A high-strength and high-toughness tungsten-based plate for nuclear applications and its preparation method
By designing layered structures and optimizing processes in tungsten-based materials, the brittleness problem of tungsten-based materials under multi-field coupling conditions was solved, achieving a combination of high strength and high toughness, which meets the requirements of nuclear fusion reactors.
Patent Information
- Application Number
- CN202411482884.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-23
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-10-23
AI Technical Summary
Existing tungsten-based materials suffer from brittleness under multi-field coupling conditions, especially low-temperature brittleness, recrystallization brittleness, and irradiation embrittlement, which prevents them from meeting the requirements of future nuclear fusion reactors. Furthermore, materials prepared by existing layered toughening methods have low tensile strain and insufficient strength-plasticity matching.
The design adopts a layered structure with a tantalum layer at the center, and a titanium-tantalum hybrid layer, a titanium layer, a tungsten-titanium hybrid layer, and a tungsten layer arranged sequentially on both sides. The titanium-tantalum hybrid layer and the tungsten-titanium hybrid layer are combined to form a small gradient strength change, and the interfacial bonding force is improved by vacuum pressure sintering and multi-stage rolling process.
It significantly improves the tensile strength and toughness of tungsten-based plates, ensuring improved performance in terms of high strength and machinability, avoiding interfacial cracking, and enhancing the overall performance of the material.
Smart Images

Figure CN119348243B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of nuclear structural material preparation technology, and in particular relates to a high-strength and high-toughness tungsten-based plate for nuclear use and its preparation method. Background Technology
[0002] Tungsten possesses advantages such as a high melting point, high thermal conductivity, high creep resistance, good high-temperature strength, low tritium retention, and high sputtering resistance, making it considered one of the most promising plasma-oriented materials for nuclear fusion reactors. The main problem faced by tungsten-based materials during service is brittleness under multi-field coupling conditions, including low-temperature brittleness, recrystallization brittleness, and irradiation embrittlement, which makes them unsuitable for future fusion reactor requirements. Therefore, improving the brittleness of tungsten, or rather, increasing its toughness, has become a key challenge in tungsten-based material research.
[0003] Tungsten is a typical body-centered cubic metal, characterized by non-planar expansion of screw dislocations, poor mobility, and intrinsic brittleness. Therefore, methods to increase the toughness of tungsten mainly include alloying, grain refinement, second-phase strengthening, fiber toughening, and layered toughening. The first three methods primarily improve the inherent properties of tungsten to increase toughness. However, because tungsten is highly sensitive to impurities and prone to recrystallization under high-temperature service conditions, these methods are not very effective in increasing tungsten toughness. Fiber toughening can improve the toughness of tungsten, but the overall strength of the material is relatively low.
[0004] Existing technologies toughen tungsten-based materials through layered toughening methods. For example, the Chinese invention patent "A Layered Gradient Structure Tungsten-Based Composite Material and Its Preparation Method" (Announcement No. CN110053328B) uses tungsten foil, titanium foil, and tantalum foil to form multiple sequentially stacked repeating units, and prepares the tungsten-based composite material through surface treatment, molding, sintering, and demolding. However, the tungsten-based composite material prepared by this method has relatively low tensile strain and insufficient strength-plasticity matching. Summary of the Invention
[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide a high-strength, high-toughness tungsten-based plate for nuclear applications. This tungsten-based plate has a layered structure with a tantalum layer at its center, and on both sides of the tantalum layer, from the inside out, a titanium-tantalum hybrid layer, a titanium layer, a tungsten-titanium hybrid layer, and a tungsten layer, forming a layered structure. This allows the tantalum, titanium, and tungsten layers to be bonded together through the titanium-tantalum hybrid layer and the tungsten-titanium hybrid layer, effectively improving the tensile strength and toughness of the tungsten-based plate and solving the problems of low tensile strain and insufficient strength-plasticity matching in tungsten-based materials prepared by existing technologies.
[0006] To achieve the above objectives, the technical solution adopted by the present invention is: a high-strength and high-toughness tungsten-based plate for nuclear applications, characterized in that the tungsten-based plate has a tantalum layer as the center, and a titanium-tantalum mixed layer, a titanium layer, a tungsten-titanium mixed layer and a tungsten layer are respectively arranged sequentially from the inside to the outside on both sides of the tantalum layer.
[0007] This invention adjusts the structure between tungsten and tantalum layers by setting a titanium layer between tungsten and tantalum layers, and a titanium-tantalum hybrid layer between tantalum and titanium layers, and a tungsten-titanium hybrid layer between titanium and tungsten layers. This results in a small gradient in strength between the metal layers, thereby improving the strength and toughness of tungsten-based plates. Tantalum has a high melting point, high thermal conductivity, good room temperature processing performance and plasticity, and exhibits low hydrogen retention and high radiation resistance when exposed to high-flux helium ion irradiation in a nuclear fusion environment, which can toughen tungsten. However, the strength of tungsten / tantalum layered composites is relatively low. To improve the strength of layered composites, titanium, which has a high melting point, high strength, low activity, and good heat resistance, is selected as an intermediate transition layer. At the same time, tungsten-titanium hybrid layers and titanium-tantalum hybrid layers are set to reduce the strength gradient between tungsten, tantalum, and titanium layers, acting as a strength transition layer and preventing interface cracking under tensile stress.
