Metal pipes for oil wells

By forming a resin coating with a specific composition on the contact surface of the metal pipe for oil wells, the problem of relaxation caused by torsion in horizontal excavation is solved, and the yield torque and wear resistance are improved, making it suitable for metal pipes for oil wells in horizontal excavation.

CN119585558BActive Publication Date: 2026-11-17NIPPON STEEL CORPORATION +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202380054159.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-07-20
Filing Date
2023-07-14
Publication Date
2026-11-17
Estimated Expiration
2043-07-14

AI Technical Summary

Technical Problem

When drilling oil wells horizontally, the metal tubing used in the well is prone to loosening due to torsion. Existing technology cannot provide metal tubing that can be tightened under high torque, resulting in insufficient wear resistance.

Method used

A resin coating is formed on the contact surfaces of the male and female threads of the metal pipe used in oil wells. The resin coating is composed of a specific ratio of base resin, nylon, TiO2, hydrated magnesium silicate, wax, fluorine additives and graphite, which improves shear strength to enhance fastening ability.

Benefits of technology

It improves the yield torque of metal pipes used in oil wells, enhances the fastening ability under horizontal digging conditions, reduces loosening, and extends service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119585558B_ABST
    Figure CN119585558B_ABST
Patent Text Reader

Abstract

The resin coating of the oil well metal pipe disclosed herein has excellent shear strength. The oil well metal pipe disclosed herein has a resin coating (100) formed as the uppermost layer of at least one of the male thread contact surface (400) and the female thread contact surface (500). The resin coating (100) contains: a base resin totaling 40.0 to 99.4% by mass, nylon 0.1 to 20.0% by mass, TiO2 0.5 to 30.0% by mass, hydrated magnesium silicate 0 to 49.4% by mass, wax 0 to 10.0% by mass, fluorine additives 0 to 30.0% by mass, graphite 0 to 10.0% by mass, anti-rust pigment 0 to 30.0% by mass, coloring pigment 0 to 10.0% by mass, and coupling agent 0 to 10.0% by mass. The total content of wax, fluorine additives and graphite in the resin coating (100) is less than 5.00 relative to the total content of TiO2, hydrated magnesium silicate and nylon.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to a metal pipe, and more specifically to a metal pipe for oil wells. Background Technology

[0002] Oil well metal tubing is used in oil wells and gas wells (hereinafter collectively referred to as "oil wells" or "gas wells"). Oil well metal tubing has threaded fittings (male or female). At the oil well production site, multiple oil well metal tubing are connected according to the depth of the oil well to form an oil well tubing connection. An oil well tubing connection may include, for example, casing and tubing. An oil well tubing connection is formed by threading the oil well metal tubing together. Furthermore, there are situations where the oil well tubing connection is inspected. In the case of inspection, the oil well tubing connection is pulled up and the threads are loosened. The oil well metal tubing is then removed from the oil well tubing connection by loosening the threads for inspection. After inspection, the oil well metal tubing is re-threaded and reused as part of the oil well tubing connection.

[0003] The metal pipe for oil wells has a male thread and a female thread. The male thread has a male thread contact surface, including an external thread, on the outer circumferential surface of the end of the metal pipe. The female thread has a female thread contact surface, including an internal thread, on the inner circumferential surface of the end of the metal pipe. In this specification, the external thread and the internal thread are collectively referred to as the "threaded portion". It should be noted that the male thread contact surface may also include a non-threaded metal contact portion, which includes a male thread sealing surface and a male thread shoulder surface. Similarly, the female thread contact surface may also include a non-threaded metal contact portion, which includes a female thread sealing surface and a female thread shoulder surface.

[0004] The male and female threaded contact surfaces of metal pipes used in oil wells are repeatedly subjected to strong friction during thread tightening and loosening. Therefore, repeated tightening and loosening can easily lead to seizing (irreparable wear) on these surfaces. Consequently, metal pipes used in oil wells require sufficient durability against friction, i.e., excellent wear resistance.

[0005] Previously, composite greases containing heavy metal powders, known as dopants, were used to improve the wear resistance of metal pipes used in oil wells. Applying composite grease to the contact surfaces of the male and / or female threads can improve the wear resistance of these pipes. However, there is a possibility that the heavy metal powders such as Pb, Zn, and Cu contained in the composite grease may have environmental impacts. Therefore, it is desirable to develop a type of metal pipe for oil wells that exhibits excellent wear resistance even without the use of composite grease.

[0006] Techniques for improving the wear resistance of metal pipes used in oil wells have been proposed, for example, in Japanese Patent Application Publication No. 2003-021278 (Patent Document 1) and International Publication No. 2006 / 104251 (Patent Document 2).

[0007] Patent Document 1 discloses a metal pipe for oil wells with a threaded joint, comprising a male thread and a female thread, each having a contact surface including a threaded portion and a non-threaded metal contact portion. Furthermore, at least one of the male and female thread surfaces has a solid lubricant coating composed of a solid lubricant and a binder. In the thickness direction section of the solid lubricant coating, the area fraction of secondary particles of the solid lubricant with an equivalent diameter of 15–60 μm is 5–90%. Patent Document 1 discloses that, according to this metal pipe for oil wells, wear resistance and airtightness can be stably ensured without applying a composite grease.

[0008] Patent Document 2 discloses a metal pipe for oil wells with a threaded joint, consisting of a male thread and a female thread, each having a threaded portion and a non-threaded metal contact surface respectively. Furthermore, the contact surface of at least one of the male and female thread components has a viscous liquid or semi-solid lubricating film and a dry solid film formed thereon. Patent Document 2 discloses that, according to this metal pipe for oil wells, rust is suppressed without the use of composite grease, and it exhibits excellent wear resistance and airtightness.

[0009] Existing technical documents

[0010] Patent documents

[0011] Patent Document 1: Japanese Patent Application Publication No. 2003-021278

[0012] Patent Document 2: International Publication No. 2006 / 104251 Summary of the Invention

[0013] The problem the invention aims to solve

[0014] However, in oil and gas extraction, vertical drilling (excavating vertically) and inclined drilling (excavating at an angle relative to the vertical direction) are commonly used. On the other hand, one method of oil and gas extraction is horizontal drilling. Horizontal drilling refers to the method of gradually curving the vertically drilled well towards the horizontal, ultimately excavating horizontally along the oil and gas reservoir. Compared to conventional vertical and inclined drilling, horizontal drilling allows for greater contact with the oil and gas reservoir, increasing the oil and gas production per unit of well. In recent years, the use of horizontal drilling in oil and gas extraction has increased. Therefore, there is a demand for metal pipes for oil wells that can be used in well pipe connections designed for horizontal drilling.

[0015] In horizontal excavation, the well tubing bends as the excavation direction changes from vertical to horizontal. During this bend, the well tubing is rotated circumferentially while excavating to reach the target oil and gas reservoir. Therefore, particularly at the bend, the well tubing is subjected to torsion due to both bending and circumferential rotation. Applying torsion under high loads makes the well tubing prone to loosening. In vertical excavation, circumferential torsion is primarily applied to the well tubing. However, in horizontal excavation, in addition to circumferential torsion, torsion due to bending is also applied. Consequently, compared to vertical excavation, horizontal excavation applies excessive torsion to the well tubing, making it more prone to loosening.

[0016] If the oil well tubing can be tightened with a higher torque than before, it will be less likely to loosen at bends in the tubing connector during horizontal excavation. Therefore, for use in horizontal excavation, there is a need for oil well tubing that can be tightened with a higher torque than before.

[0017] The purpose of this disclosure is to provide a resin-coated metal pipe for oil wells with improved shear strength.

[0018] Solution for solving the problem

[0019] The metal pipe for oil wells disclosed herein comprises a pipe body including a first end and a second end.

[0020] The pipe body includes:

[0021] The male fastener is formed at the first end; and

[0022] The female buckle portion is formed at the second end.

[0023] The male thread portion has a male thread contact surface including an external thread portion.

[0024] The female threaded portion has a female threaded portion contact surface.

[0025] The oil well metal pipe also has a resin coating formed as the uppermost layer of at least one of the male thread contact surface and the female thread contact surface.

[0026] The resin coating contains:

[0027] The base resin is selected from one or more of the group consisting of epoxy resin, phenolic resin, acrylic resin, urethane resin, polyester resin, polyamide-imide resin, polyimide resin, and polyetheretherketone resin, with a total content of 40.0 to 99.4% by mass.

[0028] Nylon: 0.1–20.0% by mass

[0029] TiO2: 0.5–30.0% by mass

[0030] Hydrous magnesium silicate: 0–49.4% by mass

[0031] Wax: 0-10.0% by weight

[0032] Fluorine additives: 0–30.0% by weight

[0033] Graphite: 0–10.0% by mass

[0034] Rust-preventive pigments: 0–30.0% by weight

[0035] Coloring pigments: 0–10.0% by mass, and

[0036] Coupling agent: 0–10.0% by mass

[0037] The total content of the wax, the fluorine additives and the graphite in the resin coating, expressed as a percentage by mass, is less than 5.00 relative to the total content of the nylon, the TiO2 and the hydrated magnesium silicate, expressed as a percentage by mass.

