Improved writing feel with protective film
By controlling the ratio of the writing feel improvement layer to the protective film adhesive layer and the thickness of the adhesive layer, the problem of the writing feel improvement film floating and peeling under temperature changes was solved, ensuring the quality of film preservation, handling and processing.
Patent Information
- Application Number
- CN202280094533.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2022-12-02
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-12-02
AI Technical Summary
Existing writing feel improvement films suffer from float-up and peeling issues due to temperature changes during storage, handling, and processing, affecting their quality.
By controlling the ratio of the maximum height of the rounded waviness curve (WEM) of the writing feel improvement layer to the thickness a of the protective film adhesive layer (WEM/a) to be above 0.01 and below 1.00, and ensuring that the adhesive layer thickness is above 5μm and below 50μm, and the interlayer peel force is below 800mN/25mm, the occurrence of lifting and peeling is suppressed.
It effectively suppresses bubbling and peeling under temperature changes, maintaining a writing feel and improving the quality and performance of the membrane.
Smart Images

Figure CN119136979B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a writing feel improvement film having a protective film, obtained by laminating a protective film on a writing feel improvement film for improving the writing feel of a stylus in a touch panel or the like. Background Technology
[0002] In recent years, image display devices (touch panels) with position detection functions, which combine display devices and input units, have been frequently used in various electronic devices.
[0003] For this type of touch panel, a film (hereinafter referred to as "writing feel improvement film") was studied to be pasted on the outermost surface of the touch panel to improve the writing feel of the stylus.
[0004] Regarding writing feel improvement films, for example, the following have been disclosed: a writing feel improvement film having a writing feel improvement layer with specific friction (Patent Document 1); an anti-glare hard coating film for touch panels that specifies the pen tip resistance and oleic acid contact angle of a stylus (Patent Document 2); a transparent film having a specific total light transmittance and a specific maximum height of the rounded corrugation curve (Patent Document 3); a tactile film including linear protrusions forming a mesh structure (Patent Document 4); and a transparent laminated film having a specific maximum height of the rounded corrugation curve and an arithmetic mean roughness (Patent Document 5), etc.
[0005] However, these documents do not contain any records of laminates with protective films superimposed on writing feel improvement films.
[0006] Existing technical documents
[0007] Patent documents
[0008] Patent Document 1: WO2020 / 122172 (US2022 / 0033600A1)
[0009] Patent Document 2: Japanese Patent Application Publication No. 2014-232276
[0010] Patent Document 3: Japanese Patent Application Publication No. 2014-97649 (US2015 / 0291828A1)
[0011] Patent Document 4: Japanese Patent Application Publication No. 2015-54417
[0012] Patent Document 5: Japanese Patent Application Publication No. 2016-196113 (US2018 / 0030229A1) Summary of the Invention
[0013] The problem that the invention aims to solve
[0014] After manufacturing, this type of writing-enhancing film undergoes storage, transportation, and processing. Therefore, to protect the surface of the writing-enhancing film until it is used in a touch panel, a protective film is sometimes pre-attached (layered) to the film surface. In addition, writing-enhancing films with a protective film layered on their surface (hereinafter referred to as "writing-enhancing films with protective films") are sometimes exposed to high temperatures (40-60°C) for extended periods during storage and transportation, or are processed at high temperatures (50-90°C).
[0015] However, due to the application of this temperature change, the membrane floats (tunnels) and peels off, resulting in a decrease in the quality of the membrane that improves writing feel.
[0016] The present invention was made in view of the above-mentioned actual situation, and its object is to provide a writing feel improved film with a protective film that suppresses the occurrence of floating and peeling caused by temperature changes.
[0017] means for solving problems
[0018] In order to solve the above-mentioned problem, the inventors conducted in-depth research on writing feel improvement films with protective films. Their results showed that by making the ratio (WEM / a) of the maximum height of the rounded waviness curve of the writing feel improvement layer to the thickness a (μm) of the adhesive layer of the protective film have a specific relationship, the problem can be solved, thus completing the present invention.
[0019] Therefore, according to the present invention, a writing feel improved film with a protective film as described in [1] to [3] can be provided.
[0020] [1] A writing feel improvement film with a protective film, characterized in that it is a writing feel improvement film having a writing feel improvement film substrate layer and a writing feel improvement layer, and a protective film having an adhesive layer and a protective film substrate layer, wherein the writing feel improvement layer of the aforementioned writing feel improvement film is in contact with the adhesive layer of the aforementioned protective film.
[0021] The ratio of the maximum height (WEM) of the rounded ripple curve of the aforementioned writing feel improvement layer to the thickness a (μm) of the aforementioned adhesive layer (WEM / a) is 0.01 or more and 1.00 or less.
[0022] [2] The writing feel improvement film with protective film according to [1] is characterized in that the maximum height (WEM) of the rounded ripple curve of the aforementioned writing feel improvement layer is more than 0.1 μm and less than 20 μm.
[0023] [3] The writing feel improved film with protective film according to [1] or [2] is characterized in that the thickness a (μm) of the aforementioned adhesive layer is 5 μm or more and 50 μm or less.
[0024] [4] The writing feel improvement film with a protective film according to [1] or [2], wherein the interlayer peel force between the aforementioned writing feel improvement film and the protective film is less than 800mN / 25mm.
[0025] Invention Effects
[0026] The writing feel improvement film with a protective film according to the present invention can suppress the occurrence of floating and peeling caused by temperature changes during storage, transportation, and processing, thus maintaining the quality of the writing feel improvement film. Attached Figure Description
[0027] Figure 1 This is a schematic diagram illustrating an example of the layer structure of the writing feel improvement film with protective film of the present invention. Detailed Implementation
[0028] The improved writing feel film with a protective film of the present invention is characterized in that it is a writing feel improved film having a writing feel improved film substrate layer and a writing feel improved layer, and a protective film having an adhesive layer and a protective film substrate layer, wherein the writing feel improved layer of the aforementioned writing feel improved film and the adhesive layer of the aforementioned protective film are in contact, and the ratio (WEM / a) of the maximum height of the rounded waviness curve (WEM) of the aforementioned writing feel improved layer to the thickness a (μm) of the aforementioned adhesive layer is 0.01 or more and 1.00 or less.
[0029] The following is a detailed description of the writing feel improvement film with a protective film of the present invention.
[0030] 1) Improved writing feel membrane
[0031] The writing feel improvement film described in this embodiment has a writing feel improvement film substrate layer and a writing feel improvement layer.
[0032] (1) Improved writing feel of the film substrate layer
[0033] The writing feel improvement film substrate layer described in this embodiment serves to support the writing feel improvement layer.
[0034] As the material for the substrate layer of the writing feel improvement film, a transparent material can be appropriately selected from the existing known materials used as optical substrates.
[0035] Examples include, for instance, polyester films such as polyethylene terephthalate (PET), polybutylene terephthalate (PET), and polyethylene naphthalate (PAN); polyolefin films such as polyethylene (PE) and polypropylene (PP); cellulose diacetate (CDI), cellulose triacetate (TJ), cellulose acetate butyrate (CAT), polyvinyl chloride (PVC), polyvinylidene chloride (PVD), polyvinyl alcohol (PVA), ethylene-vinyl acetate copolymer (EVA) films, polystyrene (PS), polycarbonate (PC), polymethylpentene (PMC), polysulfone (PS), polyetheretherketone (PEEK), polyethersulfone (PES), polyetherimide (PEI), polyimide (PEI), fluoropolymer films, polyamide films, acrylic resin films, polyurethane resin films, norbornene polymer films, cyclic olefin polymer films, cyclic conjugated diene polymer films, vinyl alicyclic hydrocarbon polymer films, polyphenylene sulfide (PPS) films, liquid crystal polymer films; cellophane; glass; and their laminated films, etc.
[0036] In combination with the writing feel improvement layer, from the viewpoint of maintaining the writing feel of the stylus well, polyethylene terephthalate film, polycarbonate film, acrylic resin film, norbornene polymer film, etc. are preferred, and polyethylene terephthalate film, polycarbonate film, polymethyl methacrylate film, and composite substrates thereof are particularly preferred.
[0037] For the writing feel improvement film substrate layer, in order to improve the adhesion of the writing feel improvement layer to its surface, the surface on which the writing feel improvement layer is formed may be subjected to surface treatments such as oxidation, embossing, etc., and primer treatments, as desired.
[0038] Examples of oxidation methods include corona discharge treatment, plasma discharge treatment, chromating treatment (wet), flame treatment, hot air treatment, and ozone / ultraviolet treatment.
[0039] Examples of methods for creating an uneven surface include sandblasting and solvent treatment.
[0040] Primer treatment can be performed using known methods such as coating the surface of the writing-feel-enhancing film substrate layer with an adhesive resin material.
