS 4 and the like, compounds containing Li, P and S. The conditions for the heat treatment are not particularly limited, but for example, it is preferably maintained at a temperature of 100 to 500° C. for 0.1 to 5 hours.

[0077] (Lithium source)

[0078] The raw materials used in the production method include Li and SO 4 The lithium source is obtained by an aqueous solution, and the SO 4 The ratio to Li is 0.1 mol% or more.

[0079] The sulfide-based solid electrolyte obtained by the present production method contains at least lithium as described above. Therefore, the raw material contains the above-mentioned substance (component) containing Li. Furthermore, the raw material contains the above-mentioned lithium source as at least a part of the substance (component) containing Li.

[0080] The lithium source can be obtained from a mixture containing Li and SO 4 AndSO 4 The aqueous solution (hereinafter sometimes referred to as "specific aqueous solution") in which the ratio of Li to the aqueous solution is 0.1 mol% or more.

[0081] It should be noted that this means the following. That is, the lithium source obtained from the specific aqueous solution refers to a lithium source obtained without a process of concentrating the lithium element in the aqueous solution by membrane separation or the like, or a process of removing components other than components containing the lithium element, until the lithium source is obtained from the specific aqueous solution. In other words, the aqueous solution before obtaining the lithium source contains Li and SO in the sense that the aqueous solution does not include a high-purification treatment of the aqueous solution by membrane separation or the like. 4 , and SO 4 If the ratio of Li to Li is 0.1 mol% or more, the lithium source is a lithium source obtained from a specific aqueous solution. This does not necessarily mean that the specific aqueous solution has not been subjected to a high-purification treatment of the aqueous solution. In other words, it is also possible to consider that the aqueous solution obtained by a process such as membrane separation in advance is equivalent to the specific aqueous solution.

[0082] Examples of a method for obtaining a lithium source from a specific aqueous solution include a method of directly obtaining a solid lithium compound from the specific aqueous solution and a method of further synthesizing a lithium compound using the solid lithium compound obtained from the specific aqueous solution.

[0083] Examples of lithium compounds directly obtained from the specific aqueous solution include lithium hydroxide (LiOH), lithium carbonate (Li 2 CO 3 ), lithium halide (LiHa), etc.

[0084] Lithium hydroxide can be obtained, for example, by a method of directly evaporating a specific aqueous solution.

[0085] In addition, lithium carbonate can be obtained, for example, by blowing carbonic acid into a specific aqueous solution and precipitating it. The precipitated lithium carbonate can be recovered by a natural drying method, a method of drying and solidifying by heating, a solid-liquid separation method such as precipitation separation. Alternatively, it can be obtained by adding a carbonate such as sodium carbonate to precipitate lithium carbonate, and the obtained lithium carbonate is recovered by solid-liquid separation such as precipitation separation. In the case of obtaining lithium carbonate by blowing carbonic acid into a specific aqueous solution to precipitate it, it is preferred to blow carbonic acid to a pH of about 5 to 9. In addition, in order to make lithium carbonate easy to precipitate, it is preferred to heat the specific aqueous solution, and the temperature is preferably 80°C to 100°C, and more preferably 80°C to 95°C. In addition, for lithium halides, such as lithium chloride, for example, can be synthesized by mixing a specific aqueous solution with hydrochloric acid and drying it.

[0086] When a solid lithium compound obtained from a specific aqueous solution is used to further synthesize a lithium compound, examples of the lithium compound obtained include lithium hydroxide and lithium sulfide (Li 2 S), lithium halide (LiHa), etc. Here, Ha represents at least one element selected from halogen elements.

[0087] Lithium hydroxide is synthesized by, for example, a method of reacting calcium hydroxide with the above-mentioned lithium carbonate.

[0088] Lithium sulfide is synthesized by, for example, reacting the above-mentioned lithium hydroxide or lithium carbonate with a gas containing sulfur element such as hydrogen sulfide.

[0089] The lithium halide is synthesized, for example, by reacting the above-mentioned lithium hydroxide or lithium carbonate with a hydrohalic acid. For example, lithium bromide can be synthesized by reacting lithium carbonate with hydrobromic acid.

[0090] The specific type of the lithium source is not particularly limited depending on the type of the sulfide-based solid electrolyte to be produced, but lithium sulfide and lithium halide are preferred from the viewpoint of easy handling and easy synthesis.

[0091] In addition, the lithium source obtained from the specific aqueous solution may contain impurities derived from components in the specific aqueous solution in addition to the above-mentioned lithium compounds. Examples of such impurities include Li 2 SO 4 , Li 2 PO 4 、Al 2 O 3 、LiF、AlF 3 The lithium source may contain these in total, for example, 0 to 10% by mass, or 0 to 5% by mass.

[0092] In addition, the lithium source may contain 0.1 mol% to 2 mol% of SO 4 , preferably 0.1 mol% to 1 mol%. Here, relative to the SO 4 The content of SO in the lithium source may be 0.1 mol% or more, and may be 2 mol% or less, and preferably 1 mol% or less. 4 It refers to Li 2 SO 4 SO 4 etc. from SO in aqueous solution 4 (SO 4 2- ) and SO 4 .

[0093] It should be noted that the oxidation resistance of the sulfide-based solid electrolyte may be improved by including F in the sulfide-based solid electrolyte. 2 O 3In the case where Al is contained in the form of, the lithium ion conductivity may be improved by promoting the crystallization of the sulfide solid electrolyte. From this viewpoint, the lithium source may contain 0.01 mol% to 10 mol% of Al element relative to the Li element, preferably 0.1 mol% to 5 mol%. Here, the content of the Al element relative to the above-mentioned Li element may be 0.01 mol% or more, preferably 0.1 mol% or more, and may be 10 mol% or less, preferably 5 mol% or less. In addition, similarly, from the above viewpoint, the lithium source may contain 0.01 mol% to 10 mol% of F element relative to the Li element, preferably 0.1 mol% to 5 mol%. Here, the content of the F element relative to the above-mentioned Li element may be 0.01 mol% or more, preferably 0.1 mol% or more, and may be 10 mol% or less, preferably 5 mol% or less.

[0094] (Specific aqueous solution)

[0095] As mentioned above, the specific aqueous solution contains Li and SO 4 AndSO 4 An aqueous solution having a ratio of Li of 0.1 mol% or more. The specific aqueous solution typically includes an aqueous solution containing an extract obtained by immersing a treated material of a used lithium ion secondary battery in water (hereinafter sometimes simply referred to as an "extract").

[0096] That is, if the treated product obtained by calcining a used lithium ion secondary battery is immersed in water, lithium elements (lithium ions) can be separated from non-aqueous metal elements such as Co, Mn, and Ni and extracted into water. On the other hand, impurities from various materials contained in the lithium ion secondary battery can be extracted together with the lithium element in water. As one of them, SO 4 , which comes from, for example (CF 3 SO 2 ) 2 NLi, (C 2 F 5 SO 2 ) 2 NLi and other electrolyte additives. It was previously considered difficult to obtain SO containing more than a certain ratio relative to Li. 4 A lithium source is directly obtained from an aqueous solution of sulfide and used as a material for lithium ion secondary batteries. In addition, according to the inventors, this is also the case when focusing on the production of sulfide-based solid electrolytes. That is, if SO containing a predetermined ratio or more relative to Li 4If a lithium source is obtained directly from an aqueous solution and a raw material containing the lithium source is used in a general solid phase reaction method, synthesis does not proceed due to impurities hindering the reaction, the reaction takes time or homogeneous synthesis cannot be performed, and therefore the properties of the obtained sulfide-based solid electrolyte are sometimes insufficient.

