Polymer-type conductive paste, conductive film, and solid electrolytic capacitor element
By adding specific additives to the conductive paste, the moisture resistance of the polymer-type conductive paste is improved, and the problem of silver ion migration in solid electrolytic capacitor elements is solved, and the high-reliability conductive layer is realized in a high humidity environment .
Patent Information
- Application Number
- CN202380039037.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-05-09
- Filing Date
- 2023-04-18
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-04-18
AI Technical Summary
The prior art is difficult to effectively suppress silver ions in the conductive layer in the solid electrolytic capacitor element under a high humidity environment, resulting in low component reliability and limited improvement of moisture resistance of the polyvinyl butyral resin used.
Polymer type conductive paste containing conductive metal powder, polyvinyl butyral resin, organic solvents and specific additives, including stearic acid, lauric acid, octadecenyl succinic acid, benzoic acid, acetyl Aminophenol, aminophenol, catechol and N,N-bis(2-hydroxyethyl)coa alkylamine, etc., the moisture resistance of the conductive layer is significantly improved through these additives.
The moisture permeability of the conductive layer is significantly reduced, the ionization of silver ions is suppressed, and the reliability of solid electrolytic capacitor elements is improved, especially in high humidity environments.
Smart Images

Figure CN119096318A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a polymer conductive paste, a conductive film and a solid electrolytic capacitor element, which can be suitably used for forming a conductor layer in a solid electrolytic capacitor element such as a tantalum capacitor or an electrode of a multilayer ceramic electronic component. Background Art
[0002] The polymer conductive paste of the present invention is used, for example, in a method for producing a solid electrolyte capacitor element.
[0003] Solid electrolytic capacitor elements generally have the following structure: the surface of the anode body made of valve metal is chemically treated to form a dielectric layer, and an electrolyte layer made of a conductive polymer, a carbon layer, and a cathode layer made of a conductive paste are sequentially formed on the surface. The cathode layer is bonded to the cathode lead terminal using a conductive adhesive, the anode body is joined to the anode lead terminal by welding, and a molded resin is applied to the outside of these to form a capacitor component.
[0004] Figure 1 An example of the structure of a solid electrolytic capacitor element is shown.
[0005] The solid electrolytic capacitor element 1 has a structure including a valve metal sintered body 11 obtained by sintering a valve metal such as tantalum, niobium, titanium, or aluminum, an oxide film layer 12 formed on the surface of the sintered body 11, and a solid electrolyte layer 13, a carbon layer 14, and a conductor layer 15 formed thereon. Here, the sintered body 11 is used as an anode body, the oxide film layer 12 is used as a dielectric layer, and the carbon layer 14 and the conductor layer 15 on the solid electrolyte layer 13 are used as cathode bodies.
[0006] The oxide film layer 12 is preferably formed by oxidizing the sintered body itself, but may be formed of other oxides.
[0007] As the solid electrolyte layer 13 , manganese dioxide, conductive polymers, and the like are widely used.
[0008] The carbon layer 14 is usually formed by applying and drying a carbon paste in which carbon powder is dispersed in an organic vehicle. The carbon layer 14 is believed to reduce the contact resistance between the solid electrolyte layer 13 and the conductor layer 15 and reduce ESR (equivalent series resistance).
[0009] The conductor layer 15 is generally formed by applying a conductive paste in which metal powder such as silver is dispersed in an organic vehicle, followed by drying and / or curing.
[0010] As described in Patent Documents 1 and 2, such solid electrolytic capacitor elements are conventionally known.
[0011] In recent years, these solid electrolytic capacitor elements are often used in high-humidity environments. In the conductive layer containing silver powder, silver is ionized and so-called migration occurs, which is one of the causes of deterioration of element reliability such as short circuits.
