A yellowing-resistant polyvinylidene fluoride heat shrink tubing and its preparation method

By adding sarin resin and NOR-type hindered amine stabilizer to polyvinylidene fluoride heat shrink tubing, and combining extrusion and irradiation processes, the problem of yellowing of polyvinylidene fluoride resin was solved, and the transparency and flexibility of the material were improved.

CN119192754BActive Publication Date: 2026-11-17SHENZHEN WOER HEAT SHRINKABLE MATERIAL
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411043708.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2026-11-17
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

Polyvinylidene fluoride resin is prone to yellowing during processing and manufacturing, which affects the appearance and transparency of the product and limits its widespread application.

Method used

Using sarin resin and NOR-type hindered amine stabilizers as additives, yellowing-resistant polyvinylidene fluoride heat shrink tubing was prepared through extrusion, irradiation, and expansion molding processes. The sarin resin consumed hydrogen fluoride, and the NOR-type hindered amine stabilizers inhibited free radical reactions and reduced the formation of conjugated structures.

Benefits of technology

It effectively reduces the yellowing phenomenon of polyvinylidene fluoride during processing and use, improves the transparency and flexibility of the material, and meets the requirements of product appearance and use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0005078141990000071
    Figure GDA0005078141990000071
  • Figure GDA0005078141990000141
    Figure GDA0005078141990000141
  • Figure GDA0005078141990000151
    Figure GDA0005078141990000151
Patent Text Reader

Abstract

This invention discloses a yellowing-resistant polyvinylidene fluoride (PVDF) heat shrink tubing, which is prepared from PVDF resin and sarin resin. By adding sarin resin, on the one hand, as a cationic polymer, it can consume hydrofluoric acid, effectively reducing the yellowing phenomenon of PVDF resin during processing and use, reducing the formation of conjugated structures in the PVDF resin structure, and minimizing yellowing of the product appearance; on the other hand, as a nucleating agent, it can improve the transparency and flexibility of the material, which is beneficial for the widespread application of PVDF materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of materials improvement technology, and in particular to a yellowing-resistant polyvinylidene fluoride heat shrink tubing and its preparation method. Background Technology

[0002] Polyvinylidene fluoride (PVDF) is a linear, semi-crystalline polymer whose polymer chain structure is mainly composed of repeating monomer units -[CH2CF2]- linked end-to-end. It primarily refers to PVDF homopolymers or copolymers of PVDF with other small amounts of fluorinated vinyl monomers. It combines the characteristics of fluoropolymers and general-purpose resins, exhibiting excellent chemical resistance, high-temperature resistance, oxidation resistance, weather resistance, and radiation resistance. PVDF has a lower melting point than most fluoroplastics, approximately between 165 and 172°C, thus its processing temperature is also lower, comparable to that of polyolefins. Over the past half-century, it has been widely used in outdoor decorative films and coatings, corrosion-resistant equipment, and flame-retardant electronic insulation.

[0003] However, polyvinylidene fluoride resin has poor thermal stability during melt processing. When subjected to thermoplastic processing such as injection molding or extrusion, the products are prone to yellowing and darkening, and the transparency decreases. This phenomenon is very common in the processing and manufacturing of PVDF resin and is generally referred to as "yellowing". This yellowing phenomenon affects the appearance of the product and greatly limits the widespread application of PVDF materials. Summary of the Invention

[0004] To address the problem of poor overall application performance caused by yellowing during the processing and manufacturing of polyvinylidene fluoride (PVDF) resin in existing technologies, this invention provides a yellowing-resistant PVDF heat shrink tubing.

[0005] The above-mentioned objective of this invention is achieved through the following technical solution:

[0006] In a first aspect, the present invention provides a yellowing-resistant polyvinylidene fluoride heat shrink tubing, wherein the material for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing comprises the following raw materials in parts by weight:

[0007] 100 parts of polyvinylidene fluoride resin;

[0008] 2-10 parts of saline resin.

[0009] In some embodiments, the material for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing further includes the following raw material: 0.5 to 3 parts of NOR-type hindered amine stabilizer.

[0010] In some embodiments, the NOR-type hindered amine stabilizer is a monomolecular N-alkoxy hindered amine stabilizer.

[0011] In some embodiments, the polyvinylidene fluoride is a copolymerized polyvinylidene fluoride.

[0012] In some embodiments, the copolymerized polyvinylidene fluoride has a melt index of 1–15 g / 10 min (230 °C / 5 kg) and a melt viscosity of 500–2500 Pa·s (230 °C, 100 s). -1 ).

[0013] In some embodiments, the sarin resin is at least one of zinc salt, sodium salt, and lithium salt ionic polymers of ethylene-(meth)acrylate.

[0014] In some embodiments, the material for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing further includes the following raw material: 0.1 to 2 parts of crosslinking sensitizer.

[0015] In some embodiments, the crosslinking sensitizer is at least one of trimethylallyl isocyanate and its derivatives, triallyl cyanurate and its derivatives, triargyl cyanurate and its derivatives, trimethylolpropane trimethacrylate and its derivatives, and trimethylolpropane triacrylate and its derivatives.

[0016] In a second aspect, the present invention provides a method for preparing the above-mentioned yellowing-resistant polyvinylidene fluoride heat shrink tubing, comprising the following steps:

[0017] Masterbatch processing: Polyvinylidene fluoride resin and Salin resin are mixed evenly, and then extruded, drawn into strips, and granulated through an extrusion device to obtain masterbatch granules;

[0018] Extrusion into pipes: The masterbatch granules obtained above are extruded into pipes through an extrusion device to obtain semi-finished pipes;

[0019] Irradiation process: The above semi-finished pipes are irradiated by an irradiation device, and the irradiation dose is controlled at 5-15 Mrad to obtain irradiated pipes;

[0020] Expansion molding: The irradiated tubing is expanded, cooled, and shaped to obtain yellowing-resistant polyvinylidene fluoride heat shrink tubing.