[0041] These surface treatments can be selected appropriately based on the material of the substrate layer.
[0042] From the viewpoints of appropriately supporting the writing feel improvement layer, processability, protection of the touch panel, and durability against stylus writing, the thickness of the writing feel improvement film substrate layer is preferably 30–300 μm, more preferably 90–250 μm, particularly preferably 120–220 μm, and even more preferably 150–200 μm.
[0043] (2) Improved writing feel layer
[0044] The writing feel improvement layer described in this embodiment has the function of improving the writing feel of the stylus.
[0045] Here, "improving the writing feel of the stylus" means that when writing with the stylus on the writing feel improvement layer, the vibration sensation when writing on paper with a ballpoint pen and the resistance sensation (degree of friction) when writing on paper with a ballpoint pen can be reproduced.
[0046] The writing feel improvement layer can be formed using a writing feel improvement layer forming composition.
[0047] The composition for forming a writing feel improvement layer can be prepared by, for example, mixing curing components, microparticles, surface conditioners, etc.
[0048] (2-1) Curing components
[0049] The composition for forming the writing feel improvement layer described in this embodiment preferably uses a curing component as the main component.
[0050] Curing agents are those that cure using active energy rays such as visible light, ultraviolet rays, and electron beams, or heat. Examples include active energy ray curing agents and thermosetting agents.
[0051] From the perspectives of the hardness of the formed writing feel improvement layer and the heat resistance of the writing feel improvement film substrate layer, an active energy ray curable component is preferred. A writing feel improvement film with a writing feel improvement layer formed from this material tends to have a desired WEM value and easily meets the aforementioned WEM / a value.
[0052] Examples of active energy ray-curable components include multifunctional (meth)acrylate monomers, (meth)acrylate prepolymers, and active energy ray-curable polymers. Among these, from the perspective of achieving a specified hardness and improving the writing feel of a stylus, multifunctional (meth)acrylate monomers and / or (meth)acrylate prepolymers are preferred, and multifunctional (meth)acrylate monomers are more preferred. A writing feel improvement film with a writing feel improvement layer formed from such a material readily possesses a desired WEM value and easily satisfies the aforementioned WEM / a value.
[0053] Multifunctional (meth)acrylate monomers and (meth)acrylate prepolymers can be used alone or in combination.
[0054] It should be noted that in this specification, (meth)acrylate refers to acrylate and / or methacrylate. Other similar terms are the same.
[0055] Examples of multifunctional (meth)acrylate monomers include 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate with hydroxypentanoic acid, dicyclopentyl di(meth)acrylate, caprolactone-modified dicyclopentenyl di(meth)acrylate, ethylene oxide-modified di(meth)acrylate phosphate, allylated cyclohexyl di(meth)acrylate, isocyanurate di(meth)acrylate, and trimethylolpropane tri(meth)acrylate. Multifunctional (meth)acrylates include pentaerythritol tri(meth)acrylate, propionic acid modified pentaerythritol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propylene oxide modified trimethylolpropane tri(meth)acrylate, tri(acryloyloxyethyl)isocyanurate, pentaerythritol tetra(meth)acrylate, propionic acid modified pentaerythritol penta(meth)acrylate, pentaerythritol hexa(meth)acrylate, ethylene oxide modified pentaerythritol hexa(meth)acrylate, and caprolactone modified pentaerythritol hexa(meth)acrylate.
[0056] They can be used individually or in combination of two or more.
[0057] Examples of (meth)acrylate prepolymers include prepolymers of polyester acrylates, epoxy acrylates, urethane acrylates, and polyol acrylates.
[0058] Polyester acrylate prepolymers can be obtained by esterifying the hydroxyl groups of a polyester oligomer with two terminal hydroxyl groups obtained by condensation of a polycarboxylic acid and a polyol using (meth)acrylic acid, or by esterifying the terminal hydroxyl groups of an oligomer obtained by adding an epoxide to a polycarboxylic acid using (meth)acrylic acid.
[0059] Epoxy acrylate prepolymers can be obtained by reacting (meth)acrylic acid with the ethylene oxide ring of bisphenol-type epoxy resin or phenolic varnish-type epoxy resin with a lower molecular weight and then esterifying them.
[0060] Carbamate acrylate prepolymers can be obtained by esterifying polyurethane oligomers obtained by reacting polyether polyols, polyester polyols and polyisocyanates with (meth)acrylic acid.
[0061] Polyol acrylate prepolymers can be obtained by esterifying the hydroxyl groups of polyether polyols with (meth)acrylic acid.
[0062] These prepolymers can be used alone or in combination of two or more.
[0063] (2-2) Particles
[0064] The composition for forming the writing feel improvement layer described in this embodiment preferably contains microparticles. By containing microparticles, the surface of the formed writing feel improvement layer is appropriately roughened, making it easy to adjust the average, maximum, minimum, and standard deviation of the friction force (described later) to the desired range. As a result, the obtained writing feel improvement film exhibits appropriate friction and vibration when written on with a stylus, effectively reproducing the writing feel when writing on paper with a ballpoint pen. Furthermore, the obtained writing feel improvement film readily possesses the desired WEM value, easily satisfying the aforementioned WEM / a value.
[0065] The aforementioned microparticles refer to particles with an average particle size larger than the silica nanoparticles described later. For example, the average particle size is preferably 1–30 μm, more preferably 3–24 μm, particularly preferably 6–18 μm, further preferably 9–16 μm, and even more preferably 11–14 μm. By using microparticles with an average particle size within the above range, the average, maximum, minimum, and standard deviation of the friction force described later can be easily adjusted to the desired range, imparting a moderate frictional and tactile sensation to the writing feel improvement layer, and well reproducing the writing feel when writing on paper with a ballpoint pen. In addition, the WEM can be easily adjusted to the desired value, especially when combined with a protective film, thereby easily achieving excellent anti-peeling effect. It should be noted that the average particle size of the aforementioned microparticles is set to the following value: obtained by measuring a few drops of a 5% by mass dispersion prepared using methyl ethyl ketone as the dispersion medium using a laser diffraction scattering particle size distribution measuring device.
[0066] The microparticles can be inorganic microparticles, organic microparticles, or resin microparticles that possess both inorganic and organic properties. From the viewpoint of improving the hardness of the resulting writing feel layer and facilitating the adjustment of the WEM to the desired value, inorganic microparticles or resin microparticles that possess both inorganic and organic properties are preferred, and resin microparticles that possess both inorganic and organic properties are particularly preferred.
[0067] Inorganic microparticles include those formed from silicon dioxide, aluminum oxide, titanium dioxide, zirconium oxide, tin oxide, indium oxide, cadmium oxide, and antimony oxide. Among these, silicon dioxide microparticles are preferred.
[0068] Examples of organic microparticles include melamine-based resin microparticles, acrylic resin microparticles (such as polymethyl methacrylate resin microparticles), acrylic-styrene copolymer microparticles, polycarbonate microparticles, polyethylene microparticles, polystyrene microparticles, and benzoguanamine resin microparticles. The resin constituting the microparticles may be cross-linked. Among these, acrylic resin microparticles are preferred from the viewpoint of optical properties and hardness, and polymethyl methacrylate resin microparticles are more preferred.
[0069] As resin microparticles that possess both inorganic and organic properties, organosilicon microparticles (such as the Tospearl series manufactured by Momentive) can be listed as suitable materials.
[0070] To further improve dispersibility, the surface of the particles is preferably modified with a surface modifier.
[0071] Furthermore, the shape of the particles can be spherical or non-spherical. In the case of non-spherical particles, they can be irregular shapes, or shapes with a large aspect ratio such as needle-like or scale-like. It should be noted that in this specification, "irregular shape" does not refer to regular shapes such as spheres or ellipses, but rather to irregular shapes with multiple corners or faces. Regarding the resulting improved writing feel layer, from the viewpoints of easily adjusting the average, maximum, minimum, and standard deviation of the friction force (described later) to the desired range and easily adjusting the WEM to the desired value, the shape of the particles is preferably spherical, and especially preferably truly spherical.
[0072] One type of microparticle can be used alone, or two or more types can be used in combination.
[0073] The particulate content in the composition for forming the writing feel improvement layer is preferably 0.1 to 20 parts by weight, more preferably 0.5 to 17 parts by weight, further preferably 1 to 14 parts by weight, even more preferably 3 to 12 parts by weight, and most preferably 6 to 11 parts by weight, relative to 100 parts by weight of the curing component. By keeping the particulate content within the above range, it is easy to adjust the average, maximum, minimum, and standard deviation of the friction force of the resulting writing feel improvement layer (described later) to the desired range, and it is easy to adjust the WEM to the desired value. In particular, by combining it with a protective film, it is easy to achieve excellent anti-peel effect.