[0097] In contrast, the present inventors have conducted intensive research and found that, according to the method of heating and melting the raw materials in an atmosphere containing sulfur, even if the raw materials contain a certain amount of sulfur derived from SO 4 Even when there are impurities of elemental sulfur, the influence of impurities can be suppressed, and a sulfide-based solid electrolyte with excellent lithium ion conductivity can be obtained, thereby completing the present invention. The reason is considered to be as follows: when the raw material is heated and melted in an atmosphere containing sulfur, SO in the melt 4 At least part of the sulfur dioxide generated by the reaction with sulfur excessively present in the melt or in the atmosphere containing sulfur elements to form gaseous sulfur dioxide is derived from SO 4 The impurities are removed. The reaction is represented by the following reaction formula.

[0098] SO 4 +S → 2SO 2 ↑

[0099] In addition, it is believed that the reaction in the melt produces a bubbling effect, which makes the melt more uniform. If the melt becomes more uniform, the resulting sulfide-based solid electrolyte will also become more uniform, and the lithium ion conductivity can be expected to be improved.

[0100] Therefore, it has been considered difficult to reuse an aqueous solution containing impurities of a predetermined amount or more such as a specific aqueous solution without separation of impurities and concentration of lithium components by membrane separation, but according to the present invention, a lithium source obtained using a specific aqueous solution can be directly used as a raw material to produce a sulfide-based solid electrolyte. Therefore, lithium can be efficiently reused without high purification treatment by membrane separation or the like.

[0101] In a specific aqueous solution, SO 4 The ratio of SO to Li is 0.1 mol% or more, preferably 0.1 to 10 mol%, more preferably 0.5 to 5 mol%, and further preferably 1 to 2 mol%. 4 The ratio of SO in the aqueous solution is 0.1 mol% or more, preferably 0.5 mol% or more, and more preferably 1 mol% or more. This makes it easier to handle the extract obtained by immersing the treated material of the used lithium ion secondary battery in water, and it is easier to reuse lithium more efficiently. On the other hand, from the viewpoint of suppressing the excessive amount of sulfur element required in the heating and melting step described later, the SO in the specific aqueous solution is 0.1 mol% or more, preferably 0.5 mol% or more, and more preferably 1 mol% or more. 4The ratio to Li is preferably 10 mol % or less, more preferably 5 mol % or less, and further preferably 2 mol % or less.

[0102] The specific aqueous solution preferably further contains Al. The ratio of Al to Li is preferably 0.01 to 5 mol%, more preferably 0.1 to 2 mol%, and further preferably 0.3 to 1 mol%. Among them, Al is a component that can be contained in the extract from the electrode of a lithium ion secondary battery, etc. In addition, when the specific aqueous solution contains Al, the lithium source obtained from the specific aqueous solution may contain Al. 2 O 3 , but Al 2 O 3 Oxides such as Al and Li sometimes improve the crystallinity of sulfide-based solid electrolytes. From these viewpoints, in the specific aqueous solution, the ratio of Al to Li is preferably 0.01 mol% or more, preferably 0.1 mol% or more, and more preferably 0.3 mol% or more. On the other hand, from the viewpoint of easy preparation of a specific aqueous solution, the ratio of Al to Li in the specific aqueous solution is preferably 5 mol% or less, more preferably 2 mol% or less, and further preferably 1 mol% or less.

[0103] The Al in the specific aqueous solution is not limited to Al derived from the extract, and may be Al intentionally added in order to obtain the above-mentioned effect.

[0104] The specific aqueous solution preferably further contains F. The ratio of F to Li is preferably 0.01 to 15 mol%, more preferably 0.1 to 10 mol%, and further preferably 1 to 5 mol%. Here, F is LiPF derived from a lithium ion secondary battery. 6 Ingredients that can be included in the extract by electrolytes such as F. In addition, by making the sulfide-based solid electrolyte contain F, the oxidation resistance of the sulfide-based solid electrolyte is sometimes improved. From these viewpoints, in the specific aqueous solution, the ratio of F to Li is preferably 0.01 mol% or more, preferably 0.1 mol% or more, and more preferably 1 mol% or more. On the other hand, the ratio of F to Li in the specific aqueous solution is preferably 15 mol% or less, more preferably 10 mol% or less, and further preferably 5 mol% or less from the viewpoint of ease of preparation.

[0105] The F in the specific aqueous solution is not limited to the F derived from the extract, and may be F intentionally added in order to obtain the above-mentioned effect.

[0106] That is, the specific aqueous solution preferably further contains at least one of Al and F, and in the specific aqueous solution, the ratio of Al to Li or the ratio of F to Li is preferably 0.01 mol% or more. According to the present production method, in addition to melting the raw materials, the above-mentioned bubbling effect can be obtained, so when it is desired to contain at least one of Al and F in the sulfide-based solid electrolyte, it can be contained more uniformly.

[0107] The specific aqueous solution may be composed of an extract obtained by immersing a treated material of a used lithium ion secondary battery in water, or may be an aqueous solution containing the extract.

[0108] For example, the specific aqueous solution may be selected from SO 4 , Al and F and Li content ratio of one or more components. As a method for adjusting the content of SO 4 , Al and F and Li content ratio of one or more components, for example, a method of adding a substance containing Al, a substance containing F, a substance containing Li, etc. to the extract, a method of mixing the extract with a solution having a different concentration of a specific component than the extract.

[0109] It should be noted that the above-mentioned extract may contain LiPF 6 Isolyte and PO 4 However, according to the present production method, it can be considered that even if the raw material contains PO 4 impurities, and can also suppress their influence, and can obtain a sulfide-based solid electrolyte with excellent lithium ion conductivity. 4 When impurities are present, the homogenization of the melt may be hindered or the synthesis of the sulfide-based solid electrolyte may be hindered. In contrast, in the present manufacturing method, the bubbling effect is generated during the heating and melting process, which promotes the homogenization of the melt, thereby eliminating or suppressing the impurities from PO. 4 Therefore, in a specific aqueous solution, PO 4 The content ratio of Li can be, for example, 0.1 mol % or more relative to Li.

[0110] Li and SO contained in specific aqueous solution 4 , Al, F and PO 4 The various components such as Li and SO are typically contained in a specific aqueous solution in the form of ions. The form of the ions is not particularly limited, and each component may form an ion alone or a complex ion. For example, Li, SO 4 , Al, F and PO 4 In a specific aqueous solution, it can be Li + 、SO 42- 、Al(OH) 4 - 、F - and PO 4 3- .

[0111] (Composition containing lithium halide)

[0112] The above-mentioned (raw materials), (lithium source) and (specific aqueous solution) have described in detail the raw materials used for producing the sulfide-based solid electrolyte. The present invention also relates to a composition containing a lithium halide.

[0113] That is, the lithium halide-containing composition according to the present embodiment is a composition containing lithium halide and containing 10% by mass or less of SO 4 , used to manufacture sulfide-based solid electrolytes.

[0114] The above-mentioned lithium halide-containing composition is effective as a lithium source, but in addition, it can also be used as a halogen-containing raw material, a S-containing raw material, or a raw material containing both.

[0115] As the lithium halide, as described above, LiCl, LiBr, and LiI are more preferred. These compounds may be used alone or in combination of two or more.

[0116] The composition contains less than 10% by mass of SO 4 , preferably 0.01 to 10 mass %, more preferably 0.02 to 5 mass %, and still more preferably 0.03 to 5 mass %. Here, from the viewpoint of avoiding excessive reduction in the amount of lithium halide component in the composition, SO 4 The content of SO is 10% by mass or less, preferably 5% by mass or less. 4 From the perspective of the homogenization effect brought by SO 4 The content of is preferably 0.01% by mass or more, more preferably 0.02% by mass or more, and further preferably 0.03% by mass or more.