[0021] In some embodiments, during the masterbatch processing step, when the polyvinylidene fluoride resin and sarin resin are mixed, at least one of a NOR-type hindered amine stabilizer and a crosslinking sensitizer is also added for mixing.

[0022] Alternatively, in the tube extrusion step, the extrusion temperature of the extrusion equipment is 180-250℃;

[0023] Alternatively, in the extrusion tube forming step, the stretch ratio of the extruded tube is controlled to be 8-40;

[0024] Alternatively, in the expansion molding step, the expansion temperature is 150-170℃.

[0025] The sarin resin in the yellowing-resistant polyvinylidene fluoride heat shrink tubing of this invention, on the one hand, as a cationic polymer, can consume hydrogen fluoride, which can effectively reduce the yellowing phenomenon of polyvinylidene fluoride during processing and use, reduce the formation of conjugated structures in the polyvinylidene fluoride resin structure, and reduce the yellowing phenomenon of the product appearance; on the other hand, as a nucleating agent, it can improve the transparency and flexibility of the material, which is conducive to the widespread application of polyvinylidene fluoride materials. Specific Implementation

[0026] It should be understood that the specific embodiments described herein are merely illustrative of the invention and are not intended to limit the invention.

[0027] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0028] In this invention, the terms "first," "second," etc., are used for descriptive purposes only and should not be construed as indicating or implying their relative importance or implicitly specifying the number of technical features indicated. Therefore, a feature defined with "first" or "second" may explicitly or implicitly include at least one of that feature. Furthermore, the technical solutions of the various embodiments can be combined with each other, but only on the basis of being achievable by those skilled in the art. If the combination of technical solutions is contradictory or impossible to implement, such a combination of technical solutions should be considered non-existent and not within the scope of protection claimed by this invention.

[0029] Polyvinylidene fluoride resin is commonly used to produce sheaths and main insulators for wire and cable products, especially heat shrink tubing. The following problems exist in the preparation and use process: (1) The extrusion molding process requires high temperature of 200-300℃; (2) The irradiation crosslinking process requires high-energy electron beam irradiation crosslinking modification; (3) During use, it is exposed to high temperature (100-200℃) environment. These high temperatures and high-energy electron beams will cause the polyvinylidene fluoride molecular chain to undergo dehalogenation reaction, generating hydrogen fluoride. With the formation of conjugated double bond structure, the material color turns yellow and darkens, and the transparency decreases.

[0030] Yellowing not only alters the appearance and color of polyvinylidene fluoride (PVDF) products but also reduces their transparency, failing to meet the demands of customers with stringent aesthetic requirements. Furthermore, yellowing is accompanied by a decrease in material toughness; the deeper the yellowing, the more brittle the PVDF pipes become. This embrittlement directly impacts product performance and lifespan, creating disadvantages and instability for downstream customers. Therefore, developing a formula that effectively improves the yellowing phenomenon in PVDF materials has significant production benefits, fundamentally improving product appearance, ensuring product consistency, reducing defect rates, extending product lifespan, and ultimately gaining customer approval—among other advantages.

[0031] Based on this, in a first aspect, the present invention provides a yellowing-resistant polyvinylidene fluoride heat shrink tubing, wherein the material for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing comprises the following raw materials in parts by weight:

[0032] 100 parts of polyvinylidene fluoride resin;

[0033] 2-10 parts of saline resin.

[0034] The sarin resin in the yellowing-resistant polyvinylidene fluoride heat shrink tubing of this invention, on the one hand, as a cationic polymer, can consume hydrogen fluoride, which can effectively reduce the yellowing phenomenon of polyvinylidene fluoride during processing and use, reduce the formation of conjugated structures in the polyvinylidene fluoride resin structure, and reduce the yellowing phenomenon of the product appearance; on the other hand, as a nucleating agent, it can improve the transparency and flexibility of the material, which is conducive to the widespread application of polyvinylidene fluoride materials.

[0035] In some embodiments, the material for preparing yellowing-resistant polyvinylidene fluoride heat shrink tubing further includes the following raw materials in parts by weight: 0.5 to 3 parts of NOR-type hindered amine stabilizer.

[0036] Understandably, NOR-type hindered amine stabilizers effectively inhibit and consume hydrogen fluoride. The introduction of alkoxy groups reduces the electron cloud density around the active nitrogen atoms, allowing them to participate in the free radical capture cycle and maintain the stability of the polymer material, thus reducing the impact of yellowing. Furthermore, the addition of only 0.5-3 parts is relatively small, minimizing its impact on the transparency of heat shrink tubing. In contrast, traditional hindered amine stabilizers have weaker anti-yellowing properties and are highly alkaline, readily reacting with acidic substances to form salts that precipitate, affecting the transparency of the heat shrink tubing. The amount of NOR-type hindered amine stabilizer affects the transparency of products made from polyvinylidene fluoride (PVDF). Too many parts, while improving anti-yellowing effects, decrease product transparency; too few parts, and they have no anti-yellowing effect.

[0037] Preferably, the NOR-type hindered amine stabilizer is a monomolecular N-alkoxy hindered amine stabilizer; preferably, the melting range is 108-123℃.

