A polylactic acid oriented thin film and its preparation method

By blending polyhydroxyalkanoate copolymers with polylactic acid resin and subjecting them to biaxial stretching and annealing, polylactic acid oriented films with both low heat shrinkage and high barrier properties are prepared. This solves the problems of excessive heat shrinkage and insufficient barrier properties of polylactic acid films under high temperature conditions, making them suitable for high-temperature food packaging and the protection of sensitive products.

CN119592033BActive Publication Date: 2026-11-17JIANGSU JICUI ADVANCED POLYMER MATERIAL RES INST CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411901496.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-12-23
Publication Date
2026-11-17
Estimated Expiration
2044-12-23

AI Technical Summary

Technical Problem

Polylactic acid film has an excessively high heat shrinkage rate after biaxial stretching, which cannot meet the requirements for use in high-temperature environments, and its barrier properties are insufficient to protect sensitive products.

Method used

Polylactic acid oriented films were prepared by blending polyhydroxyalkanoate copolymers with polylactic acid resin and then by biaxial stretching and annealing heat setting processes. The combination of crystalline and amorphous polyhydroxyalkanoate copolymers enhanced the barrier properties of the films and suppressed thermal shrinkage.

Benefits of technology

While maintaining high barrier properties, it significantly reduces the thermal shrinkage rate of the film, making it suitable for food packaging in high-temperature environments and for protecting oxygen- and moisture-sensitive products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119592033B_ABST
    Figure CN119592033B_ABST
Patent Text Reader

Abstract

This invention discloses a polylactic acid (PLA) oriented film and its preparation method, belonging to the field of polymeric material film technology. The PLA oriented film comprises the following raw materials in parts by weight: 1-25 parts of polyhydroxyalkanoate copolymer, 67-98 parts of polylactic acid resin, 0.1-0.2 parts of thickener and compatibilizer, 1-5 parts of plasticizer, and 0.1-0.2 parts of compounded antioxidant; the polyhydroxyalkanoate copolymer includes polyhydroxyalkanoate copolymer P1 and polyhydroxyalkanoate copolymer P2; the content of repeating structural units in polyhydroxyalkanoate copolymer P1 is greater than 90 mol%, and the content of repeating structural units in polyhydroxyalkanoate copolymer P2 is greater than 50 mol% and less than 90 mol%. This invention prepares a PLA oriented film by blending and modifying polylactic acid resin and polyhydroxyalkanoate copolymer, orienting them, and then subjecting them to high-temperature annealing and shrinkage treatment, resulting in a film that exhibits both low heat shrinkage and high barrier properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of polymer thin film technology, specifically relating to a polylactic acid oriented thin film and its preparation method. Background Technology

[0002] Polylactic acid (PLA), a biodegradable thermoplastic aliphatic semi-crystalline polyester derived from crops and plant straw, has been widely used in express packaging, disposable tableware, and biomedicine due to its renewable resource characteristics and good biodegradability. However, PLA's slow crystallization rate results in low crystallinity, which in turn affects the heat resistance of the products. Furthermore, PLA's poor toughness and high oxygen permeability limit its application in packaging films.

[0003] Biaxial stretching is a film preparation process that involves stretching amorphous polymer sheets laterally and longitudinally between their glass transition temperature and cold crystallization temperature. After biaxial stretching, polylactic acid (PLA) sheets experience a macroscopic reduction in physical thickness and a microscopically ordered arrangement of polymer molecular chains along the stretching orientation direction, resulting in improved physical properties. For crystalline polymers, the crystallinity of the film is significantly increased after orientation, leading to substantial gains in barrier, optical, and mechanical properties. However, the thermal shrinkage rate of biaxially oriented PLA (BOPLA) films increases significantly after biaxial stretching, failing to meet the requirements for use in food or industrial packaging applications at high temperatures.

[0004] Patent CN118386581B proposes a solution that constructs a PLA stereocomposite crystal by compounding left-handed / right-handed PLA, and utilizes a biaxial stretching process during spinning to create a highly oriented hybrid-like tandem crystal structure, significantly reducing the thermal shrinkage rate of PLA fibers in boiling water. Although BOPLA film offers significantly improved barrier properties compared to ordinary polylactic acid, its application in packaging products sensitive to oxygen and moisture, such as tea and pharmaceuticals, may not provide sufficient barrier protection, making the products susceptible to oxidation and moisture absorption, thus shortening their shelf life.