[0117] It should be noted that the above SO 4 The content of SO is the same as described above (specific aqueous solution), 4The ratio of SO to Li is preferably 0.1 to 10 mol%, more preferably 0.5 to 5 mol%, and further preferably 1 to 2 mol%. Here, the above ratio is preferably 0.1 mol% or more, more preferably 0.5 mol% or more, and further preferably 1 mol% or more. As a result, it is easy to simplify the treatment of the extract obtained by immersing the treated material of the used lithium ion secondary battery in water, and it is easy to reuse lithium more efficiently. On the other hand, from the viewpoint of suppressing the amount of sulfur element required in the heating and melting process described later from becoming excessive, SO 4 The ratio to Li is preferably 10 mol % or less, more preferably 5 mol % or less, and further preferably 2 mol % or less.

[0118] It should be noted that SO 4 It refers to Li 2 SO 4 SO 4 etc. from SO in aqueous solution 4 (SO 4 2- ) and the substances contained.

[0119] In the composition containing lithium halide, the halogen element constituting the lithium halide is a halogen element other than F, and preferably further contains at least one of Al and F. Here, the lithium halide whose constituting halogen element is a halogen element other than F is preferably LiCl, LiBr, or LiI, for example.

[0120] Al is a component that may be contained in the extract from the electrode of a lithium ion secondary battery. 2 O 3 Oxides such as these may improve the crystallinity of the sulfide-based solid electrolyte.

[0121] F is LiPF from lithium-ion secondary battery 6 In addition, the inclusion of F may improve the oxidation resistance of the sulfide-based solid electrolyte.

[0122] In the above-mentioned composition containing lithium halide, the ratio of Al to Li is preferably 0.01 to 5 mol%, more preferably 0.1 to 2 mol%, and further preferably 0.3 to 1 mol%. Here, the ratio of Al is preferably 0.01 mol% or more, preferably 0.1 mol% or more, and more preferably 0.3 mol% or more. On the other hand, from the viewpoint of avoiding excessive reduction of the amount of lithium halide component in the composition, the ratio of Al to Li is preferably 5 mol% or less, more preferably 2 mol% or less, and further preferably 1 mol% or less.

[0123] In the above-mentioned composition containing lithium halide, the ratio of F to Li is preferably 0.01 to 15 mol%, more preferably 0.1 to 10 mol%, and further preferably 1 to 5 mol%. Here, the ratio of F is preferably 0.01 mol% or more, preferably 0.1 mol% or more, and more preferably 1 mol% or more. On the other hand, from the viewpoint of easy preparation, the ratio of F to Li is preferably 15 mol% or less, more preferably 10 mol% or less, and further preferably 5 mol% or less.

[0124] (Composition containing lithium sulfide)

[0125] The above-mentioned (raw material), (lithium source), and (specific aqueous solution) describe in detail the raw materials used for producing the sulfide-based solid electrolyte. The present invention also relates to a composition containing lithium sulfide.

[0126] That is, the lithium sulfide-containing composition according to the present embodiment is a composition containing lithium sulfide, and contains 10 mass % or less of SO 4 , used to manufacture sulfide-based solid electrolytes.

[0127] The above-mentioned composition containing lithium sulfide is effective as a lithium source, but in addition, it can also be used as a raw material containing S.

[0128] The composition contains more than 0.5 mass % and less than 10 mass % of SO 4 , preferably 0.51 to 5% by mass, more preferably 0.8 to 3% by mass. Here, from the viewpoint of avoiding excessive reduction of the lithium sulfide component in the composition, SO 4 The content of SO is 10% by mass or less, preferably 5% by mass or less, and more preferably 3% by mass or less. 4 From the perspective of the homogenization effect brought by SO 4 The content of is greater than 0.5% by mass, preferably 0.51% by mass or more, and more preferably 0.8% by mass or more.

[0129] It should be noted that the above SO 4 The content of SO is the same as described above (specific aqueous solution), 4 The ratio of SO to Li is preferably 0.1 to 10 mol%, more preferably 0.5 to 5 mol%, and further preferably 1 to 2 mol%. Here, the above ratio is preferably 0.1 mol% or more, more preferably 0.5 mol% or more, and further preferably 1 mol% or more. As a result, it is easy to simplify the treatment of the extract obtained by immersing the treated material of the used lithium ion secondary battery in water, and it is easy to reuse lithium more efficiently. On the other hand, from the viewpoint of suppressing the amount of sulfur element required in the heating and melting process described later from becoming excessive, SO 4The ratio to Li is preferably 10 mol % or less, more preferably 5 mol % or less, and further preferably 2 mol % or less.

[0130] It should be noted that SO 4 It refers to Li 2 SO 4 SO 4 etc. from SO in aqueous solution 4 (SO 4 2- ) and SO 4 .

[0131] The lithium sulfide-containing composition preferably further contains at least one of Al and F.

[0132] Al is a component that may be contained in the extract from the electrode of a lithium ion secondary battery. 2 O 3 Oxides such as these may improve the crystallinity of the sulfide-based solid electrolyte.

[0133] F is LiPF from lithium-ion secondary battery 6 In addition, the inclusion of F may improve the oxidation resistance of the sulfide-based solid electrolyte.

[0134] In the above-mentioned composition containing lithium sulfide, the ratio of Al to Li is preferably 0.01 to 5 mol%, more preferably 0.1 to 2 mol%, and even more preferably 0.3 to 1 mol%. Here, the ratio of Al is preferably 0.01 mol% or more, preferably 0.1 mol% or more, and even more preferably 0.3 mol% or more. On the other hand, from the viewpoint of avoiding an excessive decrease in the amount of lithium sulfide component in the composition, the ratio of Al to Li is preferably 5 mol% or less, more preferably 2 mol% or less, and even more preferably 1 mol% or less.

[0135] In the above-mentioned composition containing lithium sulfide, the ratio of F to Li is preferably 0.01 to 15 mol%, more preferably 0.1 to 10 mol%, and further preferably 1 to 5 mol%. Here, the ratio of F is preferably 0.01 mol% or more, preferably 0.1 mol% or more, and more preferably 1 mol% or more. On the other hand, from the viewpoint of easy preparation, the ratio of F to Li is preferably 15 mol% or less, more preferably 10 mol% or less, and further preferably 5 mol% or less.

[0136] (Method for producing sulfide-based solid electrolyte)

[0137] Figure 1is a flow chart illustrating the present production method. That is, the present production method at least includes step S11 of heating and melting the raw materials in a gas atmosphere containing sulfur. The raw materials used in step S11 include a raw material containing Li and SO 4 The lithium source is obtained by an aqueous solution of SO 4 The ratio of Li is 0.1 mol% or more. This step S11 corresponds to the heating and melting step described in detail later.

[0138] In addition, the present manufacturing method may further include using a mixture containing Li and SO 4 AndSO 4 A step of obtaining a lithium source from an aqueous solution having a ratio of Li to 0.1 mol % or more. Figure 2 This is a flowchart illustrating the present production method in this case. Figure 2 The manufacturing method exemplified in the above includes using a mixture containing Li and SO 4 AndSO 4 Step S21 of obtaining a lithium source from an aqueous solution having a ratio of Li to 0.1 mol % or more, and Step S22 of heating and melting the raw material including the lithium source obtained in Step S21 in a gas atmosphere containing sulfur.

[0139] In addition, the present production method further includes a step of preparing an aqueous solution used in step S21. Figure 3 This is a flowchart illustrating the present production method in this case. Figure 3 The manufacturing method exemplified in the above includes preparing a 4 AndSO 4 Step S31 of preparing an aqueous solution having a ratio of 0.1 mol% to Li or more, step S32 of obtaining a lithium source using the aqueous solution obtained in step S31, and step S33 of heating and melting the raw material containing the lithium source obtained in step S32 in a gas atmosphere containing sulfur. The specific method of step S31 is not particularly limited, for example, step S31 may include the steps of immersing the treated material of the used lithium ion secondary battery in water to obtain an extract, adjusting the extract to be selected from SO 4 , a step of determining the content ratio of one or more components of Al and F to Li, etc. When an extracting solution is used in step S31, the extracting solution may be prepared in advance.