[0038] In some embodiments, the polyvinylidene fluoride is a copolymer of polyvinylidene fluoride.

[0039] In some embodiments, the copolymerized polyvinylidene fluoride has a melt index of 1–15 g / 10 min (230 °C / 5 kg) and a melt viscosity of 500–2500 Pa·s (230 °C, 100 s). -1 ).

[0040] Melt index (MI) is an important parameter for measuring the flowability of thermoplastics in the molten state. It is measured using a melt index tester under specified conditions, by measuring the mass of material passing through a standard die capillary over a certain period of time (usually 10 minutes), with the unit being g / 10min. This parameter is crucial for ensuring the quality of thermoplastics and their products, and for adjusting production processes. A higher melt index indicates lower viscosity, smaller molecular weight, better flowability, and better processability of the raw material; conversely, a lower melt index indicates higher viscosity, larger molecular weight, poorer flowability, and poorer processability, but higher physical and mechanical properties.

[0041] Melt viscosity refers to the ability of a melt to resist irreversible changes in the position of its volume elements (flow). Numerically, it is the ratio of the melt's shear stress to its shear rate, and the unit is Pa·s. For non-Newtonian fluids, viscosity varies with shear rate, and the resulting viscosity is called the apparent shear viscosity at the corresponding shear rate.

[0042] Melt index is 1–15 g / 10 min (230℃ / 5 kg), melt viscosity is 500–2500 Pa·s (230℃, 100 s). -1 The copolymer PVDF has good processing performance, physical and mechanical properties, and good transparency.

[0043] In some embodiments, the sarin resin is at least one of zinc salt, sodium salt, and lithium salt ionic polymers of ethylene-(meth)acrylate.

[0044] Understandably, sarin resin has extremely high transparency, which is due to the partial deposition of metal ions (Zn) onto ethylene-methacrylic acid copolymer (EMAA). 2+ Or Na + Or Li + It is a thermoplastic resin containing covalent bonds, produced by neutralization. On the one hand, it can consume hydrogen fluoride as a cationic polymer, and on the other hand, it can improve the transparency and flexibility of the material as a nucleating agent.

[0045] In some embodiments, the material for preparing yellowing-resistant polyvinylidene fluoride heat shrink tubing further includes the following raw materials in parts by weight: 0.1 to 2 parts of crosslinking sensitizer.

[0046] In some embodiments, the crosslinking sensitizer is at least one selected from trimethylallyl isocyanate and its derivatives, triallyl cyanurate and its derivatives, triargyl cyanurate and its derivatives, trimethylolpropane trimethacrylate and its derivatives, and trimethylolpropane triacrylate and its derivatives. The addition of the crosslinking sensitizer increases the number of active free radicals in the system, thereby reducing the energy of the electron beam originally required, and thus reducing the occurrence of dehalogenation reactions. Furthermore, even if some dehalogenation reaction inevitably occurs, sufficient active free radicals can reopen the C=C double bonds generated in the dehalogenation reaction, promoting the desired crosslinking reaction while consuming the conjugated double bonds. The use of sarin resin or NOR-type hindered amine stabilizers further ensures that the PVDF resin does not yellow during processing, and the product can maintain its original color.

[0047] In a second aspect, the present invention provides a method for preparing the above-mentioned yellowing-resistant polyvinylidene fluoride heat shrink tubing, comprising the following steps:

[0048] Masterbatch processing: Polyvinylidene fluoride resin and Salin resin are mixed evenly, and then extruded, drawn into strips, and granulated through an extrusion device to obtain masterbatch granules;

[0049] Extrusion into pipes: The masterbatch granules obtained above are extruded into pipes through an extrusion device to obtain semi-finished pipes;

[0050] Irradiation process: The above semi-finished pipes are irradiated by an irradiation device, and the irradiation dose is controlled at 5-15 Mrad to obtain irradiated pipes;

[0051] Expansion molding: The irradiated tubing is expanded, cooled, and shaped to obtain yellowing-resistant polyvinylidene fluoride heat shrink tubing.

[0052] Understandably, masterbatch processing involves adding polyvinylidene fluoride resin and sarin resin to a mixer according to a specified ratio, controlling the material temperature at 170±10℃, mixing for 8-15 minutes to obtain a mixture, and then extruding the mixture through an extrusion device, such as a twin-screw extruder or a single-screw extruder, extruding, drawing, and pelletizing to obtain masterbatch granules.

[0053] Extrusion into pipes: The above-mentioned granulated masterbatch particles are extruded into pipes through an extruder, such as a single-screw extruder or a twin-screw extruder, to obtain semi-finished pipes;

[0054] Irradiation process: The above semi-finished pipes are subjected to irradiation equipment, such as an electron accelerator irradiation device or a radioactive isotope irradiation device, and the irradiation dose is controlled at 5-15 Mrad to obtain irradiated pipes; by adding sarin resin, even if the irradiation dose is slightly higher during the irradiation process, yellowing will not occur.

[0055] Expansion molding: The irradiated tubing is expanded, cooled, and shaped to obtain yellowing-resistant polyvinylidene fluoride heat shrink tubing.

[0056] In some embodiments, during the masterbatch processing step, when the polyvinylidene fluoride resin and sarin resin are mixed, at least one of a NOR-type hindered amine stabilizer and a crosslinking sensitizer is also added for mixing.

[0057] In some embodiments, during the extrusion tube forming step, the extrusion temperature of the extrusion equipment is 180-250°C. It is understood that an extrusion temperature of 180-250°C not only ensures that the tube can be melt-extruded with a smooth surface, but also reduces the occurrence of yellowing.