[0005] The present invention aims to solve the above problems, and in order to provide a polylactic acid oriented film that has both low heat shrinkage and high barrier properties, meets the requirements for use in high-temperature environments, and provides better protection for sensitive products. Summary of the Invention

[0006] In view of the above-mentioned problems in the prior art, this application provides a polylactic acid oriented film and its preparation method, which has low heat shrinkage performance and good water vapor and oxygen barrier properties.

[0007] To address the above problems, the present invention provides the following technical solution:

[0008] In a first aspect, this application provides a polylactic acid oriented film comprising the following raw materials: polyhydroxyalkanoate copolymer, polylactic acid resin, thickener and compatibilizer, plasticizer and compounded antioxidant; wherein the polyhydroxyalkanoate copolymer comprises polyhydroxyalkanoate copolymer P1 and polyhydroxyalkanoate copolymer P2.

[0009] In one embodiment of this application, a polylactic acid oriented film comprises the following raw materials in parts by weight: 1-25 parts of polyhydroxyalkanoate copolymer, 67-98 parts of polylactic acid resin, 0.1-0.2 parts of thickener and compatibilizer, 1-5 parts of plasticizer, and 0.1-0.2 parts of compounded antioxidant; the polyhydroxyalkanoate copolymer includes polyhydroxyalkanoate copolymer P1 and polyhydroxyalkanoate copolymer P2.

[0010] In one embodiment of this application, a polylactic acid oriented film comprises the following raw materials in parts by weight: 0.5-20 parts of polyhydroxyalkanoate copolymer P1, 0.5-6 parts of polyhydroxyalkanoate copolymer P2, 67-98 parts of polylactic acid resin, 0.1-0.2 parts of thickener and compatibilizer, 1-5 parts of plasticizer, and 0.1-0.2 parts of compounded antioxidant.

[0011] In one embodiment of this application, the content of repeating structural units in the polyhydroxyalkanoate copolymer P1 is greater than 90 mol%.

[0012] In one embodiment of this application, the content of repeating structural units in the polyhydroxyalkanoate copolymer P2 is greater than 50 mol% and less than 90 mol%.

[0013] In one embodiment of this application, the polyhydroxy fatty acid ester copolymer is a copolymer with polyhydroxybutyrate as the main component.

[0014] In one embodiment of this application, polyhydroxybutyrate is preferably poly-3-hydroxybutyrate.

[0015] In one embodiment of this application, poly(3-hydroxybutyrate) may be selected from one or more of poly(3-hydroxybutyrate-3-hydroxyvalerate) (PHBV), poly(3-hydroxybutyrate-hydroxyhexanoate) (P3HB3HH), and poly(3-hydroxybutyrate-4-hydroxybutyrate) (P3HB4HB).

[0016] In one embodiment of this application, the 3-hydroxybutyrate structural unit content of the polyhydroxyalkanoate copolymer P1 is greater than 94 mol%.

[0017] In one embodiment of this application, the 3-hydroxybutyrate structural unit content of the polyhydroxyalkanoate copolymer P1 is greater than 97 mol%.

[0018] In one embodiment of this application, the content of 3-hydroxybutyrate structural units in the polyhydroxyalkanoate copolymer P2 is greater than 50 mol% and less than 90 mol%.

[0019] In one embodiment of this application, the melting temperature of polylactic acid resin is 150-170°C.

[0020] In one embodiment of this application, the content of dextrorotatory polylactic acid in the polylactic acid resin is 1-4 wt.%.

[0021] In one embodiment of this application, the tackifier and compatibilizer is an epoxy oligomer chain extender, such as ADR4468.

[0022] In one embodiment of this application, the plasticizer is a citrate ester compound, selected from one or more of tributyl citrate (TBC) and acetylated tributyl citrate (ATBC).

[0023] In one embodiment of this application, the compound antioxidant is a compound antioxidant of hindered phenols and phosphites, such as Irganox B225 and Irganox B215.

[0024] Secondly, this application provides a method for preparing a polylactic acid oriented film, comprising the following steps:

[0025] The polyhydroxyalkanoate copolymer and polylactic acid resin were dehumidified and dried pretreated. The raw materials were weighed according to the weight parts and mixed in a high-speed mixer to obtain a blend.

