A large-size graphite electrode for silicon metal smelting and its preparation method
By optimizing the binder and process, and combining it with nanomaterial modification, the problems of poor mixing and dispersion and low interfacial interaction in the preparation of large-size graphite electrodes were solved, thus realizing the preparation of high-performance electrodes to meet the needs of industrial silicon smelting.
Patent Information
- Application Number
- CN202411616112.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-13
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-11-13
AI Technical Summary
In the existing technology, large-size graphite electrodes suffer from poor mixing and dispersion and low interfacial interaction during the preparation process, resulting in poor electrode performance, especially high resistivity and poor mechanical and thermal properties.
High-temperature modified asphalt is used as a binder. By optimizing the kneading process, vertical vibration and horizontal extrusion molding and controlled calcination, graphitization process, and combined with nanomaterial modification treatment, the kneading and carbon residue properties of the binder are improved, thereby enhancing the density and conductivity of the electrode.
High-performance, large-scale graphite electrodes with resistivity below 12 μΩ·m and thermal expansion coefficients between 2.6 and 2.9 × 10⁻⁶ were fabricated to ensure safe use of the electrodes in industrial silicon furnaces and to prevent breakage.
Abstract
Description
Technical Field
[0001] This invention relates to the field of graphite electrode technology, specifically a large-size graphite electrode for metal silicon smelting and its preparation method. Background Technology
[0002] In recent years, with the development of the solar energy and photovoltaic industries, the demand and application of silicon-based raw materials such as monocrystalline silicon and polycrystalline silicon have been increasing daily, greatly promoting the development of silicon-based raw materials in production and other aspects. Currently, in the smelting of metallic silicon, the limitation of electrode specifications on the capacity of electric furnaces restricts its rapid development; therefore, based on meeting the diameter requirements and application performance of graphite electrodes for large industrial silicon smelting furnaces, it is urgent to increase the capacity of industrial silicon furnaces, increase the radius of silicon furnace electrode crucibles, and manufacture large-size electrodes for use in large industrial silicon furnaces.
[0003] In existing technologies, graphite electrodes are typically obtained by kneading graphite fragments, graphite tar, and binders, followed by calcination and graphitization. Due to the large size of large-scale graphite electrodes and the large amount of raw materials involved, problems such as poor kneading dispersion and low interfacial interaction exist, leading to substandard performance of the graphitized electrodes. The binder is one of the key factors in this problem; generally, the binder needs to have good kneading fluidity, high interfacial interaction, and high residual carbon content. A common binder is pitch; however, current high-temperature pitch has defects such as poor binder properties and high volatile content, resulting in high air permeability in the prepared large-scale graphite electrodes, leading to high resistivity and poor mechanical and thermal properties.
[0004] In summary, solving the above problems and preparing a large-scale graphite electrode specifically for silicon metal smelting is of great significance. Summary of the Invention
[0005] The purpose of this invention is to provide a large-size graphite electrode for metal silicon smelting and its preparation method, so as to solve the problems mentioned in the background art.
[0006] To solve the above-mentioned technical problems, the present invention provides the following technical solution:
[0007] A method for preparing a large-size graphite electrode specifically for silicon metal smelting includes the following steps:
[0008] Step 1: Dry mix calcined petroleum coke and electrode graphite powder evenly, add high-temperature modified asphalt, heat to 140-150℃ and knead for 15-30 minutes, heat to 160-170℃ and knead for 10-20 minutes to obtain a paste.
[0009] Step 2: Cool the paste to 130-140℃ and use a vertical vibration extrusion process with a vertical pressure of 17-22 kg / cm². 2The electrode is first pressed and then vibrated, cooled in a cold water tank for 6-8 hours, and then left to stand in the water for 48 hours to obtain the electrode.
[0010] Step 3: The electrode is subjected to calcination and graphitization to obtain a large-size graphite electrode.
[0011] In a more optimized manner, during the calcination process, a heating curve of 1100–1250 hours is set to heat to 880–900°C, calcination is carried out for 200–300 hours, and the product is naturally cooled and removed from the furnace to obtain the calcined product; during the graphitization process, a heating rate of 10–15°C / min is set to heat to 2400–2800°C, power is supplied for 50–80 hours, power is cut off, and the product is cooled to obtain a large-size graphite electrode.
[0012] In a more optimized manner, the raw materials of the paste include the following components: by weight fraction, 75-80 parts calcined petroleum coke, 20-25 parts electrode graphite fragments, and 20-30 parts high-temperature modified pitch;
[0013] The calcined petroleum coke comprises materials with the following particle sizes: 40-50 parts of calcined petroleum coke A with a particle size of 1-10 mm, and 30-35 parts of calcined petroleum coke B with a particle size of 0.1-0.15 mm; the electrode graphite fragments comprise materials with the following particle sizes: 9-12 parts of electrode graphite fragments A with a particle size of 0.1-4 mm, 5-7 parts of electrode graphite fragments B with a particle size of 4-8 mm, and 4-6 parts of electrode graphite fragments C with a particle size of 8-15 mm.
