Partially Crystalline Outer Coating for Marine Optical Fibers and its Preparation Method
By using partially crystalline polyurethane acrylate prepolymer and optimizing the fiber drawing process, the strength and weather resistance issues of marine optical fiber coatings have been solved, achieving high-strength and low-loss optical fiber performance suitable for long-term environmental use in marine optical fibers.
Patent Information
- Application Number
- CN202411912348.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-12-24
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-12-24
AI Technical Summary
Existing fiber optic coatings cannot meet the requirements of ultra-low loss and high strength for marine optical fibers. Conventional coatings are insufficient in terms of resistance to mechanical shock, thermal shock and weathering, making it difficult to meet the requirements for long-term environmental use.
Partially crystalline polyurethane acrylate prepolymer was used as the outer coating of optical fiber. By adjusting the crystallinity and mechanical properties and combining them with the fiber drawing process, an optical fiber outer coating with excellent performance was prepared. This included the use of a high-crystallinity hexamethylene diisocyanate and a low-crystallinity isophorone diisocyanate compounded with polycaprolactone diol and polypropylene glycol to control crystallinity and water resistance, and to optimize the fiber drawing speed and curing temperature.
It achieves a significant improvement in fiber strength and flexibility while ensuring low attenuation, meeting the high strength requirements of marine optical fibers, and taking into account good environmental performance and production efficiency.
Smart Images

Figure BDA0005206017950000041 
Figure BDA0005206017950000051 
Figure BDA0005206017950000052
Abstract
Description
Technical Field
[0001] This invention belongs to the field of coating technology, and specifically relates to an outer coating for optical fibers. Background Technology
[0002] Submarine optical cables, due to their advantages such as long transmission distance, strong anti-interference capability, high security, and good confidentiality, have gradually replaced coaxial cables and satellite communications, becoming one of the main media for global information transmission. With the development of the global digital economy, 95% of international communication traffic is transmitted via submarine optical cables, with an annual growth rate of 30%. In recent years, global internet traffic has shown a continuous growth trend, and the sustained increase in bandwidth demand has accelerated the construction of submarine optical cables. Currently, there are over 400 submarine optical cables in use worldwide, with a total length exceeding 1.4 million kilometers. The core of submarine optical cable communication is to achieve high-capacity communication transmission while ensuring long-term reliability. International marine communication giants regard submarine fiber optic cables as a systems engineering project, which has long created technological barriers and market monopolies.
[0003] At the fiber optic level, due to the need for long-distance transmission, the fiber optic cable is required to have higher strength and lower loss, which also places higher demands on the performance of fiber optic coatings. However, conventional fiber optic coatings on the market cannot meet the requirements of ultra-low loss and high strength for marine optical fibers.
[0004] Current fiber optic outer coatings typically use epoxy acrylate or a blend of epoxy acrylate and polyurethane acrylate as the oligomer component. However, epoxy acrylate is brittle, has poor resistance to mechanical and thermal shock, and poor weather resistance, making it unsuitable for the long-term environmental requirements of marine optical fibers. Conventional photocurable polyurethane acrylates offer high toughness and good weather resistance, but their use alone is insufficient to meet the high strength requirements of marine optical fibers. Research on crystalline polyurethanes has primarily focused on polyurethane elastomers, thermoplastic polyurethanes, and polyurethane adhesives, with no research on their application in marine optical fibers. These formulations and preparation processes are also unsuitable for use as fiber optic outer coatings. While crystalline polyurethanes improve the strength of polyurethane, if crystallinity is not effectively controlled, the cured film can become overly brittle and lack sufficient toughness, ultimately degrading the strength, attenuation, and other mechanical and environmental properties of the optical fiber. Therefore, balancing the strength, toughness, and weather resistance of the coating is the key and challenging aspect of outer coatings for marine optical fibers. Summary of the Invention
[0005] To address the aforementioned shortcomings in existing technologies, this invention provides a partially crystalline optical fiber outer coating and a curing method. This coating exhibits excellent mechanical properties. By matching the coating formulation with the fiber drawing process, the crystallinity is adjusted, thereby adjusting the mechanical properties. This allows the drawn optical fiber to achieve higher fiber strength while ensuring low attenuation, meeting the requirements for use in marine optical fibers.