[0058] In some embodiments, controlling the stretch ratio of the extruded tube to 8-40 during the extrusion tube forming step can improve the transparency of the polyvinylidene fluoride heat shrink tubing.

[0059] Understandably, in the extrusion tubing process, the die and mandrel are typically selected based on dimensional requirements, and the traction and extrusion speeds are controlled to obtain tubing with different draw ratios. The draw ratio of the extruded tubing is related to the transparency of the PVC heat shrink tubing. If the draw ratio is too low, the transparency of the PVC heat shrink tubing deteriorates; if the draw ratio is too high, the mechanical properties of the PVC heat shrink tubing decrease. Furthermore, 0.5-3 parts of NOR-type hindered amine stabilizer have a synergistic effect with draw ratios in the range of 8-40, which can further improve the transparency and mechanical properties of the heat shrink tubing.

[0060] In some embodiments, the expansion temperature in the expansion molding step is 150-170°C.

[0061] The present invention will be further described in detail below with reference to specific embodiments.

[0062] Determination of stretch ratio

[0063] A single-screw extruder is used, with the following die specifications: die diameter D1 (mm), mandrel diameter D2 (mm). The extruded tube dimensions are as follows: inner diameter d1 (mm), wall thickness w (mm). (Depending on the tube dimensions, the appropriate extruder, die, and mandrel model must be selected.) During the extrusion process, we control the traction speed and extrusion speed to obtain tubes with different draw ratios. The draw ratio calculation formula is as follows:

[0064]

[0065] The present invention relates to a yellowing-resistant polyvinylidene fluoride heat shrink tubing, which is illustrated in the following examples and comparative examples.

[0066] Example 1

[0067] Please refer to Table 1. The raw materials for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment include the following parts by weight:

[0068] 100 parts of polyvinylidene fluoride resin (Arkema, 2800-20);

[0069] Two parts of saline resin (DuPont, 8940).

[0070] The preparation method of this yellowing-resistant polyvinylidene fluoride heat shrink tubing is as follows:

[0071] Masterbatch processing: Polyvinylidene fluoride resin and sarin resin are added to a mixer according to the ratio. The material temperature is controlled at 170±10℃ and the mixture is mixed for 8 to 15 minutes to obtain a mixture. Then the mixture is crushed, extruded, drawn into strands, and air-cooled into pellets at a temperature of 160 to 220℃ to obtain masterbatch pellets.

[0072] Extrusion into tubes: The masterbatch granules obtained above are extruded into tubes at an extrusion temperature of 180-250℃ using a single screw extruder, and the stretch ratio of the extruded tube is controlled to be 5 to obtain a semi-finished tube.

[0073] Irradiation process: The above semi-finished tubing is irradiated using an electron accelerator device, with the irradiation dose controlled at 8Mrad, and cross-linked by irradiation to obtain the irradiated tubing.

[0074] Expansion molding: The irradiated tubing is expanded twice its original size using an expansion device at 150-170°C; then cooled and shaped to obtain the finished heat shrink tubing.

[0075] Example 2

[0076] The raw material formulation for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is the same as that in Example 1, please refer to Table 1.

[0077] The preparation method of the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is basically the same as that in Example 1, except that the stretch ratio of the extruded tubing is controlled to be 50 in the extrusion tubing step, as shown in Table 1.

[0078] Example 3

[0079] The raw material formulation for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is basically the same as that in Example 1, except for the proportions of each component, as shown in Table 1:

[0080] 100 parts of polyvinylidene fluoride resin (Arkema, 2800-20);

[0081] Six parts of saline resin (DuPont, 8940).

[0082] The preparation method of the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is basically the same as that in Example 1, except that the composition and quantity of each raw material are different in the masterbatch processing step, please refer to Table 1.

[0083] Example 4

[0084] The raw material formulation for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is basically the same as that in Example 1, except for the proportions of each component, as shown in Table 1:

[0085] 100 parts of polyvinylidene fluoride resin (Arkema, 2800-20);

[0086] Six parts of saline resin (DuPont, 8940).

[0087] The preparation method of the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is basically the same as that in Example 1, except that the composition and quantity of each raw material are different in the masterbatch processing step; in the extrusion tube forming step, the stretch ratio of the extruded tube is controlled to be 50, please refer to Table 1.

[0088] Example 5

[0089] The raw material formulation for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is basically the same as that in Example 1, except for the composition and proportion of each component, as shown in Table 1:

[0090] 100 parts of polyvinylidene fluoride resin (Arkema, 2800-20);

[0091] 10 parts of saline resin (DuPont, 8940).

[0092] The preparation method of the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is basically the same as that in Example 1, except that the composition and quantity of each raw material are different in the masterbatch processing step, please refer to Table 1.

[0093] Example 6

[0094] The raw material formulation for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is basically the same as that in Example 1, except for the composition and proportion of each component, as shown in Table 1:

[0095] 100 parts of polyvinylidene fluoride resin (Arkema, 2800-20);

[0096] 10 parts of saline resin (DuPont, 8940).

[0097] The preparation method of the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is basically the same as that in Example 1, except that the composition and quantity of each raw material are different in the masterbatch processing step; in the extrusion tube forming step, the stretch ratio of the extruded tube is controlled to be 50, please refer to Table 1.

[0098] Example 7

[0099] The raw material formulation for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is basically the same as that in Example 3, except for the composition and proportion of each component, as shown in Table 1:

[0100] 100 parts of polyvinylidene fluoride resin (Arkema, 2800-20);

[0101] 6 parts of saline resin (DuPont, 8940);

[0102] NOR-type hindered amine stabilizer: (BASF, NOR116) 0.5 parts.