[0014] A more optimized method for preparing the high-temperature modified asphalt is as follows:
[0015] Step 1: (1) Add nanomaterials and epoxy macromolecular silane coupling agent to anhydrous toluene, and add triethylamine dropwise; reflux at 110-115℃ for 2-3 hours under nitrogen atmosphere; wash and dry to obtain modified nanomaterials; (2) Add modified nanomaterials to 0.1-0.12 mol / L sulfuric acid solution, heat to 50-55℃ and stir for 6-8 hours, filter and wash to obtain pre-activated nanomaterials; (3) Disperse pre-activated nanomaterials in deionized water, add 0.1-0.12 mol / L sodium periodate solution, stir at room temperature for 4-6 hours; wash and dry to obtain aldehyde-based nanomaterials;
[0016] Step 2: Mix high-temperature asphalt, anthracene oil, trioxymethylene, aldehyde-modified nanomaterials, and p-toluenesulfonic acid evenly; under a nitrogen atmosphere, heat to 140-160℃ and stir for 18-24 hours, then stop heating to obtain high-temperature modified asphalt.
[0017] In a more optimized manner, the nanomaterials include graphene, carbon nanotubes, and molybdenum disilicide in a mass ratio of 0.5–0.6:0.2–0.3:0.1.
[0018] In a more optimized manner, the raw materials for the high-temperature modified asphalt include the following components: by mass parts, 55 parts high-temperature asphalt, 15-20 parts anthracene oil, 5-8 parts paraformaldehyde, 12-15 parts aldehyde-modified nanomaterials, and 10-12 parts p-toluenesulfonic acid.
[0019] In a more optimized manner, the ratio of nanomaterials, epoxy macromolecular silane coupling agent, and triethylamine in the raw materials of the modified nanomaterials is 1g:6-8mL:0.15-0.18mL; the ratio of modified nanomaterials and sulfuric acid solution in the raw materials of the pre-activated nanomaterials is 1g:18-20mL; and the ratio of pre-activated nanomaterials, deionized water, and sodium periodate solution in the raw materials of the aldehyde-modified nanomaterials is 1g:18-20mL:4-4.5mL.
[0020] A more optimized method for preparing the epoxy-based macromolecular silane coupling agent is as follows:
[0021] S1-1: Sodium sand, 1,2-dimethyl-1,1,2,2-tetrachlorodisilane, and diethylene glycol dimethyl ether were added sequentially to tetrahydrofuran. Under a nitrogen atmosphere, the mixture was stirred at room temperature for 5–8 minutes. The temperature was then raised to 40–50 °C. Methylvinyl dichlorosilane, methylphenyl dichlorosilane, and dibromomethane were added dropwise. After the addition was complete, the reaction was continued for 3–4 hours. Chlorodimethylsilane borate and trimethylchlorosilane were added sequentially, and the mixture was stirred for 0.5–1 hour. The mixture was then filtered, washed, and distilled under reduced pressure to obtain liquid vinyl polycarbosilane.
[0022] S1-2: Liquid vinyl polycarbosilane and formic acid are added to toluene, and concentrated sulfuric acid is added dropwise; the temperature is raised to 30-35°C, and hydrogen peroxide is added dropwise; the temperature is raised to 60-70°C and the reaction is carried out for 4-6 hours; the mixture is washed until neutral, and the solvent is evaporated to obtain epoxy polycarbosilane.
[0023] S1-3: Epoxy-based polycarbosilane, aminosilane coupling agent, and ferroceneamine are added to toluene in sequence, heated to 60-65℃ and reacted for 6-8 hours. The solvent is then evaporated to obtain the epoxy-based macromolecular silane coupling agent.
[0024] More preferably, the raw material for the liquid vinyl polycarbosilane includes the following components by mass fraction: 3-4 parts sodium sand, 3-5 parts 1,2-dimethyl-1,1,2,2-tetrachlorodisilane, 14-17 parts methyl vinyl dichlorosilane, 12-15 parts methyl phenyl dichlorosilane, 34-38 parts dibromomethane, 6-8 parts dichlorodimethylsilane borate, 4-6 parts trimethylchlorosilane, 5-10 parts diethylene glycol dimethyl ether, and 125-130 parts tetrahydrofuran;
[0025] The raw materials for the epoxy-based polycarbosilane include the following components: by mass fraction, 10 parts liquid vinyl polycarbosilane, 1.5 to 1.8 parts formic acid, 0.2 to 0.5 parts concentrated sulfuric acid, and 6 to 7 parts hydrogen peroxide; the raw materials for the epoxy-based macromolecular silane coupling agent include 10 parts epoxy-based polycarbosilane, 0.3 to 0.5 parts aminosilane coupling agent, and 0.05 to 0.08 parts ferroceneamine.