[0038] The effects of the invention

[0039] The resin-coated metal pipe for oil wells disclosed herein exhibits excellent shear strength. Attached Figure Description

[0040] Figure 1 This is a schematic diagram of a metal pipe used in oil wells when the threads are tightened.

[0041] Figure 2 It is a cross-sectional view of the area near the resin coating when the threads are tightened, perpendicular to the pipe axis of the metal pipe used in oil wells.

[0042] Figure 3 This is a graph showing the relationship between the shear strength and yield torque of the resin coating.

[0043] Figure 4 This is a graph showing the relationship between the shear material ratio in the resin coating and the shear strength of the resin coating.

[0044] Figure 5This is a structural diagram illustrating an example of a T&C type (Threaded and Coupled) metal pipe for oil wells according to this embodiment.

[0045] Figure 6 It means Figure 5 The image shows a partial sectional view of the coupling of the metal pipe for oil wells, in a section (longitudinal section) parallel to the pipe axis.

[0046] Figure 7 yes Figure 6 The diagram shows a cross-sectional view of the portion near the male thread in a metal pipe for oil wells, parallel to the pipe axis.

[0047] Figure 8 yes Figure 6 The diagram shows a cross-sectional view of the portion near the female thread in the oil well tubing, parallel to the pipe axis.

[0048] Figure 9 This is a diagram illustrating an example of a metal pipe for oil wells, where the male thread portion includes the external thread portion but excludes the male thread portion sealing surface and the male thread portion shoulder surface, and the female thread portion includes the internal thread portion but excludes the female thread portion sealing surface and the female thread portion shoulder surface.

[0049] Figure 10 This is a structural diagram of the integral metal pipe for oil wells involved in this embodiment.

[0050] Figure 11 yes Figure 7 An enlarged view of the male fastener contact surface shown.

[0051] Figure 12 yes Figure 8 An enlarged view of the contact surface of the female buckle shown. Detailed Implementation

[0052] Hereinafter, this embodiment will be described in detail with reference to the accompanying drawings. The same or equivalent parts in the drawings will be labeled with the same reference numerals and will not be described repeatedly.

[0053] The inventors have studied a metal pipe for oil wells that can be tightened with a higher torque than before, and is applicable to oil well pipe connections used in horizontal drilling. As a result, the following insights were obtained.

[0054] As described above, an oil well pipe connection is formed by threading oil well metal pipes together. When the oil well metal pipes are threaded together, the torque increases with the number of revolutions. Especially in the final stage of thread tightening, the torque increases sharply. On the other hand, if the torque during thread tightening becomes too high, the oil well metal pipes may yield. In this specification, the torque at which the oil well metal pipes yield during thread tightening is referred to as the "yield torque." The higher the yield torque, the higher the torque at which the oil well metal pipes can be tightened. In other words, the yield torque can be used as an indicator of whether the oil well metal pipes can be tightened with a higher torque.

[0055] To date, methods for increasing the tightening torque of metal pipes used in oil wells have included increasing the coefficient of friction of the resin coating formed on the pipes. The idea is that when the metal pipes are threaded together, if the resin coating with a higher coefficient of friction comes into contact and slides, the tightening torque will increase. Therefore, by increasing the coefficient of friction of the resin coating, it is possible to increase the yield torque. Therefore, the present inventors have adjusted the coefficient of friction of the resin coating by including hydrated magnesium silicate powder and / or TiO2 as solid powders, and investigated the relationship between the coefficient of friction and the yield torque. However, contrary to the present inventors' expectations, it has been found that the correlation between the coefficient of friction and the yield torque is weak. The results of the present inventors' investigation have clarified that simply increasing the coefficient of friction of the resin coating is not an effective way to increase the yield torque.

[0056] Therefore, the inventors further investigated oil well metal pipes that can be tightened with high torque. First, the inventors focused on the behavior of the resin coating during the final stage of thread tightening. During the final stage of thread tightening, the resin coatings contact each other with high surface pressure and slide along the circumferential direction of the oil well metal pipe.

[0057] Figure 1 This is a schematic diagram of a metal pipe used in oil wells during thread tightening. (Refer to...) Figure 1 The thread tightening is performed, for example, as follows: Secure the well metal pipe 1a. Insert the male thread 40 of the well metal pipe 1b into the female thread 50 of the secured well metal pipe 1a. Rotate the inserted well metal pipe 1b along its circumference.

[0058] Figure 2 This is a cross-sectional view perpendicular to the axis of the oil well metal pipe near the resin coating when the threads are tightened. It is assumed that the oil well metal pipe 1a is fixed, and the threads are tightened while rotating the oil well metal pipe 1b along the circumferential direction. Here, the surface of the resin coating 100a on the side of the resin coating 100b is called the surface. The surface of the resin coating 100a on the side of the oil well metal pipe 1a is called the back surface. (Refer to...) Figure 2When the well metal pipe 1b is rotated along its circumferential direction to tighten the threads, a pushing force F1 is generated on the resin coating 100b formed on the well metal pipe 1b, in the same direction as the rotation of the well metal pipe 1b. In the final stage of thread tightening, the surface pressure pressing the resin coatings 100a and 100b radially along the well metal pipes 1a and 1b is high. If the threads are tightened under high surface pressure, the resin coating 100a slides while being forcefully pressed against the resin coating 100b. Therefore, a pushing force F1 in the same direction as the rotation of the well metal pipe 1b is also generated in the resin coating 100a. Since the resin coating 100a is fixed to the surface of the well metal pipe 1a, a force F2 in the opposite direction to F1 is generated on the back side of the resin coating 100a. That is, in the final stage of thread tightening, the surface and back of the resin-coated 100a are subjected to opposite forces in the circumferential direction of the oil well metal pipe 1. The same applies to the resin-coated 100b; in the final stage of thread tightening, the surface and back of the resin-coated 100b are subjected to opposite forces in the circumferential direction of the oil well metal pipe 1.

[0059] Shear force refers to the force of equal magnitude and opposite direction acting on two parallel surfaces within an object. It is argued that if the shear strength of the resin coating 100 is high, even if sliding occurs between the surface and back of the resin coating 100 due to thread tightening, deformation and damage are unlikely, and the sliding resistance increases. If the resin coating 100 deforms and is damaged under low torque, the torque remains low, and the rotational speed of the oil well metal pipe 1 increases. In this case, the yield torque cannot be increased. On the other hand, it is argued that if deformation and damage of the resin coating 100 are suppressed during thread tightening, and the sliding resistance is high, the resin coating 100 can maintain a shape close to that before thread tightening until the final stage of thread tightening, and the torque can also be increased. In this case, it is believed that a high torque can be obtained relative to the rotational speed of the oil well metal pipe 1. That is, it is believed that by increasing the shear strength of the resin coating 100, the yield torque is increased.

[0060] The inventors conducted a detailed investigation into the relationship between the shear strength of the resin coating and the yield torque of the metal pipe for oil wells. Figure 3 This is a graph showing the relationship between the shear strength and yield torque of the resin coating. Figure 3 The horizontal axis represents the shear strength (MPa) of the resin coating. Figure 3 The vertical axis represents the yield torque (ft.lbs) when the resin-coated metal pipe thread of an oil well is tightened.

[0061] Reference Figure 3 The correlation coefficient R between the shear strength and yield torque of the resin coating 2The value was 0.874. Based on this result, a strong positive correlation was confirmed between the shear strength and yield torque of the resin coating. That is, the detailed research conducted by the inventors clarified that increasing the shear strength of the resin coating can effectively increase the yield torque of the metal pipe for oil wells.

[0062] The inventors have studied a method for improving the shear strength of a resin coating 100. The inventors focused on hydrogen bonds and electrostatic interactions in the resin coating 100. Hereinafter, hydrogen bonds and electrostatic interactions will be referred to as gravitational interactions. When there are many gravitational interactions in the resin coating 100, it is necessary to break more gravitational interactions to cause deformation and damage to the resin coating 100. The inventors believe that by increasing the gravitational interactions in the resin coating 100, the shear strength of the resin coating 100 can be improved.

[0063] The inventors have investigated a method for increasing the gravitational interactions in the resin coating 100. The results showed that if the resin coating 100 contains nylon, it is possible to increase the gravitational interactions within the resin coating 100.

[0064] Nylon is a general term for polymers having a repeating structure containing amide bonds (CONH) and hydrocarbon (CH2) units. The hydrogen (H) contained in the amide bonds forms hydrogen bonds with other elements. Therefore, it is believed that if a base resin containing functional groups that form hydrogen bonds with the hydrogen contained in the amide bonds and a nylon resin coating 100 are used, the hydrogen bonds increase, and the attractive interactions increase. The inventors have conducted research and concluded that if a resin coating 100 containing a total of 40.0 to 99.4% by mass of one or more base resins selected from the group consisting of epoxy resins, phenolic resins, acrylic resins, urethane resins, polyester resins, polyamide-imide resins, polyimide resins, and polyetheretherketone resins, and 0.1 to 20.0% by mass of nylon, the attractive interactions of the resin coating 100 can be increased.