[0008] The above-mentioned high-strength and high-toughness tungsten-based plate for nuclear applications is characterized in that the mass percentage of tungsten in the tungsten-titanium mixed layer is not less than 95%, and the mass percentage of tantalum in the titanium-tantalum mixed layer is not less than 20%.
[0009] The above-mentioned high-strength and high-toughness tungsten-based plate for nuclear applications is characterized in that the tensile strength of the tungsten-based plate is not less than 1500 MPa, and the elongation of the tungsten-based plate is not less than 10%.
[0010] In addition, the present invention also discloses a method for preparing the above-mentioned high-strength and high-toughness tungsten-based plate for nuclear applications, characterized in that the method includes the following steps:
[0011] Step 1: Mix tungsten powder and titanium powder to obtain tungsten-titanium mixed powder, and mix titanium powder and tantalum powder to obtain titanium-tantalum mixed powder;
[0012] Step 2: Ball mill the tungsten-titanium mixed powder and the titanium-tantalum mixed powder obtained in Step 1 respectively.
[0013] Step 3: The tungsten powder, titanium powder, tantalum powder, and the ball-milled tungsten-titanium mixed powder and titanium-tantalum mixed powder from Step 1 are subjected to cold isostatic pressing to obtain tungsten powder slabs, titanium powder slabs, tantalum powder slabs, tungsten-titanium mixed powder slabs, and titanium-tantalum mixed powder slabs.
[0014] Step 4: Place the slabs obtained in Step 3 into the mold in the following order: tungsten powder slab, tungsten-titanium mixed powder slab, titanium powder slab, titanium-tantalum mixed powder slab, tantalum powder slab, titanium-tantalum mixed powder slab, titanium powder slab, tungsten-titanium mixed powder slab, and tungsten powder slab, and perform vacuum pressure sintering to obtain tungsten-based composite material slabs.
[0015] Step 5: The tungsten-based composite material billet obtained in Step 4 is subjected to open rolling and second rolling under argon atmosphere protection to obtain the rolled tungsten-based composite material.
[0016] Step 6: Heat treat the rolled tungsten-based composite material billet obtained in Step 5 to obtain tungsten-based plates.
[0017] The above-mentioned method for preparing a high-strength and high-toughness tungsten-based plate for nuclear applications is characterized in that, in step one, the tungsten powder has a purity of not less than 99.99%, a Fisher particle size of not more than 30 μm, and an oxygen content of not more than 300 ppm; the titanium powder has a purity of not less than 99.99%, a Fisher particle size of 30 μm to 50 μm, and an oxygen content of not more than 300 ppm; the tantalum powder has a purity of not less than 99.99%, a Fisher particle size of 20 μm to 50 μm, and an oxygen content of not more than 300 ppm.
[0018] This invention reduces impurities by controlling the purity of raw materials, preventing a large number of impurities from becoming nucleation centers and promoting particle growth, thereby reducing particle size. It also controls the dispersibility and reactivity of the raw material powder by controlling the Fisher particle size; smaller Fisher particle size and finer powder particles are more conducive to uniform distribution in subsequent chemical reactions, thus promoting more uniform nucleation and growth, and reducing the size of the oxide and nitride particles ultimately formed inside the board. Furthermore, controlling the oxygen content of the raw materials effectively reduces the formation of metal oxides and nitrides, while also reducing the growth time of oxide particles, thereby lowering the size of the formed oxide and nitride particles and increasing the dispersion strengthening effect of the second phase. In summary, controlling the purity, Fisher particle size, and oxygen content of raw materials improves the processing performance of the board, thereby enhancing its mechanical properties.
[0019] The above-mentioned method for preparing a high-strength and high-toughness tungsten-based plate for nuclear applications is characterized in that, in step two, titanium balls are used for ball milling, the ball milling time is 2h to 10h, and the ball milling speed is 150r / min to 350r / min.
[0020] The above-mentioned method for preparing a high-strength and high-toughness tungsten-based plate for nuclear applications is characterized in that the cold isostatic pressing pressure in step three is 200MPa to 300MPa, the cold isostatic pressing time is 10min to 20min, and the thickness of the tungsten-titanium mixed powder slab and the titanium-tantalum mixed powder slab is not greater than 1mm.
[0021] This invention uses tungsten-titanium mixed powder slabs and titanium-tantalum mixed powder slabs with a thickness of no more than 1 mm as transition interfaces between tungsten powder slabs, titanium powder slabs, and tantalum powder slabs. Compared with sintering through direct contact between tungsten layers and titanium layers, and titanium layers and tantalum layers, the addition of transition interfaces can effectively enhance the interfacial bonding ability.
[0022] The above-mentioned method for preparing a high-strength, high-toughness tungsten-based nuclear material is characterized in that the vacuum pressure sintering temperature in step four is 1300℃~1600℃, and the vacuum degree of the vacuum pressure sintering is not greater than 10. -4 Pa, the pre-pressure of the vacuum pressure sintering is 30MPa to 50MPa.
[0023] The above-mentioned method for preparing a high-strength and high-toughness tungsten-based plate for nuclear applications is characterized in that, in step five, the rolling temperature of the initial rolling is 1200℃~1400℃, and the total deformation of the initial rolling is 50%~70%; the temperature of the second rolling is 400℃~600℃, and the deformation per pass of the second rolling is 10%~15%; the second rolling process is as follows: the first pass of rolling is carried out along the width direction, and then alternating rolling is carried out along the length direction and the width direction in sequence, and stress-relief annealing is performed in an argon atmosphere between each pass of rolling; the stress-relief annealing time is 10min~15min, and the stress-relief annealing temperature is 400℃~600℃.