[0074] (2-3) Surface conditioner
[0075] The composition for forming the writing feel improvement layer described in this embodiment preferably contains a surface conditioner.
[0076] By incorporating surface modifiers, streaks and unevenness are suppressed in the resulting writing feel improvement layer. This results in a more uniform film thickness, a superior appearance for the writing feel improvement film, and easier attainment of desired optical properties (haze value and total transmittance, etc.). Furthermore, the surface of the writing feel improvement layer tends to exhibit good surface condition, making it easier to adjust the average, maximum, minimum, and standard deviation of the friction force (described later) to the desired range, thus improving the writing feel of the writing feel layer. Additionally, WEM (Waste Elevation Material) can be easily adjusted to the desired value, especially when combined with a protective film, thereby easily achieving excellent anti-warping effects.
[0077] Examples of surface modifiers include silicone-based surface modifiers containing silicone polymers, fluorinated surface modifiers containing fluorinated polymers, acrylic-based surface modifiers containing acrylic polymers, and vinyl-based surface modifiers containing vinyl polymers.
[0078] Here, silicone-based polymers refer to polymers that primarily contain polysiloxane chains, and fluorinated polymers refer to polymers with fluorinated monomers as the main monomer units. Additionally, acrylic polymers refer to polymers with acrylates as the main monomer units. Furthermore, vinyl polymers refer to polymers that contain vinyl monomers as the main monomer units.
[0079] A single surface conditioner can be used alone, or two or more can be used in combination.
[0080] Among these, from the viewpoint of surface conditioning performance and compatibility with other components, organosilicon-based surface conditioners and fluorine-based surface conditioners are preferred.
[0081] As an organosilicon-based surface conditioner, a surface conditioner containing polydimethylsiloxane or modified polydimethylsiloxane is preferred, and a surface conditioner containing polydimethylsiloxane is more preferred.
[0082] As a fluorinated surface modifier, a surface modifier comprising a compound having a perfluoroalkyl or fluorinated alkenyl group in the main chain or side chain is preferred. Examples of commercially available products include BYK-340 manufactured by BYK Corporation, FTERGENT650A manufactured by Neos Corporation, Mega facRS-75 and Mega facRS-90 manufactured by DIC Corporation, and V-8FM manufactured by Osaka Organic Chemical Industry Co., Ltd., but are not limited to these.
[0083] When the composition for forming the writing feel improvement layer contains a surface modifier, the content of the surface modifier in the composition is preferably 0.01 to 10 parts by weight relative to 100 parts by weight of the curing component, more preferably 0.1 to 5 parts by weight, particularly preferably 0.5 to 3 parts by weight, and even more preferably 0.8 to 2 parts by weight. By setting the content of the surface modifier within the above range, the appearance of the writing feel improvement film can be improved. In addition, the average value, maximum value, minimum value, and standard deviation of the friction force (described later) can be easily adjusted to the desired range, resulting in a better writing feel for the writing feel improvement layer.
[0084] (2-4) Other ingredients
[0085] The composition for forming a writing feel improvement layer may also contain other components besides those mentioned above. Examples of such other components include silica nanoparticles, photopolymerization initiators, ultraviolet absorbers, antioxidants, light stabilizers, antistatic agents, silane coupling agents, antioxidants, thermal polymerization inhibitors, surfactants, preservation stabilizers, plasticizers, lubricants, defoamers, organic fillers, wetting modifiers, and coating modifiers.
[0086] By incorporating silica nanoparticles into the composition for forming the writing feel improvement layer, the hardness and scratch resistance of the formed writing feel improvement layer can be effectively improved, thereby facilitating peel resistance. Furthermore, the optical properties (haze value and total transmittance, etc.) of the writing feel improvement film are improved, effectively suppressing roughness during use.
[0087] The average particle size of the silica nanoparticles is preferably 1–300 nm, more preferably 5–100 nm, and particularly preferably 10–50 nm. It should be noted that the average particle size of the silica nanoparticles can be determined using a laser diffraction scattering particle size distribution measuring device.
[0088] Furthermore, silica nanoparticles can be in the form of an organosol (colloidal). By being in the form of an organosol, the dispersibility of silica nanoparticles becomes better, improving the homogeneity and light transmittance of the resulting writing feel enhancement layer.
[0089] When the composition for forming the writing feel improvement layer contains silica nanoparticles, the content of silica nanoparticles in the composition for forming the writing feel improvement layer is preferably 5 to 50 parts by weight relative to 100 parts by weight of the curing component, more preferably 10 to 35 parts by weight, and particularly preferably 15 to 25 parts by weight.
[0090] By setting the mixing ratio of silica nanoparticles to the above range, the homogeneity and light transmittance of the formed writing feel improvement layer can be maintained better.
[0091] When the composition for forming a writing feel improvement layer contains an active energy ray curable component as a curing component, it preferably also contains a photopolymerization initiator. By containing a photopolymerization initiator, the curing reaction achieved by active energy ray irradiation can be carried out more easily.
[0092] Examples of photopolymerization initiators used include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin n-butyl ether, benzoin isobutyl ether, acetophenone, dimethylaminoacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 2-hydroxy-2-methyl-1-phenylpropane-1-one, 1-hydroxycyclohexylphenyl ketone, and 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propane-1-yl ... Benzyl ketone, 4-(2-hydroxyethoxy)phenyl-2-(hydroxy-2-propyl) ketone, benzophenone, p-phenylbenzophenone, 4,4'-diethylaminobenzophenone, dichlorobenzophenone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 2-aminoanthraquinone, 2-methylthioxanthone, 2-ethylthioxanthone, 2-chlorothioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, benzyl dimethyl ketal, acetophenone dimethyl ketal, p-dimethylamino benzoate, etc. These can be used alone or in combination of two or more.
[0093] When the composition for forming a writing feel improvement layer contains a photopolymerization initiator, from the viewpoint of the effect of adding a photopolymerization initiator, the content of the photopolymerization initiator in the composition for forming a writing feel improvement layer is preferably 1 to 20 parts by mass relative to 100 parts by mass of the curing component, more preferably 2 to 10 parts by mass.
[0094] To improve coatability, adjust viscosity, and adjust solid component concentration, the composition for forming a writing feel improvement layer may contain a solvent.
[0095] There are no particular limitations on the solvents used, as long as the curing components dissolve and the particles disperse. Specific examples of solvents include alcohols such as methanol, ethanol, isopropanol, butanol, and octanol; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; esters such as ethyl acetate, butyl acetate, ethyl lactate, and γ-butyrolactone; ethers such as ethylene glycol monomethyl ether (methyl cellosolve), ethylene glycol monoethyl ether (ethyl cellosolve), diethylene glycol monobutyl ether (butyl cellosolve), and propylene glycol monomethyl ether; aromatic hydrocarbons such as benzene, toluene, and xylene; and amides such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone.
[0096] These solvents can be used alone, or in combination of two or more.
[0097] The solvent content is typically 10 to 300 parts by mass relative to 100 parts by mass of the curing component, preferably 30 to 200 parts by mass.
[0098] (3) Methods for forming the writing feel improvement layer
[0099] The writing feel improvement layer can be formed as follows: the writing feel improvement layer forming composition is coated on the aforementioned writing feel improvement film substrate layer in such a way that it becomes a desired film thickness, and the resulting coating film is dried and cured, thereby forming the layer.
[0100] As a method for forming a coating composition for improving writing feel, existing known coating methods can be used, such as rod coating, knife coating, roller coating, plate coating, mold coating, gravure coating, etc.
[0101] The drying temperature of the coating film of the composition for forming the writing feel improvement layer is typically 40–120°C, and the drying time is typically about 30 seconds to 5 minutes.
[0102] When the curing component in the composition for forming a writing feel improvement layer has the curing property of active energy rays, the coating film can be cured by irradiating the coating film of the composition for forming a writing feel improvement layer with active energy rays such as ultraviolet rays or electron rays.
[0103] Ultraviolet (UV) irradiation can be achieved using high-pressure mercury lamps, Heraeus H lamps, xenon lamps, etc. The optimal UV irradiation dose is 50–1000 mW / cm². 2 Light intensity 50–1000 mJ / cm 2 More preferably, the illuminance is 100–500 mW / cm². 2 Light intensity 100–500 mJ / cm 2 .
[0104] Electron beam irradiation can be carried out using electron beam accelerators, etc., and the preferred irradiation dose is about 10 to 1000 krad.
[0105] When the curing component in the composition for forming a writing feel improvement layer is thermosetting, the coating film can be cured by heating the coating film of the composition for forming a writing feel improvement layer at a specified temperature for a specified time.