[0065] However, the resin coating 100 having the above composition does not necessarily improve the shear strength of the resin coating 100. Therefore, the inventors conducted a further detailed study on the composition of the resin coating 100. The results showed that if the above composition is present, and the ratio of the total content (by mass%) of wax, fluorine-based additives, and graphite to the total content (by mass%) of TiO2, hydrated magnesium silicate, and nylon is 5.00 or less, then the shear strength of the resin coating 100 is improved.

[0066] The ratio of the total content of wax, fluorine additives and graphite (in mass%) to the total content of TiO2, hydrated magnesium silicate and nylon (in mass%) is defined as the "shear material ratio". Figure 4This is a graph showing the relationship between the shear material ratio in the resin coating 100 and the shear strength of the resin coating 100. Figure 4 This is an excerpt of the results of the embodiments described later. Figure 4 The horizontal axis represents the shear ratio of the material. Figure 4 The vertical axis represents the shear strength (MPa) of the resin coating 100. (Refer to...) Figure 4 If the shear ratio is below 5.00, the shear strength of the resin-coated 100 will be above 58.0 MPa.

[0067] Wax, fluorinated additives, and graphite are added to reduce the coefficient of friction of the resin coating 100. However, wax, fluorinated additives, and graphite essentially lack functional groups that can form hydrogen bonds with hydrogen atoms within amide bonds. Therefore, they are not considered to contribute to the increase in shear force resulting from increased gravitational interactions. It is believed that if the content of wax, fluorinated additives, and graphite relative to nylon is too high, the gravitational interactions cannot be sufficiently increased, and the shear strength of the resin coating 100 cannot be improved. TiO2 and hydrated magnesium silicate are considered to have high shear strength. Therefore, it is believed that when the content of nylon, TiO2, and hydrated magnesium silicate is high, the shear strength of the resin coating 100 is improved.

[0068] In summary, it is clear that, unlike previous understandings, simply increasing the friction coefficient of the resin coating is insufficient to effectively increase the yield torque; only by increasing the shear strength of the resin coating can the yield torque be effectively increased. Furthermore, it is clear that only by adjusting the components of the resin coating as described above can the shear strength of the resin coating be improved. By increasing the shear strength of the resin coating to increase the yield torque, it is possible to obtain metal pipes for oil wells that can also be used in horizontal drilling. The metal pipe for oil wells disclosed herein is based on the above understanding and has the following structure. [1]

[0070] A type of metal pipe for oil wells.

[0071] It has a tube body including a first end and a second end.

[0072] The pipe body includes:

[0073] The male fastener is formed at the first end; and

[0074] The female buckle portion is formed at the second end.

[0075] The male thread portion has a male thread contact surface including an external thread portion.

[0076] The female threaded portion has a female threaded portion contact surface.

[0077] The oil well metal pipe also has a resin coating formed as the uppermost layer of at least one of the male thread contact surface and the female thread contact surface.

[0078] The resin coating contains:

[0079] The base resin is selected from one or more of the group consisting of epoxy resin, phenolic resin, acrylic resin, urethane resin, polyester resin, polyamide-imide resin, polyimide resin, and polyetheretherketone resin, with a total content of 40.0 to 99.4% by mass.

[0080] Nylon: 0.1–20.0% by mass

[0081] TiO2: 0.5–30.0% by mass

[0082] Hydrous magnesium silicate: 0–49.4% by mass

[0083] Wax: 0-10.0% by weight

[0084] Fluorine additives: 0–30.0% by weight

[0085] Graphite: 0–10.0% by mass

[0086] Rust-preventive pigments: 0–30.0% by weight

[0087] Coloring pigments: 0–10.0% by mass, and

[0088] Coupling agent: 0–10.0% by mass

[0089] The total content of the wax, the fluorine additives and the graphite in the resin coating, expressed as a percentage by mass, is less than 5.00 relative to the total content of the nylon, the TiO2 and the hydrated magnesium silicate, expressed as a percentage by mass.

[0090] [2] According to the metal pipe for oil wells described in [1], wherein,

[0091] The ratio of the nylon content (in mass%) to the total content (in mass%) of the base resin is 0.30 or less.

[0092] [3] According to [1] or [2], the metal pipe for oil wells, wherein,

[0093] The contact surface of the male fastener also includes a male fastener sealing surface and a male fastener shoulder surface.

[0094] The contact surface of the female buckle also includes the sealing surface of the female buckle and the shoulder surface of the female buckle.

[0095] The following is a detailed description of the metal pipe for oil wells involved in this embodiment.

[0096] [Structure of metal pipes for oil wells]

[0097] First, the structure of the metal pipe for oil wells according to this embodiment will be described. The metal pipe for oil wells has a well-known structure. There are T&C type metal pipes and integral type metal pipes for oil wells. The following is a detailed description of each type of metal pipe for oil wells.

[0098] [For the case where the metal pipe for the oil well is of type T&C]

[0099] Figure 5 This is a structural diagram showing an example of the metal pipe 1 for oil wells according to this embodiment. Figure 5 This is a structural diagram of what is known as T&C type metal tubing for oil wells (Type 1). (Refer to...) Figure 5 The oil well metal pipe 1 has a pipe body 10.

[0100] The tube body 10 extends along the tube axis. The cross-section of the tube body 10 perpendicular to the tube axis is circular. The tube body 10 includes a first end 10A and a second end 10B. The first end 10A is the end opposite to the second end 10B. Figure 5 In the T&C type oil well metal pipe 1 shown, the pipe body 10 has a male threaded pipe body 11 and a coupling 12. The coupling 12 is installed at one end of the male threaded pipe body 11. More specifically, the coupling 12 is fastened to one end of the male threaded pipe body 11 by means of threads.

[0101] Figure 6 It means Figure 5 The image shows a partial sectional view (longitudinal section) of the coupling 12 of the oil well metal pipe 1, parallel to the pipe axis. (Refer to...) Figure 5 and Figure 6 The pipe body 10 includes a male threaded portion 40 and a female threaded portion 50. The male threaded portion 40 is formed at the first end 10A of the pipe body 10. When tightening, the male threaded portion 40 is inserted into the female threaded portion 50 of another oil well metal pipe 1 (not shown), thereby tightening it to the female threaded portion 50 of the other oil well metal pipe 1 by means of threads.

[0102] The female thread 50 is formed at the second end 10B of the pipe body 10. When tightening, the male thread 40 of another oil well metal pipe 1 is inserted into the female thread 50, thereby tightening the male thread 40 of the other oil well metal pipe 1 by means of threads.

[0103] [Regarding the structure of the male fastener 40]

[0104] Figure 7 yes Figure 6 A cross-sectional view of the portion near the male thread 40 of the oil well metal pipe 1, shown, parallel to the pipe axis direction of the oil well metal pipe 1. Figure 7 The dashed line indicates the structure of the female threaded portion 50 of the other oil well metal pipe 1 when it is fastened to other oil well metal pipes 1. (Refer to...) Figure 7 The male thread 40 has a male thread contact surface 400 on the outer peripheral surface of the first end 10A of the pipe body 10. When fastened to other oil well metal pipes 1, the male thread contact surface 400 is screwed into the female thread 50 of the other oil well metal pipe 1 and contacts the female thread contact surface 500 of the female thread 50 (as described later).

[0105] The male thread contact surface 400 includes at least an external thread portion 41 formed on the outer peripheral surface of the first end portion 10A. The male thread contact surface 400 may also include a male thread sealing surface 42 and a male thread shoulder surface 43. Figure 7 In this design, the male thread shoulder surface 43 is disposed on the top surface of the first end portion 10A, and the male thread sealing surface 42 is disposed on the outer peripheral surface of the first end portion 10A, further from the top surface of the first end portion 10A than the external thread portion 41. That is, the male thread sealing surface 42 is disposed between the external thread portion 41 and the male thread shoulder surface 43. The male thread sealing surface 42 is tapered. Specifically, in the male thread sealing surface 42, in the longitudinal direction (pipe axis direction) of the first end portion 10A, the outer diameter gradually decreases from the external thread portion 41 toward the male thread shoulder surface 43.

[0106] When fastened to other oil well metal pipes 1, the male thread sealing surface 42 contacts the female thread sealing surface 52 of the female thread 50 of the other oil well metal pipe 1 (as described later). More specifically, during fastening, the male thread 40 is inserted into the female thread 50 of the other oil well metal pipe 1, and the male thread sealing surface 42 contacts the female thread sealing surface 52. Then, the male thread 40 is further screwed into the female thread 50 of the other oil well metal pipe 1, and the male thread sealing surface 42 and the female thread sealing surface 52 are tightly sealed. Thus, during fastening, the male thread sealing surface 42 and the female thread sealing surface 52 are tightly sealed to form a seal based on metal-metal contact. Therefore, air tightness can be improved in the mutually fastened oil well metal pipes 1.