[0103] The preparation method of the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is basically the same as that in Example 3, except that the composition and quantity of each raw material are different in the masterbatch processing step, please refer to Table 1.

[0104] Example 8

[0105] The raw material formulation for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is basically the same as that in Example 3, except for the composition and proportion of each component, as shown in Table 1:

[0106] 100 parts of polyvinylidene fluoride resin (Arkema, 2800-20);

[0107] 6 parts of saline resin (DuPont, 8940);

[0108] NOR-type hindered amine stabilizer: (BASF, NOR116) 0.5 parts.

[0109] The preparation method of the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is basically the same as that in Example 3, except that the composition and quantity of each raw material are different in the masterbatch processing step; in the extrusion tube forming step, the stretch ratio of the extruded tube is controlled to be 50, please refer to Table 1.

[0110] Example 9

[0111] The raw material formulation for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is basically the same as that in Example 3, except for the composition and proportion of each component, as shown in Table 1:

[0112] 100 parts of polyvinylidene fluoride resin (Arkema, 2800-20);

[0113] 6 parts of saline resin (DuPont, 8940);

[0114] NOR-type hindered amine stabilizer: (BASF, NOR116) 1.8 parts.

[0115] The preparation method of the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is basically the same as that in Example 3, except that the composition and quantity of each raw material are different in the masterbatch processing step, please refer to Table 1.

[0116] Example 10

[0117] The raw material formulation for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is basically the same as that in Example 3, except for the composition and proportion of each component, as shown in Table 1:

[0118] 100 parts of polyvinylidene fluoride resin (Arkema, 2800-20);

[0119] 6 parts of saline resin (DuPont, 8940);

[0120] NOR-type hindered amine stabilizer: (BASF, NOR116) 3 parts.

[0121] The preparation method of the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is basically the same as that in Example 1, except that the composition and quantity of each raw material are different in the masterbatch processing step, please refer to Table 1.

[0122] Example 11

[0123] The raw material formulation for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is basically the same as that in Example 3, except for the composition and proportion of each component, as shown in Table 1:

[0124] 100 parts of polyvinylidene fluoride resin (Arkema, 2800-20);

[0125] 6 parts of saline resin (DuPont, 8940);

[0126] NOR-type hindered amine stabilizer: (BASF, NOR116) 3 parts.

[0127] The preparation method of the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is basically the same as that in Example 1, except that the composition and quantity of each raw material are different in the masterbatch processing step; in the extrusion tube forming step, the stretch ratio of the extruded tube is controlled to be 50, please refer to Table 1.

[0128] Example 12

[0129] The raw material formulation for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is the same as that in Example 3, please refer to Table 1.

[0130] The preparation method of the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is basically the same as that in Example 3, except that the irradiation dose is changed to 5 Mrad in the irradiation process step. Please refer to Table 1.

[0131] Example 13

[0132] The raw material formulation for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is the same as that in Example 3, please refer to Table 1.

[0133] The preparation method of the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is basically the same as that in Example 3, except that the irradiation dose is changed to 12 Mrad in the irradiation process step. Please refer to Table 1.

[0134] Example 14

[0135] The raw material formulation for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is the same as that in Example 3, please refer to Table 1.

[0136] The preparation method of the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is basically the same as that in Example 3, except that the irradiation dose is changed to 15 Mrad in the irradiation process step. Please refer to Table 1.

[0137] Example 15

[0138] The raw material formulation for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is the same as that in Example 3, please refer to Table 1.

[0139] The preparation method of the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is basically the same as that in Example 3, except that in the extrusion tubing step, the stretch ratio of the extruded tubing is controlled to be 8, as shown in Table 1.

[0140] Example 16

[0141] The raw material formulation for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is the same as that in Example 3, please refer to Table 1.

[0142] The preparation method of the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is basically the same as that in Example 3, except that the stretch ratio of the extruded tubing is controlled to be 24 in the extrusion tubing step, as shown in Table 1.

[0143] Example 17

[0144] The raw material formulation for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is the same as that in Example 3, please refer to Table 1.

[0145] The preparation method of the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is basically the same as that in Example 3, except that the stretch ratio of the extruded tubing is controlled to be 40 in the extrusion tubing step, as shown in Table 1.

[0146] Example 18

[0147] The raw material formulation for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is the same as that in Example 7, please refer to Table 1.

[0148] The preparation method of the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is basically the same as that in Example 7, except that in the extrusion tubing step, the stretch ratio of the extruded tubing is controlled to be 8, as shown in Table 1.

[0149] Example 19

[0150] The raw material formulation for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is the same as that in Example 10, please refer to Table 1.

[0151] The preparation method of the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is basically the same as that in Example 10, except that in the extrusion tubing step, the stretch ratio of the extruded tubing is controlled to be 8, as shown in Table 1.

[0152] Example 20

[0153] The raw material formulation for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is the same as that in Example 7, please refer to Table 1.

[0154] The preparation method of the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is basically the same as that in Example 7, except that the stretch ratio of the extruded tubing is controlled to be 40 in the extrusion tubing step, as shown in Table 1.

[0155] Example 21

[0156] The raw material formulation for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is the same as that in Example 11, please refer to Table 1.

[0157] The preparation method of the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this embodiment is basically the same as that in Example 11, except that the stretch ratio of the extruded tubing is controlled to be 40 in the extrusion tubing step, as shown in Table 1.