[0140] (Heating and melting process)

[0141] The present production method includes the step of heating and melting the raw material including the above-mentioned lithium source in an atmosphere containing sulfur element (heating and melting step).

[0142] Heating and melting can be carried out by, for example, placing the raw materials in a heating furnace or a heat-resistant container and heating the heating furnace or the heat-resistant container. Alternatively, a heat-resistant container can be placed in the heating furnace and the raw materials can be placed in the heat-resistant container.

[0143] The heat-resistant container is not particularly limited, and examples thereof include heat-resistant containers made of carbon, heat-resistant containers containing oxides such as quartz, quartz glass, borosilicate glass, aluminosilicate glass, aluminum oxide, zirconium oxide, and mullite, heat-resistant containers containing nitrides such as silicon nitride and boron nitride, and heat-resistant containers containing carbides such as silicon carbide. In addition, these heat-resistant containers may be a main body formed of the above-mentioned materials, or may be a container formed with a layer of carbon, oxide, nitride, carbide, etc. In addition, heating may be performed in a vacuum-sealed state.

[0144] The method of feeding the raw materials into the heating furnace or heat-resistant container is not particularly limited and may be appropriately selected from known methods according to the desired production method, etc. The raw materials may be fed continuously in a fixed amount or intermittently in a predetermined amount.

[0145] In addition, the method of heating the heating furnace and the heat-resistant container is not particularly limited, and for example, a known heating method such as an external heating device can be used. Hereinafter, the containers used in the heating and melting process such as the heating furnace and the heat-resistant container are sometimes simply collectively referred to as the heating furnace.

[0146] The heating temperature in the heating and melting step is preferably 600°C to 900°C, preferably 650°C to 850°C, and more preferably 700°C to 800°C. Here, the heating temperature is preferably 600°C or higher, more preferably 650°C or higher, and more preferably 700°C or higher. By setting the heating temperature to the above value or higher, the raw material is easily melted, which is preferred. In addition, by setting the heating temperature to the above value or higher, SO 4 +S → 2SO 2 The heating temperature is preferably 900°C or lower, more preferably 850°C or lower, and further preferably 800°C or lower. The heating temperature is preferably below the above value because the amount of components separated from the raw material during heating and melting is less likely to be excessive.

[0147] The time for heating and melting is preferably 0.1 to 100 hours, more preferably 0.5 to 50 hours, further preferably 0.7 to 24 hours, and further preferably 1 to 24 hours. Here, from the viewpoint of improving the homogeneity of the melt and the obtained sulfide-based solid electrolyte, the time for heating and melting is preferably 0.1 hours or more, more preferably 0.5 hours or more, further preferably 0.7 hours or more, and further preferably 1 hour or more. In addition, as long as the degradation and decomposition of the components in the melt due to heating are within an allowable range, the upper limit of the time for heating and melting is not particularly limited and can be longer. As a practical range, it is preferably less than 100 hours, more preferably less than 50 hours, and further preferably less than 24 hours. As described above, heating and melting can be carried out continuously or batchwise.

[0148] The pressure during heating and melting is not particularly limited, but is preferably normal pressure or slightly increased pressure, and more preferably normal pressure.

[0149] The heating and melting step is performed in an atmosphere containing sulfur. By placing the melt obtained by melting the raw materials in a gas atmosphere containing sulfur, the SO in the melt can be reduced as described above. 4 (or PO 4 ) reacts with sulfur in the melt or in a gas atmosphere containing elemental sulfur and is removed as a gas. In addition, by heating and melting in a gas atmosphere containing elemental sulfur, it is possible to suppress the volatilization of sulfur components into a gas atmosphere containing elemental sulfur with a high sulfur partial pressure. Thus, it is easy to control the composition of the obtained sulfide-based solid electrolyte.

[0150] As a method for forming a gas atmosphere containing sulfur in the heating furnace, a method of introducing a component containing sulfur into the heating furnace can be cited. Specifically, at least one of a method of introducing a gas containing sulfur and a solid containing sulfur into the heating furnace and a method of mixing an excess amount of a solid containing sulfur into the raw material can be cited. When the component containing sulfur is introduced into the heating furnace, the timing may be after the raw material is previously placed in a container and heated to obtain a melt, or it may be performed simultaneously with the placement of the raw material in the container.

[0151] As a method for introducing the sulfur-containing gas, for example, a method of introducing the sulfur-containing gas prepared in advance outside the heating furnace into the heating furnace can be cited. The method for preparing the sulfur-containing gas outside the heating furnace is not particularly limited, and for example, it is preferred to heat a sulfur source outside the heating furnace to obtain the sulfur-containing gas.

[0152] The sulfur source is not particularly limited as long as it is a sulfur-containing gas obtained by heating, such as elemental sulfur or sulfur compounds. Examples thereof include elemental sulfur, hydrogen sulfide, organic sulfur compounds such as carbon disulfide, iron sulfide (FeS, Fe 2 S3 , FeS 2 , Fe 1-x S, etc.), bismuth sulfide (Bi 2 S 3 ), copper sulfide (CuS, Cu 2 S, Cu 1-x S, etc.), polysulfides such as lithium polysulfide and sodium polysulfide, polysulfides, rubber vulcanized with sulfur, etc.

[0153] For example, these sulfur sources are heated in a separately provided sulfur source heating unit to generate a gas containing sulfur element, and N 2 An inert gas such as argon, helium, or the like is delivered into the heating furnace as a carrier gas, thereby forming a gas atmosphere containing sulfur element in the heating furnace.

[0154] The temperature for heating the sulfur source can be appropriately selected according to the type of sulfur source used. For example, when the sulfur source is elemental sulfur, the temperature for heating the sulfur source is preferably 200°C to 450°C.

[0155] Alternatively, a sulfur-containing solid may be introduced into the heating furnace to form a sulfur-containing gas atmosphere in the heating furnace. In this case, a sulfur-containing gas atmosphere may be obtained by heating the sulfur-containing solid in the heating furnace. Examples of the sulfur-containing solid include elemental sulfur, H 2 S.Bi 2 S 3 , iron sulfide, copper sulfide, CS 2 For example, the solid sulfur source can be introduced into the heating furnace by conveying the solid sulfur source in a fine state such as powder to the heating part through a carrier gas.

[0156] Alternatively, a gas atmosphere containing sulfur element can be formed in the heating furnace by mixing an excess amount of a solid containing sulfur element into the raw material. In this case, a gas containing sulfur element can be obtained by heating a solid containing sulfur element in a heating furnace to form a gas atmosphere containing sulfur element. As the solid containing sulfur element, the same substance as in the case of introducing a solid containing sulfur element into the heating furnace can be used. It should be noted that mixing an excess amount of a solid containing sulfur element into the raw material means that when the composition ratio of each element in the raw material is adjusted by considering only the desired composition of the sulfide-based solid electrolyte, a solid containing sulfur element is mixed into the raw material in such a way that the ratio of sulfur element is excessive.

[0157] In the sulfur-containing gas atmosphere, the sulfur partial pressure is preferably set to 10 -3 ~10 0By achieving this sulfur partial pressure, sulfur can be introduced efficiently at low cost without complicating the equipment.

[0158] In the heating furnace, the dew point is preferably -20°C or lower from the viewpoint of preventing side reactions with water vapor, oxygen, etc. The lower limit is not particularly limited, but is generally about -80°C. In addition, the oxygen concentration is preferably 1000 ppm (volume basis) or lower.

[0159] (Cooling process)

[0160] The present manufacturing method preferably further includes a step of cooling the melt obtained by heating and melting to obtain a solid. The cooling can be performed using a known method, and the method is not particularly limited. After the heating and melting step, the melt can be continued to cool in the heating furnace, or the melt can be taken out of the heating furnace for cooling. When the melt is taken out of the heating furnace for cooling, the melt is discharged from the above-mentioned sulfide-based solid electrolyte discharge portion, for example.