[0107] exist Figure 7 In the middle, the male buckle shoulder surface 43 is disposed on the top surface of the first end portion 10A. That is, in Figure 7In the male thread portion 40 shown, an external thread portion 41, a male thread portion sealing surface 42, and a male thread portion shoulder surface 43 are sequentially arranged from the center of the pipe body 10 toward the first end 10A. When fastened to other oil well metal pipes 1, the male thread portion shoulder surface 43 faces and contacts the female thread portion shoulder surface 53 of the female thread portion 50 of the other oil well metal pipe 1 (as described later). More specifically, during fastening, the male thread portion 40 is inserted into the female thread portion 50 of the other oil well metal pipe 1, and the male thread portion shoulder surface 43 contacts the female thread portion shoulder surface 53. As a result, a high torque can be obtained during fastening. In addition, the positional relationship between the male thread portion 40 and the female thread portion 50 in the fastened state can be stabilized.

[0108] It should be noted that the male thread contact surface 400 of the male thread portion 40 includes at least the external thread portion 41. That is, the male thread contact surface 400 may include the external thread portion 41 but does not include the male thread sealing surface 42 and the male thread shoulder surface 43. The male thread contact surface 400 may include the external thread portion 41 and the male thread shoulder surface 43 but does not include the male thread sealing surface 42. The male thread contact surface 400 may include the external thread portion 41 and the male thread sealing surface 42 but does not include the male thread shoulder surface 43.

[0109] [Regarding the structure of the female fastener 50]

[0110] Figure 8 yes Figure 6 A cross-sectional view of the portion near the female threaded portion 50 of the oil well metal pipe 1, shown, parallel to the pipe axis direction of the oil well metal pipe 1. Figure 8 The dashed line indicates the structure of the male thread 40 of the other oil well metal pipe 1 when it is fastened to other oil well metal pipes 1. (Refer to...) Figure 8 The female thread 50 has a female thread contact surface 500 on the inner circumferential surface of the second end 10B of the pipe body 10. When fastened to other oil well metal pipes 1, the female thread contact surface 500 is screwed into the male thread 40 of the other oil well metal pipe 1 and contacts the male thread contact surface 400 of the male thread 40.

[0111] The female thread contact surface 500 includes at least an internal thread portion 51 formed on the inner circumferential surface of the second end 10B. During tightening, the internal thread portion 51 engages with the external thread portion 41 of the male thread portion 40 of the other well metal pipe 1.

[0112] The female snap-fit ​​contact surface 500 may further include a female snap-fit ​​sealing surface 52 and a female snap-fit ​​shoulder surface 53. Figure 8In this design, the female thread sealing surface 52 is located on the inner circumferential surface of the second end 10B, further from the tube body 10 than the internal thread portion 51. Specifically, the female thread sealing surface 52 is positioned between the internal thread portion 51 and the female thread shoulder surface 53. The female thread sealing surface 52 is tapered. More specifically, in the female thread sealing surface 52, along the length direction (tube axis direction) of the second end 10B, the inner diameter gradually decreases from the internal thread portion 51 toward the female thread shoulder surface 53.

[0113] When fastened to other oil well metal pipes 1, the sealing surface 52 of the female thread 52 contacts the sealing surface 42 of the male thread 40 of the other oil well metal pipe 1. More specifically, during fastening, as the male thread 40 of the other oil well metal pipe 1 is screwed into the female thread 50, the sealing surface 52 of the female thread 52 contacts the sealing surface 42 of the male thread 40, and through further screwing, the sealing surface 52 of the female thread 52 and the sealing surface 42 of the male thread 42 are tightly sealed. Thus, during fastening, the sealing surface 52 of the female thread 52 and the sealing surface 42 of the male thread 42 are tightly sealed to form a seal based on metal-metal contact. Therefore, in the mutually fastened oil well metal pipes 1, air tightness can be improved.

[0114] The female threaded portion shoulder surface 53 is positioned further from the pipe body 10 than the female threaded portion sealing surface 52. Specifically, in the female threaded portion 50, the female threaded portion shoulder surface 53, the female threaded portion sealing surface 52, and the internal thread portion 51 are sequentially arranged from the center of the pipe body 10 toward the top of the second end 10B. When fastened to other well metal pipes 1, the female threaded portion shoulder surface 53 faces and contacts the male threaded portion shoulder surface 43 of the male threaded portion 40 of the other well metal pipe 1. More specifically, during fastening, the female threaded portion shoulder surface 53 contacts the male threaded portion shoulder surface 43 by inserting the male threaded portion 40 of the other well metal pipe 1 into the female threaded portion 50. This allows for high torque during fastening. Furthermore, it stabilizes the positional relationship between the male threaded portion 40 and the female threaded portion 50 in the fastened state.

[0115] The female contact surface 500 includes at least an internal thread portion 51. During tightening, the internal thread portion 51 of the female contact surface 500 corresponds to and contacts the external thread portion 41 of the male contact surface 400. The female sealing surface 52 corresponds to and contacts the male sealing surface 42. The female shoulder surface 53 corresponds to and contacts the male shoulder surface 43.

[0116] When the male thread contact surface 400 includes an external thread portion 41 but excludes the male thread sealing surface 42 and the male thread shoulder surface 43, the female thread contact surface 500 includes an internal thread portion 51 but excludes the female thread sealing surface 52 and the female thread shoulder surface 53. When the male thread contact surface 400 includes an external thread portion 41 and the male thread shoulder surface 43 but excludes the male thread sealing surface 42, the female thread contact surface 500 includes an internal thread portion 51 and the female thread shoulder surface 53 but excludes the female thread sealing surface 52. When the male thread contact surface 400 includes an external thread portion 41 and the male thread sealing surface 42 but excludes the male thread shoulder surface 43, the female thread contact surface 500 includes an internal thread portion 51 and the female thread sealing surface 52 but excludes the female thread shoulder surface 53.

[0117] The male thread contact surface 400 may include multiple external thread portions 41, or multiple male thread sealing surfaces 42, or multiple male thread shoulder surfaces 43. For example, in the male thread contact surface 400 of the male thread portion 40, the male thread shoulder surface 43, male thread sealing surface 42, external thread portion 41, male thread sealing surface 42, male thread shoulder surface 43, male thread sealing surface 42, and external thread portion 41 may be arranged sequentially from the top of the first end 10A toward the center of the tube body 10. In this case, in the female thread contact surface 500 of the female thread portion 50, the internal thread portion 51, female thread sealing surface 52, female thread shoulder surface 53, female thread sealing surface 52, internal thread portion 51, female thread sealing surface 52, and female thread shoulder surface 53 may be arranged sequentially from the top of the second end 10B toward the center of the tube body 10.

[0118] exist Figure 7 and Figure 8 The diagram illustrates a so-called advanced connector where the male thread portion 40 includes an external thread portion 41, a male thread portion sealing surface 42, and a male thread portion shoulder surface 43, and the female thread portion 50 includes an internal thread portion 51, a female thread portion sealing surface 52, and a female thread portion shoulder surface 53. However, as described above, the male thread portion 40 may include the external thread portion 41 but not the male thread portion sealing surface 42 and the male thread portion shoulder surface 43. In this case, the female thread portion 50 includes the internal thread portion 51 but not the female thread portion sealing surface 52 and the female thread portion shoulder surface 53. Figure 9 This is a diagram illustrating an example of a metal pipe 1 for oil wells, wherein the male thread portion 40 includes an external thread portion 41 but does not include the male thread portion sealing surface 42 and the male thread portion shoulder surface 43, and the female thread portion 50 includes an internal thread portion 51 but does not include the female thread portion sealing surface 52 and the female thread portion shoulder surface 53.

[0119] [In the case where the metal pipe for oil wells is a single piece]

[0120] Figure 5 , Figure 6 and Figure 9The oil well metal pipe 1 shown is a so-called T&C type oil well metal pipe 1, with the pipe body 10 including the male threaded pipe body 11 and the coupling 12. However, the oil well metal pipe 1 of this embodiment may not be T&C type, but integral type.

[0121] Figure 10 This is a structural diagram of the integral oil well metal pipe 1 involved in this embodiment. (Refer to...) Figure 10 The integral type oil well metal pipe 1 includes a pipe body 10. The pipe body 10 includes a first end 10A and a second end 10B. The first end 10A is located on the side opposite to the second end 10B. As described above, in the T&C type oil well metal pipe 1, the pipe body 10 includes a male threaded pipe body 11 and a coupling 12. That is, in the T&C type oil well metal pipe 1, the pipe body 10 is constructed by fastening two separate components (the male threaded pipe body 11 and the coupling 12). In contrast, in the integral type oil well metal pipe 1, the pipe body 10 is formed integrally.

[0122] A male threaded portion 40 is formed at the first end 10A of the pipe body 10. During tightening, the male threaded portion 40 is inserted into and screwed into the female threaded portion 50 of another integral type oil well metal pipe 1, thus tightening the pipe body 1. A female threaded portion 50 is formed at the second end 10B of the pipe body 10. During tightening, a male threaded portion 40 of another integral type oil well metal pipe 1 is inserted into and screwed into the female threaded portion 50, thus tightening the pipe body 1.

