A polishing pad for CVD diamond coarse polishing and its preparation method

By designing and selecting the materials for the polishing pad, the problem of low polishing efficiency of polycrystalline CVD diamond was solved, achieving a high-efficiency and low-cost polishing effect suitable for large-scale production.

CN119369288BActive Publication Date: 2026-11-17HENAN UNION ABRASIVES
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411617644.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-11-13
Publication Date
2026-11-17
Estimated Expiration
2044-11-13

AI Technical Summary

Technical Problem

Polishing polycrystalline CVD diamond using existing technologies is difficult. Traditional mechanical grinding and abrasive wheel polishing are inefficient, costly, and fail to meet the high crystal quality requirements of the semiconductor industry.

Method used

A polishing pad is used, which contains a high resin content and extremely tough abrasive blocks. It uses diamond-silicon carbide abrasive and glass fiber, combined with a specific ratio and shape design, to achieve rapid removal of the subsurface damage layer and improve polishing efficiency.

Benefits of technology

Polishing pads can quickly remove the subsurface damage layer of polycrystalline CVD diamond, improve polishing efficiency, reduce costs, are suitable for large-scale production, and have low equipment requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119369288B_ABST
    Figure CN119369288B_ABST
Patent Text Reader

Abstract

This invention belongs to the technical field of grinding tools, and relates to a grinding pad for rough polishing of CVD diamond and its preparation method. The grinding pad of this invention includes a substrate and grinding blocks with flat top surfaces disposed on the substrate. The ratio of the diameter or side length of the grinding blocks to the gap distance between adjacent grinding blocks is 10-15:1-1.5; the top of the grinding blocks is rounded; the raw materials for preparing the grinding blocks include diamond-silicon carbide abrasive, binder, glass fiber, and filler; the roundness of the diamond-silicon carbide abrasive is 0.80-0.85, and the D50 particle size is 40-60μm; the grinding pad of this invention has high strength and modulus, good stability, and high grinding and polishing efficiency. The grinding blocks of the grinding pad are densely distributed, with a large grinding area. The grinding blocks have chamfers and gaps, which can prevent scratches during CVD diamond polishing and also remove debris; the abrasive in the grinding pad has high strength, good self-sharpening properties, and good holding force, thus ensuring that the grinding pad has strong grinding ability and good processing effect during the rough polishing process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of abrasive tool technology, and more particularly to an abrasive pad and its preparation method. Background Technology

[0002] In recent years, driven by emerging industries such as electric vehicles and 5G communications, the third-generation semiconductor industry, primarily based on silicon carbide and gallium nitride, has received widespread attention and ushered in a period of rapid development. Diamond is the most promising candidate material for next-generation power devices, possessing a higher bandgap (5.5 eV), thermal conductivity (2000 W / m·K), and breakdown field strength (>10 MV / cm) than silicon carbide, along with stable chemical properties and extremely strong radiation resistance. Diamond devices are mostly fabricated using CVD methods. Polycrystalline CVD diamond films, with their high thermal conductivity and high surface flatness, can significantly improve the heat dissipation capacity of semiconductor power devices when introduced into their structures, thus offering broader application areas and prospects. The processing of polycrystalline CVD diamond film materials is a complex process, in which ultra-precision polishing technology plays a crucial role in reducing surface roughness and removing subsurface damage. Due to the semiconductor industry's high requirements for crystal quality, coupled with diamond's extremely high hardness and excellent chemical stability, polishing is more difficult. Currently, there is no complete processing route or a suitable fine polishing method.

[0003] Currently, the processing of polycrystalline CVD diamond primarily utilizes mechanical grinding, employing fluid abrasives with cast iron discs. This process can thin polycrystalline CVD diamond substrates. This three-body grinding process requires strict control over the abrasive particle size; even a few large particles can easily cause scratches and deep damage, resulting in high roughness and a significant damage layer on the ground diamond surface. Subsequent polishing with resin-bonded diamond wheels can take over 20 hours. While these wheels are effective at polishing due to their high diamond content, numerous cutting edges, and certain elasticity, reducing the roughness of polycrystalline CVD diamonds, they also have drawbacks. Resin-bonded diamond wheels are expensive, and because the resin matrix has some elasticity, polishing polycrystalline CVD diamonds is time-consuming and inefficient. Therefore, it is necessary to develop a polishing product with moderate matrix hardness that can rapidly reduce roughness. Summary of the Invention

[0004] To address the technical problems of diamond polishing in existing technologies, this invention proposes an abrasive pad for CVD diamond coarse polishing and its preparation method. This abrasive pad features a special formulation system with high resin content and extremely high toughness. The abrasive used in the system has high strength and unique properties. This product can rapidly remove the subsurface damage layer of the product, which is more efficient than polishing with a grinding wheel alone. Furthermore, the manufacturing process is simple, the cost is low, the equipment requirements are not high, and the polishing cycle is short, improving production efficiency. It is suitable for large-scale production.

[0005] To achieve the above objectives, the technical solution of the present invention is implemented as follows: A polishing pad for CVD diamond coarse polishing, the polishing pad comprising a substrate and a plurality of polishing blocks with flat top surfaces disposed on the substrate, wherein the ratio of the diameter or side length of the polishing block to the gap distance between adjacent polishing blocks is 10-15:1-1.5; the top of the polishing block is rounded; the raw materials for preparing the polishing block are: diamond-silicon carbide abrasive, binder, glass fiber and filler.

[0006] Preferably, the top surface diameter or side length of the grinding block is 10-15mm, and the gap is 1-1.5mm; the radius R of the rounded corner at the top of the grinding block is 0.5-1mm.