[0024] This invention improves the strength of sheet metal by employing a process of initial billet rolling followed by a second rolling with small deformation. By controlling the initial billet rolling temperature to 1200℃~1400℃, which is higher than the recrystallization temperature of tungsten, the tungsten-based composite billet can obtain a dense, coarse equiaxed recrystallized structure under large deformation reduction. Then, by performing multiple passes of alternating small deformation rolling on the tungsten-based composite billet, a fine fibrous structure distributed along the main deformation direction is formed, resulting in a significant strengthening effect on the sheet metal and thus improving its strength.
[0025] The above-mentioned method for preparing a high-strength and high-toughness tungsten-based plate for nuclear applications is characterized in that the heat treatment in step six is a precise temperature-controlled heat treatment process under atmosphere protection, wherein the heat treatment temperature is 400℃~600℃, the temperature deviation in the uniform temperature zone is no more than 10℃, and the annealing time of the heat treatment is 10min~30min.
[0026] This invention employs an atmosphere-protected, precise temperature-controlled heat treatment process to prevent metal oxidation at high temperatures. This process precisely controls the atmosphere and temperature within the heat treatment furnace by using computer simulation to preset temperature curves, heating rates, holding times, atmosphere composition, the arrangement of heating elements within the furnace, and full circulation of furnace gas.
[0027] Compared with the prior art, the present invention has the following advantages:
[0028] 1. The present invention forms a layered structure with a tantalum layer as the center and a titanium-tantalum hybrid layer, a titanium layer, a tungsten-titanium hybrid layer and a tungsten layer arranged sequentially from the inside to the outside on both sides of the tantalum layer. This allows the tantalum layer, titanium layer and tungsten layer to be bonded through the titanium-tantalum hybrid layer and the tungsten-titanium hybrid layer, thereby improving the interfacial bonding force between the tantalum layer and the titanium layer, and between the titanium layer and the tungsten layer, thus improving the tensile strength and toughness of the tungsten-based plate.
[0029] 2. This invention controls the mass percentage of tungsten in the tungsten-titanium mixed layer to be no less than 95%, and the mass percentage of tantalum in the titanium-tantalum mixed layer to be no less than 20%. This results in the formation of a (β-Ti, W) solid solution region in the tungsten-titanium mixed layer and a (β-Ti, Ta) solid solution region in the titanium-tantalum mixed layer. These two solid solutions enable good bonding between the tungsten / titanium interface and the titanium / tantalum interface, forming a stable interface structure. This results in high strength in the composite material, and the presence of multiple interfaces in the plate further enhances its strength and toughness. Simultaneously, by forming solid solution regions between the tungsten, titanium, and tantalum layers, the thermal expansion coefficient of the composite material is also transitioned, reducing subsequent rolling cracking.
[0030] 3. This invention employs a process combining vacuum pressure sintering and multi-stage rolling, enabling the formation of (β-Ti, W) solid solutions and (β-Ti, Ta) solid solutions in tungsten-titanium mixed powder slabs and titanium-tantalum mixed powder slabs. Under vacuum pressure, the solid solution elements diffuse to both sides of the interface, effectively improving the interfacial bonding ability between slabs and reducing defects such as pores at the tungsten / titanium and titanium / tantalum interfaces. This makes the tungsten-based plates less prone to delamination during multi-stage rolling, increasing the plate's machinability.
[0031] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Attached Figure Description
[0032] Figure 1 This is a microscopic image of the tungsten-based substrate in Embodiment 1 of the present invention. Detailed Implementation
[0033] Example 1
[0034] In this embodiment, the tungsten-based plate has a tantalum layer as the center, and a titanium-tantalum hybrid layer, a titanium layer, a tungsten-titanium hybrid layer and a tungsten layer are sequentially arranged on both sides of the tantalum layer from the inside to the outside. The tungsten-titanium hybrid layer has a tungsten element mass percentage of 97%, and the titanium-tantalum hybrid layer has a tantalum element mass percentage of 25%.
[0035] The preparation method of the tungsten-based plate in this embodiment includes the following steps:
[0036] Step 1: Mix tungsten powder and titanium powder to obtain tungsten-titanium mixed powder, and mix titanium powder and tantalum powder to obtain titanium-tantalum mixed powder; the tungsten powder has a purity of 99.995%, a Fisher particle size of 20μm, and an oxygen content of 245ppm; the titanium powder has a purity of 99.993%, a Fisher particle size of 35μm, and an oxygen content of 240ppm; the tantalum powder has a purity of 99.992%, a Fisher particle size of 40μm, and an oxygen content of 240ppm; the tungsten powder accounts for 97% of the mass of the tungsten-titanium mixed powder, and the tantalum powder accounts for 25% of the mass of the titanium-tantalum mixed powder.