[0006] To achieve the above objectives, the following technical solution is adopted:
[0007] A partially crystalline optical fiber outer coating, the composition of which is as follows (parts by weight):
[0008] The mixture consists of 90-110 parts of partially crystalline polyurethane acrylate prepolymer, 20-40 parts of acrylate reactive monomer diluent, 1-7 parts of photoinitiator, and 0-5 parts of additives. In the optimized formulation, the additives are 1-5 parts.
[0009] The method for preparing the partially crystalline polyurethane acrylate prepolymer is as follows: A polyol, isocyanate, and catalyst are mixed and heated to react. Then, (meth)acrylate hydroxyl ester and a polymerization inhibitor are added, and the reaction continues until the isocyanate is completely consumed, thus obtaining the partially crystalline polyurethane acrylate prepolymer. The structure, molecular weight, and crystallinity of the self-made polyurethane acrylate prepolymer can be flexibly controlled as needed.
[0010] According to the above scheme, the preparation method of the partially crystalline polyurethane acrylate prepolymer includes the following steps:
[0011] (1) Add polyol, isocyanate and catalyst sequentially to the reaction vessel, heat to 60±2℃, and keep the temperature for 2 to 2.5 hours.
[0012] (2) Add (meth)acrylate hydroxy ester and polymerization inhibitor, and continue the reaction at 65±2℃ for 2 to 3 hours until the isocyanate group content is zero, thus obtaining a partially crystalline polyurethane acrylate prepolymer;
[0013] The raw materials used, by weight, are as follows: 80-110 parts of polycaprolactone diol, 80-100 parts of polypropylene glycol, 30-50 parts of isocyanate (HDI and IPDI), 25-35 parts of (meth)acrylate hydroxy ester, 0.1-0.4 parts of catalyst, and 0.1-0.4 parts of polymerization inhibitor.
[0014] According to the above scheme, the polyol is a mixture of polyester polyol and polyether polyol. Polycaprolactone diol is easy to crystallize and is suitable for use as the soft segment of polyurethane acrylate in this invention. However, its water resistance is poor, and its use alone can easily lead to excessive crystallinity. Therefore, it is used in combination with polypropylene glycol for performance adjustment. In order to further adjust the crystallinity and water resistance, polycaprolactone diol with a molecular weight of 1000-3000 is preferred. The higher the molecular weight of polycaprolactone diol, the easier it is to crystallize. Based on the drawing speed and the contribution of other components to crystallinity commonly used in actual production, polycaprolactone diol with a molecular weight in this range can obtain suitable crystallinity while taking into account good water resistance.
[0015] According to the above scheme, in order to more flexibly control the crystallinity of the coating, the isocyanate is selected by using a combination of high-crystallinity isocyanate and low-crystallinity isocyanate. As the hard segment in polyurethane acrylate, appropriately increasing the crystallinity of isocyanate can increase the strength of the final coating; however, if its crystallinity is too high, it will also lead to insufficient toughness of the cured coating and affect the performance of the optical fiber. Therefore, this invention uses a combination of high-crystallinity hexamethylene diisocyanate (HDI) and low-crystallinity isophorone diacrylate (IPDI), and controls the final crystallinity by reasonably adjusting the ratio of the two.
[0016] According to the above scheme, the hydroxy methacrylate used for end capping is specifically selected from one or more of the following: hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, dipentaerythritol monohydroxypentamethacrylate, 2-hydroxyoctyl methacrylate, pentaerythritol trimethacrylate, glycerol dimethacrylate, 4-hydroxycyclohexyl methacrylate, trimethylolpropane dimethacrylate, and trimethylolethane dimethacrylate.
[0017] According to the above scheme, the catalyst is one or a mixture of two or more of the following: dibutyltin dilaurate, bismuth carboxylate, bismuth isooctanoate, N,N-dimethylcyclohexylamine, bis(2-dimethylaminoethyl) ether, N,N,N',N'-tetramethylalkylene diamine, triethylamine, N,N-dimethylbenzylamine, solidamine, N-ethylmorpholine, N,N'-diethylpiperazine, triethanolamine, dimethylaminoethanol, pyridine, and N,N'-dimethylpyridine; the amount used is 0.1wt% to 1wt% of the total mass of the reactants.
[0018] According to the above scheme, the polymerization inhibitor is one of hydroquinone and p-hydroxyanisole; the amount used is 0.1wt% to 1wt% of the total mass of the reactants.