[0007] If the spacing ratio between the grinding blocks is too large, or the radius of the fillet R is too large, the contact area with the workpiece during processing will be less, affecting the surface processing quality. If the spacing ratio is too small or the fillet radius is too small, it will affect the demolding process of the grinding particles and the chip removal during the grinding process.

[0008] Preferably, the ratio of the height of the grinding block (01) to the gap distance between adjacent grinding blocks (01) is 2-3:1; the roundness of the diamond-silicon carbide abrasive is 0.80-0.85, and the D50 particle size is 40-60μm; the binder is an epoxy resin polymer.

[0009] Preferably, the method for preparing the diamond-silicon carbide abrasive includes the following steps: a) Diamond powder with a Raman value of 3.0 or higher is obtained by airflow crushing, shaping, sedimentation and classification to obtain diamond powder with a D50 of about 40-60μm. Diamond-silicon carbide composite abrasive is prepared by the composite abrasive preparation method in patent CN118061074A. The raw material diamond has a Raman value of 3.0 or higher. b) The obtained diamond-silicon carbide composite abrasive is mixed with diamond powder with D50 of 10-30μm and D50 of 90-110μm, and then placed in a steel cylinder. The volume of the diamond is less than half the volume of the cylinder. At the same time, a certain amount of steel balls are added to the cylinder. Then, a vertical three-dimensional mixer is used for mixing and stirring. After the mixing is completed, the resulting mixture is sieved through 230# and 400# sieves to obtain diamond-silicon carbide abrasive powder with a roundness coefficient of 0.80-0.85 and a D50 range of 40-60μm.

[0010] Preferably, the roundness of the diamond-silicon carbide composite abrasive in step (a) is 0.7 or higher.

[0011] Preferably, in step (b), the mass ratio of diamond-silicon carbide composite abrasive, diamond powder with a D50 of 20 μm, and diamond powder with a D50 of 100 μm is 1:1:2 to 1:1:4.

[0012] Because diamond-silicon carbide composite abrasives are slightly less hard than diamond powder, their roundness can be efficiently shaped through ball milling with diamond particles of varying sizes. The resulting diamond-silicon carbide composite abrasives exhibit high roundness and particle size concentration. This differs from traditional ball milling processes, which involve mixing abrasives of different sizes together for shaping, resulting in lower efficiency. The diamond surface produced by this ball milling method is rough, and the resin matrix's holding force reduces the risk of abrasive detachment during processing.

[0013] The technical method in this invention is possible because the surface layer of the diamond-silicon carbide composite abrasive is basically silicon carbide with a thickness of 2-3 μm and a strength slightly lower than that of pure diamond micro powder. By using diamonds of different particle sizes, the raw material can be efficiently shaped. At the same time, compared with single-crystal diamond, the diamond-silicon carbide composite material is easier to shape, and the diamond-silicon carbide composite material has better self-sharpening properties, which can ensure a stronger cutting force.

[0014] High-grade diamond micron powder with a Raman value of 3.0 or higher is used because the grinding pad has higher grinding force and processing efficiency during the coarse polishing of polycrystalline CVD. The outer surface thickness of the diamond-silicon carbide composite abrasive can be controlled by the sintering process. The composite abrasive is mixed with diamond powder with D50≈20 and D50≈100μm to better sieve the abrasive with the target particle size after ball milling and shaping.

[0015] The above-mentioned quality ratio is to ensure the shaping effect. The amount of material and time for each shaping are also for the shaping effect, ensuring that the roundness of the composite abrasive is between 0.8 and 0.85. If the roundness is too low, it will affect the polishing quality of the grinding pad. If the roundness is too high, the cutting force will be insufficient, which will affect the processing efficiency.

[0016] Preferably, the adhesive is bisphenol A type epoxy resin, bisphenol S type epoxy resin, bisphenol F type epoxy resin or H type epoxy resin; the diameter of the glass fiber is 5-10 μm.

[0017] The binder has high strength and high modulus, giving the polishing pad a high overall hardness and ensuring polishing performance. Glass fiber enhances the hardness and rigidity of the binder.

[0018] Preferably, the filler is one or any combination of calcium silicate, magnesium carbonate, sodium silicate, and phosphate; the D50 particle size of the filler is 2-5 μm. Controlling the particle size of the filler within the above range can ensure the self-sharpening property of the grinding pad during the grinding process while guaranteeing the surface quality of the workpiece.

[0019] The substrate (02) includes an adhesive layer (03), a substrate layer (04), and a backing adhesive layer (05); the adhesive layer (03) is formed by screen printing and then curing with adhesive, and the adhesive is a mixture of epoxy thermosetting resin and inorganic powder; the substrate layer (04) is made of PC board, PET board or PP board.

[0020] To facilitate the fixing of the polishing pad to the upper and lower surfaces of the polishing machine during use, the substrate also includes an adhesive backing layer, which is disposed on the side of the substrate layer away from the adhesive layer.

[0021] Preferably, the mass fractions of the raw materials diamond-silicon carbide abrasive, binder, glass fiber and filler are 10-20%, 50-60%, 5-10% and 10-35% respectively, and the total mass fraction of the raw materials is 100%.

[0022] Controlling the mass ratio of diamond-silicon carbide composite abrasive, binder, glass fiber, and filler within the aforementioned range ensures that the grinding block has high strength and rigidity, maintains shape stability under stress, and is not prone to deformation. This improves the overall strength of the grinding pad, reduces its yielding, and guarantees both cutting efficiency and surface finish of the workpiece.