[0037] Step 2: The tungsten-titanium mixed powder and the titanium-tantalum mixed powder obtained in Step 1 are respectively subjected to ball milling at a speed of 250 r / min for 5 hours; the ball milling uses titanium balls;
[0038] Step 3: The tungsten powder, titanium powder, tantalum powder, and the ball-milled tungsten-titanium mixed powder and titanium-tantalum mixed powder from Step 1 are subjected to cold isostatic pressing for 15 minutes to obtain tungsten powder blanks, titanium powder blanks, tantalum powder blanks, tungsten-titanium mixed powder blanks, and titanium-tantalum mixed powder blanks; the cold isostatic pressing pressure is 280 MPa, and the thickness of the tungsten-titanium mixed powder blanks and the titanium-tantalum mixed powder blanks is 0.5 mm;
[0039] Step 4: Place the slabs obtained in Step 3 into a mold in the following order: tungsten powder slab, tungsten-titanium mixed powder slab, titanium powder slab, titanium-tantalum mixed powder slab, tantalum powder slab, titanium-tantalum mixed powder slab, titanium powder slab, tungsten-titanium mixed powder slab, and tungsten powder slab. Perform vacuum pressure sintering to obtain a tungsten-based composite material slab. The vacuum pressure sintering temperature is 1400℃, and the vacuum degree is 10. -4 Pa, the pre-pressure of vacuum pressure sintering is 40 MPa;
[0040] Step 5: The tungsten-based composite material billet obtained in Step 4 is subjected to a first rolling and a second rolling process to obtain the rolled tungsten-based composite material. The rolling temperature for the first rolling is 1300℃, and the deformation is 55%. The temperature for the second rolling is 450℃, and the deformation per pass is 10%. The second rolling process is as follows: the first pass is rolled along the width direction, and then the rolling is performed alternately along the length and width directions. An argon atmosphere stress-relief annealing treatment is performed between each pass. The stress-relief annealing treatment takes 10 minutes and is performed at a temperature of 400℃.
[0041] Step 6: Perform precise temperature-controlled heat treatment on the rolled tungsten-based composite material billet obtained in Step 5 under atmosphere protection to obtain tungsten-based plates; the heat treatment temperature is 400℃, the temperature deviation in the uniform temperature zone is no more than 10℃, and the annealing time of the heat treatment is 15min.
[0042] Microscopic analysis was performed on the tungsten-based substrate obtained in this embodiment, such as... Figure 1 As shown, the metal layers of the tungsten-based plate are well bonded together, and no defects such as pores are present.
[0043] The tungsten-based plate prepared in this embodiment has a tensile strength of 1614 MPa and an elongation of 15.6%, as tested.
[0044] Example 2
[0045] In this embodiment, the tungsten-based plate has a tantalum layer as the center, and a titanium-tantalum hybrid layer, a titanium layer, a tungsten-titanium hybrid layer and a tungsten layer are sequentially arranged on both sides of the tantalum layer from the inside to the outside. The tungsten-titanium hybrid layer has a tungsten element mass percentage of 99%, and the titanium-tantalum hybrid layer has a tantalum element mass percentage of 20%.
[0046] The preparation method of the tungsten-based plate in this embodiment includes the following steps:
[0047] Step 1: Mix tungsten powder and titanium powder to obtain tungsten-titanium mixed powder, and mix titanium powder and tantalum powder to obtain titanium-tantalum mixed powder; the tungsten powder has a purity of 99.993%, a Fisher particle size of 15μm, and an oxygen content of 264ppm; the titanium powder has a purity of 99.991%, a Fisher particle size of 25μm, and an oxygen content of 280ppm; the tantalum powder has a purity of 99.995%, a Fisher particle size of 36μm, and an oxygen content of 278ppm; the tungsten powder accounts for 99% of the mass of the tungsten-titanium mixed powder, and the tantalum powder accounts for 20% of the mass of the titanium-tantalum mixed powder.
[0048] Step 2: The tungsten-titanium mixed powder and the titanium-tantalum mixed powder obtained in Step 1 are respectively subjected to ball milling at a speed of 350 r / min for 10 hours; the ball milling uses titanium balls;
[0049] Step 3: The tungsten powder, titanium powder, tantalum powder, and the ball-milled tungsten-titanium mixed powder and titanium-tantalum mixed powder from Step 1 are subjected to cold isostatic pressing for 20 minutes to obtain tungsten powder blanks, titanium powder blanks, tantalum powder blanks, tungsten-titanium mixed powder blanks, and titanium-tantalum mixed powder blanks; the cold isostatic pressing pressure is 300 MPa, and the thickness of the tungsten-titanium mixed powder blanks and the titanium-tantalum mixed powder blanks is 1 mm;
[0050] Step 4: Place the slabs obtained in Step 3 into a mold in the following order: tungsten powder slab, tungsten-titanium mixed powder slab, titanium powder slab, titanium-tantalum mixed powder slab, tantalum powder slab, titanium-tantalum mixed powder slab, titanium powder slab, tungsten-titanium mixed powder slab, and tungsten powder slab. Perform vacuum pressure sintering to obtain tungsten-based composite material blanks. The vacuum pressure sintering temperature is 1600℃, and the vacuum degree of vacuum pressure sintering is 10. -4 Pa, the pre-pressure of vacuum pressure sintering is 50 MPa;
[0051] Step 5: The tungsten-based composite material billet obtained in Step 4 is subjected to a first rolling and a second rolling process to obtain the rolled tungsten-based composite material. The rolling temperature for the first rolling is 1400℃, and the deformation amount is 70%. The temperature for the second rolling is 600℃, and the deformation amount per pass in the second rolling is 15%. The second rolling process is as follows: the first pass is rolled along the width direction, and then the rolling is carried out alternately along the length and width directions. An argon atmosphere stress-relief annealing treatment is performed between each pass. The stress-relief annealing treatment time is 15 minutes, and the stress-relief annealing treatment temperature is 600℃.