[0123] The structure of the male thread 40 of the integral metal pipe 1 for oil wells and Figure 7 The male thread 40 of the T&C type oil well metal pipe 1 shown has the same structure. Similarly, the female thread 50 of the integral type oil well metal pipe 1 has the same structure. Figure 8 The structure of the female thread 50 of the T&C type oil well metal pipe 1 shown is the same. It should be noted that... Figure 7 and Figure 8 In the male thread portion 40, a male thread shoulder surface 43, a male thread sealing surface 42, and an external thread portion 41 are sequentially arranged from the top of the first end 10A toward the center of the pipe body 10. Therefore, in the female thread portion 50, an internal thread portion 51, a female thread sealing surface 52, and a female thread shoulder surface 53 are sequentially arranged from the top of the second end 10B toward the center of the pipe body 10. However, similar to the male thread contact surface 400 of the male thread portion 40 of the T&C type oil well metal pipe 1, the male thread contact surface 400 of the integral type oil well metal pipe 1 only needs to include at least the external thread portion 41. Similarly, similar to the female thread contact surface 500 of the female thread portion 50 of the T&C type oil well metal pipe 1, the female thread contact surface 500 of the integral type oil well metal pipe 1 only needs to include at least the internal thread portion 51.

[0124] The metal pipe 1 for oil wells in this embodiment can be either T&C type or integral type.

[0125] [Resin Coating 100]

[0126] The oil well metal pipe 1 of this embodiment has a resin coating 100 formed as the uppermost layer of at least one of the male thread contact surface 400 and the female thread contact surface 500. Figure 11 yes Figure 7 An enlarged view of the male fastener contact surface 400 shown. Figure 12 yes Figure 8 An enlarged view of the female buckle contact surface 500 shown. (See diagram below.) Figure 11 and Figure 12 As shown, the oil well metal pipe 1 according to this embodiment may have a resin coating 100 as the uppermost layer on both the male thread contact surface 400 and the female thread contact surface 500. However, the oil well metal pipe 1 according to this embodiment may also have the resin coating 100 as the uppermost layer on only one of the male thread contact surface 400 or the female thread contact surface 500. For example, as Figure 11 As shown, when the male contact surface 400 has a resin coating 100, the female contact surface 500 may not have a resin coating 100. Additionally, as... Figure 12 As shown, when the female thread contact surface 500 has a resin coating 100, the male thread contact surface 400 may not have a resin coating 100. In other words, the oil well metal pipe 1 according to this embodiment has a resin coating 100 as the uppermost layer on the male thread contact surface 400 and / or the female thread contact surface 500.

[0127] [Composition of Resin Coating 100]

[0128] The resin coating 100 has the following composition.

[0129] Base resin: 40.0–99.4% by mass in total.

[0130] The base resin is the substrate of the resin coating 100. The base resin is selected from one or more of the group consisting of epoxy resin, phenolic resin, acrylic resin, urethane resin, polyester resin, polyamide-imide resin, polyimide resin, and polyetheretherketone resin. These base resins have moderate hardness and contain a large number of functional groups that form hydrogen bonds with hydrogen (H) in nylon. Therefore, these base resins increase the attractive interactions in the resin coating 100, improving the shear strength of the resin coating 100. When the total content of the base resin is less than 40.0% by mass, the hardness of the resin coating 100 decreases, thus failing to improve the shear strength of the resin coating 100. On the other hand, when the content of the base resin exceeds 99.4% by mass, the wear resistance and yield torque of the oil well metal pipe 1 may decrease because it cannot contain sufficient amounts of other components, including nylon and TiO2. Therefore, the total content of the base resin is 40.0% to 99.4% by mass. In the case of multiple base resins, the total content of the base resin refers to the total content of all base resins.

[0131] The lower limit of the total content of the base resin is preferably 42.0% by mass, more preferably 50.0% by mass, more preferably 55.0% by mass, more preferably 60.0% by mass, more preferably 65.0% by mass, and more preferably 70.0% by mass.

[0132] The upper limit of the total content of the base resin is preferably 95.0% by mass, more preferably 90.0% by mass, more preferably 88.0% by mass, and more preferably 87.0% by mass.

[0133] Nylon: 0.1–20.0% by mass

[0134] It is believed that nylon facilitates the formation of hydrogen bonds between its internal hydrogen (H) and functional groups in the base resin, thereby improving the shear strength of the resin coating 100. When the nylon content is less than 0.1% by mass, this effect cannot be achieved. On the other hand, when the nylon content exceeds 20.0% by mass, the content of other components cannot be adequately ensured. In this case, poor formation of the resin coating 100 or a decrease in the wear resistance and yield torque of the resin coating 100 may occur. Therefore, the nylon content is 0.1% to 20.0% by mass.

[0135] The lower limit of the nylon content is preferably 0.3% by mass, more preferably 0.5% by mass, more preferably 0.8% by mass, more preferably 1.0% by mass, more preferably 2.0% by mass, more preferably 2.5% by mass, more preferably 3.0% by mass, more preferably 4.0% by mass, and more preferably 5.0% by mass. The upper limit of the nylon content is preferably 19.0% by mass, more preferably 17.0% by mass, and more preferably 15.0% by mass.

[0136] TiO2: 0.5–30.0% by mass

[0137] Titanium dioxide (TiO2) improves the shear strength of the resin coating 100. TiO2 is in powder form. Hydroxyl groups and titanium-containing polar groups are exposed on the surface of TiO2. Therefore, TiO2 readily forms hydrogen bonds with hydrogen (H) in nylon and functional groups in the base resin. It is believed that the shear strength of the resin coating 100 is improved through the formation of hydrogen bonds between TiO2 and the nylon and base resin. This effect cannot be obtained when the TiO2 content is less than 0.5% by mass. On the other hand, when the TiO2 content exceeds 30.0% by mass, it may promote abrasive wear, reducing the wear resistance of the metal pipe 1 for oil wells. Therefore, the TiO2 content is 0.5% to 30.0% by mass.

[0138] The lower limit of the TiO2 content is preferably 0.7% by mass, more preferably 1.0% by mass, and even more preferably 1.2% by mass. The upper limit of the TiO2 content is preferably 28.0% by mass, more preferably 26.0% by mass, more preferably 25.0% by mass, more preferably 23.0% by mass, and even more preferably 21.0% by mass.

[0139] hydrated magnesium silicate: 0–49.4% by mass

[0140] Hydrous magnesium silicate is an optional component and can be omitted. That is, the content of hydrous magnesium silicate can be 0% by mass. Hydrous magnesium silicate is in powder form. When included, i.e., when the content of hydrous magnesium silicate exceeds 0% by mass, it further improves the shear strength of the resin coating 100. Hydroxyl groups and magnesium-containing polar groups are exposed on the surface of the hydrous magnesium silicate. Therefore, hydrous magnesium silicate readily forms hydrogen bonds or electrostatic interactions with hydrogen (H) in nylon and functional groups in the substrate resin. It is believed that the shear strength of the resin coating 100 is improved through hydrogen bonding formed by hydrous magnesium silicate within nylon and the substrate resin. The above-mentioned effects can be achieved to a certain extent with only a small amount of hydrous magnesium silicate.

[0141] On the other hand, when the content of hydrated magnesium silicate exceeds 49.4% by mass, the resin coating 100 forms poorly. Therefore, the content of hydrated magnesium silicate is 0–49.4% by mass.

[0142] The lower limit of the content of hydrated magnesium silicate is preferably 0.1% by mass, more preferably 0.3% by mass, more preferably 5.0% by mass, more preferably 7.0% by mass, and more preferably 10.0% by mass.

[0143] The upper limit of the content of hydrated magnesium silicate is preferably 45.0% by mass, more preferably 42.0% by mass, more preferably 40.0% by mass, more preferably 35.0% by mass, and more preferably 30.0% by mass.

[0144] Wax: 0-10.0% by mass

[0145] The type of wax contained in the resin coating 100 of this embodiment is not particularly limited. The wax may be one or more selected from the group consisting of animal wax, plant wax, mineral wax, and synthetic wax. Preferably, the wax is selected from the group consisting of beeswax, whale wax (all animal-derived), wood wax, carnauba wax, candelilla wax, rice bran wax (all plant-derived), paraffin wax, microcrystalline wax, petrolatum, lignite wax, ozokelite, ceresin (all mineral-derived), oxidized wax, polyethylene wax, polypropylene wax, Fischer-Tropsch wax, amide wax, and hydrogenated castor oil (Castorwax) (all synthetic wax).

[0146] Further preferred waxes are selected from one or more of the group consisting of polyethylene waxes and polypropylene waxes. The resin coating 100 may also contain multiple waxes. In the case of multiple waxes, the wax content is the total content of all waxes.

[0147] Wax is an optional component, which can be included or excluded. That is, the wax content can be 0% by mass. When included, i.e., when the wax content exceeds 0% by mass, the wax improves the lubricity of the resin coating by 100%. Even a small amount of wax can achieve the aforementioned effect to some extent.

[0148] On the other hand, when the wax content exceeds 10.0% by mass, the hardness of the resin coating 100 decreases, and the resin becomes brittle due to the reduced substrate ratio. This makes the resin coating 100 prone to peeling when repeatedly tightening and loosening the threads. Therefore, the wax content should be between 0% and 10.0% by mass.