[0161] As a more specific cooling method, for example, a method of cooling the molten metal by flowing out onto a plate-like body such as carbon, a method of thinly molding the molten metal by pouring the molten metal into a narrow gap, etc. can be cited. In the case of cooling the molten metal by flowing out onto a plate-like body, from the viewpoint of improving the cooling efficiency, the thickness of the molten metal after flowing out and the obtained solid is preferably thinner. Specifically, the thickness is preferably less than 10 mm, more preferably less than 5 mm. The lower limit of the thickness is not particularly limited, and may be more than 0.01 mm, or more than 0.02 mm. In the case of thinly molding by pouring into a narrow gap, the cooling efficiency is excellent, and a flaky molded body, a fibrous molded body, a powdery molded body, etc. can be obtained. The obtained solid is crushed to a size that is easy to handle, and any shape can be obtained. Among them, it is preferred to obtain a block-like solid that is easy to recycle. Blocks also include plate-like, flaky or fibrous situations.

[0162] From the viewpoint of maintaining the composition obtained by the heating and melting process, the cooling rate is preferably 0.01°C / sec or more, more preferably 0.05°C / sec or more, and further preferably 0.1°C / sec or more. In addition, the upper limit of the cooling rate is not particularly limited, but it is generally believed that the cooling rate of the twin rolls with the fastest rapid cooling rate is 1,000,000°C / sec or less.

[0163] Here, in the case of making the obtained solid an amorphous sulfide-based solid electrolyte, it is preferred to quench the melt obtained by heating and melting to obtain a solid. Specifically, the cooling rate during quenching is preferably 10°C / sec or more, more preferably 100°C / sec or more, further preferably 500°C / sec or more, and further preferably 700°C / sec or more. In addition, the upper limit of the cooling rate is not particularly limited, and it is generally believed that the cooling rate of the twin rolls with the fastest quenching rate is 1,000,000°C / sec or less.

[0164] On the other hand, during the cooling process, slow cooling is performed to crystallize at least a portion of the solid, and a sulfide-based solid electrolyte having a specific crystal structure or a sulfide-based solid electrolyte composed of a crystalline phase and an amorphous phase can also be obtained. The cooling rate during slow cooling is preferably 0.01 to 500°C / sec, and more preferably 0.05 to 450°C / sec. Here, the above cooling rate is preferably greater than 0.01°C / sec, and more preferably greater than 0.05°C / sec. In addition, the cooling rate is preferably less than 500°C / sec, and more preferably less than 450°C / sec. The cooling rate can be less than 10°C / sec, and can also be less than 5°C / sec. It should be noted that the cooling rate can be appropriately adjusted according to the conditions of crystallization.

[0165] Here, the crystal contained in the sulfide-based solid electrolyte is preferably an ion-conducting crystal. Specifically, the ion-conducting crystal refers to a crystal having a lithium ion conductivity greater than 10 -4 S / cm, more preferably greater than 10 -3 S / cm crystals.

[0166] When the solid obtained after cooling is to be a sulfide-containing solid electrolyte containing a crystalline phase, it is preferred that the melt obtained in the heating and melting step contains a compound that becomes a crystal nucleus. As a result, crystals are easily precipitated in the cooling step. The method of making the melt contain a compound that becomes a crystal nucleus is not particularly limited, and examples thereof include adding a compound that becomes a crystal nucleus to a raw material or a raw material heating material, and adding a compound that becomes a crystal nucleus to a melt being heated and melted.

[0167] Examples of the compound that serves as a crystal nucleus include oxides, oxynitrides, nitrides, carbides, other chalcogenides, halides, etc. The compound that serves as a crystal nucleus is preferably a compound that has a certain degree of compatibility with the melt. It should be noted that a compound that is completely incompatible with the melt cannot serve as a crystal nucleus.

[0168] In the case where the solid obtained after cooling is intended to be a sulfide-based solid electrolyte containing a crystalline phase, the content of the compound that becomes the crystal nucleus in the melt is preferably 0.01 to 20% by mass, more preferably 0.1 to 10% by mass, and further preferably 1 to 10% by mass. Here, the above content is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, and further preferably 1% by mass or more. On the other hand, from the viewpoint of suppressing the decrease in lithium ion conductivity, the content of the compound that becomes the crystal nucleus in the melt is preferably 20% by mass or less, and more preferably 10% by mass or less.

[0169] In the case of a sulfide-based solid electrolyte in which the solid obtained after cooling is to be amorphous, it is preferred that the melt does not contain a compound that becomes a crystal nucleus or its content is less than a specified amount. Specifically, the content of the compound that becomes a crystal nucleus in the melt is preferably 1% by mass or less, more preferably 0.1% by mass or less. The content of the compound that becomes a crystal nucleus in the melt may also be less than 0.01% by mass.

[0170] The present manufacturing method may further include a step of performing a known post-treatment on the sulfide-based solid electrolyte obtained by cooling the melt. As the post-treatment step, for example, there can be mentioned a step of further heat-treating the sulfide-based solid electrolyte from the viewpoint of obtaining desired properties or promoting crystallization, a step of pulverizing from the viewpoint of obtaining a desired shape, etc.

[0171] The lithium ion conductivity of the sulfide-based solid electrolyte obtained by the present production method varies depending on its composition and is not particularly limited. However, from the viewpoint of improving battery characteristics when used in a lithium ion secondary battery, it is preferably 2.0×10 -3 S / cm or more, more preferably 3.0×10 -3 S / cm or more, more preferably 4.0×10 -3 More preferably, when the sulfide-based solid electrolyte to be measured is made into a powder having an average particle size of 10 μm and pressed into a powder body under a pressure of 380 MPa, the lithium ion conductivity measured at 25° C. is within the above range.

[0172] According to the present manufacturing method, even when the raw material contains a predetermined amount of impurities such as those mentioned above, the influence of the impurities can be suppressed, and the sulfide-based solid electrolyte can be appropriately manufactured. Thus, the lithium source obtained from the aqueous solution containing lithium and impurities can be directly used as the raw material to manufacture the sulfide-based solid electrolyte, and there is no need to perform high-purification treatment of the aqueous solution using membrane separation, etc., so lithium can be efficiently reused. The sulfide-based solid electrolyte obtained by the present manufacturing method can be appropriately used as a solid electrolyte material for lithium-ion secondary batteries, for example.

[0173] Example

[0174] The present invention is specifically described below with reference to the following examples, but the present invention is not limited thereto. Examples 2, 4 to 15 are examples, and Examples 1 and 3 are comparative examples.

[0175] (Preparation of Extract)

[0176] The used lithium-ion secondary battery is calcined and the obtained product is immersed in water to obtain an extract. The extract contains Li, Al, F and SO 4 In the extract, the concentration of Li is 3017 mg / L, the concentration of Al is 80.3 mg / L, the concentration of F is 219.2 mg / L, and the concentration of SO 4 The concentration of SO in the extract is 305.7 mg / L. 4 The content ratio of O is 0.73 mol %, the content ratio of Al is 0.68 mol %, and the content ratio of F is 2.65 mol %.

[0177] (Example 1)

[0178] The extract was purified by using a lithium selective permeable membrane with reference to the method described in Patent Document 2 to obtain an impurity-free aqueous solution containing lithium. The aqueous solution was confirmed to contain no SO 4 , Al, F. It should be noted that the time required for the high-purification treatment was 14 days.

[0179] Lithium bromide is obtained as a lithium source from the above aqueous solution. Specifically, first, carbonic acid is blown into the aqueous solution to precipitate lithium in the form of lithium carbonate. The conditions during precipitation are about pH 7 and temperature 85°C. The precipitated lithium carbonate is recovered by solid-liquid separation. Then, the recovered lithium carbonate is reacted with hydrobromic acid to synthesize lithium bromide. Hydrobromic acid uses a 48% by mass aqueous solution made by Kanto Chemical. The obtained lithium bromide aqueous solution is added to a vibration drying device (trade name VH type, made by Central Chemical Machinery Co., Ltd.), and is heated and dried under reduced pressure at a maximum temperature of 160°C to obtain lithium bromide. The obtained lithium bromide is crushed into powder in a mortar.