[0026] The blend is added to a twin-screw extruder, extruded and granulated to obtain composite modified granules, which are then dehumidified and dried.

[0027] The dried composite modified granules are melted and plasticized in a single screw extruder, and then extruded, cast, and rolled through a die to obtain polylactic acid composite sheets.

[0028] Polylactic acid composite sheets are placed in a biaxial stretching apparatus and simultaneously biaxially stretched at a predetermined rate and ratio, followed by annealing and heat setting to obtain polylactic acid oriented films.

[0029] In one embodiment of this application, the blend is obtained by mixing for 1-10 minutes.

[0030] In one embodiment of this application, the blend is obtained by mixing for 5 minutes.

[0031] In one embodiment of this application, the operating temperature range of the twin-screw extruder is 100-180°C.

[0032] In one embodiment of this application, the operating temperature range of the twin-screw extruder is set to 100°C, 130°C, 155°C, 160°C, 160°C, 165°C, 170°C, 170°C, 165°C, 160°C, and 160°C.

[0033] In one embodiment of this application, the feeding speed of the twin-screw extruder is 10-20 kg / h.

[0034] In one embodiment of this application, the temperature range of the single-screw extruder is 160-180°C.

[0035] In one embodiment of this application, the temperature of the single-screw extruder is 170°C.

[0036] In one embodiment of this application, the rotational speed of the single-screw extruder is 40-60 rpm.

[0037] In one embodiment of this application, the single-screw extruder rotates at 50 rpm.

[0038] In one embodiment of this application, a polylactic acid composite sheet with a thickness of 300 μm is subjected to biaxial stretching molding.

[0039] In one embodiment of this application, the temperature for biaxial stretching is 80-100°C.

[0040] In one embodiment of this application, the biaxial stretching rate is 50-150% / s.

[0041] In one embodiment of this application, the biaxial stretching ratio is (1-3)×(1-3).

[0042] In one embodiment of this application, the annealing heat setting temperature is 110-130°C.

[0043] In one embodiment of this application, the annealing heat setting time is 1-3 minutes.

[0044] In one embodiment of this application, during the annealing and heat setting step, the polylactic acid composite sheet shrinks in both the MD and TD directions.

[0045] In one embodiment of this application, the shrinkage ratio is 5-10%.

[0046] Compared with the prior art, the present invention has the following advantages:

[0047] This invention relates to a polylactic acid (PLA) oriented film prepared by blending and modifying PLA resin with a polyhydroxyalkanoate (PHA) copolymer and then orienting it. The combination of crystalline and amorphous PHA copolymers is employed. The lower viscosity of the amorphous PHA copolymer toughens the PLA, while the crystalline PHA copolymer, after orientation, exhibits a crystalline distribution. This not only enhances barrier properties together with the PLA crystals, effectively isolating water vapor and oxygen, but also acts as an anchor point to suppress thermal shrinkage, thus improving heat shrinkage resistance. Furthermore, the high-temperature annealing shrinkage treatment during the biaxial orientation heat setting process further reduces the film's thermal shrinkage rate, resulting in a final product that maintains high barrier properties while exhibiting excellent heat shrinkage resistance. This PLA film can meet the needs of packaging foods at high temperatures, packaging foods requiring secondary heating, secondary processing such as printing and heat sealing, and other related applications. Attached Figure Description

[0048] Figure 1 This is a schematic diagram of the internal structure of the polylactic acid oriented film of the present invention;

[0049] Figure 2 The water vapor and oxygen permeability diagrams are shown for the thin films prepared in the examples and comparative examples.

[0050] Figure 3 This is a comparison diagram of the heat resistance of films prepared in the examples and comparative examples after annealing and heat shrinkage treatment.

[0051] Figure 4 The mechanical properties of the films prepared in the examples and comparative examples are shown in the diagram.

[0052] Figure 5 The graph shows the results of film thermal shrinkage under different heat treatment conditions in Example 6. Detailed Implementation

[0053] The technical solutions in the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments.

[0054] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of the particular range. The range defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range.

[0055] Unless otherwise stated, when this invention relates to percentages between liquids, it is volume / volume percentage; when this invention relates to percentages between liquids and solids, it is volume / weight percentage; when this invention relates to percentages between solids and liquids, it is weight / volume percentage; the rest are weight / weight percentage.