[0158] Comparative Example 1

[0159] The raw material formulation for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this comparative example is basically the same as that in Example 3, except for the proportions of each component, as shown in Table 1:

[0160] 100 parts of polyvinylidene fluoride resin (Arkema, 2800-20).

[0161] The preparation method of the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this comparative example is basically the same as that in Example 3, except that the proportions of each component in the masterbatch processing step are different, as shown in Table 1.

[0162] Comparative Example 2

[0163] The raw material formulation for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this comparative example is basically the same as that in Example 3, except for the proportions of each component, as shown in Table 1:

[0164] 100 parts of polyvinylidene fluoride resin (Arkema, 2800-20);

[0165] One part of saline resin (DuPont, 8940).

[0166] The preparation method of the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this comparative example is basically the same as that in Example 3, except that the proportions of each component in the masterbatch processing step are different, as shown in Table 1.

[0167] Comparative Example 3

[0168] The raw material formulation for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this comparative example is basically the same as that in Example 3, except for the proportions of each component, as shown in Table 1:

[0169] 100 parts of polyvinylidene fluoride resin (Arkema, 2800-20);

[0170] 12 parts of saline resin (DuPont, 8940).

[0171] The preparation method of the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this comparative example is basically the same as that in Example 3, except that the proportions of each component in the masterbatch processing step are different, as shown in Table 1.

[0172] Comparative Example 4

[0173] The raw material formulation for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this comparative example is basically the same as that in Example 3, except for the composition and proportion of each raw material, as shown in Table 1:

[0174] 100 parts of polyvinylidene fluoride resin (Arkema, 2800-20);

[0175] 6 parts of saline resin (DuPont, 8940);

[0176] NOR-type hindered amine stabilizer: (BASF, NOR116) 0.3 parts.

[0177] The preparation method of the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this comparative example is basically the same as that in Example 3, except that the composition and quantity of each raw material are different in the masterbatch processing step, please refer to Table 1.

[0178] Comparative Example 5

[0179] The raw material formulation for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this comparative example is basically the same as that in Example 3, except for the composition and proportion of each raw material, as shown in Table 1:

[0180] 100 parts of polyvinylidene fluoride resin (Arkema, 2800-20);

[0181] 6 parts of saline resin (DuPont, 8940);

[0182] NOR-type hindered amine stabilizer: (BASF, NOR116) 4 parts.

[0183] The preparation method of the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this comparative example is basically the same as that in Example 3, except that the composition and quantity of each raw material are different in the masterbatch processing step, please refer to Table 1.

[0184] Comparative Example 6

[0185] The raw material formulation for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this comparative example is basically the same as that in Example 3, except for the composition and proportion of each raw material, as shown in Table 1:

[0186] 100 parts of polyvinylidene fluoride resin (Arkema, 2800-20);

[0187] 6 parts of saline resin (DuPont, 8940);

[0188] Three parts of hindered amine stabilizer (BASF, 944).

[0189] The preparation method of the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this comparative example is basically the same as that in Example 3, except that the composition and quantity of each raw material are different in the masterbatch processing step, please refer to Table 1.

[0190] Comparative Example 7

[0191] The raw material formulation for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this comparative example is the same as that in Example 3, please refer to Table 1.

[0192] The preparation method of the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this comparative example is basically the same as that in Example 3, except that the irradiation dose is changed to 3 Mrad in the irradiation process step. Please refer to Table 1.

[0193] Comparative Example 8

[0194] The raw material formulation for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this comparative example is the same as that in Example 3, please refer to Table 1.

[0195] The preparation method of the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this comparative example is basically the same as that in Example 3, except that the irradiation dose is changed to 17 Mrad in the irradiation process step. Please refer to Table 1.

[0196] Comparative Example 9

[0197] The raw material formulation for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this comparative example is basically the same as that in Example 3, except for the composition and proportion of each raw material, as shown in Table 1:

[0198] 100 parts of polyvinylidene fluoride resin (Arkema, 2800-20);

[0199] 6 parts of saline resin (DuPont, 8940);

[0200] NOR-type hindered amine stabilizer: (BASF, NOR116) 0.3 parts.

[0201] The preparation method of the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this comparative example is basically the same as that in Example 3, except that the composition and proportion of each raw material are different in the masterbatch processing step; in the extrusion tube forming step, the stretch ratio of the extruded tube is controlled to be 50, please refer to Table 1.

[0202] Comparative Example 10

[0203] The raw material formulation for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this comparative example is basically the same as that in Example 3, except for the composition and proportion of each raw material, as shown in Table 1:

[0204] 100 parts of polyvinylidene fluoride resin (Arkema, 2800-20);

[0205] 6 parts of saline resin (DuPont, 8940);

[0206] NOR-type hindered amine stabilizer: (BASF, NOR116) 4 parts.

[0207] The preparation method of the yellowing-resistant polyvinylidene fluoride heat shrink tubing in this comparative example is basically the same as that in Example 3, except that the composition and proportion of each raw material are different in the masterbatch processing step; in the extrusion tube forming step, the stretch ratio of the extruded tube is controlled to be 50, please refer to Table 1.

[0208] The yellowing index, light transmittance, and elongation at break of the finished product were measured. The results of the tests in the examples and comparative examples are shown in Table 2. The test methods are as follows:

[0209] Determination of yellowing index

[0210] The tristimulus values ​​X, Y, and Z of the material color were measured using a ColorSpectrum CS-820N spectrophotometer under a standard C light source. The yellowing index YI was calculated using the following formula: YI = 100(1.28X - 1.06Z) / Y. Generally, a yellowing index below 2.0 indicates normal use.