[0023] Preferably, in step (2), the abrasive is mixed using a vertical three-dimensional mixer, and the mixing time is 1-3 hours.

[0024] Preferably, the method for preparing the polishing pad for CVD diamond coarse polishing includes the following steps: 1) Prepare a mold, which has multiple grooves for forming grinding blocks, the shape of which matches the shape of the grinding blocks; The diamond-silicon carbide abrasive, binder, glass fiber and filler are mixed and stirred to form a slurry; 2) Fill the prepared slurry into each groove of the mold, ensuring even filling. Then, apply adhesive to cover the slurry filling the grooves. Next, lay a layer of screen mesh on top of the adhesive coating on the mold surface, impregnating the mesh with the adhesive. Then, press a substrate with double-sided adhesive on one side onto the screen mesh surface, ensuring the adhesive layer faces away from the mesh. Finally, demold after heat curing. The adhesive-impregnated screen mesh and substrate support ensure the integrity of the abrasive block after demolding. The adhesive comprises epoxy thermosetting resin and inorganic powder; the inorganic powder includes any one of calcium silicate, magnesium carbonate, sodium silicate, and phosphate; the screen mesh is either nylon or glass fiber. Nylon and glass fiber meshes have stronger holding power for the abrasive particles compared to non-woven fabrics. The mass ratio of epoxy thermosetting resin to inorganic powder is 6-7:3-4.

[0025] The mold is made of metal, and the grooves and chamfers on the mold are laser-engraved. Compared with silicone molds, metal molds have better strength and hardness. In this patent, the spacing between the grinding blocks is small, which ensures the integrity and operability of demolding this special structure of grinding blocks.

[0026] The present invention has the following beneficial effects: 1. The grinding pad structure for CVD diamond rough polishing in this invention features a unique design. Compared to ordinary grinding pads, the grinding blocks are more densely distributed and have a larger grinding area. This prevents scratches on the CVD diamond during polishing, while maintaining a certain gap between the grinding blocks to remove debris. Furthermore, the spacing ratio between the grinding blocks facilitates chip removal and demolding during the grinding process. The rounded corners also aid in demolding during processing and ensure the quality of the processed surface. The dense distribution of grinding blocks and the larger grinding area ensure sufficient contact area between the grinding pad and the workpiece during grinding, thereby improving the surface quality of the workpiece.

[0027] 2. The grinding blocks used in this invention for CVD diamond coarse polishing pads have a suitable raw material ratio, high resin content, high hardness and modulus, and extremely high toughness. Simultaneously, the addition of a certain amount of glass fiber to the grinding pad system ensures that the overall grinding pad has high strength, maintains shape stability under stress, and is not prone to deformation, thus guaranteeing polishing efficiency. The abrasive uses specially formulated diamond-silicon carbide abrasive (the raw material diamond has a Raman value above 3.0), which has high hardness, strong self-sharpening properties, and high grinding efficiency. This enables rapid removal of the subsurface damage layer of the product, reducing additional damage to the CVD diamond. The roundness control (shape factor of 0.8-0.85) improves the abrasive's holding force while ensuring processing quality, thereby increasing the polishing efficiency and service life of the grinding pad.

[0028] 3. The manufacturing process of the CVD diamond coarse polishing pad of the present invention is simple, the cost is low, the equipment requirements are not high, and the polishing cycle is short, which improves the production efficiency and is suitable for large-scale production. Attached Figure Description

[0029] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0030] Figure 1 This is a schematic diagram of the structure of the CVD diamond coarse polishing pad of the present invention; Figure 2 This is a cross-sectional schematic diagram of the CVD diamond coarse polishing pad of the present invention; Among them, 01-grinding block, 02-substrate, 03-adhesive layer, 04-substrate layer, and 05-back adhesive layer. Detailed Implementation

[0031] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0032] The diamond-silicon carbide composite abrasives used in the following embodiments are prepared by a method including the following steps: a mixed powder composed of diamond particles and graphite-coated silicon particles is subjected to heat treatment in an oxygen-free atmosphere to vaporize silicon; the material obtained after heat treatment is ground and then naturally settled and classified to remove impurity silicon carbide; then, hydrofluoric acid is used to clean and remove impurity silicon, thus obtaining the diamond-silicon carbide composite abrasive; the diamond particles are bare diamond material and / or carbon-coated diamond particles; the heat treatment temperature is 1400~1600℃, and the heat treatment time is 2~5h.

[0033] Example 1 This embodiment uses a polishing pad for CVD diamond coarse polishing, such as... Figure 1 and Figure 2 As shown, the device includes a substrate 02 and a grinding block 01 disposed on the substrate. The substrate 02 includes, from bottom to top, a backing adhesive layer 05, a substrate layer 04, and an adhesive layer 03, which are formed by impregnating nylon mesh with adhesive and then curing it. The grinding block 01 is a square with a top side length of 10 mm, and the spacing between adjacent grinding blocks 01 is 1 mm. The four corners of the upper surface of the grinding block 01 have a radius of 0.5 mm. The grinding block 01 is made of the following raw materials in the following mass percentages: 15% diamond-silicon carbide composite abrasive, 55% bisphenol A type epoxy resin binder, 5% glass fiber, and 25% filler. The diameter of the glass fiber used is 5 μm. The filler is calcium silicate with a D50 particle size of 2 μm. The diamond-silicon carbide composite abrasive has a D50 particle size of 50 μm and a roundness of 0.80, and is prepared by a method including the following steps: Step 1: Mixing: Mix diamond-silicon carbide composite abrasive with diamond powder of D50≈20μm and D50≈100μm, wherein the ratio of the three is 1:1:2 (composite abrasive: diamond powder D50≈20μm : diamond powder D50≈100μm). The second step is ball milling: Pour the mixed abrasive into the mixing tank, add a certain amount of steel balls, and make sure the total volume does not exceed 1 / 2 of the tank. Then, use a vertical three-dimensional mixer to stir for 1 hour.