[0149] The lower limit of the wax content is preferably 0.1% by mass, more preferably 0.5% by mass, more preferably 0.8% by mass, more preferably 1.0% by mass, and more preferably 2.0% by mass.

[0150] The upper limit of the wax content is preferably 9.0% by mass, more preferably 8.0% by mass, and even more preferably 7.5% by mass.

[0151] Fluorine-based additives: 0–30.0% by mass

[0152] In this specification, fluorinated additives are collectively referred to as fluorinated additives. Fluorinated additives are, for example, one or two selected from the group consisting of perfluoropolyether (PFPE) and polytetrafluoroethylene (PTFE). The resin coating 100 may also contain multiple fluorinated additives. In the case of multiple fluorinated additives, the content of the fluorinated additives is the total content of the multiple fluorinated additives.

[0153] In this embodiment, the fluorinated additive is a component that can be included arbitrarily, or it can be absent. That is, the content of the fluorinated additive can be 0% by mass. When it is included, that is, when the content of the fluorinated additive exceeds 0% by mass, the fluorinated additive improves the lubricity of the resin coating 100. The above-mentioned effects can be obtained to a certain extent even with only a small amount of fluorinated additive.

[0154] On the other hand, when the content of fluorinated additives exceeds 30.0% by mass, the hardness of the resin coating 100 decreases and it becomes brittle. As a result, the resin coating 100 is easily peeled off when the threads are repeatedly tightened and loosened. Therefore, the content of fluorinated additives is 0–30.0% by mass.

[0155] The lower limit of the content of fluorine-based additives is preferably 0.1% by mass, more preferably 0.5% by mass, more preferably 1.0% by mass, more preferably 2.0% by mass, more preferably 3.0% by mass, more preferably 4.5% by mass, more preferably 5.0% by mass, and more preferably 7.5% by mass.

[0156] The upper limit of the content of fluorinated additives is preferably 25.0% by mass, more preferably 20.0% by mass, more preferably 18.0% by mass, more preferably 15.0% by mass, and more preferably 12.5% ​​by mass.

[0157] Graphite: 0–10.0% by mass

[0158] In this embodiment, graphite is a component that can be included arbitrarily, or it can be absent. That is, the graphite content can be 0% by mass. When included, that is, when the graphite content exceeds 0% by mass, graphite improves the lubricity of the resin coating 100. The above-mentioned effects can be obtained to a certain extent even with only a small amount of graphite.

[0159] On the other hand, when the graphite content exceeds 10.0% by mass, the hardness of the resin coating 100 decreases and it becomes brittle. As a result, the resin coating 100 is easily peeled off when the threads are repeatedly tightened and loosened. Therefore, the graphite content is 0–10.0% by mass.

[0160] The lower limit of the graphite content is preferably 0.1% by mass, more preferably 0.5% by mass, more preferably 0.8% by mass, more preferably 1.0% by mass, more preferably 2.0% by mass, and more preferably 3.0% by mass.

[0161] The upper limit of the graphite content is preferably 9.0% by mass, more preferably 8.0% by mass, more preferably 7.0% by mass, and more preferably 6.0% by mass.

[0162] Rust-preventive pigments: 0–30.0% by mass

[0163] In this embodiment, the rust-preventive pigment is not particularly limited as long as it is a well-known pigment that improves the rust resistance of the resin coating 100. For example, the rust-preventive pigment may be one or more selected from the group consisting of zinc phosphate, aluminum tripolyphosphate, aluminum phosphite, carboxylic acid metal soaps, and sulfonates. The resin coating 100 may also contain multiple rust-preventive pigments. When multiple rust-preventive pigments are contained, the content of the rust-preventive pigments refers to the total content of the multiple rust-preventive pigments.

[0164] In this embodiment, the rust-preventive pigment is an optional component, or it may be absent altogether. That is, the content of the rust-preventive pigment can be 0% by mass. When it is present, that is, when the content of the rust-preventive pigment exceeds 0% by mass, the rust-preventive pigment improves the rust resistance of the resin coating 100. Even a small amount of rust-preventive pigment is sufficient to achieve the aforementioned effects.

[0165] On the other hand, when the content of the rust-preventive pigment exceeds 30.0% by mass, the resin coating 100 forms poorly. Therefore, the content of the rust-preventive pigment is 0 to 30.0% by mass.

[0166] The lower limit of the content of the rust-preventive pigment is preferably 1.0% by mass, more preferably 1.5% by mass, more preferably 2.0% by mass, more preferably 3.0% by mass, and more preferably 3.5% by mass.

[0167] The upper limit of the content of the rust-preventive pigment is preferably 25.0% by mass, more preferably 20.0% by mass, and even more preferably 10.0% by mass.

[0168] Coloring pigment: 0–10.0% by mass

[0169] In this embodiment, the coloring pigment is not particularly limited as long as it is a well-known pigment capable of coloring the resin coating 100. For example, the coloring pigment may be one or more selected from the group consisting of copper phthalocyanine, zinc oxide, yellow iron oxide, iron oxide, and chromium hydroxide. The resin coating 100 may also contain multiple coloring pigments. When multiple coloring pigments are present, the content of the coloring pigment is the total content of all coloring pigments.

[0170] In this embodiment, the coloring pigment is an optional component, or it may be absent altogether. That is, the content of the coloring pigment can be 0% by mass. When it is present, that is, when the content of the coloring pigment exceeds 0% by mass, the coloring pigment colors the resin coating 100. As a result, damage to the resin coating 100 is easily visually identifiable. The above-mentioned effects can be achieved to a certain extent even with only a small amount of coloring pigment.

[0171] On the other hand, when the content of the coloring pigment exceeds 10.0% by mass, the resin coating 100 forms poorly. Therefore, the content of the coloring pigment is 0 to 10.0% by mass.

[0172] The lower limit of the content of the coloring pigment is preferably 0.1% by mass, more preferably 0.2% by mass, more preferably 0.5% by mass, and more preferably 0.8% by mass.

[0173] The upper limit of the content of the coloring pigment is preferably 8.0% by mass, more preferably 5.0% by mass, more preferably 3.0% by mass, and more preferably 2.0% by mass.

[0174] Coupling agent: 0–10.0% by mass

[0175] In this embodiment, the coupling agent is not particularly limited. The coupling agent may be, for example, one or two selected from the group consisting of silane coupling agents and titanium coupling agents. The resin coating 100 may also contain multiple coupling agents. In the case of multiple coupling agents, the content of the coupling agent is the total content of the multiple coupling agents.

[0176] In this embodiment, the coupling agent is a component that can be included arbitrarily or not included at all. That is, the content of the coupling agent can be 0% by mass. When included, that is, when the content of the coupling agent exceeds 0% by mass, the coupling agent improves the adhesion of the resin coating 100. Therefore, when the threads of the oil well metal pipe 1 are repeatedly tightened and loosened, peeling of the resin coating 100 is suppressed. The above-mentioned effect can be obtained to a certain extent even with only a small amount of coupling agent.

[0177] On the other hand, when the coupling agent content exceeds 10.0% by mass, the resin coating 100 forms poorly. Therefore, the coupling agent content is 0 to 10.0% by mass.

[0178] The lower limit of the coupling agent content is preferably 0.1% by mass, more preferably 0.2% by mass, more preferably 0.5% by mass, more preferably 0.7% by mass, and more preferably 1.0% by mass.

[0179] The upper limit of the coupling agent content is preferably 8.0% by mass, more preferably 6.0% by mass, more preferably 5.0% by mass, and more preferably 4.0% by mass.

[0180] The resin coating 100 may be composed of the above-mentioned components, or may contain the above-mentioned components and the balance being 0 to 1.0% by mass of impurities.

[0181] [Shear Material Ratio]

[0182] In the resin coating 100 of this embodiment, the ratio of the total content of wax, fluorine additives, and graphite (in mass%) to the total content of nylon, TiO2, and hydrated magnesium silicate (in mass%) is 5.00 or less. Hereinafter, the ratio of the total content of wax, fluorine additives, and graphite (in mass%) to the total content of nylon, TiO2, and hydrated magnesium silicate (in mass%) will also be referred to as the shear material ratio.

[0183] As stated above, it is believed that wax, fluorine-based additives, and graphite do not contribute to the increase in shear force resulting from the increased gravitational interactions in the resin coating 100. If the total content of wax, fluorine-based additives, and graphite is excessive relative to the total content of nylon, TiO2, and hydrated magnesium silicate, the gravitational interactions cannot be sufficiently increased, and the shear strength of the resin coating 100 cannot be improved. Therefore, based on the above composition, the shear-to-material ratio of the resin coating 100 is 5.00 or less.

[0184] The upper limit of the shear ratio is preferably 4.50, more preferably 4.00, more preferably 3.50, more preferably 3.00, and more preferably 2.90. The lower limit of the shear ratio is not particularly limited, for example, it is 0.00, for example, it is 0.10.

[0185] With the resin coating 100 having the above-described composition, and a shear material ratio of 5.00 or less, the shear strength is improved. As a result, the yield torque of the oil well metal pipe 1 equipped with the resin coating 100 is increased.