[0180] Next, in a dry nitrogen atmosphere, to become Li 5.5 PS 4.3 Cl 0.8 Br 0.8 Lithium sulfide powder (manufactured by Sigma, purity 99.98%), phosphorus pentasulfide powder (manufactured by Sigma, purity 99%), lithium chloride powder (manufactured by Sigma, purity 99.99%) and synthesized lithium bromide powder were weighed in a composition ratio to prepare a mixture.

[0181] The mixture was placed in a heat-resistant container and heated to melt for 0.5 hours under the conditions of 1 atm and 750°C. At this time, sulfur gas obtained by heating elemental sulfur at 350°C was supplied so that the partial pressure of the sulfur gas was 0.1 atm, and N 2 A gas atmosphere containing sulfur element was obtained as a carrier gas, and sulfur was introduced into the melt by heating and melting in the gas atmosphere. The content of sulfur gas in the gas atmosphere containing sulfur element was 0.1 vol%.

[0182] Then, the solid is cooled at a cooling rate of 1 to 1000°C / sec to obtain a solid sulfide-based solid electrolyte including an amorphous phase and an argyrodite-type crystal phase. Next, the solid is crystallized at 450°C for 1 hour in a nitrogen atmosphere to obtain a sulfide-based solid electrolyte including argyrodite-type crystals.

[0183] (Example 2)

[0184] The extract was not subjected to high-purification treatment, and the same procedure as in Example 1 was followed to obtain a composition containing lithium bromide as a lithium source from the extract. Analysis confirmed that the obtained composition containing lithium bromide contained 0.17 mass % of SO 4 , 0.04 mass % Al, and 0.11 mass % F. The obtained lithium source was used as a raw material in the same manner as in Example 1, and a sulfide-based solid electrolyte containing argyrodite-type crystals was obtained by the same method as in Example 1.

[0185] (Example 3)

[0186] Lithium bromide was obtained as a lithium source from the extract in the same manner as in Example 1 except that the extract was not subjected to a high-purification treatment.

[0187] Next, in a dry nitrogen atmosphere, to become Li 5.5 PS 4.3 Cl 0.8 Br 0.8 Lithium sulfide powder (manufactured by Sigma, purity 99.98%), phosphorus pentasulfide powder (manufactured by Sigma, purity 99%), lithium chloride powder (manufactured by Sigma, purity 99.99%), and synthesized lithium bromide powder are weighed in a composition ratio. After mixing them in the same atmosphere using a mixer, they are further mixed using a planetary ball mill (manufactured by Ito Seisakusho Co., Ltd., LP-M2) to obtain a raw material mixture. The mixing using a planetary ball mill is carried out at 400 rpm for 20 hours using balls with a particle size of 10 mm. The obtained raw material mixture is vacuum-sealed in a quartz tube and the tube is sealed, and heated and calcined at 450°C for 5 hours, thereby precipitating argyrodite-type crystals to obtain a sulfide-based solid electrolyte containing argyrodite-type crystals.

[0188] (Example 4)

[0189] To the extract, a LiOH aqueous solution prepared from lithium hydroxide monohydrate (manufactured by Sigma, purity 99.95%) and distilled water was added, and the content ratio of each component relative to Li was adjusted to obtain an aqueous solution. In the obtained aqueous solution, the content of SO relative to Li 4 The content ratio of SO was 0.15 mol%, the content ratio of Al was 0.14 mol%, and the content ratio of F was 0.53 mol%. The same procedure as in Example 1 was performed except that this aqueous solution was used to obtain a composition containing lithium bromide as a lithium source. The obtained composition containing lithium bromide was confirmed by analysis to contain 0.03 mass % of SO 4 , 0.01 mass % Al, and 0.02 mass % F. The obtained lithium source was used as a raw material in the same manner as in Example 1, and a sulfide-based solid electrolyte containing argyrodite-type crystals was obtained by the same method as in Example 1.

[0190] (Example 5)

[0191] Hydrofluoric acid is added to the extract to obtain an aqueous solution having an adjusted content ratio of F to Li. In the obtained extract, SO 4 The content ratio of SO was 0.73 mol%, the content ratio of Al was 0.68 mol%, and the content ratio of F was 5.30 mol%. A composition containing lithium bromide was obtained in the same manner as in Example 1 except that the aqueous solution was used as a lithium source. The obtained composition containing lithium bromide was confirmed by analysis to contain 0.17 mass % of SO 4 , 0.04 mass % Al, and 0.21 mass % F. The obtained lithium source was used as a raw material in the same manner as in Example 1, and a sulfide-based solid electrolyte containing argyrodite-type crystals was obtained by the same method as in Example 1.

[0192] (Example 6)

[0193] Hydrobromic acid was directly added to the extract not subjected to high-purity treatment used in (Example 2) to prepare a lithium bromide aqueous solution. A 48% by mass aqueous solution of hydrobromic acid manufactured by Kanto Chemical was used. The obtained lithium bromide aqueous solution was added to a vibration drying device (trade name VH type, manufactured by Central Chemical Industry Co., Ltd.), and heated under reduced pressure and dried at a maximum temperature of 160° C., thereby obtaining a composition containing lithium bromide. The obtained composition containing lithium bromide was crushed into powder in a mortar.

[0194] The obtained lithium bromide-containing composition was confirmed to contain 0.78 mass % of SO 4, 0.20 mass % Al, and 0.56 mass % F. The obtained lithium source was used as a raw material in the same manner as in Example 1, and a sulfide-based solid electrolyte containing argyrodite-type crystals was obtained by the same method as in Example 1.

[0195] (Example 7)

[0196] SO was prepared using lithium hydroxide monohydrate (manufactured by Sigma, purity 99.95%), lithium sulfate (manufactured by Sigma, purity 99.99%), and distilled water. 4 A specific aqueous solution containing 0.10 mol% of Li. Hydrobromic acid is directly added to the prepared specific aqueous solution to prepare a lithium bromide aqueous solution. A 48% by mass aqueous solution of hydrobromic acid manufactured by Kanto Chemical is used. The obtained lithium bromide aqueous solution is added to a vibration drying device (trade name VH type, manufactured by Central Chemical Industry Co., Ltd.), and is heated and dried under reduced pressure at a maximum temperature of 160°C to obtain a composition containing lithium bromide. The obtained composition containing lithium bromide is crushed into powder in a mortar.

[0197] The obtained lithium bromide-containing composition was confirmed by analysis to contain 0.11 mass % of SO 4 The obtained lithium source was used as a raw material in the same manner as in Example 1, and a sulfide-based solid electrolyte containing argyrodite-type crystals was obtained by the same method as in Example 1.

[0198] (Example 8)

[0199] SO was prepared using lithium hydroxide monohydrate (manufactured by Sigma, purity 99.95%), lithium sulfate (manufactured by Sigma, purity 99.99%), and distilled water. 4 A specific aqueous solution containing 1.02 mol% of Li. Hydrobromic acid is directly added to the prepared specific aqueous solution to prepare a lithium bromide aqueous solution. A 48% by mass aqueous solution of hydrobromic acid manufactured by Kanto Chemical is used. The obtained lithium bromide aqueous solution is added to a vibration drying device (trade name VH type, manufactured by Central Chemical Industry Co., Ltd.), and is heated and dried under reduced pressure at a maximum temperature of 160°C to obtain a composition containing lithium bromide. The obtained composition containing lithium bromide is crushed into powder in a mortar.

[0200] The obtained lithium bromide-containing composition was confirmed by analysis to contain 1.10 mass % of SO 4 The obtained lithium source was used as a raw material in the same manner as in Example 1, and a sulfide-based solid electrolyte containing argyrodite-type crystals was obtained by the same method as in Example 1.