[0106] The thickness of the formed writing feel improvement layer is not particularly limited, but is preferably 0.8–30 μm, more preferably 1–20 μm, particularly preferably 2–15 μm, more preferably 3–12 μm, more preferably 4–10 μm, and most preferably 5–8 μm. By making the thickness of the writing feel improvement layer within the above range, the writing feel when writing on paper with a ballpoint pen can be reproduced better. In addition, the WEM can be easily adjusted to the desired value, especially when combined with a protective film, thereby easily achieving excellent anti-warping effects.
[0107] The surface of the writing feel improvement layer described in this invention has a moderately textured surface. The maximum height (WEM) of the rounded waviness curve of the writing feel improvement film (writing feel improvement layer) is preferably 0.1 μm or more, more preferably 0.5 μm or more, particularly preferably 1.0 μm or more, and even more preferably 2.0 μm or more. Furthermore, the maximum height (WEM) of the rounded waviness curve of the writing feel improvement layer is preferably 20 μm or less, more preferably 16.0 μm or less, particularly preferably 12.0 μm or less, even more preferably 8.0 μm or less, and most preferably 5.0 μm or less, and most preferably 3.0 μm or less.
[0108] If the WEM (Wide Surface Elevation) falls within this range, it can be inferred that when inputting with a stylus on a touch panel, the stylus tip can moderately scrape the raised areas, allowing for a relatively constant adjustment of the writing feel at the beginning and throughout the writing process. Furthermore, the average, maximum, minimum, and standard deviation of the friction force (described later) can be easily adjusted to the desired range, resulting in a better writing feel from the improved writing feel layer. Moreover, when a writing feel improved layer with a surface shape exhibiting the aforementioned WEM range is adhered to the writing feel improved layer using the adhesive layer of a protective film, the thickness of the adhesive layer and the moderately uneven surface shape of the writing feel improved layer exhibit appropriate adhesion. Therefore, even when subjected to temperature changes during storage, handling, or processing, peeling can be suppressed.
[0109] Furthermore, as described later, the design should be such that the ratio of the WEM to the thickness a (μm) of the adhesive layer of the protective film (WEM / a) is 0.01 or more and 1.00 or less, preferably more than 0.01 and less than 1.00, more preferably 0.03 or more and 0.80 or less, particularly preferably 0.06 or more and 0.70 or less, and even more preferably 0.07 or more and 0.60 or less.
[0110] The maximum height (WEM) of the rounded waviness curve of the writing feel improvement layer can be measured according to JIS B0610:2001. Specifically, it can be measured using the method described in the examples below.
[0111] The arithmetic mean roughness (Ra) of the writing feel improvement film (writing feel improvement layer) is preferably 0.1 to 1 μm, more preferably 0.2 to 0.9 μm, particularly preferably 0.3 to 0.8 μm, and even more preferably 0.4 to 0.7 μm.
[0112] The ten-point average roughness (RzJIS) of the writing feel improvement film (writing feel improvement layer) is preferably 1 to 15 μm, preferably 3 to 10 μm, and particularly preferably 5 to 8 μm.
[0113] Because the arithmetic mean roughness (Ra) and ten-point mean roughness (Rz) of the writing feel improvement film (writing feel improvement layer) are of this value, it is easy to adjust the average, maximum, minimum, and standard deviation of the friction force (described later) to the desired range, thereby improving the writing feel of the writing feel improvement layer. Furthermore, complementing the WEM mentioned above, the writing feel improvement layer exhibits a moderately uneven surface shape, and when the adhesive layer of the protective film is adhered to this writing feel improvement layer, the adhesive layer and the writing feel improvement layer exhibit moderate adhesion. As a result, even when subjected to temperature changes during storage, handling, processing, etc., peeling can be suppressed.
[0114] Arithmetic mean roughness (Ra) and ten-point mean roughness (RzJIS) can be measured according to JIS B0601:2013 using a surface roughness measuring device.
[0115] The average friction force between the writing feel improvement film (writing feel improvement layer) and the stylus pen during writing is preferably 100 to 1200 mN, more preferably 200 to 800 mN, particularly preferably 250 to 500 mN or more, and even more preferably 300 to 400 mN.
[0116] The maximum friction force between the writing feel improvement film (writing feel improvement layer) and the stylus pen during writing is preferably 200 to 1500 mN, particularly preferably 250 to 1000 mN, and even more preferably 300 to 600 mN.
[0117] The minimum friction between the writing feel improvement film (writing feel improvement layer) and the stylus pen during writing is preferably 80 to 1200 mN, more preferably 120 to 1000 mN, particularly preferably 200 to 700 mN, and even more preferably 240 to 500 mN.
[0118] The standard deviation of the friction force between the writing feel improvement film (writing feel improvement layer) and the stylus pen during writing is preferably 10 to 60 mN, more preferably 12 to 45 mN, particularly preferably 14 to 30 mN, and even more preferably 16 to 20 mN.
[0119] By ensuring that the average, maximum, minimum, and standard deviation of the aforementioned frictional forces fall within the range described above, the vibration sensation transmitted to the hand holding the stylus can be easily and accurately reproduced from the vibration sensation obtained when writing on paper with a ballpoint pen. It should be noted that the physical properties related to the aforementioned frictional forces can be measured using the methods described in the embodiments below.
[0120] The writing feel improvement film of the present invention exhibits excellent scratch resistance on the surface of the writing feel improvement layer. In the scratch resistance evaluation using steel wool, no visible change is preferred. Specifically, for the surface of the writing feel improvement layer, according to JIS K5600-5-10, #0000 steel wool is used at 250 g / cm³. 2 After being subjected to a load of 10cm and 10 back-and-forth rubbing, the surface preferably has 3 or fewer scratches, and more preferably no damage. Therefore, when used on the surface of displays such as touch panels, it provides excellent surface protection and maintains the aesthetic appearance of the touch panel.
[0121] The evaluation of scratch resistance can be carried out using the methods described in the test examples below.
[0122] The writing feel improvement film (writing feel improvement layer) of the present invention preferably has a pencil hardness of H or higher, more preferably 2H or higher, particularly preferably 3H or higher, and even more preferably 4H or higher. Furthermore, the pencil hardness is typically 9H or lower, preferably 7H or lower, and more preferably 5H or lower. This hardness provides excellent scratch resistance, resulting in superior surface protection when used on the surface of displays such as touch panels. In particular, the surface is less prone to damage, thus maintaining the aesthetic appearance of the touch panel.
[0123] Pencil hardness can be determined according to JIS K5600 using a pencil scratch hardness tester.
[0124] The total light transmittance (%) of the writing feel improvement film of the present invention is preferably 80% or more, more preferably 85% or more, and even more preferably 90% or more. Therefore, the writing feel improvement film has excellent transparency and can also provide good image recognition when applied to touch panels. The upper limit of the total light transmittance is typically 100%.
[0125] Total transmittance can be measured using a haze meter according to JIS K 7361-1, after calibration with blank material, by illuminating the writing feel improvement layer from the side.
[0126] The writing feel improvement film (writing feel improvement layer) of the present invention preferably has a haze of 0-50%, more preferably 1-40%, particularly preferably 5-30%, and even more preferably 10-22%. Therefore, the writing feel improvement film has excellent transparency and can also provide good image recognition when applied to touch panels.
[0127] Haze can be measured according to JIS K 7136:2000 using a haze meter.
[0128] 2) Protective film
[0129] The writing feel improvement film with a protective film described in this invention uses a protective film having a protective film substrate layer and an adhesive layer. The protective film serves to prevent surface damage and dirt adhesion to the writing feel improvement film.
[0130] (1) Protective film substrate layer
[0131] The material used for the protective film substrate layer described in this embodiment is not particularly limited, and existing known materials used as protective film substrate layers for optical films can be listed. Specifically, materials identical to those exemplified as the aforementioned writing feel improvement film substrate layer can be listed.
[0132] From the viewpoints of processability, ease of acquisition, and easier attainment of the effects of the present invention, the preferred materials are polyethylene terephthalate film, polyethylene terephthalate film, polyethylene naphthalate film, polycarbonate film, polypropylene film, polyimide film, polyetherimide film, polymethylpentene film, polyphenylene sulfide film, and liquid crystal polymer film, and more preferably polyethylene terephthalate film, polypropylene film, and polycarbonate film.
[0133] The protective film substrate layer can be a single layer formed from one of these films, or it can be a layer formed by stacking two or more of these films.
[0134] The protective film substrate layer can undergo surface treatments such as oxidation and embossing, as well as primer treatments, similar to those described in the section on writing feel improvement film substrate layers. These surface treatment methods are appropriately selected depending on the type of protective film substrate layer.