[0012] Patent document 1 describes a solid electrolytic capacitor element having at least a dielectric layer, a solid electrolyte layer, a carbon layer including a first resin component, and a conductive layer including a second resin component on the surface of an anode body, wherein the difference between the hydrogen bonding component value on the surface of the carbon layer and the hydrogen bonding component value on the surface of the conductive layer is set within a specific range, thereby obtaining a solid electrolytic capacitor element in which ESR degradation is reduced and the deviation of ESR changes over time for each product is suppressed.
[0013] Patent document 2 solves the above problem by dispersing conductive polymer particles in a solid electrolyte layer and using a polymer with controlled water content as a resin component in the conductor layer. Specifically, by dispersing thiophene polymer particles in a solid electrolyte layer to suppress the movement of silver ions, and using a vinyl acetal polymer with a small amount of residual hydroxyl groups in the polymer as a resin component of the conductor layer, the water content of the conductor layer can be reduced. It should be noted that the residual amount of hydroxyl groups in Patent document 2 is less than 35 mol%, preferably more than 10 mol% and less than 25 mol%. As an example of such a polymer, "BH-S" (polyvinyl butyral resin) manufactured by Sekisui Chemical Co., Ltd. can be cited.
[0014] Prior art literature
[0015] Patent Literature
[0016] Patent Document 1: International Publication No. 2013 / 111438
[0017] Patent Document 2: U.S. Patent Application Publication No. 2018 / 0137988 Summary of the invention
[0018] Technical problem solved by the invention
[0019] However, the dispersion of conductive polymer particles into the solid electrolyte layer can only inhibit the movement of silver ions in the solid electrolyte layer, but cannot inhibit the occurrence of migration itself. In addition, in Patent Document 1 based on the present applicant, polyvinyl butyral resins such as "BH-S" and "KS-5" with a residual hydroxyl content of less than 35 mol% are used in the conductor layer, and the reliability of the case of long-term placement in a high-humidity environment is insufficient. According to the research / inquiry of the present inventors, by using a polyvinyl butyral resin with a small residual hydroxyl content, the effect of inhibiting the occurrence of migration can be expected to a certain extent, but the effect is limited and insufficient, and does not necessarily improve the reliability of the component.
[0020] If epoxy resins that form a dense cured film are used instead of polyvinyl butyral resins, moisture resistance is improved. However, epoxy resin cured films are very hard and therefore not suitable for certain uses. Therefore, it is often desired to improve the moisture resistance of pastes using polyvinyl butyral resins.
[0021] According to the research and study by the present inventors, moisture resistance can be improved to a certain extent by adding compounds such as 5-amino-2-hydroxybenzoic acid, naphthol, cresol, and salicylic acid to a conductive paste using a polyvinyl butyral resin, but the improvement is not necessarily sufficient.
[0022] Based on the above background, the present inventors conducted intensive studies on polymer conductive pastes using polyvinyl butyral resins and found that moisture resistance in polymer conductive pastes can be significantly improved by adding specific compounds to the paste, thereby completing the present invention.
[0023] That is, an object of the present invention is to provide a polymer conductive paste capable of obtaining a highly reliable conductive layer even in a high-humidity environment.
[0024] Technical means of solving problems
[0025] The present invention which solves the above-mentioned problems relates to the following polymer conductive paste, conductive film, and solid electrolytic capacitor element.
[0026] (1) A polymer-type conductive paste comprising a conductive metal powder, a binder resin, an organic solvent and a specific additive, wherein:
[0027] The binder resin is polyvinyl butyral resin,
[0028] The specific additive is one or more selected from stearic acid, lauric acid, octadecenylsuccinic acid, benzoic acid, acetaminophenol, aminophenol, catechol and N,N-bis(2-hydroxyethyl)coconut alkylamine,
[0029] The polymer conductive paste contains the specific additive in an amount within a range of 0.01 parts by mass to 3.0 parts by mass, both inclusive, based on 100 parts by mass of the conductive metal powder.
[0030] (2) The polymer conductive paste according to (1), wherein
[0031] The specific additive is octadecenylsuccinic acid.
[0032] (3) The polymer conductive paste according to (1), wherein
[0033] The polyvinyl butyral resin contains hydroxyl groups in an amount of 30 mol % or less.