[0026] Compared with the prior art, the beneficial effects achieved by the present invention are as follows:
[0027] (1) The scheme uses high-quality calcined petroleum coke and adds a certain proportion of electrode graphite fragments, with high-temperature modified pitch as a binder; optimizes the proportions and uses two-stage kneading to ensure the homogeneity and good plasticity of the kneaded paste; adopts vertical vibration and horizontal extrusion molding process to ensure the density and homogeneity of the electrode; and uses a cold water pool for cooling and water immersion after molding to effectively release the pressure components of the electrode precursor; by controlling the heating curves or rates of the calcination and graphitization processes, and controlling the temperature and time, the uniformity of the graphite electrode product performance during processing is maintained; so that the resistivity of the prepared large-scale electrode is <12μΩ. . m, coefficient of thermal expansion is 2.6~2.9×10 -6 This ensures that the dimensions of the male and female electrodes and the gap between their cross-sections are within a 0.1–0.4 mm thermal expansion gap, guaranteeing a tight and uniform connection between the two electrodes and ensuring safe and unbreakable use of the electrodes in industrial silicon furnaces.
[0028] (2) In this application, high-temperature modified asphalt is obtained by using nanomaterials to modify high-temperature asphalt; it is used as a binder to effectively improve the kneadability of the electrode and increase the residual carbon of the binder; it effectively reduces the air permeability after graphitization; it reduces the resistivity of large-size graphite electrodes and improves their mechanical or thermal properties.
[0029] Due to the dispersibility and agglomeration issues of nanomaterials, the nanomaterials are surface-modified with epoxy-based macromolecular silane coupling agents, and then the epoxy groups are reacted to form aldehyde groups, thus obtaining aldehyde-based nanomaterials which are introduced into high-temperature asphalt. Utilizing the dispersibility of the high-temperature modified asphalt in the electrode substrate, the nanomaterials are effectively and uniformly dispersed in the substrate, improving the performance of the graphite electrode.
[0030] In this process, aldehyde-based nanomaterials are used to crosslink and polymerize high-temperature asphalt. Anthracene oil modification increases the fluidity of the modified asphalt, facilitating mixing and improving interfacial adhesion. The introduced aldehyde-based nanomaterials enhance cohesive strength, suppress volatilization at high temperatures, maximize carbon retention, reduce air reaction yield, and decrease electrode resistivity.
[0031] Firstly, the nanomaterial is composed of graphene, carbon nanotubes, and molybdenum disilicide. These three components act as structure-directing agents, effectively catalyzing the carbonization of high-temperature modified asphalt to form highly conductive and carbon-based electrothermal materials. The addition of graphene effectively promotes graphitization, increases sp2 carbon content, and reduces defects. Carbon nanotubes, with a morphology different from graphene, can increase the carrier concentration after carbonization, improving conductivity; simultaneously, their embedding within the graphite electrode promotes subsequent release of external forces, enhancing mechanical strength. The introduction of molybdenum disilicide, due to the introduction of epoxy-based macromolecular silane coupling agents containing polycarbosilane segments during the modification process, can promote the formation of nano-sized SiC grains, improve density, alleviate pressure on micropores, and enhance mechanical properties; furthermore, its molybdenum ions can improve the thermal and electrical conductivity of the graphite electrode.
[0032] Secondly, the epoxy-based macromolecular silane coupling agent is based on esterified liquid vinyl polycarbosilane, obtained through epoxidation, followed by grafting of aminosilane coupling agents and ferrocene amine onto some epoxy groups. It contains the main chain of liquid vinyl polycarbosilane, which, when introduced into high-temperature asphalt, can improve the asphalt's bonding performance and reduce its volatile matter content. Furthermore, the main chain is a C-Si-C chain with low oxygen content, which can subsequently generate silicon carbide to improve mechanical properties, reduce the thermal expansion coefficient of graphite electrodes, and enhance their stability under temperature changes. In addition, the liquid vinyl polycarbosilane contains boron groups and is grafted with iron-containing segments; the low boron content can increase the number of p-type charge carriers in graphite carbon, improving conductivity; while the iron content, in conjunction with molybdenum disilicide, effectively catalyzes and promotes the growth of graphite microcrystals, increasing graphitization and order, and enhancing conductivity and thermal stability. Detailed Implementation
[0033] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0034] It should be noted that the following proportions are by weight. There are no special restrictions on the manufacturers of the raw materials involved in this invention. Exemplary examples include: Ferroceneamine (CAS number 1273-82-1); high-temperature asphalt (original specification 0-3mm, purchased from Hebei Xiangbei New Material Technology Co., Ltd.); it was pulverized and ground before use, and then passed through a 0.2mm sieve. Calcined petroleum coke A has a specification of 1-10mm; calcined petroleum coke B has a specification of 0.1-0.15mm; electrode graphite fragments A have a specification of 0.1-4mm; electrode graphite fragments B have a specification of 4-8mm; and electrode graphite fragments C have a specification of 8-15mm. The hydrogen peroxide has a mass fraction of 30%. All other raw materials involved are commercially available.