[0034] The third step is screening: the ball-milled abrasive is screened through 230# and 400# metal woven screens to separate the diamond-silicon carbide composite abrasive.

[0035] The fourth step is cleaning: the sieved diamond-silicon carbide composite abrasive is ultrasonically cleaned and dried to obtain diamond-silicon carbide composite abrasive with a roundness of 0.8.

[0036] The abrasive pad in this embodiment is prepared using a method including the following steps: 1) Prepare a metal mold with multiple grooves for forming the grinding block 01. The shape of the grooves matches the shape of the grinding block 01. Diamond-silicon carbide composite abrasive, binder, glass fiber and filler are dispersed in a polytetrafluoroethylene tank and a slurry is formed by double planetary mixing. 2) Fill the prepared slurry into each metal groove, ensuring even filling. Scrape off the adhesive from the grooves, leaving the adhesive covering the slurry filling the grooves. Then, lay a layer of nylon mesh on top of the adhesive applied to the mold surface, allowing the adhesive to impregnate the mesh. Next, press a PC sheet with double-sided adhesive on one side onto the mesh surface, ensuring the adhesive layer is away from the nylon mesh. Finally, demold after heat curing. The adhesive-impregnated mesh and the support provided by the PC sheet ensure the integrity of the grinding block 01 after demolding.

[0037] Example 2 This embodiment uses a polishing pad for CVD diamond coarse polishing, such as... Figure 1 and Figure 2 As shown, it includes a substrate 02 and an abrasive block 01 disposed on the substrate; the substrate 02 includes, from bottom to top, a backing adhesive layer 05, a substrate layer 04, and an adhesive layer 03, which are formed by impregnating nylon mesh with adhesive and then curing it; the abrasive block 01 is a square with a top side length of 15mm, the spacing between adjacent abrasive blocks 01 is 1.5mm, and the four corners of the upper surface of the abrasive block 01 have a radius of 0.5mm; the abrasive block 01 is made of the following raw materials in the following mass percentages: 15% diamond-silicon carbide composite abrasive, 55% bisphenol S type epoxy resin binder, 5% glass fiber, and 25% filler; the diameter of the glass fiber used is 5μm; the filler is calcium silicate with a D50 particle size of 2μm; the diamond-silicon carbide composite abrasive has a D50 particle size of 50μm and a roundness of 0.80, and is prepared by a method including the following steps: Step 1: Mixing: Mix diamond-silicon carbide composite abrasive with diamond powder of D50≈10 and D50≈90μm, wherein the ratio of the three is 1:1:2 (composite abrasive: diamond powder D50≈10μm: diamond powder D50≈90μm). The second step is ball milling: Pour the mixed abrasive into the mixing tank, add a certain amount of steel balls, and make sure the total volume does not exceed 1 / 2 of the tank. Then, use a vertical three-dimensional mixer to stir for 1 hour.

[0038] The third step is screening: the ball-milled abrasive is screened through 230# and 400# metal woven screens to separate the diamond-silicon carbide composite abrasive.

[0039] The fourth step is cleaning: the sieved diamond-silicon carbide composite abrasive is ultrasonically cleaned and dried to obtain diamond-silicon carbide composite abrasive with a roundness of 0.8.

[0040] The abrasive pad in this embodiment is prepared using a method including the following steps: 1) Prepare a metal mold with multiple grooves for forming the grinding block 01. The shape of the grooves matches the shape of the grinding block 01. Diamond-silicon carbide composite abrasive, binder, glass fiber and filler are dispersed in a polytetrafluoroethylene tank and a slurry is formed by double planetary mixing. 3) Fill the prepared slurry into each metal groove, ensuring even filling. Afterward, scrape off the adhesive. The adhesive is a mixture of epoxy thermosetting resin and calcium silicate in a 7:3 ratio. Cover the slurry filling the grooves with the adhesive, then lay a layer of fiberglass mesh on top of the adhesive coating on the mold surface, allowing the adhesive to impregnate the mesh. Next, press a PC sheet with double-sided adhesive on one side onto the mesh surface, ensuring the adhesive layer is away from the fiberglass mesh. Finally, demold after heat curing. The adhesive-impregnated mesh and the supporting PC sheet ensure the integrity of the grinding block 01 after demolding.

[0041] Example 3 This embodiment uses a polishing pad for CVD diamond coarse polishing, such as... Figure 1 and Figure 2 As shown, the device includes a substrate 02 and abrasive blocks 01 disposed on the substrate. The substrate 02 includes, from bottom to top, a backing adhesive layer 05, a substrate layer 04, and an adhesive layer 03, which are formed by impregnating nylon mesh with adhesive and then curing it. The abrasive blocks 01 are squares with a top side length of 10 mm, and the spacing between the abrasive blocks 01 is 1 mm. The four corners of the upper surface of the abrasive blocks 01 have a radius of 1 mm. The abrasive blocks 01 are made of the following raw materials in the following mass percentages: 15% diamond-silicon carbide composite abrasive, 55% bisphenol A type epoxy resin binder, 5% glass fiber, and 25% filler. The diameter of the glass fiber used is 5 μm. The filler is calcium silicate with a D50 particle size of 2 μm. The diamond-silicon carbide composite abrasive has a D50 particle size of 50 μm and a roundness of 0.80, and is prepared by a method including the following steps: Step 1: Mixing: Mix diamond-silicon carbide composite abrasive with diamond powder of D50≈30 and D50≈110μm, wherein the ratio of the three is 1:1:2 (composite abrasive: diamond powder D50≈30μm: diamond powder D50≈110μm). The second step is ball milling: Pour the mixed abrasive into the mixing tank, add a certain amount of steel balls, and make sure the total volume does not exceed 1 / 2 of the tank. Then, use a vertical three-dimensional mixer to stir for 1 hour.