[0034] (4) The polymer conductive paste according to (3), wherein
[0035] The polyvinyl butyral resin contains hydroxyl groups in an amount of 25 mol % or less.
[0036] (5) The polymer conductive paste according to (1), wherein
[0037] The conductive metal powder is silver powder.
[0038] (6) A conductive film formed from the polymer conductive paste according to any one of (1) to (5) above.
[0039] (7) A solid electrolytic capacitor element having at least a dielectric layer, a solid electrolyte layer, a carbon layer and a conductor layer on the surface of an anode body, wherein:
[0040] The conductor layer includes the conductive film described in (6).
[0041] Effects of the Invention
[0042] The conductive layer formed from the polymer conductive paste of the present invention has low moisture permeability even in a high-humidity environment. Therefore, ionization of silver in the conductive layer can be suppressed, and a conductive layer with high reliability can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] [ Figure 1 ] Figure 1 FIG. 1 is a diagram showing an example of a solid electrolytic capacitor element. DETAILED DESCRIPTION
[0044] In addition, the term "polymer-type conductive paste" in this specification is in contrast to the term "fired-type conductive paste" in which the organic components in the coating film are dispersed by firing and only the inorganic components remain in the resulting conductive film. It refers to a type of paste in which an organic component containing a binder resin remains in the conductive film obtained by drying and / or curing the coating film.
[0045] The polymer conductive paste of the present invention is not limited to the application, and can be used for wiring of common circuits, electronic components, such as electrode formation of multilayer ceramic electronic components, and is particularly preferably used for forming a conductor layer in a solid electrolytic capacitor element such as a tantalum capacitor, so that the effects of the present invention can be fully obtained. Figure 1 An example of a solid electrolytic capacitor element is shown.
[0046] The conductor layer 15 mainly comprises conductive metal powder and polyvinyl butyral resin, and is obtained by applying the polymer conductive paste of the present invention onto the carbon layer 14, heating to about 120° C. to 220° C., removing the organic solvent, and drying.
[0047] The polymer conductive paste of the present invention contains at least conductive metal powder, a polyvinyl butyral resin as a binder resin, an organic solvent capable of dissolving the binder resin, and a specific additive.
[0048] The conductive metal powder contained in the polymer conductive paste is not particularly limited, and metal powders generally used in conductive pastes such as silver, copper, nickel, palladium, and aluminum can be used.
[0049] Among them, silver powder is particularly preferred. In addition to pure silver powder, it can be silver-coated powder in which the surface of metal powder other than silver is coated with silver, composite silver powder in which the surface of silver powder is coated with inorganic and / or organic substances, and silver alloy powder in which silver and metal other than silver are alloyed. Hereinafter, these are collectively referred to as "silver powder" in this specification. By using silver powder, the effect of the present invention can be further achieved, and it is also advantageous from the viewpoint of conductivity and cost. In addition, mixed powders obtained by mixing these silver powders with other conductive metal powders such as palladium, platinum, copper, and metal oxides can be used. In any case, the content of the silver component relative to the entire conductive metal powder is preferably 10% by mass or more.
[0050] In addition, the shape of the conductive metal powder may be spherical, flake, dendritic, or any other conventionally used shape, and two or more types having different average particle diameters, particle size distributions, shapes, etc. may be mixed and used. In the present invention, a spherical silver-based powder and a flake silver-based powder are mixed and used, because the conductivity, moisture resistance, etc. can be easily controlled, and this is particularly preferred.