[0019] According to the above scheme, the acrylate active monomer diluent is any one or a mixture of tripropylene glycol diacrylate, tripropylene glycol dimethacrylate, triethylene glycol dimethacrylate, diethylene glycol dimethacrylate, 1,4-butanediol dimethacrylate, tricyclodecanediethanol diacrylate, dioxanediol diacrylate, ethylene glycol dimethacrylate, isobornyl acrylate, isobornyl methacrylate, cyclohexyl methacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, ethoxylated trimethylolpropane triacrylate, propionyl trimethylolpropane triacrylate, propionyl glycerol triacrylate, trimethylolpropane trimethacrylate, ethoxylated trimethylolpropane trimethacrylate, pentaerythritol tetraacrylate, and bis(trimethylolpropane tetraacrylate).
[0020] According to the above scheme, the photoinitiator is one or a mixture of two or more of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 2-hydroxy-2-methyl-1-phenylpropanone, 1-hydroxycyclohexylbenzophenone, benzoin dimethyl ether, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, and 2-methyl-1-(4-methylthiophenyl)-2-morpholine-1-propanone.
[0021] According to the above scheme, the additives include any one or any combination of defoamers, leveling agents, antioxidants, and stabilizers.
[0022] The above-mentioned (meth)acrylate hydroxy esters, catalysts, polymerization inhibitors, acrylate reactive monomer diluents, photoinitiators and additives are all conventional raw materials. The specific types can be selected reasonably based on their objective properties.
[0023] A method for preparing an outer coating for partially crystalline optical fibers includes simultaneously preparing an optical fiber surface coating during the optical fiber drawing process; the surface coating adopts the aforementioned outer coating for partially crystalline optical fibers; the optical fiber drawing process involves a drawing speed of 500-2000 m / min, a curing temperature of 35-55℃, and an ultraviolet curing lamp power of 300-700W.
[0024] The crystallinity of the partially crystalline fiber outer coating after final curing can be adjusted by the curing conditions during the fiber drawing process to obtain optimal fiber performance. 500-2000 m / min is a commonly used fiber drawing speed in actual fiber production; speeds below 500 m / min are too inefficient, while speeds above 2000 m / min make it difficult to guarantee quality. The coating formulation of this application can be matched with currently used drawing speeds and adjusted accordingly based on changes in the specific drawing speed, ensuring fiber production efficiency while improving fiber performance.
[0025] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0026] (1) Since the preparation method of the outer coating of optical fiber is to coat the outer coating while drawing the fiber, the drawing process has an orientation effect on the coating, which can improve the crystallinity of the coating. Increasing the crystallinity of polyurethane can improve the strength. Therefore, the applicant creatively uses partially crystallized polyurethane acrylate coating to prepare the outer coating of optical fiber. Based on the contribution of the commonly used drawing speed in actual production to the crystallinity, the component ratio is reasonably set. The crystallinity of the outer coating is adjusted by the drawing process and the coating formulation. At the same time, good strength and flexibility are obtained, ensuring production efficiency. While taking into account the low attenuation of optical fiber and excellent environmental performance, the strength of optical fiber is significantly improved, ensuring the long-distance transmission of marine optical fiber on the seabed.
[0027] (2) Regarding the composition and ratio, PCL and PPG were selected as polyols based on their water resistance and crystallinity, and the molecular weight of PCL was further optimized to further improve the tensile strength of the optical fiber. In order to further control the crystallinity, HDI and IPDI were selected as a compound of isocyanates in a certain proportion.
[0028] (3) This invention selects partially crystalline polyurethane acrylate as the oligomer component of the outer coating for marine optical fibers. While retaining the original excellent properties of polyurethane materials, it improves the strength of polyurethane by introducing crystalline segments to meet the high strength requirements of marine optical fibers. The crystallinity of this polyurethane acrylate material can be adjusted by changing the type and ratio of raw materials, thereby adjusting the mechanical properties. Specifically, the soft segment of this polyurethane acrylate is selected by compounding polycaprolactone diol with a molecular weight of 1000-3000 with polypropylene glycol to obtain a suitable degree of crystallinity and good water resistance; the hard segment is selected by compounding hexamethylene diisocyanate (HDI) with high crystallinity and isophorone diacrylate (IPDI) with low crystallinity to obtain a suitable degree of crystallinity. In addition, the stretching induction during the fiber drawing process also affects the crystallinity of the coating, which can further adjust the performance of the optical fiber. The suitable drawing process is: drawing speed 500-2000 m / min, curing temperature 35-55℃, and UV curing lamp power 300-700W. Detailed Implementation
[0029] The following embodiments further illustrate the technical solution of the present invention, but are not intended to limit the scope of protection of the present invention.