[0035] Unless otherwise specified, the preparation process of the aldehyde-based nanomaterials in the following embodiments is as follows:
[0036] Step 1: (1) Add 3.5g sodium sand, 3.2g 1,2-dimethyl-1,1,2,2-tetrachlorodisilane, and 10g diethylene glycol dimethyl ether to 130g tetrahydrofuran in sequence. Stir at room temperature for 5 minutes under a nitrogen atmosphere. Heat to 50℃. Add 16g methylvinyl dichlorosilane, 13g methylphenyl dichlorosilane, and 36g dibromomethane dropwise. After the addition is complete, continue the reaction for 4 hours. Add 6g dichlorodimethylsilane boronic acid ester and 5g trimethylchlorosilane in sequence, and continue stirring for 1 hour. Filter, wash, and distill under reduced pressure to obtain the desired product. (1) Add 10g of liquid vinyl polycarbosilane and 1.6g of formic acid to toluene, and add 0.32g of concentrated sulfuric acid; heat to 35°C, and add 6.9g of hydrogen peroxide; heat to 65°C and react for 6 hours; wash until neutral, evaporate the solvent, and obtain epoxy polycarbosilane; (2) Add 10g of epoxy polycarbosilane, 0.5g of γ-aminopropyltriethoxysilane and 20.05g of ferrocene to toluene in sequence, heat to 60°C and react for 6 hours, evaporate the solvent, and obtain epoxy macromolecular silane coupling agent;
[0037] Step 2: (1) Graphene, carbon nanotubes and molybdenum disilicide in a mass ratio of 0.6:0.3:0.1 are mixed evenly to obtain nanomaterials; (2) 1g of nanomaterials and 8mL of epoxy macromolecular silane coupling agent are added to 10mL of anhydrous toluene, and 0.16mL of triethylamine is added dropwise; under a nitrogen atmosphere, the mixture is refluxed at 110℃ for 3 hours; washed and dried to obtain modified nanomaterials; (3) 1g of modified nanomaterials is added to 20mL of 0.1mol / L sulfuric acid solution, heated to 50℃ and stirred for 8 hours, filtered and washed to obtain pre-activated nanomaterials; (4) 1g of pre-activated nanomaterials is dispersed in 20mL of deionized water, and 4.5mL of 0.1mol / L sodium periodate solution is added, and stirred at room temperature for 5 hours; washed and dried to obtain aldehyde-based nanomaterials;
[0038] This process can be scaled up proportionally.
[0039] Example 1: A method for preparing a large-size graphite electrode for silicon metal smelting, comprising the following steps:
[0040] Pre-preparation: Mix 55 parts of high-temperature asphalt, 16 parts of anthracene oil, 5 parts of paraformaldehyde, 14 parts of aldehyde-modified nanomaterials, and 10 parts of p-toluenesulfonic acid evenly; under a nitrogen atmosphere, heat to 150℃ and stir for 20 hours, then stop heating to obtain high-temperature modified asphalt.
[0041] Step 1: Dry mix 78 parts of calcined petroleum coke (45 parts of calcined petroleum coke A and 33 parts of calcined petroleum coke B) and 22 parts of electrode graphite fragments (10 parts of electrode graphite fragments A, 7 parts of electrode graphite fragments B and 5 parts of electrode graphite fragments C) evenly, add 26 parts of high-temperature modified asphalt, heat to 150℃ and knead for 30 minutes, heat to 170℃ and knead for 15 minutes to obtain a paste;
[0042] Step 2: Cool the paste to 140℃ and use a vertical vibration extrusion process with a vertical pressure of 20 kg / cm². 2 The electrode was first pressed and then vibrated, cooled in a cold water tank for 6 hours, and then left to stand in the water for 48 hours to obtain the electrode.
[0043] Step 3: The electrode is first subjected to calcination treatment. During the process, a 1250-hour heating curve is set to heat to 900℃, calcination is carried out for 250 hours, and the product is cooled naturally to obtain the calcined product. Then, it is subjected to graphitization treatment. During the process, a heating rate of 10℃ / min is set to heat to 2600℃, power is supplied for 60 hours, power is turned off, and the product is cooled to obtain a large-size graphite electrode.
[0044] Example 2: A method for preparing a large-size graphite electrode for silicon metal smelting, comprising the following steps:
[0045] Pre-preparation: Mix 55 parts of high-temperature asphalt, 20 parts of anthracene oil, 8 parts of paraformaldehyde, 15 parts of aldehyde-modified nanomaterials, and 12 parts of p-toluenesulfonic acid evenly; under a nitrogen atmosphere, heat to 150℃ and stir for 20 hours, then stop heating to obtain high-temperature modified asphalt.
[0046] Step 1: Dry mix 80 parts of calcined petroleum coke (50 parts of calcined petroleum coke A and 30 parts of calcined petroleum coke B) and 20 parts of electrode graphite fragments (9 parts of electrode graphite fragments A, 7 parts of electrode graphite fragments B and 4 parts of electrode graphite fragments C) evenly, add 30 parts of high-temperature modified asphalt, heat to 150℃ and knead for 30 minutes, then heat to 170℃ and knead for 15 minutes to obtain a paste.