[0135] From the perspectives of operability and cost, the thickness of the protective film substrate layer can be appropriately set. The thickness of the protective film substrate layer is preferably 10–300 μm, more preferably 20–200 μm, particularly preferably 25–150 μm or more, further preferably 30–120 μm, and more preferably 35–110 μm. Therefore, the interlayer peel strength, as described later, can easily be within a specified range.
[0136] (2) Adhesive layer
[0137] The adhesive layer enables the protective film substrate layer to be bonded to the writing feel improvement film more easily and firmly.
[0138] As the adhesive constituting the adhesive layer, adhesives commonly used in optical film applications can be used. Examples include acrylic adhesives, rubber adhesives, silicone adhesives, urethane adhesives, polyester adhesives, and polyvinyl ether adhesives. Furthermore, the adhesive can be any of the following: emulsion type, solvent type, or solvent-free type. Moreover, the adhesive may or may not have a cross-linked structure.
[0139] Among these, from the viewpoint of exhibiting excellent desired adhesion, optical properties, and durability, acrylic adhesives containing (meth)acrylate polymers as the base polymer are preferred, and acrylic adhesives containing (meth)acrylate polymers as the base polymer and having a cross-linked structure are more preferred. It should be noted that in this specification, "polymer" also includes the concept of "copolymer".
[0140] From the perspectives of transparency and adhesion, the monomer units constituting the above-mentioned (meth)acrylate polymers can be appropriately selected, and monomers containing alkyl (meth)acrylates and reactive functional groups within the molecule are particularly preferred (monomers containing reactive functional groups).
[0141] (Meth)acrylate polymers exhibit preferred adhesive properties by containing alkyl (meth)acrylates as monomeric units constituting the polymer. Alkyl (meth)acrylates are preferably those with 1 to 20 carbon atoms in the alkyl group. The alkyl group can be linear, branched, or have a cyclic structure.
[0142] Alkyl methacrylates having 1 to 20 carbon atoms as alkyl groups include, for example, methyl methacrylate, ethyl methacrylate, propyl methacrylate, n-butyl methacrylate, n-pentyl methacrylate, n-hexyl methacrylate, 2-ethylhexyl methacrylate, isooctyl methacrylate, n-decyl methacrylate, n-dodecyl methacrylate, myristyl methacrylate, palmitate methacrylate, stearate methacrylate, cyclohexyl methacrylate, isobornyl methacrylate, and adamantyl methacrylate. Among these, methyl methacrylate and 2-ethylhexyl methacrylate are preferred from the viewpoint of easily adjusting the interlayer peel strength (described later) to the desired value. They can be used alone or in combination of two or more.
[0143] In (meth)acrylate polymers, as monomer units constituting the polymer, it is preferable to contain 30 to 99.9% by mass of alkyl (meth)acrylates relative to all monomer units, particularly preferably 50 to 99.5% by mass, and even more preferably 70 to 99% by mass. By using this range, the interlayer peel strength, described later, can be easily adjusted to the desired value.
[0144] (Meth)acrylate polymers contain monomers with reactive functional groups as monomer units constituting the polymer. These monomers react with a crosslinking agent (described later) via the reactive functional groups derived from the monomers containing reactive functional groups, thereby forming a crosslinked structure (three-dimensional network structure) and obtaining an adhesive with desired cohesive strength.
[0145] Monomers containing reactive functional groups are preferably examples of monomers with intramolecular hydroxyl groups (hydroxyl-containing monomers), monomers with intramolecular carboxyl groups (carboxyl-containing monomers), and monomers with intramolecular amino groups (amino-containing monomers). Among these, hydroxyl-containing monomers or carboxyl-containing monomers are preferred from the viewpoints of easily adjusting crosslinking density, easily obtaining adhesives with desired cohesive strength, and interlayer peel strength (described later). These monomers containing reactive functional groups can be used alone or in combination of two or more.
[0146] Examples of hydroxyl-containing monomers include 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 3-hydroxypropyl methacrylate, 2-hydroxybutyl methacrylate, 3-hydroxybutyl methacrylate, 4-hydroxybutyl methacrylate, and other hydroxyalkyl methacrylates. Among these, hydroxyalkyl methacrylates having 1 to 4 carbon atoms are preferred. They can be used alone or in combination of two or more.
[0147] Examples of carboxyl-containing monomers include olefinic unsaturated carboxylic acids such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, itaconic acid, and citraconic acid. Among these, acrylic acid is preferred from the viewpoint of easily satisfying the interlayer peel strength described later. They can be used alone or in combination of two or more.
[0148] In (meth)acrylate polymers, as monomer units constituting the polymer, it is preferable to contain 0.1 to 20% by mass of monomers containing reactive functional groups, more preferably 0.5 to 10% by mass, and particularly preferably 0.8 to 3% by mass, relative to all monomer units. Therefore, the (meth)acrylate polymer readily undergoes the desired crosslinking reaction between crosslinking agents, resulting in an adhesive that readily exhibits good cohesive strength and easily adjusts the interlayer peel strength (described later) to the desired value.
[0149] In (meth)acrylate polymers, other monomers may also be included as constituent monomers. Examples of such other monomers include (meth)acrylates containing an alicyclic structure, such as glycidyl methacrylate, dicyclopentyl methacrylate, adamantyl methacrylate, isobornyl methacrylate, dicyclopentenyl methacrylate, and dicyclopentenoxyethyl methacrylate; (meth)acrylate alkoxyalkyl methacrylates such as methoxyethyl methacrylate and ethoxyethyl methacrylate; non-crosslinked acrylamides such as acrylamide and methacrylamide; non-crosslinked (meth)acrylates with tertiary amino groups such as N,N-dimethylaminoethyl methacrylate and N,N-dimethylaminopropyl methacrylate; vinyl acetate; and styrene. From the viewpoints of the cohesive strength of the resulting (meth)acrylate polymer (A) and the interlayer peel strength (described later), glycidyl methacrylate is preferred, and particularly preferred. These monomers may be used alone or in combination of two or more.
[0150] In (meth)acrylate polymers, as monomer units constituting the polymer, it is preferable to contain 0.1 to 10% by mass of other monomers relative to all monomer units, particularly preferably 0.2 to 5% by mass, and even more preferably 0.3 to 1% by mass. As a result, the resulting adhesive readily exhibits good cohesive strength, and the interlayer peel strength (described later) can be easily adjusted to the desired value.
[0151] The polymerization method of the (meth)acrylate polymer in this embodiment is not particularly limited; it can be a random polymer or a block polymer. Furthermore, the acrylic polymer can be obtained by polymerizing the above-mentioned monomers using conventional methods. It can be prepared by polymerization methods such as emulsion polymerization, solution polymerization, suspension polymerization, bulk polymerization, and aqueous solution polymerization. From the viewpoint of stability during polymerization and ease of handling during use, solution polymerization in an organic solvent is preferred.
[0152] The weight-average molecular weight of the (meth)acrylate polymer is preferably 100,000 to 3,000,000, more preferably 300,000 to 2,000,000, particularly preferably 450,000 to 1,500,000, and even more preferably 600,000 to 1,000,000. Therefore, the resulting adhesive readily exhibits good cohesive strength, and the interlayer peel strength (described later) can be easily adjusted to the desired value.
[0153] It should be noted that the adhesive composition described in this embodiment may contain one of the above-mentioned (meth)acrylate polymers, or it may contain two or more. Furthermore, the adhesive composition described in this embodiment may contain both the above-mentioned (meth)acrylate polymer and other (meth)acrylate polymers.
[0154] By including a crosslinking agent, the above-mentioned (meth)acrylate polymer can be crosslinked by heating the adhesive composition, thus forming a good three-dimensional network structure. This further improves the cohesive strength of the resulting adhesive, making it easier to adjust the interlayer peel strength (described later) to the desired value.
[0155] Examples of crosslinking agents are preferably those that react with the reactive functional groups present in (meth)acrylate polymers. Examples include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, amine-based crosslinking agents, melamine-based crosslinking agents, aziridine-based crosslinking agents, hydrazine-based crosslinking agents, aldehyde-based crosslinking agents, oxazoline-based crosslinking agents, metal alkoxide-based crosslinking agents, metal chelate-based crosslinking agents, metal salt-based crosslinking agents, and ammonium salt-based crosslinking agents.
[0156] Among the aforementioned crosslinking agents, isocyanate-based, epoxy-based, and aziridine-based crosslinking agents are preferred from the viewpoints of readily reacting with the reactive functional groups of (meth)acrylate polymers and readily adjusting the interlayer peel strength to the desired value. One type of crosslinking agent may be used alone, or two or more may be used in combination.