[0201] (Example 9)

[0202] SO was prepared using lithium hydroxide monohydrate (manufactured by Sigma, purity 99.95%), lithium sulfate (manufactured by Sigma, purity 99.99%), and distilled water. 4 A specific aqueous solution containing 5.12 mol% of Li. Hydrobromic acid is directly added to the prepared specific aqueous solution to prepare a lithium bromide aqueous solution. A 48% by mass aqueous solution of hydrobromic acid manufactured by Kanto Chemical is used. The obtained lithium bromide aqueous solution is added to a vibration drying device (trade name VH type, manufactured by Central Chemical Industry Co., Ltd.), and is heated and dried under reduced pressure at a maximum temperature of 160°C to obtain a composition containing lithium bromide. The obtained composition containing lithium bromide is crushed into powder in a mortar.

[0203] The obtained lithium bromide-containing composition was confirmed by analysis to contain 5.00 mass % of SO 4 The obtained lithium source was used as a raw material in the same manner as in Example 1, and a sulfide-based solid electrolyte containing argyrodite-type crystals was obtained by the same method as in Example 1.

[0204] (Example 10)

[0205] SO was prepared using lithium hydroxide monohydrate (manufactured by Sigma, purity 99.95%), lithium sulfate (manufactured by Sigma, purity 99.99%), and distilled water. 4 A specific aqueous solution containing 11.81 mol% of Li. Hydrobromic acid is directly added to the prepared specific aqueous solution to prepare a lithium bromide aqueous solution. A 48% by mass aqueous solution of hydrobromic acid manufactured by Kanto Chemical is used. The obtained lithium bromide aqueous solution is added to a vibration drying device (trade name VH type, manufactured by Central Chemical Industry Co., Ltd.), and is heated and dried under reduced pressure at a maximum temperature of 160°C to obtain a composition containing lithium bromide. The obtained composition containing lithium bromide is crushed into powder in a mortar.

[0206] The obtained lithium bromide-containing composition was confirmed by analysis to contain 10.00 mass % of SO 4 The obtained lithium source was used as a raw material in the same manner as in Example 1, and a sulfide-based solid electrolyte containing argyrodite-type crystals was obtained by the same method as in Example 1.

[0207] (Example 11)

[0208] The unpurified extract used in Example 2 was placed in a vibration drying device (trade name VH model, manufactured by Chuo Kakoki Co., Ltd.) and dried under reduced pressure at a maximum temperature of 85° C. to obtain lithium hydroxide. The obtained lithium hydroxide was pulverized into powder in a mortar.

[0209] Then, the lithium hydroxide powder was placed in a vibration drying device (trade name: VH type, manufactured by Chuo Kakoki Co., Ltd.), and reacted at 200° C. while introducing hydrogen sulfide, thereby obtaining a composition containing lithium sulfide.

[0210] The obtained lithium sulfide-containing composition was confirmed to contain 2.94 mass % of SO 4 , 0.77 mass% Al, and 2.12 mass% F.

[0211] Next, in a dry nitrogen atmosphere, to become Li 5.5 PS 4.3 Cl 0.8 Br 0.8 Phosphorus pentasulfide powder (manufactured by Sigma, purity 99%), lithium bromide powder (manufactured by Sigma, purity 99.99%), lithium chloride powder (manufactured by Sigma, purity 99.99%) and synthesized lithium sulfide powder were weighed in a composition ratio of 99.99% to prepare a mixture.

[0212] The mixture was placed in a heat-resistant container and heated to melt for 0.5 hours under the conditions of 1 atm and 750°C. At this time, sulfur gas obtained by heating elemental sulfur at 350°C was supplied so that the partial pressure of the sulfur gas was 0.1 atm, and N 2 A gas atmosphere containing sulfur element was obtained as a carrier gas, and sulfur was introduced into the melt by heating and melting in the gas atmosphere. The content of sulfur gas in the gas atmosphere containing sulfur element was 0.1 volume %.

[0213] Then, the solid is cooled at a cooling rate of 1 to 1000°C / sec to obtain a solid sulfide-based solid electrolyte including an amorphous phase and an argyrodite-type crystal phase. Next, the solid is crystallized at 450°C for 1 hour in a nitrogen atmosphere to obtain a sulfide-based solid electrolyte including argyrodite-type crystals.

[0214] (Example 12)

[0215] SO was prepared using lithium hydroxide monohydrate (manufactured by Sigma, purity 99.95%), lithium sulfate (manufactured by Sigma, purity 99.99%), and distilled water. 4 A specific aqueous solution containing 0.12 mol% of Li was prepared. The obtained specific aqueous solution was added to a vibration drying device (trade name VH type, manufactured by Central Chemical Industry Co., Ltd.) and dried by heating under reduced pressure at a maximum temperature of 85° C., thereby obtaining lithium hydroxide. The obtained lithium hydroxide was crushed into powder in a mortar.

[0216] Then, the lithium hydroxide powder was placed in a vibration drying device (trade name: VH type, manufactured by Chuo Kakoki Co., Ltd.), and reacted at 200° C. while introducing hydrogen sulfide, thereby obtaining a composition containing lithium sulfide.

[0217] The obtained lithium sulfide-containing composition was confirmed to contain 0.51 mass % of SO 4 .

[0218] The obtained lithium source was used as a raw material in the same manner as in Example 1, and a sulfide-based solid electrolyte containing argyrodite-type crystals was obtained by the same method as in Example 1.

[0219] (Example 13)

[0220] SO was prepared using lithium hydroxide monohydrate (manufactured by Sigma, purity 99.95%), lithium sulfate (manufactured by Sigma, purity 99.99%), and distilled water. 4 A specific aqueous solution containing 0.25 mol% of Li. The obtained specific aqueous solution was added to a vibration drying device (trade name VH type, manufactured by Central Chemical Industry Co., Ltd.), and heated under reduced pressure at a maximum temperature of 85°C to dry, thereby obtaining lithium hydroxide. The obtained lithium hydroxide was crushed into powder in a mortar.

[0221] Then, the lithium hydroxide powder was placed in a vibration drying device and reacted at 200° C. while introducing hydrogen sulfide, thereby obtaining a composition containing lithium sulfide.

[0222] The obtained lithium sulfide-containing composition was confirmed to contain 1.02 mass % of SO 4 .

[0223] The obtained lithium source was used as a raw material in the same manner as in Example 1, and a sulfide-based solid electrolyte containing argyrodite-type crystals was obtained by the same method as in Example 1.

[0224] (Example 14)

[0225] SO was prepared using lithium hydroxide monohydrate (manufactured by Sigma, purity 99.95%), lithium sulfate (manufactured by Sigma, purity 99.99%), and distilled water. 4 A specific aqueous solution containing 1.02 mol% of Li was prepared. The obtained specific aqueous solution was added to a vibration drying device (trade name VH type, manufactured by Central Chemical Industry Co., Ltd.) and heated under reduced pressure at a maximum temperature of 85° C. to obtain lithium hydroxide. The obtained lithium hydroxide was crushed into powder in a mortar.

[0226] Then, the lithium hydroxide powder was placed in a vibration drying device and reacted at 200° C. while introducing hydrogen sulfide, thereby obtaining a composition containing lithium sulfide.

[0227] The obtained lithium sulfide-containing composition was confirmed to contain 4.16 mass % of SO 4 .

[0228] The obtained lithium source was used as a raw material in the same manner as in Example 1, and a sulfide-based solid electrolyte containing argyrodite-type crystals was obtained by the same method as in Example 1.

[0229] (Example 15)

[0230] SO was prepared using lithium hydroxide monohydrate (manufactured by Sigma, purity 99.95%), lithium sulfate (manufactured by Sigma, purity 99.99%), and distilled water. 4 A specific aqueous solution containing 2.55 mol% of Li was prepared. The obtained specific aqueous solution was added to a vibration drying device (trade name VH type, manufactured by Central Chemical Industry Co., Ltd.) and heated under reduced pressure at a maximum temperature of 85° C. to obtain lithium hydroxide. The obtained lithium hydroxide was crushed into powder in a mortar.