[0186] [Ratio of base resin to nylon]

[0187] Preferably, the ratio of the nylon content (by mass%) to the total content (by mass%) of the base resin is 0.30 or less. As described above, by forming hydrogen bonds between hydrogen (H) in the nylon and functional groups in the base resin, the attractive interaction increases, thereby improving the shear strength of the resin coating 100. When the ratio of the nylon content to the total content of the base resin is 0.30 or less, the number of functional groups increases, further promoting the formation of hydrogen bonds in the resin coating 100. As a result, the shear strength of the resin coating 100 is further improved.

[0188] The upper limit of the ratio of nylon content to the total content of the base resin is more preferably 0.25, further preferably 0.20, further preferably 0.18, and even more preferably 0.15. The lower limit of the ratio of nylon content to the total content of the base resin is not particularly limited, for example, it is 0.01. The lower limit of the ratio of nylon content to the total content of the base resin is preferably 0.02, further preferably 0.03.

[0189] Shear strength

[0190] The shear strength of the resin coating 100 is not particularly limited, but a higher shear strength is preferred. When the shear strength of the resin coating 100 is 58.0 MPa or higher, the yield torque of the oil well metal pipe 1 equipped with the resin coating 100 can be further stably improved. Therefore, the shear strength of the resin coating 100 is preferably 58.0 MPa or higher. The lower limit of the shear strength of the resin coating 100 is further preferably 58.5 MPa, and more preferably 59.0 MPa. The upper limit of the shear strength of the resin coating 100 is not particularly limited, but is, for example, 70.0 MPa.

[0191] [Methods for determining shear strength]

[0192] The shear strength of the resin coating 100 can be determined by the following method: A test piece is cut from an oil well metal pipe 1 equipped with the resin coating 100. The test piece is, for example, 10mm × 10mm in surface area and 10mm in thickness. However, the size of the test piece is not particularly limited; for example, the surface area of ​​the test piece could be 30mm × 30mm. The resin coating 100 is formed on the surface of the test piece. This surface corresponds to the contact surface 400 or 500 of the oil well metal pipe 1 with the resin coating 100 formed.

[0193] The shear strength of the obtained test pieces was determined using a surface and interface property analysis device (e.g., DAIPLA WINTESCO.,LTD., trademark: SAICAS). Using a cutting blade with a blade width of 1 mm, the surface of the resin coating 100 was cut at a constant speed (2 μm / s horizontally, 0.2 μm / s vertically) at a 10° angle, peeling the resin coating 100 from the contact surfaces 400 and 500. It should be noted that all tests were conducted at room temperature (25±5℃). In cases where the surface of the test piece was bent, the direction for measuring the shear strength on the surface of the test piece was set perpendicular to the bending direction of the test piece (i.e., the pipe axis direction of the oil well metal pipe 1). In this case, the shear strength (MPa) of the resin coating 100 was determined based on the horizontal force, vertical force, and vertical displacement applied to the cutting blade.

[0194] [Resin coating thickness 100]

[0195] In this embodiment, the thickness of the resin coating 100 is not particularly limited. The thickness of the resin coating 100 is, for example, 1 to 100 μm. In this case, the yield torque of the oil well metal pipe 1 can be improved more stably. The lower limit of the thickness of the resin coating 100 is preferably 2 μm, more preferably 5 μm, and even more preferably 10 μm. The upper limit of the thickness of the resin coating 100 is preferably 50 μm, more preferably 40 μm, and even more preferably 30 μm.

[0196] [Method for determining the thickness of resin coating 100]

[0197] The thickness of the resin coating 100 can be determined using the following method. An electromagnetic induction thickness gauge probe is brought into contact with the male contact surface 400 or the female contact surface 500 on which the resin coating 100 is formed. The probe has an electromagnet; when it approaches a magnetic body, electromagnetic induction is generated, and the voltage varies depending on the distance between the probe and the magnetic body. The thickness of the resin coating 100 is determined based on the change in voltage. The measurement locations are 12 points along the circumference of the oil well metal pipe 1 (0°, 30°, 60°, 90°, 120°, 150°, 180°, 210°, 240°, 270°, 300°, and 330°). The arithmetic mean of the measurement results at the 12 locations is taken as the thickness of the resin coating 100.

[0198] [Other layers]

[0199] The oil well metal pipe 1 according to this embodiment may also have other layers between at least one of the male thread contact surface 400 and the female thread contact surface 500 and the uppermost resin coating 100. For example, the oil well metal pipe 1 may have other layers below the uppermost resin coating 100, i.e., between the male thread contact surface 400 and the resin coating 100. Alternatively, for example, the oil well metal pipe 1 may have other layers below the uppermost resin coating 100, i.e., between the female thread contact surface 500 and the uppermost resin coating 100.

[0200] Other layers may be, for example, one or more chemically converted coatings and / or one or more plating layers. More specifically, other layers may be, for example, one or more selected from the group consisting of phosphate coatings, plating layers, chromate coatings, and zirconium coatings. Phosphate coatings may be, for example, one or more selected from the group consisting of zinc phosphate coatings, manganese phosphate coatings, calcium phosphate coatings, and iron phosphate coatings. Plating layers may be, for example, one or more selected from the group consisting of Zn plating layers, Ni plating layers, Cu plating layers, Zn-Ni alloy plating layers, Zn-Co alloy plating layers, and Ni-W alloy plating layers. In the case of a Zn-Ni alloy plating layer, the chemical composition of the Zn-Ni alloy plating layer may consist, for example, 10 to 20% by mass of Ni, and the balance being Zn and impurities. In the case of a Cu plating layer, the chemical composition of the Cu plating layer may consist, for example, Cu and impurities. Multiple other layers may be stacked radially along the well metal pipe 1. For example, the coating may be disposed on the male contact surface 400, the chromate coating may be disposed on the coating, and the resin coating 100, as the uppermost layer, may be disposed on the chromate coating.

[0201] [Chemical composition of tube body 10]

[0202] The chemical composition of the pipe body 10 of the oil well metal pipe 1 involved in this embodiment is not particularly limited. That is, in this embodiment, the steel type of the pipe body 10 of the oil well metal pipe 1 is not particularly limited. The pipe body 10 can be formed, for example, from carbon steel, stainless steel, and alloys. That is, the oil well metal pipe 1 can be a steel pipe formed from an Fe-based alloy or an alloy pipe represented by a Ni-based alloy pipe. Here, the steel pipe is, for example, a low-alloy steel pipe, a martensitic stainless steel pipe, a duplex stainless steel pipe, etc. On the other hand, among alloys, Ni-based alloys and high alloys such as duplex stainless steel containing alloying elements such as Cr, Ni, and Mo have high corrosion resistance. Therefore, if these high alloys are used as the pipe body 10, excellent corrosion resistance can be obtained in corrosive environments containing hydrogen sulfide, carbon dioxide, etc.

[0203] [Manufacturing Method]

[0204] The manufacturing method of the metal pipe 1 for oil wells involved in this embodiment will be described below.

[0205] The method for manufacturing the metal pipe 1 for oil wells according to this embodiment includes a preparation step, a coating step, and a curing step. The curing step is performed after the coating step.

[0206] [Preparation Process]

[0207] In the preparation process, a metal pipe for oil wells, comprising a pipe body 10, is prepared. The pipe body 10 includes a male thread portion 40 and a female thread portion 50. The male thread portion 40 has a male thread contact surface 400 including an external thread portion 41, and the female thread portion 50 has a female thread contact surface 500 including an internal thread portion 51. As described above, the metal pipe for oil wells according to this embodiment has a well-known structure. That is, in the preparation process, it is sufficient to prepare a metal pipe for oil wells with a well-known structure.

[0208] [Coating Process]

[0209] In the coating process, a composition is applied to at least one of the male thread contact surface 400 and the female thread contact surface 500 of the prepared oil well metal pipe. The composition is for forming the aforementioned resin coating 100. The composition contains: a base resin totaling 40.0–99.4% by mass, nylon 0.1–20.0% by mass, TiO2 0.5–30.0% by mass, hydrated magnesium silicate 0–49.4% by mass, wax 0–10.0% by mass, fluorine additives 0–30.0% by mass, graphite 0–10.0% by mass, anti-rust pigment 0–30.0% by mass, coloring pigment 0–10.0% by mass, and a coupling agent 0–10.0% by mass. The total content of wax, fluorine additives, and graphite, expressed as a percentage by mass, is in a ratio of 5.00 or less to the total content of nylon, TiO2, and hydrated magnesium silicate, expressed as a percentage by mass. The composition also contains a solvent. The composition of the composition used to form the resin coating 100, except for the solvent, is the same as the composition of the resin coating 100 described above.

[0210] The composition can be prepared, for example, by dissolving or dispersing the base resin, nylon, TiO2, and other components as needed in a solvent and then mixing them. The solvent is, for example, one or more selected from the group consisting of water, alcohols, and organic solvents. The solvent may contain trace amounts of surfactants. The proportion of the solvent is not particularly limited. The proportion of the solvent is adjusted in a way that gives the composition a suitable viscosity according to the coating method. For example, if the total amount of all components excluding the solvent is set to 100% by mass, the proportion of the solvent is 40-60% by mass.