[0157] When the adhesive composition contains a crosslinking agent and a (meth)acrylate polymer, the content of the crosslinking agent in the adhesive composition is preferably 0.01 to 5 parts by weight relative to 100 parts by weight of the (meth)acrylate polymer, more preferably 0.1 to 4 parts by weight, particularly preferably 0.5 to 3 parts by weight, and even more preferably 1 to 2 parts by weight. As a result, the resulting adhesive readily exhibits superior cohesive strength, and the interlayer peel strength (described later) is easily adjusted to the desired value.
[0158] In addition, the adhesive layer may contain other components depending on the purpose.
[0159] Other components include tackifiers, plasticizers, antistatic agents, UV absorbers, silane coupling agents, rust inhibitors, antioxidants, light stabilizers, softeners, and refractive index modifiers. It should be noted that polymerization solvents and diluents derived from the manufacture of (meth)acrylate polymers are not included in the additives constituting the adhesive composition.
[0160] When the adhesive composition contains a plasticizer, the content of the crosslinking agent in the adhesive composition is preferably 0.1 to 50 parts by weight relative to 100 parts by weight of the (meth)acrylate polymer, more preferably 1 to 35 parts by weight, particularly preferably 4 to 20 parts by weight, and even more preferably 8 to 15 parts by weight. As a result, the resulting adhesive readily exhibits superior cohesive strength and easily adjusts the interlayer peel strength (described later) to the desired value.
[0161] The storage modulus of the adhesive described in this invention is preferably 0.010–1 MPa, more preferably 0.011–0.6 MPa, and particularly preferably 0.012–0.3 MPa. Therefore, the adhesive layer and the writing feel improvement layer easily achieve adequate adhesion, resulting in good peel resistance.
[0162] The energy storage modulus can be determined according to JIS K7244-1.
[0163] The thickness 'a' of the adhesive layer is preferably 3 μm or more, more preferably 5 μm or more, and particularly preferably 10 μm or more. Furthermore, the thickness of the adhesive layer is typically 300 μm or less. Moreover, from the viewpoint of better reproducing the writing feel of writing on paper with a ballpoint pen and from the viewpoint of reducing the overall thickness of the touch panel with the writing feel improvement film, it is preferably 200 μm or less, more preferably 100 μm or less, particularly preferably 50 μm or less, and most preferably 30 μm or less.
[0164] In addition, as will be described later, the design should be carried out in such a way that the ratio of the WEM of the writing feel improvement layer to the thickness a (μm) of the adhesive layer (WEM / a) of the aforementioned writing feel improvement film is 0.01 or more and 1.00 or less.
[0165] (3) Protective film
[0166] There are no particular limitations on the method for manufacturing a protective film with an adhesive layer. For example, it can be formed by applying an adhesive layer forming composition to a protective film substrate layer in a manner that achieves a desired film thickness using a known coating method, and then drying the resulting coating.
[0167] Compositions for forming adhesive layers typically contain a base polymer, a solvent, a crosslinking agent, and, as desired, microparticles, tackifiers, plasticizers, antistatic agents, UV absorbers, etc.
[0168] It should be noted that the protective film can also be made by forming an adhesive layer on the aforementioned writing feel improvement layer, overlapping a protective film substrate on it, and then pressing (laminating).
[0169] 3) Improved writing feel with a protective film
[0170] The writing feel improvement film with protective film of the present invention is formed by laminating the writing feel improvement layer of the aforementioned writing feel improvement film with the adhesive layer of the protective film.
[0171] The writing feel improvement film with protective film of the present invention can be long strip (strip) or short strip (single sheet).
[0172] A schematic diagram of the layer structure of the writing feel improvement film with protective film of the present invention is shown below. Figure 1 .
[0173] That is, the writing feel improvement film with protective film of the present invention is formed by laminating the writing feel improvement film 10 and the protective film 20 in such a way that the writing feel improvement layer 2 and the adhesive layer 3 of the protective film are in contact.
[0174] The method for manufacturing the writing feel improvement film with a protective film of the present invention is not particularly limited. For example, it can be manufactured by overlapping and laminating the aforementioned writing feel improvement film and protective film in such a way that the writing feel improvement layer and adhesive layer are in contact.
[0175] In addition, as described above, by forming an adhesive layer on the writing feel improvement layer of the aforementioned writing feel improvement film and laminating a protective film substrate thereon, it is also possible to produce the writing feel improvement film with a protective film of the present invention.
[0176] Regarding the writing feel improvement film with a protective film of the present invention, the ratio of the maximum height of the rounded waviness curve (WEM) of the writing feel improvement layer to the thickness a (μm) of the aforementioned adhesive layer, "WEM / a", is preferably 0.01 or more, more preferably more than 0.01, particularly preferably 0.03 or more, further preferably 0.06 or more, and preferably 0.07 or more. Furthermore, "WEM / a" is preferably 1.00 or less, more preferably less than 1.00, particularly preferably 0.80 or less, further preferably 0.70 or less, and preferably 0.60 or less.
[0177] The writing feel improvement film with protective film of the present invention is designed so that the value of "WEM / a" falls within this range. Therefore, even if temperature changes occur during storage, transportation, processing, etc., the protective film and the writing feel improvement film are not prone to floating or peeling, thus maintaining the quality of the writing feel improvement film.
[0178] In the writing feel improvement film with a protective film of the present invention, in order to make the value of "WEM / a" fall within the above range, it is preferable to use (i) a writing feel improvement film in which the thickness a of the adhesive layer of the protective film is adjusted according to the WEM value of the writing feel improvement layer or (ii) a writing feel improvement film containing a writing feel improvement layer with an appropriate WEM according to the thickness a of the adhesive layer of the protective film.
[0179] The fact that the protective film and the writing feel improvement film are unlikely to lift or peel off between the layers can be confirmed by, for example, that even if a sample (5cm × 5cm) of the writing feel improvement film with the protective film is placed in an oven maintained at 90°C for 1 hour, the peeling from the end is less than 1cm. The degree of peeling from this end is preferably less than 1cm, more preferably less than 0.5cm, particularly preferably less than 0.3cm, and even more preferably less than 0.1cm.
[0180] In the writing feel improvement film with a protective film of the present invention, the interlayer peel strength between the writing feel improvement film and the protective film is preferably 800mN / 25mm or less. This will be described in detail below.
[0181] In the writing feel improvement film with protective film of the present invention, the interlayer peel force between the writing feel improvement layer surface of the writing feel improvement film and the protective film is preferably 800mN / 25mm or less, more preferably 500mN / 25mm or less, particularly preferably 300mN / 25mm or less, further preferably 200mN / 25mm or less, and most preferably 150mN / 25mm or less after being placed in an oven maintained at 90°C for 1 hour.
[0182] Furthermore, from the viewpoint of preventing the self-writing feel improvement film from unintentionally floating or peeling when exposed to temperature changes, the lower limit of the interlayer peel force is preferably 1 mN / 25 mm or more, more preferably 3 mN / 25 mm or more, particularly preferably 6 mN / 25 mm or more, and even more preferably 10 mN / 25 mm or more.
[0183] By possessing this interlayer peeling force, it more effectively suppresses the occurrence of lifting and peeling caused by temperature changes during storage, handling, and processing, thus maintaining the quality of the writing feel improvement film and allowing the protective film to be easily peeled off from the writing feel improvement film during use.
[0184] In the writing feel improvement film with protective film of the present invention, the interlayer peel force between the writing feel improvement layer surface of the writing feel improvement film and the protective film, before the application of a thermal process accompanied by a temperature change of 90°C for 1 hour, is preferably 800 mN / 25 mm or less, more preferably 500 mN / 25 mm or less, particularly preferably 200 mN / 25 mm or less, further preferably 120 mN / 25 mm or less, and most preferably 90 mN / 25 mm or less.
[0185] Furthermore, from the viewpoint of preventing the self-writing feel improvement film from unintentionally floating or peeling when exposed to temperature changes, the lower limit of the interlayer peel force is preferably 5mN / 25mm or more, more preferably 8mN / 25mm or more, particularly preferably 11mN / 25mm or more, and even more preferably 14mN / 25mm or more.
[0186] By possessing this interlayer peeling force, the occurrence of lifting and peeling caused by temperature changes during storage, handling, and processing can be more effectively controlled, thus maintaining the quality of the writing feel improvement film and allowing the self-writing feel improvement film to be easily peeled off and the protective film removed during use.
[0187] The interlayer peel strength between the writing feel improvement film and the protective film can be measured using the method described in the examples.
[0188] The writing feel improvement film with a protective film of the present invention can be used to peel off the protective film from the writing feel improvement film and form the outermost writing feel improvement film of the touch panel (image display device with position detection function) to be used with a stylus.
[0189] Specifically, a writing feel improvement film is laminated onto a cover material in a touch panel that includes display modules such as liquid crystal (LCD) modules, light-emitting diode (LED) modules, organic electroluminescent (OLED) modules, and contact sensors, in such a manner that the aforementioned cover material contacts the writing feel improvement film substrate layer. The writing feel improvement film can be adhered using an adhesive layer.