[0056] Example 1

[0057] A polylactic acid oriented thin film, the preparation method of which is as follows:

[0058] Step S1: Raw material pretreatment and blending

[0059] Various biodegradable resins were pretreated by dehumidification and drying; the above raw materials were weighed according to the weight ratio, and then mixed in a high-speed mixer at 1000 rpm for 5 minutes to obtain a blend.

[0060] The weight proportions of each raw material are as follows: 0.5 parts of polyhydroxyalkanoate copolymer P1 (containing 95 mol% 3HB), 0.5 parts of polyhydroxyalkanoate copolymer P2 (containing 86 mol% 3HB), 1 part of plasticizer TBC, 98 parts of polylactic acid resin LX575 (2% D-co-lactic acid content, melting temperature 160-170℃), 0.1 parts of thickener and compatibilizer ADR-4468, and 0.1 parts of antioxidant Irganox B225.

[0061] Step S2: Extrusion granulation of the blended raw materials

[0062] The blend obtained in step S1 is added to a twin-screw extruder for extrusion and granulation. The temperature range of the extruder is set as follows: 100℃, 130℃, 155℃, 160℃, 160℃, 165℃, 170℃, 170℃, 165℃, 160℃, 160℃. The extruder speed is 150 rpm and the extruder feed rate is 16 kg / h. The composite modified granules are then dehumidified and dried.

[0063] Step S3: Extrusion casting of composite modified granules

[0064] The dehumidified and dried composite modified material is added to a single screw extruder for melting and plasticization, and then extruded through a die to cast and roll out a thin sheet with a thickness of 300μm. The melt extrusion processing temperature is set to 170℃ to obtain polylactic acid composite sheets.

[0065] Step S4: Biaxial stretching of polylactic acid composite sheets

[0066] In the biaxial stretching equipment, the sheet is first placed in an environment of 90°C and preheated for 30 seconds. Then, it is simultaneously biaxially stretched at a rate of 100% / s with a stretching ratio of 3×3. After orientation, it is then directly shaped and removed at 120°C.

[0067] Example 2

[0068] The difference between Example 2 and Example 1 is as follows: In step S1, the polyhydroxyalkanoate copolymer P1 is selected from 12 parts of PHBV (containing 97 mol% 3HB), the polyhydroxyalkanoate copolymer P2 is selected from 6 parts of P3HB4HB (containing 86 mol% 3HB), the plasticizer is selected from 2 parts of ATBC, the polylactic acid resin LX175 (4% ​​D-co-lactic acid content, melt temperature 150-160℃) is selected from 80 parts, the thickener and compatibilizer ADR-446 is selected from 0.2 parts, and the antioxidant Irganox B225 is selected from 0.15 parts. Subsequently, a sheet is prepared according to steps S2 and S3. In step S4, it is preheated at 90℃ for 30s, and then simultaneously biaxially stretched at a rate of 100% / s with a stretching ratio of 3×3. After orientation, it is directly shaped and removed at 110℃.

[0069] Example 3

[0070] The difference between Example 3 and Example 2 is that the polyhydroxyalkanoate copolymer P1 is PHBV (containing 95 mol% 3HB), while the other preparation process conditions are the same.

[0071] Example 4

[0072] The difference between Example 4 and Example 2 is that the polyhydroxy fatty acid ester copolymer P1 is P3HB3HH (containing 94 mol% 3HB), while the other preparation process conditions are the same.

[0073] Example 5

[0074] The difference between Example 5 and Example 1 is as follows: In step S1, the polyhydroxyalkanoate copolymer P1 is selected from 20 parts of PHBV (containing 97 mol% 3HB), the polyhydroxyalkanoate copolymer P2 is selected from 5 parts of P3HB4HB (containing 86 mol% 3HB), the plasticizer is selected from 5 parts of ATBC, the polylactic acid resin LX575 (containing 2% D-co-lactic acid, with a melting temperature of 160-170℃) is selected from 70 parts, the thickener and compatibilizer ADR-4468 is selected from 0.2 parts, and the antioxidant Irganox B215 is selected from 0.2 parts. Subsequently, a sheet is prepared according to steps S2 and S3. In step S4, it is preheated at 90℃ for 30s, and then simultaneously biaxially stretched at a rate of 100% / s with a stretching ratio of 3×3. After orientation, it is directly shaped and removed at 110℃.