[0042] The third step is screening: the ball-milled abrasive is screened through 230# and 400# metal woven screens to separate the diamond-silicon carbide composite abrasive.

[0043] The fourth step is cleaning: the sieved diamond-silicon carbide composite abrasive is ultrasonically cleaned and dried to obtain diamond-silicon carbide composite abrasive with a roundness of 0.8.

[0044] The preparation method of the abrasive pad in this embodiment is the same as that of the abrasive pad in Example 1.

[0045] Example 4 This embodiment uses a polishing pad for CVD diamond coarse polishing, such as... Figure 1 and Figure 2 As shown, the device includes a substrate 02 and grinding blocks 01 disposed on the substrate. The substrate 02 includes, from bottom to top, a backing adhesive layer 05, a substrate layer 04, and an adhesive layer 03, which are formed by impregnating nylon mesh with adhesive and then curing it. The grinding blocks 01 are squares with a top side length of 10 mm, and the spacing between the grinding blocks 01 is 1 mm. The four corners of the upper surface of the grinding blocks 01 have a radius of 0.5 mm. The grinding blocks 01 are made of the following raw materials in the following mass percentages: 15% diamond-silicon carbide composite abrasive, 55% bisphenol S type epoxy resin binder, 5% glass fiber, and 25% filler. The diameter of the glass fiber used is 5 μm. The filler is calcium silicate with a D50 particle size of 2 μm. The diamond-silicon carbide composite abrasive has a D50 particle size of 50 μm and a roundness of 0.80, and is prepared by a method including the following steps: Step 1: Mixing: Mix diamond-silicon carbide composite abrasive with diamond powder of D50≈20 and D50≈100, wherein the ratio of the three is 1:1:4 (composite abrasive: diamond powder D50≈20um: diamond powder D50≈100um). The second step is ball milling: Pour the mixed abrasive into the mixing tank, add a certain amount of steel balls, and make sure the total volume does not exceed 1 / 2 of the tank. Then, use a vertical three-dimensional mixer to stir for 1 hour.

[0046] The third step is screening: the ball-milled abrasive is screened through 230# and 400# metal woven screens to separate the diamond-silicon carbide composite abrasive.

[0047] The fourth step is cleaning: the sieved diamond-silicon carbide composite abrasive is ultrasonically cleaned and dried to obtain diamond-silicon carbide composite abrasive with a roundness of 0.8.

[0048] The preparation method of the abrasive pad in this embodiment is the same as that of the abrasive pad in Example 1.

[0049] Example 5 This embodiment uses a polishing pad for CVD diamond coarse polishing, such as... Figure 1 and Figure 2As shown, the device includes a substrate 02 and abrasive blocks 01 disposed on the substrate. The substrate 02 includes, from bottom to top, a backing adhesive layer 05, a substrate layer 04, and an adhesive layer 03, which are formed by impregnating nylon mesh with adhesive and then curing it. The abrasive blocks 01 are squares with a top side length of 10 mm, and the spacing between the abrasive blocks 01 is 1 mm. The four corners of the upper surface of the abrasive blocks 01 have a radius of 0.5 mm. The abrasive blocks 01 are made of the following raw materials in the following mass percentages: 15% diamond-silicon carbide composite abrasive, 55% bisphenol F type epoxy resin binder, 5% glass fiber, and 25% filler. The diameter of the glass fiber used is 5 μm. The filler is calcium phosphate with a D50 particle size of 2 μm. The diamond-silicon carbide composite abrasive has a D50 particle size of 50 μm and a roundness of 0.85, and is prepared by a method including the following steps: Step 1: Mixing: Mix diamond-silicon carbide composite abrasive with diamond powder of D50≈20 and D50≈100, wherein the ratio of the three is 1:1:2 (composite abrasive: diamond powder D50≈20um: diamond powder D50≈100um). The second step is ball milling: Pour the mixed abrasive into the mixing tank, add a certain amount of steel balls, and the total volume should not exceed 1 / 2 of the tank. Stir for 3 hours using a vertical three-dimensional mixer.

[0050] The third step is screening: the ball-milled abrasive is screened through 230# and 400# metal woven screens to separate the diamond-silicon carbide composite abrasive.

[0051] The fourth step is cleaning: the sieved diamond-silicon carbide composite abrasive is ultrasonically cleaned and dried to obtain diamond-silicon carbide composite abrasive with a roundness of 0.85.

[0052] The preparation method of the abrasive pad in this embodiment is the same as that of the abrasive pad in Example 1.