[0190] As a stylus that uses a writing-enhancing film, there are no particular limitations; examples include styluses with polyacetal tips, styluses with stiff felt tips, and styluses with flexible tips.
[0191] The embodiments described above are for the purpose of facilitating understanding of the present invention and are not intended to limit the present invention in any way. Therefore, the elements disclosed in the above embodiments also include all design modifications and equivalents that fall within the scope of the present invention.
[0192] For example, the writing feel improvement film with a protective film of the present invention may be laminated with other layers. Examples of other layers include an adhesive layer, a release film, etc., laminated to the writing feel improvement film substrate layer side.
[0193] It should be noted that when "X~Y" (where X and Y are arbitrary numbers) are used in this specification, unless otherwise specified, they include the meaning of "X or more and Y or less," as well as the meaning of "preferably greater than X" or "preferably less than Y." Furthermore, when "X or more" (where X is any number) is used, unless otherwise specified, it includes the meaning of "preferably greater than X," and when "Y or less" (where Y is any number) is used, unless otherwise specified, it includes the meaning of "preferably less than Y."
[0194] Example
[0195] The present invention will now be described in more detail through examples, etc., but the scope of the present invention is not limited to these examples, etc.
[0196] (Manufacturing Example 1) Preparation of Writing Sensitivity Improvement Film A
[0197] Composition A for forming a writing feel improvement layer is prepared by mixing 100 parts by mass of an active energy-curable component containing polyfunctional urethane acrylate (product name "Opstar Z7530", manufactured by Arakawa Chemical Industry Co., Ltd.; the conversion value is for solid components. The same applies to other components except solvents below.), 9.0 parts by mass of silicone microparticles (Tospearl 1100, manufactured by Momentive, average particle size: 11.0 μm, true spherical), 1.0 part by mass of a fluorinated surface conditioner (Megafac RS-90, manufactured by DIC), 0.3 parts by mass of a silicone surface conditioner (SH28, manufactured by Dow & Toray Industries, polydimethylsiloxane), and 85.5 parts by mass of 1-methoxy-2-propanol as a solvent.
[0198] On a polyethylene terephthalate (PET) film (Lumirror U403, thickness: 188 μm, manufactured by Toray Industries, Inc.) used as the substrate layer of the writing feel improvement film, a writing feel improvement layer forming composition A was formed by coating with a Mayer rod to a thickness of 7 μm, and then dried in an oven at 70°C for 1 minute.
[0199] Next, using an ultraviolet irradiation device (EYE GRANTAGEECS-401GX type, manufactured by EYEGRAPHICS), a high-pressure mercury lamp is used as the light source to irradiate the aforementioned coating under the following irradiation conditions to cure the coating and create a writing feel improvement film A.
[0200] (Ultraviolet radiation conditions)
[0201] Light power: 2kW
[0202] Transmission speed: 4.23m / min
[0203] Illuminance: 240mW / cm 2
[0204] Light intensity: 307 mJ / cm 2
[0205] The maximum height of the rounded waviness curve (WEM), the arithmetic mean roughness (Ra), and the ten-point mean roughness (RzJIS) of the writing feel improvement layer of the obtained writing feel improvement film A were determined using the method shown below.
[0206] The resulting writing feel improvement film A has a WEM of 2.40 μm, Ra of 0.66 μm, and RzJIS of 6.14 μm.
[0207] <Maximum Height of Rounded Wavy Curve (WEM)>
[0208] WEM was measured using a surface roughness shape measuring machine (SV3000S4, manufactured by Mitutoyo) under the following conditions, in accordance with JIS B0610:2001.
[0209] The shape of the measuring head's tip: spherical
[0210] The front radius of the measuring head: 800 μm
[0211] Sliding speed: 0.5mm / s
[0212] Measurement length: 16mm
[0213] <Ra,RzJIS>
[0214] For the surface of the writing feel improvement layer in writing feel improvement sheets A, B, and C, the arithmetic mean surface roughness Ra (μm) and the ten-point mean surface roughness RzJIS (μm) were measured using a surface roughness shape measuring machine (SV3000S4, manufactured by Mitutoyo) in accordance with JIS B0601:2013.
[0215] (Manufacturing Example 2) Preparation of Writing Sensitivity Improvement Film B
[0216] In Manufacturing Example 1, 1 part by mass of true spherical microparticles composed of cross-linked polymethyl methacrylate (SSX-110, average particle size: 10 μm, manufactured by Sekisui Chemicals Co., Ltd.) was used to replace 9.0 parts by mass of silicone microparticles. Otherwise, the same procedure as in Manufacturing Example 1 was followed to prepare writing feel improved film B.
[0217] The resulting writing feel improvement film B has a WEM of 6.28 μm, Ra of 0.26 μm, and Rz of 4.03 μm.
[0218] (Manufacturing Example 3) Preparation of Writing Sensitivity Improvement Film C
[0219] In Manufacturing Example 1, 1 part by mass of true spherical microparticles composed of cross-linked polymethyl methacrylate (SSX-120, average particle size: 20 μm, manufactured by Sekisui Chemicals Co., Ltd.) was used to replace 9.0 parts by mass of silicone microparticles. Otherwise, the same procedure as in Manufacturing Example 1 was followed to prepare a writing feel improvement film C.
[0220] The resulting writing feel improvement film C has a WEM of 15.5 μm, Ra of 0.34 μm, and Rz of 8.92 μm.
[0221] [Friction Measurement]
[0222] The friction between the improved writing feel films A, B, and C and the stylus (product name "ACK-2003", pen tip material: felt, pen tip diameter: 0.5 mm, manufactured by Wacom) during writing was measured using a dynamic and static friction tester (Tribomaster TL201Ts, manufactured by TrinityLab) under the following conditions.
[0223] (Measurement conditions)
[0224] Load capacity: 200g
[0225] Test length: 10–100 mm
[0226] Speed: 1.6 mm / s (Vibration measurement conditions, dynamic friction coefficient measurement conditions)
[0227] Sampling interval: 50ms
[0228] stylus tip angle: 45°
[0229] The average friction force of the writing feel improvement film A is 310 mN, the maximum friction force is 350 mN, the minimum friction force is 240 mN, and the standard deviation of the friction force is 17 mN. The average friction force of the writing feel improvement film B is 220 mN, the maximum friction force is 280 mN, the minimum friction force is 220 mN, and the standard deviation of the friction force is 17 mN. The average friction force of the writing feel improvement film C is 190 mN, the maximum friction force is 240 mN, the minimum friction force is 210 mN, and the standard deviation of the friction force is 22 mN.
[0230] [Pencil Hardness]
[0231] The writing feel improvement layer surface of the obtained writing feel improvement films A, B, and C was tested for pencil hardness using a pencil scratch hardness tester (product name "No. 553-M", manufactured by Yasuda Seiki Co., Ltd.) in accordance with JIS K5600.
[0232] The pencil hardness of the writing feel improvement film A is 4H, while the pencil hardness of the writing feel improvement films B and C is 3H.
[0233] [Scratch resistance]
[0234] For the surface of the writing feel improvement layer in films A, B, and C, according to JIS K5600-5-10, #0000 steel wool was used at 250g / cm². 2 The surface was rubbed back and forth 10 times under a load and a sliding distance of 10 cm. Afterward, the surface of the writing feel improvement layer was visually inspected under a three-wavelength fluorescent lamp for any scratches, and evaluated according to the following criteria.
[0235] ○: No changes were observed in the appearance of the writing feel improvement layer (0 scratches were detected).
[0236] △: The appearance of the improved writing feel layer has been slightly altered (the number of scratches detected is more than 1 but less than 3).
[0237] ×: The appearance of the improved writing feel layer has been significantly altered (more than 4 scratches have been identified).
[0238] As a result, the writing feel improvement films A and B were 0, and the writing feel improvement film C was △.
[0239] (Manufacturing Example 4) Preparation of Composition D for Adhesive Layer Formation
[0240] A (meth)acrylate polymer was prepared by copolymerizing 70 parts by weight of 2-ethylhexyl acrylate, 28.6 parts by weight of methyl acrylate, 0.3 parts by weight of glycidyl methacrylate, and 1.1 parts by weight of acrylic acid. The weight-average molecular weight (Mw) of the obtained (meth)acrylate polymer was 800,000 when the molecular weight was determined using the method shown below.
[0241] The weight-average molecular weight (Mw) is the weight-average molecular weight of polystyrene obtained by gel permeation chromatography (GPC) under the following conditions (GPC determination).