[0047] Step 2: Cool the paste to 140℃ and use a vertical vibration extrusion process with a vertical pressure of 20 kg / cm². 2The electrode was first pressed and then vibrated, cooled in a cold water tank for 6 hours, and then left to stand in the water for 48 hours to obtain the electrode.
[0048] Step 3: The electrode is first subjected to calcination treatment. During the process, a 1200-hour heating curve is set to heat to 880℃, calcination is carried out for 250 hours, and the product is cooled naturally to obtain the calcined product. Then, it is subjected to graphitization treatment. During the process, a heating rate of 10℃ / min is set to heat to 2600℃, power is supplied for 60 hours, power is turned off, and the product is cooled to obtain a large-size graphite electrode.
[0049] Example 3: A method for preparing a large-size graphite electrode for silicon metal smelting, comprising the following steps:
[0050] Pre-preparation: Mix 55 parts high-temperature asphalt, 15 parts anthracene oil, 5 parts paraformaldehyde, 12 parts aldehyde-modified nanomaterials, and 10 parts p-toluenesulfonic acid evenly; under a nitrogen atmosphere, heat to 150℃ and stir for 20 hours, then stop heating to obtain high-temperature modified asphalt.
[0051] Step 1: Dry mix 75 parts of calcined petroleum coke (40 parts of calcined petroleum coke A and 35 parts of calcined petroleum coke B) and 25 parts of electrode graphite fragments (12 parts of electrode graphite fragments A, 7 parts of electrode graphite fragments B and 6 parts of electrode graphite fragments C) evenly, add 20 parts of high-temperature modified asphalt, heat to 150℃ and knead for 30 minutes, heat to 170℃ and knead for 15 minutes to obtain a paste;
[0052] Step 2: Cool the paste to 140℃ and use a vertical vibration extrusion process with a vertical pressure of 20 kg / cm². 2 The electrode was first pressed and then vibrated, cooled in a cold water tank for 6 hours, and then left to stand in the water for 48 hours to obtain the electrode.
[0053] Step 3: The electrode is first subjected to calcination treatment. During the process, a 1200-hour heating curve is set to heat to 900℃, calcination is carried out for 250 hours, and the product is cooled naturally to obtain the calcined product. Then, it is subjected to graphitization treatment. During the process, a heating rate of 10℃ / min is set to heat to 2600℃, power is supplied for 60 hours, power is turned off, and the product is cooled to obtain a large-size graphite electrode.
[0054] Comparative Example 1: Based on Example 1, high-temperature asphalt (Hebei Xiangbei) was replaced with high-temperature modified asphalt, and the rest was the same as in Example 1; the details are as follows:
[0055] Step 1: Dry mix 78 parts of calcined petroleum coke (45 parts of calcined petroleum coke A and 33 parts of calcined petroleum coke B) and 22 parts of electrode graphite fragments (10 parts of electrode graphite fragments A, 7 parts of electrode graphite fragments B and 5 parts of electrode graphite fragments C) evenly, add 26 parts of high-temperature asphalt, heat to 150℃ and knead for 30 minutes, heat to 170℃ and knead for 15 minutes to obtain a paste;
[0056] Step 2: Cool the paste to 140℃ and use a vertical vibration extrusion process with a vertical pressure of 20 kg / cm². 2 The electrode was first pressed and then vibrated, cooled in a cold water tank for 6 hours, and then left to stand in the water for 48 hours to obtain the electrode.
[0057] Step 3: The electrode is first subjected to calcination treatment. During the process, a 1250-hour heating curve is set to heat to 900℃, calcination is carried out for 250 hours, and the product is cooled naturally to obtain the calcined product. Then, it is subjected to graphitization treatment. During the process, a heating rate of 10℃ / min is set to heat to 2600℃, power is supplied for 60 hours, power is turned off, and the product is cooled to obtain a large-size graphite electrode.
[0058] Comparative Example 2: Based on Example 1, nanomaterials were directly introduced into high-temperature modified asphalt, with the rest being the same as in Example 1; details are as follows:
[0059] Pre-preparation: Mix 55 parts high-temperature asphalt, 16 parts anthracene oil, 15 parts paraformaldehyde, 4 parts nanomaterials, and 10 parts p-toluenesulfonic acid evenly; under a nitrogen atmosphere, heat to 150℃ and stir for 20 hours, then stop heating to obtain high-temperature modified asphalt.
[0060] Step 1: Dry mix 78 parts of calcined petroleum coke (45 parts of calcined petroleum coke A and 33 parts of calcined petroleum coke B) and 22 parts of electrode graphite fragments (10 parts of electrode graphite fragments A, 7 parts of electrode graphite fragments B and 5 parts of electrode graphite fragments C) evenly, add 26 parts of high-temperature modified asphalt, heat to 150℃ and knead for 30 minutes, heat to 170℃ and knead for 15 minutes to obtain a paste;
[0061] Step 2: Cool the paste to 140℃ and use a vertical vibration extrusion process with a vertical pressure of 20 kg / cm². 2 The electrode was first pressed and then vibrated, cooled in a cold water tank for 6 hours, and then left to stand in the water for 48 hours to obtain the electrode.