[0231] Then, the lithium hydroxide powder was placed in a vibration drying device and reacted at 200° C. while introducing hydrogen sulfide, thereby obtaining a composition containing lithium sulfide.

[0232] The obtained lithium sulfide-containing composition was confirmed to contain 10.00 mass % of SO 4 .

[0233] The obtained lithium source was used as a raw material in the same manner as in Example 1, and a sulfide-based solid electrolyte containing argyrodite-type crystals was obtained by the same method as in Example 1.

[0234] The following evaluations were performed on Examples 1 to 15. The evaluation results are shown in Table 2.

[0235] (Productivity Evaluation)

[0236] The time required to prepare the aqueous solution for obtaining the lithium source from the extract was evaluated according to the following criteria: The preparation time does not include the time until the extract is obtained.

[0237] Pass: The time required to prepare the aqueous solution is less than 1 day.

[0238] Failure: The time required to prepare the aqueous solution is more than 1 day.

[0239] (Lithium ion conductivity evaluation)

[0240] The sulfide-based solid electrolyte of each example was crushed to obtain a sulfide-based solid electrolyte powder with an average particle size of 10 μm. The sulfide-based solid electrolyte powder was pressed into a powder body at a pressure of 380 MPa and used as a measurement sample to measure using an AC impedance measurement device (Bio-Logic Sciences Instruments, potentiostat / galvanostat VSP).

[0241] The measurement conditions were set to measurement frequency: 100 Hz to 1 MHz, measurement voltage: 100 mV, and measurement temperature: 25°C.

[0242] Pass: The lithium ion conductivity is 2 mS / cm or higher, which is a level that can be used practically as a lithium ion secondary battery.

[0243] Unqualified: The lithium ion conductivity is less than 2 mS / cm, which is too low to be practically used as a lithium ion secondary battery.

[0244] (Impurity Determination Method)

[0245] SO in aqueous solution 4 The amount of F was measured using ion chromatography, the amount of Al was measured using an ICP emission spectrometry device, and the amount of Li was measured using an atomic absorption spectrometry device.

[0246] In addition, the SO contained in the obtained lithium compound 4 , Al, F, use ultrapure water to make a solution, SO 4 The amount of F was measured using ion chromatography, the amount of Al was measured using an ICP emission spectrometry device, and the amount of Li was measured using an atomic absorption spectrometry device.

[0247] For ion chromatography, ICS-2000 manufactured by DIONEX was used, for ICP emission spectrometry, Agilent 5800 manufactured by Agilent Technologies was used, and for atomic absorption spectrometry, Z-2300 manufactured by Hitachi High-Technologies was used.

[0248] The change in oxygen content of the electrolyte sample prepared in (Example 15) was investigated. The analysis was performed using an oxygen analyzer (manufactured by LECO). The results showed that the oxygen content of the mixed raw material was 1.8% by mass, while the oxygen content of the synthesized sulfide solid electrolyte was 1.4% by mass, a decrease of 22%. This is believed to be due to the fact that by heating and melting the raw materials in a gas atmosphere containing sulfur, part of the SO 4 Become a SO 2 In addition, due to the influence of bubbling at this time, the composition is homogenized, and an electrolyte with high electrical conductivity can be synthesized.

[0249] [Table 1]

[0250]

[0251] The results are shown in Table 1. In addition, the SO 4 The relationship between the concentration and the lithium ion conductivity of the sulfide-based solid electrolyte produced using the sulfide-based solid electrolyte is shown in FIG. Figures 4 to 6 .in, Figure 4 is the result of Examples 1 to 6, Figure 5 is the result of Example 1 and Examples 7 to 10, Figure 6 These are the results of Examples 1 and 12 to 15.

[0252] According to the above results, in the manufacturing methods of Examples 2, 4 to 15 as embodiments, a sulfide-based solid electrolyte is manufactured by heating and melting the raw materials in a gas atmosphere containing sulfur element, thereby obtaining a sulfide-based solid electrolyte containing Li and SO. 4 AndSO 4 When a lithium source obtained by using an aqueous solution having a ratio of 0.1 mol% or more to Li is used as a raw material, a sulfide-based solid electrolyte having characteristics at a level that can be practically used as a lithium ion secondary battery is obtained. In addition, in the manufacturing methods of Examples 2, 4 to 15 as embodiments, the preparation of the aqueous solution for obtaining the lithium source is short and the productivity is excellent. On the other hand, in Example 1, the aqueous solution for obtaining the lithium source is prepared by subjecting the extract to a high-purification treatment. As a result, although a sulfide-based solid electrolyte having characteristics at a level that can be practically used as a lithium ion secondary battery can be obtained, the preparation of the aqueous solution takes a long time and is poor in productivity. In addition, in Example 3, in which a sulfide-based solid electrolyte is manufactured using a solid phase reaction method, a sulfide-based solid electrolyte having characteristics at a level that can be practically used as a lithium ion secondary battery cannot be obtained.

[0253] Although the present invention is described in detail with reference to specific embodiments, various changes and modifications can be made without departing from the spirit and scope of the present invention, which will be clear to those skilled in the art. This application is based on Japanese patent application (Japanese Patent Application No. 2022-073771) filed on April 27, 2022, the contents of which are incorporated herein by reference.

Claims

1. A method for producing a sulfide-based solid electrolyte, The method comprises the steps of heating and melting the raw materials in an atmosphere containing sulfur. The raw material includes a lithium source obtained by using an aqueous solution containing Li and SO4, The ratio of the SO4 to the Li in the aqueous solution is 0.1 mol% or more.

2. The method for producing a sulfide-based solid electrolyte according to claim 1, wherein: The aqueous solution further contains at least one of Al and F, In the aqueous solution, at least one of a ratio of the Al to the Li and a ratio of the F to the Li is 0.01 mol % or more.

3. The method for producing a sulfide-based solid electrolyte according to claim 1 or 2, wherein: The aqueous solution includes an extract obtained by immersing a treated material of a used lithium ion secondary battery in water.

4. The method for producing a sulfide-based solid electrolyte according to claim 3, wherein: The aqueous solution is obtained by adjusting the content ratio of one or more components selected from SO4, Al and F and Li in the extract.

5. A method for producing a sulfide-based solid electrolyte, The method comprises the steps of obtaining a lithium source by using an aqueous solution containing Li and SO4 and heating and melting a raw material containing the lithium source in an atmosphere containing sulfur. In the aqueous solution, the ratio of the SO4 to the Li is greater than 0.1 mol%.

6. The method for producing a sulfide-based solid electrolyte according to claim 5, wherein: The aqueous solution further contains at least one of Al and F, In the aqueous solution, at least one of a ratio of the Al to the Li and a ratio of the F to the Li is 0.01 mol % or more.

7. The method for producing a sulfide-based solid electrolyte according to claim 5 or 6, wherein: The aqueous solution includes an extract obtained by immersing a treated material of a used lithium ion secondary battery in water.

8. The method for producing a sulfide-based solid electrolyte according to claim 7, wherein: The method further comprises the step of preparing the aqueous solution, wherein the preparation of the aqueous solution comprises the step of adjusting the content ratio of one or more components selected from SO4, Al and F and Li in the extract.

9. A composition containing lithium halide, containing 10 mass % or less of SO4, for use in producing a sulfide-based solid electrolyte.

10. The composition containing lithium halide according to claim 9, wherein The halogen elements constituting the lithium halide are halogen elements other than F, and further contain at least one of Al and F.

11. A composition containing lithium sulfide, containing more than 0.5 mass % and less than 10 mass % of SO4, for use in producing a sulfide-based solid electrolyte.

12. The composition containing lithium sulfide according to claim 11, wherein Contains at least one of Al and F.