[0075] Example 6

[0076] The difference between Example 6 and Example 5 is that the polylactic acid resin used is LX175 (4% ​​dextrorotatory polylactic acid content, melting temperature of 150-160℃), while the other preparation process conditions are the same.

[0077] Example 7

[0078] The sheet composition of Example 7 is the same as that of Example 6. The only difference is that in step S4 of this example, the sheet is preheated at 80°C for 30s, and then simultaneously biaxially stretched at a rate of 50% / s with a stretching ratio of 2.5×2.5. After orientation, the sheet is directly shaped and removed at 110°C.

[0079] Example 8

[0080] The thin film composition in Example 8 is the same as that in Example 6, and the film is oriented using the same preheating and orientation process. The only difference is that in step S4 of this example, there is an annealing shrinkage treatment. The specific steps are as follows: the oriented film is sent into the annealing chamber, the annealing temperature is 120°C, and the film is heat-shrinked in both the MD (longitudinal) and TD (transverse) directions with a shrinkage rate of 7% and an annealing time of 2 minutes.

[0081] Example 9

[0082] The thin film composition of Example 9 is the same as that of Example 6, and the film is oriented using the same preheating and orientation process. The only difference is that the annealing shrinkage and shaping process in step S4 of this example is different. The specific steps are as follows: the oriented film is sent into the annealing chamber, the annealing temperature is 130°C, and the film is heat-shrinked in both the MD (longitudinal) and TD (transverse) directions with a shrinkage rate of 10% and an annealing time of 3 minutes.

[0083] In addition to Examples 8 and 9, Example 6 underwent a more detailed annealing heat shrinkage treatment, and the specific process parameters are shown in Table 1.

[0084] Table 1

[0085] Annealing temperature / °C Annealing time / min Heat shrinkage treatment rate / % 110 1 5 120 2 7 130 3 10

[0086] Comparative Example 1

[0087] Wires were prepared directly using polylactic acid resin LX175 (4% ​​dextrorotatory polylactic acid content, melting temperature 150-160℃). PLA sheets were prepared through step S3, then preheated at 80℃ for 30s, and simultaneously biaxially stretched at a rate of 100% / s with a stretching ratio of 3×3. After orientation, the sheets were directly shaped and removed at 110℃.

[0088] like Figure 1As shown, crystalline polyhydroxyalkanoates exhibit a crystalline distribution after film orientation. While acting as a barrier phase with PLA crystals, they can also serve as anchor points to inhibit the thermal shrinkage of the oriented polylactic acid film.

[0089] The oxygen permeability and water vapor transmission coefficient of the above comparative examples and embodiments were measured under the following conditions: 23°C and 50% RH. The test results are shown in [Figure number missing]. Figure 2 ,from Figure 2 As can be seen, when PHBV and P3HB3HH with higher 3HB molar contents are selected for the A-poly(3-hydroxybutyrate) copolymer, the water vapor permeability and oxygen permeability coefficient of the oriented film decrease significantly with the increase of the addition amount. This is because when the 3HB molar content in the poly(3-hydroxybutyrate) copolymer is higher, its crystallinity is also higher. During the orientation process, the polylactic acid molecular chains tend to be more regular and are more prone to orientation crystallization. Therefore, the overall crystallinity of the film is high, and the permeation path of water vapor and oxygen inside the film becomes more tortuous. Thus, the water vapor and oxygen barrier performance of the composite film is significantly improved. However, the coefficient changes in Examples 6 and 7-9 are not significant. Subsequently, the comparative examples and each example were placed in a 100°C oven for 10 minutes, and the dimensional changes were recorded. Figure 3 As can be seen, compared to the comparative example, the addition of poly(3-hydroxybutyrate) copolymer with a higher 3HB molar content can appropriately improve the heat resistance of the film and reduce its thermal shrinkage rate. Furthermore, after thermal shrinkage treatment during the orientation process, the heat resistance of the film is significantly improved, specifically manifested in a significant reduction in its thermal shrinkage rate. Simultaneously, the shrinkage rate of the film prepared at a magnification of 2.5 × 2.5 is significantly lower than that of the sample prepared at 3 × 3. Regarding the experimental results of annealing temperature, annealing time, and shrinkage rate parameters of the shrinkage treatment process in Example 6, from... Figure 5 It can also be found that the actual heat shrinkage rate of oriented polylactic acid film products is positively correlated with the annealing process parameters in Table 1. These parameters can be appropriately adjusted in actual production to obtain composite films with the best heat resistance.