[0053] Example 6 This embodiment uses a polishing pad for CVD diamond coarse polishing, such as... Figure 1 and Figure 2As shown, it includes a substrate 02 and abrasive blocks 01 disposed on the substrate; the substrate 02 includes, from bottom to top, a backing adhesive layer 05, a substrate layer 04, and an adhesive layer 03, which are formed by impregnating nylon mesh with adhesive and then curing it; the abrasive blocks 01 are squares with a top side length of 10mm, the spacing between the abrasive blocks 01 is 1.5mm, and the four corners of the upper surface of the abrasive blocks 01 have a radius of 0.5mm; the abrasive blocks 01 are made of the following raw materials in the following mass percentages: 15% diamond-silicon carbide composite abrasive, 50% H-type epoxy resin binder, 5% glass fiber, and 35% filler; the diameter of the glass fiber used is 5μm; the filler is magnesium carbonate with a D50 particle size of 2μm; the diamond-silicon carbide composite abrasive has a D50 particle size of 40μm and a roundness of 0.80, and is prepared by a method including the following steps: Step 1: Mixing: Mix diamond-silicon carbide composite abrasive with diamond powder of D50≈20 and D50≈100, wherein the ratio of the three is 1:1:2 (composite abrasive: diamond powder D50≈20um: diamond powder D50≈100um). The second step is ball milling: Pour the mixed abrasive into the mixing tank, add a certain amount of steel balls, and make sure the total volume does not exceed 1 / 2 of the tank. Then, use a vertical three-dimensional mixer to stir for 1 hour.

[0054] The third step is screening: the ball-milled abrasive is screened through 230# and 400# metal woven screens to separate the diamond-silicon carbide composite abrasive.

[0055] The fourth step is cleaning: the sieved diamond-silicon carbide composite abrasive is ultrasonically cleaned and dried to obtain diamond-silicon carbide composite abrasive with a roundness of 0.8.

[0056] The preparation method of the abrasive pad in this embodiment is the same as that of the abrasive pad in Example 1.

[0057] Example 7 This embodiment uses a polishing pad for CVD diamond coarse polishing, such as... Figure 1 and Figure 2As shown, the device includes a substrate 02 and abrasive blocks 01 disposed on the substrate. The substrate 02 includes, from bottom to top, a backing adhesive layer 05, a substrate layer 04, and an adhesive layer 03, which are formed by impregnating nylon mesh with adhesive and then curing it. The abrasive blocks 01 are squares with a top side length of 10 mm, and the spacing between the abrasive blocks 01 is 1 mm. The four corners of the upper surface of the abrasive blocks 01 have a radius of 0.5 mm. The abrasive blocks 01 are made of the following raw materials in the following mass percentages: 20% diamond-silicon carbide composite abrasive, 60% bisphenol A type epoxy resin binder, 5% glass fiber, and 15% filler. The diameter of the glass fiber used is 5 μm. The filler is sodium silicate with a D50 particle size of 2 μm. The diamond-silicon carbide composite abrasive has a D50 particle size of 60 μm and a roundness of 0.80, and is prepared by a method including the following steps: Step 1: Mixing: Mix diamond-silicon carbide composite abrasive with diamond powder of D50≈20 and D50≈100, wherein the ratio of the three is 1:1:2 (composite abrasive: diamond powder D50≈20um: diamond powder D50≈100um). The second step is ball milling: Pour the mixed abrasive into the mixing tank, add a certain amount of steel balls, and make sure the total volume does not exceed 1 / 2 of the tank. Then, use a vertical three-dimensional mixer to stir for 1 hour.

[0058] The third step is screening: the ball-milled abrasive is screened through 230# and 400# metal woven screens to separate the diamond-silicon carbide composite abrasive.

[0059] The fourth step is cleaning: the sieved diamond-silicon carbide composite abrasive is ultrasonically cleaned and dried to obtain diamond-silicon carbide composite abrasive with a roundness of 0.8.

[0060] The preparation method of the abrasive pad in this embodiment is the same as that of the abrasive pad in Example 1.

[0061] Example 8 This embodiment uses a polishing pad for CVD diamond coarse polishing, such as... Figure 1 and Figure 2As shown, the device includes a substrate 02 and grinding blocks 01 disposed on the substrate. The substrate 02 includes, from bottom to top, a backing adhesive layer 05, a substrate layer 04, and an adhesive layer 03, which are formed by impregnating nylon mesh with adhesive and then curing it. The grinding blocks 01 are squares with a top side length of 10 mm, and the spacing between the grinding blocks 01 is 1 mm. The four corners of the upper surface of the grinding blocks 01 have a radius of 0.5 mm. The grinding blocks 01 are made of the following raw materials in the following mass percentages: 10% diamond-silicon carbide composite abrasive, 50% bisphenol S type epoxy resin binder, 10% glass fiber, and 30% filler. The diameter of the glass fiber used is 10 μm. The filler is calcium silicate with a D50 particle size of 5 μm. The diamond-silicon carbide composite abrasive has a D50 particle size of 50 μm and a roundness of 0.80, and is prepared by a method including the following steps: Step 1: Mixing: Mix diamond-silicon carbide composite abrasive with diamond powder of D50≈20 and D50≈100, wherein the ratio of the three is 1:1:2 (composite abrasive: diamond powder D50≈20um: diamond powder D50≈100um). The second step is ball milling: Pour the mixed abrasive into the mixing tank, add a certain amount of steel balls, and make sure the total volume does not exceed 1 / 2 of the tank. Then, use a vertical three-dimensional mixer to stir for 1 hour.

[0062] The third step is screening: the ball-milled abrasive is screened through 230# and 400# metal woven screens to separate the diamond-silicon carbide composite abrasive.

[0063] The fourth step is cleaning: the sieved diamond-silicon carbide composite abrasive is ultrasonically cleaned and dried to obtain diamond-silicon carbide composite abrasive with a roundness of 0.8.

[0064] The preparation method of the abrasive pad in this embodiment is the same as that of the abrasive pad in Example 1.