[0052] Step 6: Perform precise temperature-controlled heat treatment on the rolled tungsten-based composite material billet obtained in Step 5 under atmosphere protection to obtain tungsten-based plates; the heat treatment temperature is 600℃, the temperature deviation in the uniform temperature zone is no more than 10℃, and the annealing time of the heat treatment is 30min.
[0053] The tungsten-based plate prepared in this embodiment has a tensile strength of 1589 MPa and an elongation of 14.3%, as tested.
[0054] Example 3
[0055] In this embodiment, the tungsten-based substrate has a tantalum layer as the center, and a titanium-tantalum hybrid layer, a titanium layer, a tungsten-titanium hybrid layer, and a tungsten layer are sequentially arranged on both sides of the tantalum layer from the inside to the outside. The tungsten-titanium hybrid layer has a tungsten element mass percentage of 95%, and the titanium-tantalum hybrid layer has a tantalum element mass percentage of 20%.
[0056] The preparation method of the tungsten-based plate in this embodiment includes the following steps:
[0057] Step 1: Mix tungsten powder and titanium powder to obtain tungsten-titanium mixed powder, and mix titanium powder and tantalum powder to obtain titanium-tantalum mixed powder; the tungsten powder has a purity of 99.995%, a Fisher particle size of 20μm, and an oxygen content of 245ppm; the titanium powder has a purity of 99.993%, a Fisher particle size of 35μm, and an oxygen content of 250ppm; the tantalum powder has a purity of 99.992%, a Fisher particle size of 40μm, and an oxygen content of 240ppm; the tungsten powder accounts for 95% of the mass of the tungsten-titanium mixed powder, and the tantalum powder accounts for 20% of the mass of the titanium-tantalum mixed powder.
[0058] Step 2: The tungsten-titanium mixed powder and the titanium-tantalum mixed powder obtained in Step 1 are respectively subjected to ball milling at a speed of 150 r / min for 2 hours; the ball milling uses titanium balls;
[0059] Step 3: The tungsten powder, titanium powder, tantalum powder, and the ball-milled tungsten-titanium mixed powder and titanium-tantalum mixed powder from Step 1 are subjected to cold isostatic pressing for 10 minutes to obtain tungsten powder blanks, titanium powder blanks, tantalum powder blanks, tungsten-titanium mixed powder blanks, and titanium-tantalum mixed powder blanks; the cold isostatic pressing pressure is 200 MPa, and the thickness of the tungsten-titanium mixed powder blanks and the titanium-tantalum mixed powder blanks is 0.5 mm;
[0060] Step 4: Place the slabs obtained in Step 3 into a mold in the following order: tungsten powder slab, tungsten-titanium mixed powder slab, titanium powder slab, titanium-tantalum mixed powder slab, tantalum powder slab, titanium-tantalum mixed powder slab, titanium powder slab, tungsten-titanium mixed powder slab, and tungsten powder slab. Perform vacuum pressure sintering to obtain a tungsten-based composite material slab. The vacuum pressure sintering temperature is 1200℃, and the vacuum degree is 10. -4 Pa, the pre-pressure of vacuum pressure sintering is 30 MPa;
[0061] Step 5: The tungsten-based composite material billet obtained in Step 4 is subjected to a first rolling and a second rolling process to obtain the rolled tungsten-based composite material. The rolling temperature for the first rolling is 1200℃, and the deformation amount is 50%. The temperature for the second rolling is 400℃, and the deformation amount per pass in the second rolling is 10%. The second rolling process is as follows: the first pass is rolled along the width direction, and then the rolling is carried out alternately along the length and width directions. An argon atmosphere stress-relief annealing treatment is performed between each pass. The stress-relief annealing treatment time is 10 minutes, and the stress-relief annealing treatment temperature is 400℃.
[0062] Step 6: Perform precise temperature-controlled heat treatment on the rolled tungsten-based composite material billet obtained in Step 5 under atmosphere protection to obtain tungsten-based plates; the heat treatment temperature is 400℃, the temperature deviation in the uniform temperature zone is no more than 10℃, and the annealing time of the heat treatment is 10min.
[0063] The tungsten-based plate prepared in this embodiment has a tensile strength of 1567 MPa and an elongation of 14.8%, as tested.
[0064] Example 4
[0065] In this embodiment, the tungsten-based substrate has a tantalum layer as the center, and a titanium-tantalum hybrid layer, a titanium layer, a tungsten-titanium hybrid layer, and a tungsten layer are sequentially arranged on both sides of the tantalum layer from the inside to the outside. The tungsten-titanium hybrid layer has a tungsten element mass percentage of 95%, and the titanium-tantalum hybrid layer has a tantalum element mass percentage of 20%.
[0066] The preparation method of the tungsten-based plate in this embodiment includes the following steps:
[0067] Step 1: Mix tungsten powder and titanium powder to obtain tungsten-titanium mixed powder, and mix titanium powder and tantalum powder to obtain titanium-tantalum mixed powder; the tungsten powder has a purity of 99.995%, a Fisher particle size of 20μm, and an oxygen content of 245ppm; the titanium powder has a purity of 99.99%, a Fisher particle size of 50μm, and an oxygen content of 243ppm; the tantalum powder has a purity of 99.99%, a Fisher particle size of 20μm, and an oxygen content of 243ppm; the tungsten powder accounts for 95% of the mass of the tungsten-titanium mixed powder, and the tantalum powder accounts for 20% of the mass of the titanium-tantalum mixed powder.