[0211] Measurement of transmittance

[0212] Using a Sanenshi YH600 haze meter, the incident light flux T1 and the total transmitted light flux T2 through the sample are read. The transmittance Tt is calculated using the following formula: Tt = T2 / 21 × 100%. Generally, a transmittance higher than 85% indicates better transparency.

[0213] Determination of elongation at break

[0214] The high-speed rail AI-7000-SU1 tensile testing machine was used to measure the length L0 before stretching and the length L at the point of fracture. The elongation at break ε was calculated using the following formula: (L-L0) / L0×100%. Generally, mechanical properties are better when the elongation at break is higher than 400%.

[0215] Table 1. Composition and mass fraction of each raw material, and preparation process parameters for the yellowing-resistant polyvinylidene fluoride heat shrink tubing in the examples and comparative examples.

[0216]

[0217]

[0218]

[0219] Table 2. Test results of yellowing-resistant polyvinylidene fluoride heat shrink tubing prepared in the examples and comparative examples.

[0220]

[0221]

[0222] Table 2 shows that the yellowing index of the PVC heat shrink tubing prepared in Examples 1 to 21 was all below 2.0, indicating good yellowing resistance. While the PVC heat shrink tubing prepared in Examples 1, 3, and 5 showed good yellowing resistance, its light transmittance was between 82% and 85%, indicating room for improvement. Similarly, the PVC heat shrink tubing prepared in Examples 2, 4, and 6 showed good yellowing resistance, but its elongation at break was between 350% and 370%, suggesting room for improvement in mechanical properties. The PVC heat shrink tubing prepared in Examples 12, 13, and 14 showed good yellowing resistance, with a yellowing index below 2.0 over a relatively wide irradiation dose range. However, with increasing irradiation dose, although the heat shrink tubing still exhibited good yellowing resistance, it had a certain impact on subsequent expansion processes, thus affecting the related mechanical properties and causing a certain degree of decrease in mechanical properties. Compared to Example 3, the yellowing-resistant PVC heat shrink tubing prepared in Examples 7, 9, and 10 showed improved yellowing resistance and transparency by adding a certain amount of NOR-type hindered amine stabilizer. Compared to Comparative Examples 4, 5, 9, and 10, the yellowing-resistant PVC heat shrink tubing prepared in Examples 7, 10, 8, and 11 showed improved yellowing resistance and transparency by controlling the NOR-type hindered amine stabilizer content to 0.5-3 parts, without controlling the stretch ratio range. Compared to Examples 3 and 4, the yellowing-resistant PVC heat shrink tubing prepared in Examples 15-17 showed improved yellowing resistance, transparency, and mechanical properties by controlling the stretch ratio to 8-40 without adding NOR-type hindered amine stabilizer. Compared to Examples 7 and 8, the yellowing-resistant PVC heat shrink tubing prepared in Examples 18 and 20 showed improved yellowing resistance and transparency by adding 0.5 parts of NOR-type hindered amine stabilizer. Under the condition of R-type hindered amine stabilizer, by controlling the stretch ratio within the range of 8-40, not only is the yellowing resistance good, but the light transmittance, elongation at break, transparency, and mechanical properties are also higher. Compared with the corresponding examples 10 and 11, the yellowing-resistant polyvinylidene fluoride heat shrink tubing prepared in Examples 19 and 21, with the addition of 3 parts of NOR-type hindered amine stabilizer and the stretch ratio controlled within the range of 8-40, not only has the yellowing resistance good, but also the light transmittance, elongation at break, transparency, and mechanical properties are also higher. It can be seen that 0.5-3 parts of NOR-type hindered amine stabilizer and the stretch ratio within the range of 8-40 have a synergistic effect, which can further improve the yellowing resistance, transparency, and mechanical properties of heat shrink tubing.

[0223] Comparative Example 1, without the addition of sarin resin, showed severe yellowing of the heat shrink tubing, and a significant decrease in transparency and mechanical properties.

[0224] In Comparative Example 2, the amount of sarin resin was too low, resulting in severe yellowing of the heat shrink tubing and a decrease in transparency and mechanical properties.

[0225] In Comparative Example 3, the amount of saline resin was too high. Although it helped to improve the yellowing phenomenon of heat shrink tubing, it affected the transparency and mechanical properties.

[0226] In Comparative Example 4, the amount of NOR-type hindered amine stabilizer was too low, resulting in an excessively low draw ratio of the extruded tubing and an insignificant improvement in the yellowing resistance and transparency of the heat shrink tubing.

[0227] The proportion of hindered amine stabilizer 5NOR was too high, resulting in an excessively low draw ratio of the extruded tubing. While this improved the yellowing resistance of the heat shrink tubing, it also affected its transparency.

[0228] Comparative Example 6 used other types of hindered amine stabilizers, resulting in poorer resistance to yellowing and lower transparency of the heat shrink tubing.

[0229] Comparative Example 7 showed an excessively low irradiation dose, resulting in poor mechanical properties of the heat shrink tubing.

[0230] Comparative Example 8 showed excessive irradiation dose, resulting in severe yellowing and a significant decrease in transparency of the heat shrink tubing.

[0231] The proportion of hindered amine stabilizer 9NOR type in the comparative example was too low, resulting in an excessively high draw ratio of the extruded tube and low transparency and mechanical properties of the heat shrink tubing.

[0232] The proportion of hindered amine stabilizer 10NOR type in the comparative example was too high, and the stretch ratio of the extruded tube was too high. Although it could improve the yellowing resistance of the heat shrink tube, it reduced the transparency and mechanical properties.