[0065] Comparative Example 1 The difference between the grinding pad used in this comparative example for CVD diamond coarse polishing and the grinding pad in Example 1 is that the diamond-silicon carbide composite abrasive in the grinding block 01 raw material of this comparative example was not shaped, and the roundness was about 0.7. All other aspects are the same as in Example 1. The single-crystal diamond abrasive used also has a Raman value of 3.0 or higher.

[0066] Comparative Example 2 The difference between the grinding pad used in this comparative example for CVD diamond coarse polishing and the grinding pad in Example 1 is that the diamond-silicon carbide composite abrasive in the grinding block 01 material of Example 1 is replaced with single-crystal diamond abrasive with D50≈50μm. All other aspects are the same as in Example 1. The single-crystal diamond abrasive used also has a Raman value of 3.0 or higher.

[0067] Comparative Example 3 The difference between the grinding pad used in this comparative example for CVD diamond coarse polishing and the grinding pad in Example 1 is that the grinding pad used in this comparative example is diamond-silicon carbide composite abrasive single crystal diamond abrasive with a transposition Raman value of less than 2.0 prepared from the raw material of grinding block 01 in Example 1. All other contents are the same as in Example 1.

[0068] Comparative Example 4 The difference between the grinding pad used in this comparative example for CVD diamond rough polishing and the grinding pad in Example 1 is that the ratio of each type of abrasive in the first step of the diamond-silicon carbide composite abrasive ball milling shaping method in Example 1 is adjusted to 1:1:6. All other contents are the same as in Example 1.

[0069] Comparative Example 5 The difference between the grinding pad used in this comparative example for CVD diamond rough polishing and the grinding pad in Example 1 is that the grinding time in the second step of the diamond-silicon carbide composite abrasive ball milling shaping method in Example 1 is set to 6 hours. All other contents are the same as in Example 1.

[0070] Comparative Example 6 The difference between the grinding pad used in this comparative example for CVD diamond rough polishing and the grinding pad in Example 1 is that the chamfer of the grinding block 01 in Example 1 is set to a radius R = 2mm. All other contents are the same as in Example 1.

[0071] Comparative Example 7 The difference between the grinding pad used in this comparative example for CVD diamond coarse polishing and the grinding pad in Example 1 is that the type of binder in the raw material of grinding block 01 in Example 1 is replaced with polyester acrylic resin. All other contents are the same as in Example 1.

[0072] Comparative Example 8 The difference between the abrasive layer of this comparative example and the abrasive pad of Example 1 is that the abrasive blocks 01 of this comparative example are conventionally shaped abrasive pads with a side length of 2-3 mm and a spacing of 1.5-2 mm.

[0073] Experimental Example To evaluate the grinding performance of the grinding pads in each embodiment and comparative example, grinding experiments were conducted on the grinding pads of each embodiment and comparative example. The grinding experiment used a 6B single-sided grinding mill, and the grinding pressure was kept constant at 300 g / cm. 2During grinding, the lower disc rotated at 100 rpm, the guide wheel rotated at 30 Hz, the swing frequency was 8.5 Hz, the cooling medium was water, and the grinding object was polycrystalline CVD diamond that had already undergone three-body grinding on a cast iron disc. The diamond was 2 inches in size and had a roughness Ra of 400 nm or more. During the experiment, each example or comparative example grinding pad ground five batches of polycrystalline CVD diamond, one piece per batch, and the grinding time for each batch was greater than 30 minutes.

[0074] After the experiment, the following parameters were used as evaluation indicators: (1) Roughness: To a certain extent, it represents the polishing effect of the grinding pad. The roughness is taken as the RA value, which can be directly measured by a roughness measuring instrument; the roughness of 5 points is taken for each polycrystalline CVD diamond and the average value is taken.

[0075] (2) Processing time: The processing time here is set to the time required for the roughness of the polycrystalline diamond after grinding to be below 250um.

[0076] (3) Surface damage condition: Grinding damage refers to the surface condition of polycrystalline diamond after grinding. It can reflect the degree of surface damage of the workpiece from a macroscopic perspective. The surface damage is determined by observation with a metallographic microscope. The damage can be divided into three levels: A-excellent, B-good, and C-poor. Among them, level A is a good surface condition, level B has slight abnormal damage on the surface, and level C has serious damage or pits on the surface.

[0077] For each test metric, data was collected from 5 test points and the average value was calculated. The results are shown in the table below: .

[0078] In the high-speed polishing of polycrystalline CVD diamond, the polishing pad needs to simultaneously meet the requirements of cutting force, self-sharpening, and processing quality. The diamond polishing pads prepared in Examples 1-8 meet the polishing rate requirements, have short processing times, and their surface quality meets the A-level evaluation standard. Compared with the diamond polishing pad prepared in Comparative Example 1, it does not show good polishing performance in reducing roughness. The diamonds in the polishing pad are not shaped, have low roundness, poor crystal form, and abnormal damage on the polycrystalline CVD surface. The polishing pad prepared in Comparative Example 2 reduces the overall roughness during the polishing process, but the time required is longer than that of Examples 1-8. This is because the single-crystal diamonds in Comparative Example 2 have higher strength and poorer self-sharpening properties compared to diamond-silicon carbide composite abrasives. Furthermore, the shaping process of the diamond-silicon carbide composite abrasive requires more time, resulting in a smaller overall diamond particle size and thus a longer processing time.

[0079] The polishing pad prepared in Comparative Example 3 could not effectively reduce roughness during the polishing process, and the processing time was long. This was because the diamond used was not strong enough to effectively process the polycrystalline CVD diamond, greatly affecting the polishing effect. In Examples 1-8, the high-grade diamond abrasive selected ensured the polishing efficiency and processing time of the polishing pad. The prepared diamond-silicon carbide composite abrasive, through ball milling shaping, could obtain abrasive with a higher degree of sphericity, improving processing quality. In addition, the special abrasive block structure ensured sufficient contact area between the polycrystalline CVD and the abrasive block during the polishing process, further guaranteeing the quality of the polycrystalline CVD after polishing.