[0090] Therefore, it can be seen that in the orientation process, the heat setting step after film orientation can significantly improve the heat resistance of the film product in actual use by appropriately heat shrinking the film. Subsequent mechanical property tests on the film show that by selecting poly(3-hydroxybutyrate) copolymers with different 3HB molar ratios, the rigidity and toughness of the film can be adjusted to prepare polylactic acid composite oriented films with excellent mechanical properties.

[0091] The present application has been described in detail above with reference to specific embodiments and exemplary examples. However, these descriptions should not be construed as limiting the present application. Those skilled in the art will understand that various equivalent substitutions, modifications, or improvements can be made to the technical solutions and implementation methods of the present application without departing from the spirit and scope of the present application, and all such modifications and improvements fall within the scope of the present application.

Claims

1. A polylactic acid oriented film, characterized in that, The raw materials comprise the following parts by weight: 0.5-20 parts of polyhydroxyalkanoate copolymer P1, 0.5-6 parts of polyhydroxyalkanoate copolymer P2, 67-98 parts of polylactic acid resin, 0.1-0.2 parts of tackifier and compatibilizer, 1-5 parts of plasticizer, and 0.1-0.2 parts of compounded antioxidant; wherein the polyhydroxyalkanoate copolymer is a copolymer with polyhydroxybutyrate as the main component; wherein the polyhydroxyalkanoate copolymer P1 is selected from one of PHBV, P3HB3HH, and P3HB4HB; wherein the polyhydroxyalkanoate copolymer P2 is selected from P3HB4HB; wherein the content of 3-hydroxybutyrate structural units in the polyhydroxyalkanoate copolymer P1 is greater than 94 mol%; and wherein the content of 3-hydroxybutyrate structural units in the polyhydroxyalkanoate copolymer P2 is 86 mol%. A method for preparing polylactic acid oriented thin films includes the following steps: S1: The polyhydroxyalkanoate copolymer and polylactic acid resin are dehumidified and dried pretreated. The raw materials are weighed according to the weight parts and mixed in a high-speed mixer to obtain a blend. S2: The blend is added to a twin-screw extruder, extruded and granulated to obtain composite modified granules, which are then dehumidified and dried. S3: The dried composite modified granules are melted and plasticized in a single screw extruder, and then extruded, cast, and rolled through a die to obtain polylactic acid composite sheets; S4: Polylactic acid composite sheets are placed in a biaxial stretching apparatus and simultaneously biaxially stretched at a predetermined rate and ratio. Subsequently, they are annealed and heat-set to obtain a polylactic acid oriented film. During the annealing and heat-setting process, the film undergoes shrinkage treatment in the MD and TD directions, with a shrinkage ratio of 5-10%. The temperature for biaxial stretching is 80-100℃, the speed is 50-150% / s, the ratio is (1-3)×(1-3), the annealing heat setting temperature is 110-130℃, and the annealing heat setting time is 1-3min.

2. The polylactic acid oriented film according to claim 1, characterized in that, The polylactic acid resin has a melting temperature of 150-170℃ and the content of dextrorotatory polylactic acid in the polylactic acid resin is 1-4 wt.%.

3. The polylactic acid oriented film according to claim 1, characterized in that, The thickener and compatibilizer is an epoxide chain extender; the plasticizer is a citrate ester compound; and the compound antioxidant is a compound antioxidant of hindered phenols and phosphites.

4. The polylactic acid oriented film according to claim 1, characterized in that, The twin-screw extruder has a processing temperature range of 100-180℃ and a feeding speed of 10-20 kg / h.

5. The polylactic acid oriented film according to claim 1, characterized in that, The temperature range of the single-screw extruder is 160-180℃, and the rotation speed is 40-60rpm.

Citation Information

Patent Citations

  • High-performance polylactic acid biaxially oriented film and preparation method thereof

    CN118813008A

  • Stretched film and method for producing same

    WO2023090176A1

  • Biodegradable resin composition, biodegradable film using same, and method for producing same

    WO2024215088A1