[0211] The method for applying the composition to the male contact surface 400 and / or the female contact surface 500 is not particularly limited, and any well-known method may be used. For example, the composition in a solution state can be applied to the male contact surface 400 and / or the female contact surface 500 by spraying. In this case, the viscosity of the composition is adjusted so that it can be sprayed under normal temperature and pressure. The method for applying the composition to the male contact surface 400 and / or the female contact surface 500 may also be brushing or dipping instead of spraying.

[0212] [Curing Process]

[0213] In the curing process, the coated composition is cured to form a resin film 100. The composition coated on at least one of the male contact surface 400 and the female contact surface 500 is thermally cured by heating to form a solid resin film 100. The heating method is not particularly limited and any well-known method is acceptable. For example, the heating method involves placing the oil well metal pipe 1 coated with the composition into a well-known heating furnace for heating. The heating temperature is, for example, 200–250°C, and the heating time is, for example, 5–30 minutes.

[0214] The above steps are used to manufacture the oil well metal pipe 1 according to this embodiment. It should be noted that the manufacturing method of the oil well metal pipe 1 according to this embodiment may also include other steps.

[0215] [Substrate Treatment Process]

[0216] The method for manufacturing the metal pipe 1 for oil wells according to this embodiment may include a substrate treatment step before the coating step. In the substrate treatment step, for example, one or more of the following may be performed: acid washing, spraying, and alkaline degreasing.

[0217] When acid pickling is performed, for example, the male contact surface 400 and / or the female contact surface 500 are immersed in a strong acid solution such as sulfuric acid, hydrochloric acid, nitric acid, hydrofluoric acid, or a mixture thereof, to improve the surface roughness of the male contact surface 400 and / or the female contact surface 500. When blasting is performed, for example, sandblasting is performed, i.e., a mixture of blasting material (abrasive) and compressed air is projected onto the male contact surface 400 and / or the female contact surface 500. In this case, the surface roughness of the male contact surface 400 and / or the female contact surface 500 is improved.

[0218] It should be noted that in the base treatment process, the same treatment can be applied to both the male contact surface 400 and the female contact surface 500, or different treatments can be applied. Furthermore, the base treatment process can be performed only on the male contact surface 400 or only on the female contact surface 500.

[0219] The above-described process manufactures the oil well metal pipe 1 according to this embodiment. However, the above-described manufacturing method is only one example of the manufacturing method of the oil well metal pipe 1 according to this embodiment, and is not limited to this manufacturing method. The oil well metal pipe 1 according to this embodiment can also be manufactured by other methods.

[0220] Example

[0221] The effects of the metal pipe for oil wells according to this embodiment will be further explained in detail below through examples. The conditions in the following examples are one example of conditions adopted to confirm the feasibility and effects of the metal pipe for oil wells according to this embodiment. Therefore, the metal pipe for oil wells according to this embodiment is not limited to this one example of conditions.

[0222] In the embodiments, compositions for forming resin coatings were prepared, and the shear strength of the resin coatings was evaluated. Specifically, as described below.

[0223] Prepare compositions having the compositions shown in Table 1. For each test number composition, determine the ratio of the total content (by mass%) of wax, fluorinated additives, and graphite to the total content (by mass%) of nylon, TiO2, and hydrated magnesium silicate. Show the results in the "Shear Material Ratio" column of Table 1. For each test number composition, determine the ratio (by mass%) of nylon to the total content (by mass%) of the base resin. Show the results in the "Nylon Ratio" column of Table 1. It should be noted that, in addition to the compositions listed in Table 1, the compositions also contain solvents. A mixture of water, alcohol, and surfactants was used as the solvent.

[0224] [Table 1]

[0225] Table 1

[0226]

[0227] As the metal material for simulating metal pipes used in oil wells, cold-rolled steel sheets with a length of 30 mm, a width of 30 mm, and a thickness of 2 mm were prepared (chemical composition: C≤0.15%, Mn≤0.60%, P≤0.100%, S≤0.050%, and balance: Fe and impurities). The compositions for each test number were coated onto the cold-rolled steel sheets. The target film thickness of the resin coating was 20 μm. The cold-rolled steel sheets coated with the compositions were heat-treated at 210°C for 20 minutes and then cooled to form a resin coating. The shear strength of the resin coating for each test number was determined according to the [Shear Strength Determination Method] described above. The surface area of ​​the test piece was set to 30 mm × 30 mm, and the thickness was set to 2 mm. The results are shown in Table 1.

[0228] [Evaluation Results]

[0229] Referring to Table 1, the content of each component in the resin coatings of tests 1 to 24 was appropriate, and furthermore, the shear ratio was below 5.00. As a result, these resin coatings exhibited a shear strength of over 58.0 MPa, demonstrating high shear strength.

[0230] The resin films of test numbers 1 to 23, in which the ratio of nylon content (by mass%) to the total content (by mass%) of the base resin is 0.30 or less, exhibit a shear strength of 59.0 MPa or higher. The resin films of test numbers 1 to 23 demonstrate higher shear strength compared to test number 24.

[0231] On the other hand, the nylon content of the resin-coated film in test number 25 was too low. As a result, the shear strength of the resin-coated film in test number 25 was less than 58.0 MPa, and it did not have high shear strength.

[0232] The nylon content in the resin-coated film of test number 26 was too high. As a result, the shear strength of the resin-coated film of test number 26 was less than 58.0 MPa, indicating a lack of high shear strength.

[0233] Although the resin coatings in tests 27 and 28 had appropriate component contents, their shear-to-material ratios were greater than 5.00. As a result, the shear strength of the resin coatings in tests 27 and 28 was less than 58.0 MPa, indicating a lack of high shear strength.

[0234] The TiO2 content of the resin coating in test number 29 was too low. As a result, the shear strength of the resin coating in test number 29 was less than 58.0 MPa, indicating a lack of high shear strength.

[0235] The TiO2 content of the resin coating in test number 30 was too high. As a result, the shear strength of the resin coating in test number 30 was less than 58.0 MPa, indicating that it did not have high shear strength.

[0236] The embodiments of this disclosure have been described above. However, the above embodiments are merely illustrative examples for implementing this disclosure. Therefore, this disclosure is not limited to the above embodiments, and can be implemented by appropriately modifying the above embodiments without departing from its spirit.

[0237] Explanation of reference numerals in the attached figures

[0238] 1, 1a, 1b: Metal pipes for oil wells

[0239] 10: Main body of the pipe

[0240] 10A: First end

[0241] 10B: Second end

[0242] 11: Male buckle body

[0243] 12: Joint

[0244] 40: Male buckle section

[0245] 41: External thread section

[0246] 42: Male thread sealing surface

[0247] 43: Shoulder surface of male buckle

[0248] 50: Female buckle

[0249] 51: Internal thread section

[0250] 52: Sealing surface of the female fastener

[0251] 53: Shoulder surface of the female buckle

[0252] 100, 100a, 100b: Resin-coated

[0253] 400: Male thread contact surface

[0254] 500: Female fastener contact surface

Claims

1. A metal pipe for oil wells, comprising a pipe body including a first end and a second end. The pipe body includes: The male fastener is formed at the first end; and The female buckle portion is formed at the second end. The male thread portion has a male thread contact surface including an external thread portion. The female threaded portion has a female threaded portion contact surface. The oil well metal pipe also has a resin coating formed as the uppermost layer of at least one of the male thread contact surface and the female thread contact surface. The resin coating contains: The base resin is selected from one or more of the group consisting of epoxy resin, phenolic resin, acrylic resin, urethane resin, polyester resin, polyamide-imide resin, polyimide resin, and polyetheretherketone resin, with a total content of 40.0 to 99.4% by mass. Nylon: 0.1–20.0% by mass TiO2: 0.5–30.0% by mass Hydrous magnesium silicate: 0–49.4% by mass Wax: 0-10.0% by weight Fluorine additives: 0–30.0% by weight Graphite: 0–10.0% by mass Rust-preventive pigments: 0–30.0% by weight Coloring pigments: 0–10.0% by mass, and Coupling agent: 0–10.0% by mass The total content of the wax, the fluorine additives and the graphite in the resin coating, expressed as a percentage by mass, is less than 5.00 relative to the total content of the nylon, the TiO2 and the hydrated magnesium silicate, expressed as a percentage by mass.

2. The metal pipe for oil wells according to claim 1, wherein, The ratio of the nylon content (in mass%) to the total content (in mass%) of the base resin is 0.30 or less.

3. The metal pipe for oil wells according to claim 1 or claim 2, wherein, The contact surface of the male fastener also includes a male fastener sealing surface and a male fastener shoulder surface. The contact surface of the female buckle also includes the sealing surface of the female buckle and the shoulder surface of the female buckle.

Citation Information

Patent Citations

  • Threaded joint for steel pipe

    JP2003021278A

  • Threaded joint for steel pipes

    WO2006104251A1

  • Threaded end of a tubular component for drilling or working hydrocarbon wells, and resulting connection

    CN103119106A

  • Threaded joint for steel pipe

    CN114174708A