[0030] A specific embodiment provides a method for preparing a partially crystalline polyurethane acrylate prepolymer, comprising the following steps:
[0031] (1) Add polyol, isocyanate and catalyst sequentially to the reaction vessel, heat to 60±2℃, and keep the temperature for 2 to 2.5 hours.
[0032] (2) Add (meth)acrylate hydroxyl ester and polymerization inhibitor dropwise, and continue the reaction at 65±2℃ for 2-3 hours until the isocyanate group content is zero, thus obtaining a partially crystalline polyurethane acrylate prepolymer. The specific raw materials and dosages are shown in Table 1.
[0033] Table 1 (Unit: g)
[0034]
[0035]
[0036] 100g of the partially crystalline polyurethane acrylate prepolymer obtained in Examples 1-6 above was mixed with 30g of tripropylene glycol diacrylate, 1.95g of TPO (2,4,6-trimethylbenzoyl-diphenylphosphine oxide), 1.95g of 184 (1-hydroxycyclohexylphenyl ketone), and 1.3g of DAROCURE 1173 (2-hydroxy-2-methyl-1-phenyl-1-propanone) to obtain an outer coating for optical fibers. This coating was applied to the optical fiber drawing process to simultaneously prepare a surface coating. The curing temperature was 45℃ and the UV curing lamp power was 500W. The properties of the resulting optical fiber and coating are shown in Table 2.
[0037] Table 2
[0038]
[0039] Comparative Example 1
[0040] Repeat Example 1, except that 100g of polycaprolactone diol (2000) is replaced with 50g of polycaprolactone diol (1000), and the rest remains the same.
[0041] Comparative Example 2
[0042] Repeat Example 1, except that 100g of polycaprolactone diol (2000) is replaced with 150g of polycaprolactone diol (3000), and the rest remains the same.
[0043] Comparative Example 3
[0044] Repeat Example 1, except that 100g of polycaprolactone diol (2000) and 80g of polypropylene glycol (1000) are replaced with 260g of polycaprolactone diol (2000), while the rest remain unchanged.
[0045] Comparative Example 4
[0046] Repeat Example 1, but replace 30.24g HDI and 17.76g IPDI with 43.68g HDI, leaving the rest unchanged.
[0047] Comparative Example 5
[0048] Repeat Example 1, but replace 30.24g HDI and 17.76g IPDI with 57.72g HDI, leaving the rest unchanged.
[0049] Comparative Example 6
[0050] Repeat Example 1, using a wire drawing speed of 2300 m / min, with all other parameters remaining unchanged.
[0051] Comparative Example 7
[0052] Repeat Example 1, using a wire drawing speed of 300 m / min, with all other parameters remaining unchanged.
[0053] Comparative Examples 1-7 yielded optical fiber outer coatings, which were applied to the optical fiber drawing process to simultaneously prepare surface coatings. The properties of the resulting optical fibers and coatings are shown in Table 3.
[0054] Table 3
[0055]
[0056] As demonstrated by the examples, this application has obtained a marine optical fiber outer coating formulation that matches the drawing speed through specific raw material selection and proportioning, achieving suitable crystallinity and thus realizing good strength, flexibility, water resistance, and low attenuation. Example 1 exhibits the best performance, while Examples 2-6 also demonstrate good comprehensive performance. Comparison shows that Examples 1 and 2, when drawing optical fibers at speeds of 1000 m / min and 2000 m / min respectively, both achieved high fiber strength while maintaining low attenuation and good water resistance, indicating that this formulation is well-suited to the commonly used drawing speed range of 1000-2000 m / min. Examples 3 and 4 replaced PCL2000 in Example 1 with a mixture of PCL1000 and PCL3000. After mixing, the tensile strength of the cured coating increased with the increase of the PCL3000 ratio. However, the tensile strength of the optical fibers drawn from both PCL1000 and PCL3000 decreased compared to Example 1. The water resistance and attenuation of Examples 3 and 4 were not superior to Example 1, indicating that using a mixture of PCL1000 and PCL3000 cannot fully achieve the technical effect of PCL2000. Example 1 is the optimal technical solution. Example 5 changed the ratio of PCL2000 to PPG1000 compared to Example 1. After the proportion of PCL2000 decreased, the strength of both the cured coating and the drawn optical fiber decreased. Example 6 changed the ratio of HDI and IPDI compared to Example 1. HDI can improve crystallinity, and reasonable control of its proportion can further improve the strength of the cured coating and the tensile strength of the drawn optical fiber.