[0062] Step 3: The electrode is first subjected to calcination treatment. During the process, a 1250-hour heating curve is set to heat to 900℃, calcination is carried out for 250 hours, and the product is cooled naturally to obtain the calcined product. Then, it is subjected to graphitization treatment. During the process, a heating rate of 10℃ / min is set to heat to 2600℃, power is supplied for 60 hours, power is turned off, and the product is cooled to obtain a large-size graphite electrode.
[0063] Comparative Example 3: Based on Example 1, the epoxy macromolecular silane coupling agent in the raw materials for preparing aldehyde-based nanomaterials was replaced with γ-glycidyl etheroxypropyltrimethoxysilane, while the rest remained the same as in Example 1; details are as follows:
[0064] Pre-preparation: (1) Graphene, carbon nanotubes and molybdenum disilicide were mixed evenly in a mass ratio of 0.6:0.3:0.1 to obtain nanomaterials; (2) 1g of nanomaterials and 8mL of γ-glycidyl etheroxypropyltrimethoxysilane were added to 10mL of anhydrous toluene, and 0.16mL of triethylamine was added dropwise; under a nitrogen atmosphere, the mixture was refluxed at 110℃ for 3 hours; washed and dried to obtain modified nanomaterials; (3) 1g of modified nanomaterials were added to 20mL of 0.1mol / L sulfuric acid solution, heated to 50℃ and stirred for 8 hours, filtered and washed to obtain pre-activated nanomaterials; (4) 1g of pre-activated nanomaterials were dispersed in 20mL of deionized water, and 4.5mL of 0.1mol / L sodium periodate solution was added, and stirred at room temperature for 5 hours; washed and dried to obtain aldehyde-modified nanomaterials;
[0065] (5) Mix 55 parts of high-temperature asphalt, 16 parts of anthracene oil, 5 parts of trioxymethylene, 14 parts of aldehyde-modified nanomaterials and 10 parts of p-toluenesulfonic acid evenly; under a nitrogen atmosphere, heat to 150°C and stir for 20 hours, then stop heating to obtain high-temperature modified asphalt.
[0066] Step 1: Dry mix 78 parts of calcined petroleum coke (45 parts of calcined petroleum coke A and 33 parts of calcined petroleum coke B) and 22 parts of electrode graphite fragments (10 parts of electrode graphite fragments A, 7 parts of electrode graphite fragments B and 5 parts of electrode graphite fragments C) evenly, add 26 parts of high-temperature modified asphalt, heat to 150℃ and knead for 30 minutes, heat to 170℃ and knead for 15 minutes to obtain a paste;
[0067] Step 2: Cool the paste to 140℃ and use a vertical vibration extrusion process with a vertical pressure of 20 kg / cm². 2 The electrode was first pressed and then vibrated, cooled in a cold water tank for 6 hours, and then left to stand in the water for 48 hours to obtain the electrode.
[0068] Step 3: The electrode is first subjected to calcination treatment. During the process, a 1250-hour heating curve is set to heat to 900℃, calcination is carried out for 250 hours, and the product is cooled naturally to obtain the calcined product. Then, it is subjected to graphitization treatment. During the process, a heating rate of 10℃ / min is set to heat to 2600℃, power is supplied for 60 hours, power is turned off, and the product is cooled to obtain a large-size graphite electrode.
[0069] Comparative Example 4: Based on Example 1, the nanomaterial in the high-temperature modified asphalt was a single type of graphene; the rest was the same as in Example 1; details are as follows:
[0070] Pre-preparation: (1) Graphene, carbon nanotubes and molybdenum disilicide were mixed evenly in a mass ratio of 0.6:0.3:0.1 to obtain nanomaterials; (2) 1g of nanomaterials and 8mL of epoxy macromolecular silane coupling agent were added to 10mL of anhydrous toluene, and 0.16mL of triethylamine was added dropwise; under a nitrogen atmosphere, the mixture was refluxed at 110℃ for 3 hours; washed and dried to obtain modified nanomaterials; (3) 1g of modified nanomaterials were added to 20mL of 0.1mol / L sulfuric acid solution, heated to 50℃ and stirred for 8 hours, filtered and washed to obtain pre-activated nanomaterials; (4) 1g of pre-activated nanomaterials were dispersed in 20mL of deionized water, and 4.5mL of 0.1mol / L sodium periodate solution was added, and stirred at room temperature for 5 hours; washed and dried to obtain aldehyde-based nanomaterials;
[0071] (5) Mix 55 parts of high-temperature asphalt, 16 parts of anthracene oil, 5 parts of trioxymethylene, 14 parts of aldehyde-modified nanomaterials and 10 parts of p-toluenesulfonic acid evenly; under a nitrogen atmosphere, heat to 150°C and stir for 20 hours, then stop heating to obtain high-temperature modified asphalt.