[0051] As the binder resin contained in the polymer conductive paste of the present invention, a polyvinyl butyral resin is used. As the polyvinyl butyral resin, "BH-S" (hydroxyl amount = 22 mol%) manufactured by Sekisui Chemical Co., Ltd., "KS-5" (hydroxyl amount = 25 mol%) manufactured by Sekisui Chemical Co., Ltd., "BM-5" (hydroxyl amount = 34 mol%) manufactured by Sekisui Chemical Co., Ltd., "KS-1" (hydroxyl amount = 25 mol%) manufactured by Sekisui Chemical Co., Ltd., "KS-10" (hydroxyl amount = 25 mol%) manufactured by Sekisui Chemical Co., Ltd., "SV-02" (hydroxyl amount = 22 mol%) manufactured by Sekisui Chemical Co., Ltd., "SV-06" (hydroxyl amount = 22 mol%) manufactured by Sekisui Chemical Co., Ltd., "SV-22" (hydroxyl amount = 22 mol%) manufactured by Sekisui Chemical Co., Ltd., etc. can be used.
[0052] In the polymer conductive paste of the present invention, the content of the polyvinyl butyral resin is not particularly limited and can be appropriately determined according to the properties required as the paste. As an example, the solid content of the polyvinyl butyral resin is in the range of 1.0 mass part to 20 mass parts per 100 mass parts of the conductive metal powder.
[0053] Furthermore, as long as the effects of the present invention are not impaired, a resin other than the polyvinyl butyral resin may be included as a binder resin, and examples thereof include cellulose resins, acrylic resins, methacrylic resins, epoxy resins, phenolic resins, rosin acrylic resins, and the like.
[0054] It should be noted that the residual amount of hydroxyl groups in the polyvinyl butyral resin used in the present invention is not particularly limited, but is preferably 35 mol % or less in order to improve moisture resistance, more preferably 30 mol % or less, and particularly preferably 25 mol % or less.
[0055] The organic solvent may be any solvent that dissolves the binder resin used, and for example, alcohols, ethers, esters, hydrocarbons or the like may be used. Two or more organic solvents or a mixed solvent of an organic solvent and water may be used as necessary.
[0056] The polymer conductive paste of the present invention contains one or more selected from stearic acid, lauric acid, octadecenylsuccinic acid, benzoic acid, acetaminophenol, aminophenol, catechol and N,N-bis(2-hydroxyethyl)coconut alkylamine as specific additives.
[0057] These specific additives function as moisture permeability adjusters in the paste of the present invention, and therefore are also referred to as moisture permeability adjusters in this specification.
[0058] According to the research conducted by the present inventors, when these moisture permeability regulators are compounded in a given amount in a paste using polyvinyl butyral resin as a binder, the moisture permeability (moisture permeability) of the film obtained by applying and drying the paste is significantly reduced without having almost any adverse effect on conductivity, printability (thixotropy), etc., and as a result, the moisture resistance of the film can be improved.
[0059] Among the moisture permeability regulators, octadecenylsuccinic acid is particularly preferred because the film density can be increased and an effect of reducing ESR can be expected.
[0060] The content of these moisture permeability regulators is within the range of 0.01 parts by mass or more and 3.0 parts by mass or less relative to 100 parts by mass of the conductive metal powder. When the content of the moisture permeability regulator is outside the above range, the moisture resistance deteriorates, and other properties (such as conductivity, for example) are adversely affected. The content of the moisture permeability regulator is preferably within the range of 0.1 parts by mass or more and 1.5 parts by mass or less.
[0061] Furthermore, the polymer conductive paste of the present invention may contain additives such as a common surfactant, a defoaming agent, a plasticizer, a dispersant, and an organic or inorganic filler as needed.
[0062] Example
[0063] (1) Experiment 1
[0064] <Preparation of Conductive Paste>
[0065] - Sample 1 -
[0066] 8.6 parts by mass of a polyvinyl butyral resin ("BM-5" manufactured by Sekisui Chemical Co., Ltd.; hydroxyl content = 35 mol%) was dissolved in benzyl alcohol to prepare 57.2 parts by mass of varnish A, 80 parts by mass of a flaky silver powder ("Ag-531" manufactured by Shoei Chemical Co., Ltd.) and 20 parts by mass of a spherical silver powder ("Ag-202" manufactured by Shoei Chemical Co., Ltd.) were mixed and kneaded and stirred using a three-roll mill, and then diluted with butyl acetate so that the shear rate at 25° C. using a Brookfield viscometer HA type was 9.3 s. -1 The viscosity measured below was 1 Pa·s, and the silver paste prepared in this way was designated as Sample 1.