[0242] (Measurement conditions)
[0243] • GPC measuring device: HLC-8020, manufactured by Tosoh Corporation
[0244] • GPC pillars (passing in the following order): Made by Tosoh Corporation
[0245] TSK guard column HXL-H
[0246] TSK gel GMHXL (×2)
[0247] TSK gel G2000HXL
[0248] • Solvent for determination: Tetrahydrofuran
[0249] • Measurement temperature: 40℃
[0250] Composition D for forming an adhesive layer is prepared by mixing 100 parts by mass of the (meth)acrylate polymer obtained above (representing the conversion value of solid content; the same applies to other components except solvent below), 10.0 parts by mass of dibutoxyethoxyethyl adipate as a plasticizer, 0.9 parts by mass of aziridine crosslinking agent (BXX-5134, manufactured by Toyo Chemical Co., Ltd.) as a crosslinking agent, and 87 parts by mass of toluene as a solvent.
[0251] (Manufacturing Example 5) Preparation of Composition E for Adhesive Layer Formation
[0252] In Manufacturing Example 4, 1.9 parts by weight of crosslinking agent were used instead of 0.9 parts by weight. Otherwise, the same procedure as in Manufacturing Example 4 was followed to prepare the adhesive layer forming composition E.
[0253] (Manufacturing Example 6) Preparation of Composition F for Adhesive Layer Formation
[0254] In Manufacturing Example 4, 2.8 parts by weight of crosslinking agent were used instead of 0.9 parts by weight. Otherwise, the same procedure as in Manufacturing Example 4 was followed to prepare the adhesive layer forming composition F.
[0255] (Example 1)
[0256] On a polyethylene terephthalate (PET) film (Lumirror, thickness: 38 μm, manufactured by Toray Industries, Inc.) serving as the protective film substrate layer, the adhesive layer forming composition D obtained in Manufacturing Example 4 was applied using a coater to a film thickness of 10 μm, forming an adhesive layer coating. Subsequently, the coating was placed in an oven maintained at 100°C for 1 minute to dry, resulting in a protective film comprising the protective film substrate layer and the adhesive layer.
[0257] Next, the adhesive layer of the obtained protective film is laminated with the writing feel improvement layer of the writing feel improvement film A obtained in Manufacturing Example 1 in a face-to-face contact manner to produce a writing feel improvement film with a protective film.
[0258] (Examples 2-15, Comparative Examples 1-3)
[0259] In Example 1, the type of writing feel improvement film used, the type of adhesive layer forming composition, and the thickness of the adhesive layer were set as shown in Table 1 below. Otherwise, the same procedure as in Example 1 was followed to produce writing feel improvement films with protective films for Examples 2 to 15 and Comparative Examples 1 to 3.
[0260] The maximum height (WEM) of the rounded waviness curve of the adhesive layer of the writing feel improvement film with protective film obtained in Examples 1-15 and Comparative Examples 1-3 is shown in Table 1.
[0261] For the writing feel improvement films with protective films obtained in Examples 1-15 and Comparative Examples 1-3, a peel test was conducted using the method shown below.
[0262] The results are shown in Table 1.
[0263] <Peeling Test>
[0264] The resulting writing feel improvement film with a protective film was cut into 5cm squares and used as samples. The protective film side of each sample was placed face down in an oven maintained at 90°C. After being placed in the oven for 1 hour, the peeling (cm) between the writing feel improvement layer and the protective film was measured and evaluated according to the following criteria.
[0265] It should be noted that the temperature before the experiment was 23℃.
[0266] 5: Not stripped
[0267] 4: Peeling less than 0.5 cm from the end was observed.
[0268] 3: Peeling was observed with a length of 0.5 cm or more but less than 1.0 cm from the end.
[0269] 2: Peeling was observed with a length of 1.0 cm or more but less than 1.5 cm from the end.
[0270] 1: Peeling of more than 1.5 cm was observed from the end.
[0271] In addition, the interlayer peel force (adhesion) of the protective film and the writing feel improvement film before and after the peel test, as well as the writing feel of the writing feel improvement film after the peel test, were measured by the method shown below.
[0272] The results are shown in Table 1.
[0273] <Interlayer peel strength>
[0274] The resulting writing feel improvement film with protective coating was cut into test pieces 25 mm wide and 110 mm long. For the test pieces, the interlayer peel force (N / 25 mm) when peeling the protective film from the writing feel improvement film was measured using a tensile testing machine (TENSILON, ORIENTEC) according to JIS Z0237:2009, at a peel speed of 300 mm / min and a peel angle of 180°.
[0275] <Evaluation of the writing style>
[0276] Prepare paper (product name "Campus loose-leaf", model: No-S816B, size: B5, grid width: B grid, manufactured by Kokuyo Co., Ltd., to be used in 20-sheet stacks) and a ballpoint pen (product name "Orange EG 1.0", oil-based ballpoint pen, nib diameter: 1.0mm, manufactured by BIC Co., Ltd.). The evaluator uses the ballpoint pen to write the letters "ABCDE" on the paper.
[0277] Next, the protective film was peeled off from the writing feel improvement film after the peel test, and double-sided tape was used to attach it to a glass plate (70mm long, 150mm wide, and 1.2mm thick) to expose the writing feel improvement layer. The letters "ABCDE" were then written on the surface of the writing feel improvement layer using a stylus.
[0278] The writing feel (x) of actually writing on paper with a ballpoint pen is compared with the writing feel (y) of writing with a stylus-enhanced writing layer, and the writing feel is evaluated according to the following criteria.
[0279] (Evaluation Criteria)
[0280] ◎: The writing feel (y) has a vibration and resistance feel very similar to the writing feel (x), resulting in good writing comfort.
[0281] 〇: The writing feel (y) is similar to the writing feel (x), with slight differences in vibration and resistance, but the writing comfort is good.
[0282] △: The writing feel (y) differs from the writing feel (x) in terms of vibration and resistance, but the writing comfort is within an acceptable range.
[0283] ×: Compared to writing feel (x), writing feel (y) has different vibration and resistance sensations, making it difficult to write and resulting in poor writing comfort.
[0284] [Table 1]
[0285]
[0286] According to Table 1, in the writing feel improvement films with protective films in Examples 1 to 15, where the WEM / a value is 0.01 or higher and 1.00 or lower, the peel test evaluation is 3 or higher, and the occurrence of heat-induced lifting and peeling is suppressed.
[0287] Furthermore, it can be seen that the writing feel is also good, and the quality of the writing feel improvement layer has been maintained.
[0288] On the other hand, it can be seen that in Comparative Examples 1 to 3, the peel test evaluation was 1 or 2, indicating that peeling occurred due to heat, and the quality of the writing feel improvement layer was damaged.
[0289] Explanation of reference numerals in the attached figures
[0290] 1…Improved writing feel of the film substrate layer
[0291] 2… Improved writing experience layer
[0292] 3… Adhesive layer
[0293] 4… Protective film substrate layer
[0294] 10… Improved writing feel membrane
[0295] 20…protective film
Claims
1. A writing feel-improved film with a protective film, characterized by, It is a writing-feel-improving film having a writing-feel-improving film substrate layer and a writing-feel-improving layer, and a protective film having an adhesive layer and a protective film substrate layer, wherein the writing-feel-improving layer of the writing-feel-improving film is in contact with the adhesive layer of the protective film, thus forming a writing-feel-improving film with a protective film. The maximum height (WEM) of the rounded waviness curve of the writing feel improvement layer is above 0.1 μm and below 20 μm. The arithmetic mean roughness (Ra) of the writing feel improvement layer is 0.1~1μm. The ten-point average roughness (RzJIS) of the writing feel improvement layer is 1~15μm. The average friction between the writing feel improvement film and the stylus during writing is 100~1200mN. The ratio of the maximum height (WEM) of the rounded ripple curve of the writing feel improvement layer to the thickness a (μm) of the adhesive layer (WEM / a) is greater than 0.01 and less than 1.
00.
2. The writing feel-improved film with a protective film according to claim 1, characterized by, The maximum height (WEM) of the rounded ripple curve of the writing feel improvement layer is above 0.5 μm and below 16.0 μm.
3. The writing feel-improved film with a protective film according to claim 1 or 2, characterized by, The thickness a (μm) of the adhesive layer is greater than 5 μm and less than 50 μm.
4. The writing feel-improved film with a protective film according to claim 1 or 2, wherein, The interlayer peel strength between the writing feel improvement film and the protective film is below 800mN / 25mm.
Citation Information
Patent Citations
Transparent film, method for using the same, and touch panel
JP2014097649A
Antiglare hard coat film
JP2014232276A
Transparent tactile film and method for producing the same
JP2015054417A
Transparent laminated film
JP2016196113A
Transparent film, method for using the same, and touch panel
US20150291828A1