[0080] The ball milling process for the diamond-silicon carbide composite abrasive used in Comparative Example 4 differed from that in Example 1 in that the abrasive mixing ratio was different. The resulting composite abrasive could not achieve a roundness of 0.8-0.85, leading to poor polishing and affecting processing quality. In Comparative Example 5, the ball milling process for preparing the composite abrasive was too long, resulting in smaller overall abrasive particle size, weaker cutting force, and consequently, longer processing time. In Comparative Example 6, the polishing pad had a chamfer radius of 2mm, reducing polishing time. However, compared to Examples 1-8, the surface roughness was slightly higher, the processing time was reduced, and some surface damage was present. This was because the chamfer was too large, reducing the contact area with the CVD substrate during processing, leading to high roughness and damage.

[0081] The excessively long processing time of the polishing pad prepared in Comparative Example 7 is because the adhesive used in this example is polyester acrylic resin, which has lower strength than bisphenol A epoxy resin. During polishing, the particles in the polishing block are prone to collapsing, leading to prolonged processing time. In Comparative Example 8, the polishing pad particles are traditional square-shaped, with no chamfered surfaces, small areas, and large spacing. The polishing performance is not significantly better than that of Examples 1-8 in reducing roughness, and there is significant surface damage.

[0082] In summary, the diamond polishing pads prepared in Examples 1-8 have excellent polishing performance, can effectively and quickly reduce the roughness of CVD diamond, and have less surface damage and good processing effect. At the same time, the raw materials used in the preparation methods of Examples 1-8 are inexpensive and readily available, and are suitable for large-scale industrial production.

[0083] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A polishing pad for CVD diamond rough polishing, characterized by: The grinding pad includes a substrate (02) and several grinding blocks (01) with flat top surfaces disposed on the substrate (02), the top of the grinding blocks (01) being rounded; the ratio of the diameter or side length of the grinding block (01) to the gap distance between adjacent grinding blocks (01) is 10-15:1-1.5; the raw materials for preparing the grinding blocks (01) are: diamond-silicon carbide abrasive, binder, glass fiber and filler; The ratio of the height of the grinding block (01) to the gap distance between adjacent grinding blocks (01) is 2-3:1; the roundness of the diamond-silicon carbide abrasive is 0.80-0.85, and the D50 particle size is 40-60μm; In the preparation of the diamond-silicon carbide abrasive, the Raman value of the diamond raw material is above 3.0; the preparation method of the diamond-silicon carbide abrasive is as follows: diamond-silicon carbide powder is mixed with diamond of different particle sizes and ball-milled, and then sieved to obtain the diamond-silicon carbide abrasive. The diamonds of different particle sizes include diamond powders with particle sizes of 10-30 μm and 90-110 μm; The adhesive comprises an epoxy resin polymer, wherein the epoxy resin polymer is bisphenol A type epoxy resin, bisphenol S type epoxy resin, bisphenol F type epoxy resin, or H type epoxy resin; the glass fiber has a diameter of 5-10 μm; the filler is one or any combination of calcium silicate, magnesium carbonate, sodium silicate, and phosphate; and the D50 particle size of the filler is 2-5 μm.

2. The abrasive pad for CVD diamond rough polishing according to claim 1, wherein: The top surface diameter or side length of the grinding block (01) is 10-15mm, the gap between adjacent grinding blocks (01) is 1-1.5mm, and the radius R of the rounded corner at the top of the grinding block (01) is 0.5-1mm.

3. The abrasive pad for CVD diamond rough polishing according to claim 1, wherein: The raw materials, diamond-silicon carbide abrasive, binder, glass fiber and filler, have mass fractions of 10-20%, 50-60%, 5-10% and 10-35%, respectively, and the total amount of raw materials is 100%.

4. The abrasive pad for CVD diamond rough polishing according to claim 1, wherein: The substrate (02) includes an adhesive layer (03), a substrate layer (04), and a backing adhesive layer (05); the adhesive layer (03) is formed by screen printing and then curing the adhesive; the substrate layer (04) is made of PC board, PET board, or PP board.

5. The method of making an abrasive pad for CVD diamond rough polishing according to any one of claims 1 to 4, wherein, Includes the following steps: 1) Weigh the raw materials diamond-silicon carbide abrasive, binder, glass fiber and filler according to the formula, and mix them to form a slurry; 2) Fill the prepared slurry into each groove of the mold, then apply glue to cover the slurry in the groove, then lay a layer of screen on the glue, then press a substrate with double-sided adhesive on one side onto the screen surface, with the double-sided adhesive layer facing away from the screen, and finally demold after heating and curing.

6. The method of claim 5, wherein: The adhesive comprises epoxy thermosetting resin and inorganic powder; the inorganic powder is any one of calcium silicate, magnesium carbonate, sodium silicate, and phosphate; the mesh is nylon mesh or glass fiber mesh.

Citation Information

Patent Citations

  • Method for detecting grade of diamond micro-powder by utilizing Raman spectroscopy and application of method in detecting grade of diamond micro-powder

    CN112014377A

  • Scouring pad and preparation method thereof

    CN116900960A

  • Grinding pad

    CN118061074A

  • Sheet for polishing pad, method for manufacturing the same, polishing pad, method for manufacturing the same, and polishing method

    JP2013193181A