[0067] - Sample 2 -
[0068] A silver paste obtained in the same manner as Sample 1 was designated as Sample 2, except that the polyvinyl butyral resin was changed to “KS-5” (manufactured by Sekisui Chemical Co., Ltd.; hydroxyl content = 25 mol %) as Varnish B.
[0069] - Sample 3 -
[0070] The same procedure as in Sample 2 was performed except that 0.5 parts by mass of acetaminophenol (“3-hydroxyacetanilide” manufactured by Tokyo Chemical Industry Co., Ltd.) was further added to the composition of Sample 2 based on 100 parts by mass of the silver powder. The resulting silver paste was designated as Sample 3.
[0071] - Sample 4 -
[0072] The silver paste obtained was designated as Sample 4 in the same manner as Sample 3 except that stearic acid (“Stearic Acid 90” manufactured by MIYOSHI OIL & FAT Co., Ltd.) was used instead of acetaminophen.
[0073] - Sample 5 -
[0074] The silver paste obtained was designated as Sample 5 in the same manner as Sample 3 except that lauric acid (“lauric acid” manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used instead of acetaminophen.
[0075] - Sample 6 -
[0076] The silver paste obtained was designated as Sample 6 in the same manner as Sample 3 except that octadecenylsuccinic acid (dicarboxylic acid “Hypermer KD-16” manufactured by CRODA JAPAN) was used instead of acetaminophen.
[0077] - Sample 7 -
[0078] The silver paste obtained was designated as Sample 7 in the same manner as Sample 3 except that benzoic acid (“Benzoic acid” manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) was used instead of acetaminophen.
[0079] - Sample 8 -
[0080] The silver paste obtained was designated as Sample 8 in the same manner as Sample 3 except that aminophenol (“p-aminophenol” manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used instead of acetaminophenol.
[0081] - Sample 9 -
[0082] The silver paste obtained was designated as Sample 9 in the same manner as Sample 3 except that catechol (“Catechol” manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used instead of acetaminophen.
[0083] - Sample 10 -
[0084] The silver paste obtained was designated as Sample 10 in the same manner as Sample 3 except that N,N-bis(2-hydroxyethyl)coconut alkylamine (ESOMIN “LIPONOL C / 12” manufactured by Lion Specialty Chemicals) was used instead of acetaminophenol.
[0085] - Sample 11 -
[0086] The same procedure as in Sample 3 was carried out except that stearylamine (“FARMIN 80” manufactured by Kao Corporation) was used instead of acetaminophen, and the obtained silver paste was designated as Sample 11.
[0087] (2) Experiment 2
[0088] <Preparation of Conductive Paste>
[0089] -Sample 12~21-
[0090] Silver pastes obtained in the same manner as Sample 3 were designated as Samples 12 to 21, except that the amounts of the conductive metal powder, the polyvinyl butyral resin, and acetaminophenol were the amounts described in Table 2.
[0091] (3) Experiment 3
[0092] <Preparation of Conductive Paste>
[0093] -Sample 22~25-
[0094] The same procedure as in Sample 6 was performed except that the amounts of the conductive metal powder, the polyvinyl butyral resin, and the octadecenylsuccinic acid were the amounts described in Table 3, and the obtained silver pastes were designated as Samples 22 to 25.
[0095] The following moisture permeability test was performed on each of Samples 1 to 25 of the conductive paste obtained as described above, and the moisture permeation amount of each sample was evaluated.
[0096] The evaluation results of samples 1 to 11 are shown in Table 1, the evaluation results of samples 12 to 21 are shown in Table 2, and the evaluation results of samples 22 to 25 are shown in Table 3.
[0097] It should be noted that the samples marked with a * in Tables 1 to 3 are comparative examples.