[0068] Step 2: The tungsten-titanium mixed powder and the titanium-tantalum mixed powder obtained in Step 1 are respectively subjected to ball milling at a speed of 250 r / min for 5 hours; the ball milling uses titanium balls;
[0069] Step 3: The tungsten powder, titanium powder, tantalum powder, and the ball-milled tungsten-titanium mixed powder and titanium-tantalum mixed powder from Step 1 are subjected to cold isostatic pressing for 15 minutes to obtain tungsten powder blanks, titanium powder blanks, tantalum powder blanks, tungsten-titanium mixed powder blanks, and titanium-tantalum mixed powder blanks; the cold isostatic pressing pressure is 280 MPa, and the thickness of the tungsten-titanium mixed powder blanks and the titanium-tantalum mixed powder blanks is 0.5 mm;
[0070] Step 4: Place the slabs obtained in Step 3 into a mold in the following order: tungsten powder slab, tungsten-titanium mixed powder slab, titanium powder slab, titanium-tantalum mixed powder slab, tantalum powder slab, titanium-tantalum mixed powder slab, titanium powder slab, tungsten-titanium mixed powder slab, and tungsten powder slab. Perform vacuum pressure sintering to obtain a tungsten-based composite material slab. The vacuum pressure sintering temperature is 1400℃, and the vacuum degree is 10. -4 Pa, the pre-pressure of vacuum pressure sintering is 40 MPa;
[0071] Step 5: The tungsten-based composite material billet obtained in Step 4 is subjected to a first rolling and a second rolling process to obtain the rolled tungsten-based composite material. The rolling temperature for the first rolling is 1300℃, and the deformation is 55%. The temperature for the second rolling is 450℃, and the deformation per pass is 10%. The second rolling process is as follows: the first pass is rolled along the width direction, and then the length and width directions are rolled alternately. An argon atmosphere stress-relief annealing treatment is performed between each pass. The stress-relief annealing treatment takes 12 minutes and is performed at a temperature of 450℃.
[0072] Step 6: Perform precise temperature-controlled heat treatment on the rolled tungsten-based composite material billet obtained in Step 5 under atmosphere protection to obtain tungsten-based plates; the heat treatment temperature is 500℃, the temperature deviation in the uniform temperature zone is no more than 10℃, and the annealing time of the heat treatment is 15min.
[0073] The tungsten-based plate prepared in this embodiment has a tensile strength of 1547 MPa and an elongation of 13.8%, as tested.
[0074] Example 5
[0075] In this embodiment, the tungsten-based plate has a tantalum layer as the center, and a titanium-tantalum hybrid layer, a titanium layer, a tungsten-titanium hybrid layer and a tungsten layer are sequentially arranged on both sides of the tantalum layer from the inside to the outside. The tungsten-titanium hybrid layer has a tungsten element mass percentage of 97%, and the titanium-tantalum hybrid layer has a tantalum element mass percentage of 40%.
[0076] The preparation method of the tungsten-based plate in this embodiment includes the following steps:
[0077] Step 1: Mix tungsten powder and titanium powder to obtain tungsten-titanium mixed powder, and mix titanium powder and tantalum powder to obtain titanium-tantalum mixed powder; the tungsten powder has a purity of 99.995%, a Fisher particle size of 20μm, and an oxygen content of 245ppm; the titanium powder has a purity of 99.99%, a Fisher particle size of 50μm, and an oxygen content of 243ppm; the tantalum powder has a purity of 99.99%, a Fisher particle size of 50μm, and an oxygen content of 242ppm; the tungsten powder accounts for 97% of the mass of the tungsten-titanium mixed powder, and the tantalum powder accounts for 40% of the mass of the titanium-tantalum mixed powder.
[0078] Step 2: The tungsten-titanium mixed powder and the titanium-tantalum mixed powder obtained in Step 1 are respectively subjected to ball milling at a speed of 250 r / min for 5 hours; the ball milling uses titanium balls;
[0079] Step 3: The tungsten powder, titanium powder, tantalum powder, and the ball-milled tungsten-titanium mixed powder and titanium-tantalum mixed powder from Step 1 are subjected to cold isostatic pressing for 15 minutes to obtain tungsten powder blanks, titanium powder blanks, tantalum powder blanks, tungsten-titanium mixed powder blanks, and titanium-tantalum mixed powder blanks; the cold isostatic pressing pressure is 280 MPa, and the thickness of the tungsten-titanium mixed powder blanks and the titanium-tantalum mixed powder blanks is 0.5 mm;
[0080] Step 4: Place the slabs obtained in Step 3 into a mold in the following order: tungsten powder slab, tungsten-titanium mixed powder slab, titanium powder slab, titanium-tantalum mixed powder slab, tantalum powder slab, titanium-tantalum mixed powder slab, titanium powder slab, tungsten-titanium mixed powder slab, and tungsten powder slab. Perform vacuum pressure sintering to obtain a tungsten-based composite material slab. The vacuum pressure sintering temperature is 1400℃, and the vacuum degree is 10. -4 Pa, the pre-pressure of vacuum pressure sintering is 40 MPa;
[0081] Step 5: The tungsten-based composite material billet obtained in Step 4 is subjected to a first rolling and a second rolling process to obtain the rolled tungsten-based composite material. The rolling temperature for the first rolling is 1300℃, and the deformation is 55%. The temperature for the second rolling is 450℃, and the deformation per pass is 10%. The second rolling process is as follows: the first pass is rolled along the width direction, and then the rolling is performed alternately along the length and width directions. An argon atmosphere stress-relief annealing treatment is performed between each pass. The stress-relief annealing treatment takes 13 minutes and is performed at a temperature of 550℃.