[0072] Step 1: Dry mix 78 parts of calcined petroleum coke (45 parts of calcined petroleum coke A and 33 parts of calcined petroleum coke B) and 22 parts of electrode graphite fragments (10 parts of electrode graphite fragments A, 7 parts of electrode graphite fragments B and 5 parts of electrode graphite fragments C) evenly, add 26 parts of high-temperature modified asphalt, heat to 150℃ and knead for 30 minutes, heat to 170℃ and knead for 15 minutes to obtain a paste;
[0073] Step 2: Cool the paste to 140℃ and use a vertical vibration extrusion process with a vertical pressure of 20 kg / cm². 2 The electrode was first pressed and then vibrated, cooled in a cold water tank for 6 hours, and then left to stand in the water for 48 hours to obtain the electrode.
[0074] Step 3: The electrode is first subjected to calcination treatment. During the process, a 1250-hour heating curve is set to heat to 900℃, calcination is carried out for 250 hours, and the product is cooled naturally to obtain the calcined product. Then, it is subjected to graphitization treatment. During the process, a heating rate of 10℃ / min is set to heat to 2600℃, power is supplied for 60 hours, power is turned off, and the product is cooled to obtain a large-size graphite electrode.
[0075] Performance testing: The large-scale graphite electrodes (900×900×2200mm) prepared in the examples and comparative examples were subjected to relevant performance tests; the specific results are as follows:
[0076] sample <![CDATA[Resistivity μΩ . m]]> Flexural strength (MPa) <![CDATA[Bulk density g / cm 2 > <![CDATA[Coefficient of thermal expansion ×10 -6 / °C]]> Example 1 8.7 12.8 1.78 2.61 Comparative Example 1 11.2 10.7 1.58 2.95 Comparative Example 2 10.2 11.5 1.64 2.88 Comparative Example 3 9.9 11.8 1.68 2.80 Comparative Example 4 9.3 12.1 1.70 2.73
[0077] Conclusion: The data in the table above shows that this application prepared a large-size graphite electrode with low resistivity, high strength, and high thermal performance; it effectively ensures tight and uniform communication between the two electrodes, achieving safety when used in industrial silicon furnaces. Comparing the data from Comparative Examples 1-4 with Example 1, it can be seen that in Comparative Example 1, the direct use of high-temperature asphalt resulted in a significant decrease in relevant performance. In Comparative Example 2, the direct introduction of nanomaterials without the introduction of polycarbosilane segments during the modification process reduced the residual carbon rate and graphitization furnace, leading to a decrease in performance. In Comparative Example 3, the use of small-molecule γ-glycidyl etheroxypropyltrimethoxysilane reduced cohesive viscosity, density, and residual carbon rate, resulting in a decrease in relevant performance. In Comparative Example 4, the use of only graphene as the nanomaterial reduced the sintering aid properties and slightly decreased conductivity.
[0078] Finally, it should be noted that the above descriptions are merely preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for preparing a large-size graphite electrode for silicon metal smelting, characterized in that: Includes the following steps: Step 1: Dry mix calcined petroleum coke and electrode graphite powder evenly, add high-temperature modified asphalt, heat to 140~150℃ and knead for 15~30 minutes, heat to 160~170℃ and knead for 10~20 minutes to obtain a paste. Step 2: Cool the paste to 130~140℃ and use a vertical vibration extrusion process with a vertical pressure of 17~22 kg / cm². 2 The electrode precursor is obtained by first pressing and then vibrating, cooling in a cold water tank for 6-8 hours, and then letting it stand in the water for 48 hours. Step 3: The electrode precursor is calcined and graphitized to obtain a large-size graphite electrode. The preparation method of the high-temperature modified asphalt is as follows: Step 1: (1) Add nanomaterials and epoxy macromolecular silane coupling agent to anhydrous toluene, and add triethylamine dropwise; under nitrogen atmosphere, reflux at 110~115℃ for 2~3 hours; wash and dry to obtain modified nanomaterials; (2) Add modified nanomaterials to 0.1~0.12mol / L sulfuric acid solution, heat to 50~55℃ and stir for 6~8 hours, filter and wash to obtain pre-activated nanomaterials; (3) Disperse pre-activated nanomaterials in deionized water, add 0.1~0.12mol / L sodium periodate solution, stir at room temperature for 4~6 hours; wash and dry to obtain aldehyde-based nanomaterials; Step 2: Mix high-temperature asphalt, anthracene oil, paraformaldehyde, aldehyde-modified nanomaterials, and p-toluenesulfonic acid evenly; under a nitrogen atmosphere, heat to 140~160℃ and stir for 18~24 hours, then stop heating to obtain high-temperature modified asphalt; The nanomaterials include graphene, carbon nanotubes, and molybdenum disilicide in a mass ratio of 0.5~0.6:0.2~0.3:0.
1.
2. The method for preparing a large-size graphite electrode for silicon metal smelting according to claim 1, characterized in that: During the calcination process, a heating curve of 1100~1250 hours is set to heat to 880~900℃, calcination is carried out for 200~300 hours, and the product is naturally cooled and removed from the furnace to obtain the calcined product; during the graphitization process, a heating rate of 10~15℃ / min is set to heat to 2400~2800℃, power is supplied for 50~80 hours, power is turned off and the product is cooled to obtain a large-size graphite electrode.