[0098] <Moisture Permeability Test>
[0099] The silver paste of the sample was applied onto a PET film, and then heated at 150° C. for 60 minutes and peeled off from the PET film to prepare a dry film of the sample with a thickness of 20±2 μm.
[0100] Glass containers A containing 2 g of silica gel were prepared according to the number of samples, and each opening was covered with a dry film of the sample using an instant adhesive. After the openings were completely sealed, the total mass of the glass containers A was measured.
[0101] Next, a plastic container B of a size to be placed in the glass container A was prepared, and an appropriate amount of purified water was added from the opening of the plastic container B. The glass container A was added to the plastic container B so that the purified water as described above would not enter the glass container A, and the opening of the plastic container B was completely sealed. Then, the plastic container B containing the glass container A was heated from room temperature to 65° C. and kept as it was for 15 hours.
[0102] After the holding time has passed, the slowly cooled plastic container B is unsealed, the glass container A is taken out, and the total mass of the glass container A is measured again, and the increase is taken as the moisture permeation amount (mg). In this example, samples with a moisture permeation amount of less than 20 mg are considered to be acceptable.
[0103] [Table 1]
[0104]
[0105] [Table 2]
[0106]
[0107] [Table 3]
[0108]
[0109] (For evaluation results)
[0110] As can be seen from the results shown in Table 1, the moisture permeability changes depending on the amount of hydroxyl groups in the polyvinyl butyral resin, and when the moisture permeability regulator of the present invention is included, the moisture permeability further decreases significantly.
[0111] Furthermore, from the results shown in Tables 2 and 3, it is understood that the effect of reducing the moisture permeability is reduced regardless of whether the content of the moisture permeability regulator in the conductive paste is too high or too low.
[0112] In addition, among the moisture permeability adjusting agents used in the Examples, the same experiment was conducted on substances having structural isomers, and it was confirmed that the structural isomers also have the effect of reducing the moisture permeability.
[0113] Industrial Applicability
[0114] The present invention can be applied to solid electrolytic capacitor elements and multilayer ceramic electronic components.
[0115] Explanation of symbols
[0116] 1 Solid electrolytic capacitor element
[0117] 11 Valve action metal sintered body (anode body)
[0118] 12 Oxide film layer (dielectric layer)
[0119] 13 Solid electrolyte layer
[0120] 14 Carbon layer
[0121] 15 Conductor layer
Claims
1. A polymer conductive paste comprising conductive metal powder, a binder resin, an organic solvent and a specific additive, wherein: The binder resin is polyvinyl butyral resin, The specific additive is one or more selected from stearic acid, lauric acid, octadecenylsuccinic acid, benzoic acid, acetaminophenol, aminophenol, catechol and N,N-bis(2-hydroxyethyl)coconut alkylamine, The polymer conductive paste contains the specific additive in an amount within a range of 0.01 parts by mass to 3.0 parts by mass, both inclusive, based on 100 parts by mass of the conductive metal powder.
2. The polymer conductive paste according to claim 1, wherein The specific additive is octadecenylsuccinic acid.
3. The polymer conductive paste according to claim 1, wherein The polyvinyl butyral resin contains hydroxyl groups in an amount of 30 mol % or less.
4. The polymer conductive paste according to claim 3, wherein The polyvinyl butyral resin contains hydroxyl groups in an amount of 25 mol % or less.
5. The polymer conductive paste according to claim 1, wherein The conductive metal powder is silver powder. 6 . A conductive film formed from the polymer conductive paste according to claim 1 .
7. A solid electrolytic capacitor element, comprising at least a dielectric layer, a solid electrolyte layer, a carbon layer and a conductor layer on the surface of an anode body, wherein: The conductor layer includes the conductive film according to claim 6.
Citation Information
Patent Citations
Solid electrolytic capacitor element, method for manufacturing same, and conductive paste
CN104054147A
Conductive paste
CN110574125A
Conductive paste, electronic component, and laminated ceramic capacitor
CN113227233A
Solid electrolytic capacitors for use in high humidity environments
JP2020500427A