[0082] Step 6: Perform precise temperature-controlled heat treatment on the rolled tungsten-based composite material billet obtained in Step 5 under atmosphere protection to obtain tungsten-based plates; the heat treatment temperature is 520℃, the temperature deviation in the uniform temperature zone is no more than 10℃, and the annealing time of the heat treatment is 20min.
[0083] Upon testing, the tungsten-based plate prepared in this embodiment has a tensile strength of 1523 MPa and an elongation of 12.9%.
[0084] Comparative Example 1
[0085] The difference between this comparative example and Example 1 is that the purity, Fisher particle size, and oxygen content of the raw materials in step one are different. The tungsten powder has a purity of 99.9 wt%, a Fisher particle size of 48 μm, and an oxygen content of 500 ppm; the titanium powder has a purity of 99.9 wt%, a Fisher particle size of 65 μm, and an oxygen content of 650 ppm; and the tantalum powder has a purity of 99.9 wt%, a Fisher particle size of 40 μm, and an oxygen content of 500 ppm.
[0086] Upon testing, the tungsten-based plate prepared in this embodiment has a tensile strength of 1037 MPa and an elongation of 5.4%.
[0087] The tungsten, titanium, and tantalum powders used in this comparative example had low purity, large Fisher particle size, and high oxygen content, leading to reduced tensile strength and elongation of the tungsten-based sheet. Since tungsten has a body-centered cubic structure and is brittle at room temperature, the ductile-brittle transition temperature (DBTT) is a crucial parameter characterizing the ductility and brittleness of tungsten-based materials. Above the DBTT, tungsten exhibits toughness and can undergo plastic deformation; below the DBTT, tungsten processing deformation easily results in brittle fracture. The DBTT of tungsten materials is mainly related to the purity of raw materials, oxygen content, preparation method, and impurity content. Reducing the content of non-metallic interstitial impurities such as oxygen and nitrogen can effectively lower the DBTT of tungsten-based composites and improve their elongation. On the other hand, oxygen segregation at grain boundaries reduces the bonding force of tungsten grain boundaries, thereby decreasing the mechanical properties of tungsten-based composites.
[0088] In summary, the purity, Fisher particle size, and oxygen content of the tungsten powder, titanium powder, and tantalum powder provided in this invention can help improve the strength and toughness of tungsten-based plates.
[0089] Comparative Example 2
[0090] The difference between this comparative example and Example 1 is that the vacuum pressure sintering temperature in step four is 700°C and the vacuum degree is 10. -3 Pa, with a pre-pressure of 20MPa, in step five, the tungsten-based composite material billet is heated to 900°C under argon atmosphere protection and then rolled, with a rolling deformation of 70%.
[0091] The tungsten-based composite material billet in this comparative example cracked after roughing and rolling, and delamination occurred at the interface, resulting in sample failure.
[0092] In this comparative example, the vacuum pressure sintering temperature was 700℃, which is lower than the allotropic transformation temperature of titanium (882℃). Titanium cannot transform from a close-packed hexagonal structure to a body-centered cubic structure, and tungsten and tantalum cannot diffuse through vacancies, resulting in low interfacial bonding. Furthermore, the sintering temperature was too low, and the pressure was too small (only 20 MPa), leading to insufficient bonding between powder particles, affecting the microstructure between particles, and causing cracking of the sample during subsequent rolling. Additionally, the rolling temperature in step six was too low at 900℃. Under these conditions, tungsten has extremely low fluidity and plasticity, which also leads to cracking of the sheet metal.
[0093] In summary, the vacuum pressure sintering temperature and pre-pressure set in this invention are beneficial to improving the bonding force between the metal slabs of each layer.
[0094] Comparative Example 3
[0095] The difference between this comparative example and Example 2 is that the tungsten-based plate in this comparative example has a tantalum layer as the center, and titanium layers and tungsten layers are respectively arranged on both sides of the tantalum layer from the inside to the outside.
[0096] The tungsten-based plate prepared in this embodiment has a tensile strength of 714 MPa and an elongation of 3.3%, as tested.
[0097] The tungsten-based plates used in this comparative example were slabs without tungsten-titanium mixed powder and slabs without titanium-tantalum mixed powder. Test results showed a decrease in both tensile strength and elongation. This is because during sintering, the interfaces between the tungsten and titanium layers, and between the titanium and tantalum layers, could not be completely diffused and wetted, resulting in defects such as pores at the interfaces, which affected the subsequent rolling effect. Furthermore, only a very small solid solution region was formed between the tungsten and titanium layers, and between the titanium and tantalum layers, and the reduced number of interfaces within the tungsten-based plate also led to a decrease in the strength and toughness of the tungsten-based plate.