[0233] The above are merely preferred embodiments of the present invention and do not limit the patent scope of the present invention. Any equivalent structural or procedural transformations made based on the content of the present invention specification, or direct or indirect applications in other related technical fields, are similarly included within the patent protection scope of the present invention.

Claims

1. A yellowing-resistant polyvinylidene fluoride heat shrink tubing, characterized in that, The material for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing comprises the following parts by weight: 100 parts of polyvinylidene fluoride resin, wherein the polyvinylidene fluoride is homopolymer or copolymer polyvinylidene fluoride; 2-10 parts of sarin resin; 0.5 to 3 parts of stabilizer, wherein the stabilizer is a NOR-type hindered amine stabilizer; The sarin resin is at least one of zinc salt, sodium salt, and lithium salt ionic polymers of ethylene-(meth)acrylate.

2. A yellowing-resistant polyvinylidene fluoride heat shrink tubing, characterized in that, The material for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing is composed of the following raw materials in parts by weight: 100 parts of polyvinylidene fluoride resin, wherein the polyvinylidene fluoride is homopolymer or copolymer polyvinylidene fluoride; 2-10 parts of sarin resin; The sarin resin is at least one of zinc salt, sodium salt, and lithium salt ionic polymers of ethylene-(meth)acrylate.

3. The yellowing-resistant polyvinylidene fluoride heat shrink tubing according to claim 1, characterized in that, The NOR-type hindered amine stabilizer is a monomolecular N-alkoxy hindered amine stabilizer with a melting range of 108-123℃.

4. The yellowing-resistant polyvinylidene fluoride heat shrink tubing according to claim 1 or 2, characterized in that, The polyvinylidene fluoride is a copolymerized polyvinylidene fluoride.

5. The yellowing-resistant polyvinylidene fluoride heat shrink tubing according to claim 4, characterized in that, The copolymerized polyvinylidene fluoride has a melt index of 1~15 g / 10 min at 230°C and a load of 5 kg, and a melt index of 1~15 g / 10 min at 230°C and a shear rate of 100 s⁻¹. -1 Under these conditions, the melt viscosity is 500~2500 Pa·s.

6. The yellowing-resistant polyvinylidene fluoride heat shrink tubing according to claim 1, characterized in that, It also includes the following raw materials: Crosslinking sensitizer 0.1~2 parts.

7. The yellowing-resistant polyvinylidene fluoride heat shrink tubing according to claim 6, characterized in that, The crosslinking sensitizer is at least one of trimethylallyl isocyanurate, triallyl cyanurate, triargyl cyanurate, trimethylolpropane trimethacrylate, and trimethylolpropane triacrylate.

8. A method for preparing a yellowing-resistant polyvinylidene fluoride heat shrink tubing as described in claim 1, characterized in that, Includes the following steps: Masterbatch processing: Polyvinylidene fluoride resin, Salin resin and NOR type hindered amine stabilizer are mixed evenly, and then extruded, drawn into strips and granulated by an extrusion device to obtain masterbatch granules; Extrusion into pipes: The masterbatch granules obtained above are extruded into pipes through an extrusion device to obtain semi-finished pipes; Irradiation process: The above semi-finished pipes are irradiated by an irradiation device, and the irradiation dose is controlled at 5-15 Mrad to obtain irradiated pipes; Expansion molding: The irradiated tubing is expanded, cooled, and shaped to obtain yellowing-resistant polyvinylidene fluoride heat shrink tubing; The sarin resin is at least one of zinc salt, sodium salt, and lithium salt ionic polymers of ethylene-(meth)acrylate.

9. The method for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing according to claim 8, characterized in that, In the masterbatch processing step, when the polyvinylidene fluoride resin, sarin resin and NOR-type hindered amine stabilizer are mixed, a crosslinking sensitizer is also added for mixing. Alternatively, in the tube extrusion step, the extrusion temperature of the extrusion equipment is 180-250 ℃; Alternatively, in the extrusion tube forming step, the stretch ratio of the extruded tube is controlled to be 8-40; Alternatively, in the expansion molding step, the expansion temperature is 150-170 ℃.

10. A method for preparing a yellowing-resistant polyvinylidene fluoride heat shrink tubing as described in claim 2, characterized in that, Includes the following steps: Masterbatch processing: Polyvinylidene fluoride resin and Salin resin are mixed evenly, and then extruded, drawn into strips, and granulated through an extrusion device to obtain masterbatch granules; Extrusion into pipes: The masterbatch granules obtained above are extruded into pipes through an extrusion device to obtain semi-finished pipes; Irradiation process: The above semi-finished pipes are irradiated by an irradiation device, and the irradiation dose is controlled at 5-15 Mrad to obtain irradiated pipes; Expansion molding: The irradiated tubing is expanded, cooled, and shaped to obtain yellowing-resistant polyvinylidene fluoride heat shrink tubing; The sarin resin is at least one of zinc salt, sodium salt, and lithium salt ionic polymers of ethylene-(meth)acrylate.

11. The method for preparing the yellowing-resistant polyvinylidene fluoride heat shrink tubing according to claim 10, characterized in that, In the tube extrusion step, the extrusion temperature of the extrusion equipment is 180-250 ℃; Alternatively, in the extrusion tube forming step, the stretch ratio of the extruded tube is controlled to be 8-40; Alternatively, in the expansion molding step, the expansion temperature is 150-170 ℃.

Citation Information

Patent Citations

  • Yellowing-resistant modified polyvinylidene fluoride material, heat-shrinkable tube and preparation methods of yellowing-resistant modified polyvinylidene fluoride material and heat-shrinkable tube

    CN116925482A