3. The method for preparing a large-size graphite electrode for silicon metal smelting according to claim 1, characterized in that: The raw materials of the paste include the following components: by weight fraction, 75-80 parts calcined petroleum coke, 20-25 parts electrode graphite fragments, and 20-30 parts high-temperature modified pitch; The calcined petroleum coke comprises materials with the following particle sizes: 40-50 parts of calcined petroleum coke A with a particle size of 1-10 mm, and 30-35 parts of calcined petroleum coke B with a particle size of 0.1-0.15 mm; the electrode graphite fragments comprise materials with the following particle sizes: 9-12 parts of electrode graphite fragments A with a particle size of 0.1-4 mm, 5-7 parts of electrode graphite fragments B with a particle size of 4-8 mm, and 4-6 parts of electrode graphite fragments C with a particle size of 8-15 mm.
4. The method for preparing a large-size graphite electrode for silicon metal smelting according to claim 1, characterized in that: The raw materials for the high-temperature modified asphalt include the following components: by mass, 55 parts high-temperature asphalt, 15-20 parts anthracene oil, 5-8 parts paraformaldehyde, 12-15 parts aldehyde-modified nanomaterials, and 10-12 parts p-toluenesulfonic acid.
5. The method for preparing a large-size graphite electrode for silicon metal smelting according to claim 1, characterized in that: In the raw materials of the modified nanomaterial, the ratio of nanomaterial, epoxy macromolecular silane coupling agent, and triethylamine is 1g:6~8mL:0.15~0.18mL; in the raw materials of the pre-activated nanomaterial, the ratio of modified nanomaterial and sulfuric acid solution is 1g:18~20mL; in the raw materials of the aldehyde-modified nanomaterial, the ratio of pre-activated nanomaterial, deionized water, and sodium periodate solution is 1g:18~20mL:4~4.5mL.
6. The method for preparing a large-size graphite electrode for silicon metal smelting according to claim 1, characterized in that: The preparation method of the epoxy-based macromolecular silane coupling agent is as follows: S1-1: Sodium sand, 1,2-dimethyl-1,1,2,2-tetrachlorodisilane, and diethylene glycol dimethyl ether are added sequentially to tetrahydrofuran. Under a nitrogen atmosphere, the mixture is stirred at room temperature for 5-8 minutes. The temperature is then raised to 40-50°C. Methylvinyl dichlorosilane, methylphenyl dichlorosilane, and dibromomethane are added dropwise. After the addition is complete, the reaction continues for 3-4 hours. Chlorodimethylsilane borate and trimethylchlorosilane are added sequentially, and the mixture is stirred for 0.5-1 hour. The mixture is then filtered, washed, and distilled under reduced pressure to obtain liquid vinyl polycarbosilane. S1-2: Add liquid vinyl polycarbosilane and formic acid to toluene, and add concentrated sulfuric acid dropwise; heat to 30~35℃ and add hydrogen peroxide dropwise; heat to 60~70℃ and react for 4~6 hours; wash until neutral, evaporate the solvent, and obtain epoxy polycarbosilane; S1-3: Epoxy-based polycarbosilane, aminosilane coupling agent, and ferroceneamine are added to toluene in sequence, heated to 60-65℃ and reacted for 6-8 hours. The solvent is then evaporated to obtain the epoxy-based macromolecular silane coupling agent.
7. The method for preparing a large-size graphite electrode for silicon metal smelting according to claim 6, characterized in that: The raw materials for the liquid vinyl polycarbosilane include the following components by mass fraction: 3-4 parts sodium sand, 3-5 parts 1,2-dimethyl-1,1,2,2-tetrachlorodisilane, 14-17 parts methyl vinyl dichlorosilane, 12-15 parts methyl phenyl dichlorosilane, 34-38 parts dibromomethane, 6-8 parts dichlorodimethylsilane borate, 4-6 parts trimethylchlorosilane, 5-10 parts diethylene glycol dimethyl ether, and 125-130 parts tetrahydrofuran; The raw materials for the epoxy-based polycarbosilane include the following components: by mass fraction, 10 parts liquid vinyl polycarbosilane, 1.5-1.8 parts formic acid, 0.2-0.5 parts concentrated sulfuric acid, and 6-7 parts hydrogen peroxide; the raw materials for the epoxy-based macromolecular silane coupling agent include 10 parts epoxy-based polycarbosilane, 0.3-0.5 parts aminosilane coupling agent, and 0.05-0.08 parts ferroceneamine.
8. The large-size graphite electrode prepared by the method for preparing a large-size graphite electrode for metal silicon smelting according to claim 1.
Citation Information
Patent Citations
Method for preparing graphite crucible with recycled graphite
CN105272287A
Extra-large-specification graphite electrode with diameter of 1320mm and preparation method thereof
CN111517792A