[0098] In summary, this invention demonstrates that by setting a titanium-tantalum hybrid layer between the tantalum layer and the titanium layer, and a tungsten-titanium hybrid layer between the titanium layer and the tungsten layer, it can effectively improve the strength and toughness of tungsten-based plates.
[0099] The above description is merely a preferred embodiment of the present invention and does not constitute any limitation on the present invention. Any simple modifications, alterations, or equivalent structural transformations made to the above embodiments based on the technical essence of the present invention shall still fall within the protection scope of the present invention.
Claims
1. A high-strength, high-toughness tungsten-based plate for nuclear applications, characterized in that, The tungsten-based plate has a tantalum layer at its center, and on both sides of the tantalum layer, from the inside out, a titanium-tantalum hybrid layer, a titanium layer, a tungsten-titanium hybrid layer, and a tungsten layer are respectively arranged sequentially. The tungsten-titanium hybrid layer contains a tungsten element with a mass percentage of not less than 95%, and the titanium-tantalum hybrid layer contains a tantalum element with a mass percentage of not less than 20%. The method for preparing the tungsten-based plate includes the following steps: Step 1: Mix tungsten powder and titanium powder to obtain tungsten-titanium mixed powder, and mix titanium powder and tantalum powder to obtain titanium-tantalum mixed powder; Step 2: Ball mill the tungsten-titanium mixed powder and the titanium-tantalum mixed powder obtained in Step 1 respectively; Step 3: The tungsten powder, titanium powder, tantalum powder, and the ball-milled tungsten-titanium mixed powder and titanium-tantalum mixed powder from Step 1 are subjected to cold isostatic pressing to obtain tungsten powder slabs, titanium powder slabs, tantalum powder slabs, tungsten-titanium mixed powder slabs, and titanium-tantalum mixed powder slabs. Step 4: Place the slabs obtained in Step 3 into the mold in the following order: tungsten powder slab, tungsten-titanium mixed powder slab, titanium powder slab, titanium-tantalum mixed powder slab, tantalum powder slab, titanium-tantalum mixed powder slab, titanium powder slab, tungsten-titanium mixed powder slab, and tungsten powder slab, and perform vacuum pressure sintering to obtain tungsten-based composite material slabs. Step 5: The tungsten-based composite material billet obtained in Step 4 is subjected to initial rolling and second rolling in sequence to obtain the rolled tungsten-based composite material. Step 6: Heat treat the rolled tungsten-based composite material billet obtained in Step 5 to obtain tungsten-based plates.
2. The high-strength, high-toughness tungsten-based plate for nuclear applications according to claim 1, characterized in that, The tungsten-based plate has a tensile strength of not less than 1500 MPa and an elongation of not less than 10%.
3. The high-strength, high-toughness tungsten-based plate for nuclear applications according to claim 1, characterized in that, In step one, the tungsten powder has a purity of not less than 99.99%, a Fisher particle size of not more than 30µm, and an oxygen content of not more than 300ppm; the titanium powder has a purity of not less than 99.99%, a Fisher particle size of 25µm to 50µm, and an oxygen content of not more than 300ppm; the tantalum powder has a purity of not less than 99.99%, a Fisher particle size of 20µm to 50µm, and an oxygen content of not more than 300ppm.
4. The high-strength, high-toughness tungsten-based plate for nuclear applications according to claim 1, characterized in that, In step two, titanium balls are used for ball milling, the milling time is 2h to 10h, and the milling speed is 150r / min to 350r / min.
5. The high-strength, high-toughness tungsten-based plate for nuclear applications according to claim 1, characterized in that, The cold isostatic pressing pressure in step three is 200MPa~300MPa, the cold isostatic pressing time is 10min~20min, and the thickness of the tungsten-titanium mixed powder slab and the titanium-tantalum mixed powder slab is no more than 1mm.
6. The high-strength, high-toughness tungsten-based plate for nuclear applications according to claim 1, characterized in that, The vacuum pressure sintering temperature in step four is 1200℃~1600℃, and the vacuum degree of the vacuum pressure sintering is no greater than 10. -4 Pa, the pre-pressure of the vacuum pressure sintering is 30MPa~50MPa.
7. The high-strength, high-toughness tungsten-based plate for nuclear applications according to claim 1, characterized in that, In step five, the rolling temperature for the initial rolling is 1200℃~1400℃, and the total deformation of the initial rolling is 50%~70%; the temperature for the second rolling is 400℃~600℃, and the deformation per pass of the second rolling is 10%~15%. The process of the second rolling is as follows: the first pass is rolled along the width direction, and then the rolling is carried out alternately along the length and width directions. An argon atmosphere stress-relief annealing treatment is performed between each pass; the stress-relief annealing treatment time is 10min~15min, and the stress-relief annealing treatment temperature is 400℃~600℃.
8. The high-strength, high-toughness tungsten-based plate for nuclear applications according to claim 1, characterized in that, The heat treatment described in step six is a precise temperature-controlled heat treatment process under atmosphere protection. The temperature of the heat treatment is 400℃~600℃, the temperature deviation in the uniform temperature zone is no more than 10℃, and the annealing time of the heat treatment is 10min~30min.
Citation Information
Patent Citations
A layered gradient structure tungsten-based composite material and its preparation method
CN110053328B
Layered gradient-structure tungsten-based composite material and preparation method thereof