[0057] In Comparative Example 1, only PCL1000 polyester polyol was used. Due to the low molecular weight of the resulting crystalline polyurethane soft segments, they could not effectively arrange themselves to form crystals, leading to low coating crystallinity and low optical fiber strength. In Comparative Example 2, only PCL3000 polyester polyol was used. After curing, the coating had excessively high crystallinity and was too brittle, resulting in decreased optical fiber strength and increased attenuation. In Comparative Example 3, only PCL2000 polyester polyol was used, without the addition of PPG1000 polyether polyol. The coating had excessively high crystallinity and insufficient toughness, leading to decreased optical fiber strength and increased attenuation. Furthermore, because only polyester polyol was used... The coating formulations in Comparative Example 4 had poor water resistance, leading to increased attenuation after the optical fiber was immersed in water. In Comparative Example 5, only HDI isocyanate was used, resulting in excessively high crystallinity of the polyurethane hard segment and an overly brittle coating, which in turn reduced the strength of the optical fiber and increased attenuation. In Comparative Example 6, only IPDI isocyanate was used, resulting in low crystallinity of the polyurethane hard segment, which in turn resulted in insufficient strength of the optical fiber. In Comparative Example 6, with a drawing speed of 2300, the coating was over-crystallized, significantly reducing the strength and water resistance of the optical fiber. In Comparative Example 7, with a drawing speed of 300, the production efficiency was low, and the decreased crystallinity resulted in reduced strength, high attenuation, and poor water resistance of the optical fiber.
Claims
1. A coating for the outer layer of a partially crystalline optical fiber, characterized in that... The composition, by weight, includes: Partially crystalline polyurethane acrylate prepolymer 90-110 parts, acrylate reactive monomer diluent 20-40 parts, photoinitiator 1-7 parts, additives 0-5 parts; The method for preparing the partially crystalline polyurethane acrylate prepolymer includes the following steps: (1) Add polyol, isocyanate and catalyst to the reaction vessel in sequence, heat to 60±2℃, and keep the temperature for 2~2.5 hours; (2) Add (meth)acrylate hydroxy ester and polymerization inhibitor, and continue the reaction at 65±2℃ for 2~3 hours until the isocyanate group content is zero, thus obtaining a partially crystalline polyurethane acrylate prepolymer; The raw materials of the partially crystalline polyurethane acrylate prepolymer, by weight, include: 80-110 parts of polycaprolactone diol, 80-100 parts of polypropylene glycol, 30-50 parts of HDI and IPDI combined, 25-35 parts of (meth)acrylate hydroxy ester, 0.1-0.4 parts of catalyst, and 0.1-0.4 parts of polymerization inhibitor. The mass ratio of HDI to IPDI is 1:(0.5~1.4); the molecular weight of the polycaprolactone diol is 1000-3000.
2. The coating for the outer layer of a partially crystalline optical fiber as described in claim 1, characterized in that, The ratio of 1000 molecular weight polycaprolactone diol to 3000 molecular weight polycaprolactone diol is (1~9):(1~9).
3. The coating for the outer layer of partially crystalline optical fibers as described in claim 1, characterized in that, The molecular weight of the polycaprolactone diol is 2000.
4. The coating for the outer layer of partially crystalline optical fibers as described in claim 1, characterized in that... The hydroxy methacrylate is one or a mixture of two or more of the following: hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, dipentaerythritol monohydroxypentamethacrylate, 2-hydroxyoctyl methacrylate, pentaerythritol trimethacrylate, glycerol dimethacrylate, 4-hydroxycyclohexyl methacrylate, trimethylolpropane dimethacrylate, and trimethylolethane dimethacrylate.
5. The coating for the outer layer of partially crystalline optical fibers as described in claim 1, characterized in that... The catalyst is one or a mixture of two or more of the following: dibutyltin dilaurate, bismuth carboxylate, bismuth isooctanoate, N,N-dimethylcyclohexylamine, bis(2-dimethylaminoethyl) ether, N,N,N',N'-tetramethylalkylene diamine, triethylamine, N,N-dimethylbenzylamine, solidamine, N-ethylmorpholine, N,N'-diethylpiperazine, triethanolamine, dimethylaminoethanol, pyridine, and N,N'-dimethylpyridine; the amount used is 0.1wt% to 1wt% of the total mass of the reactants.
6. The coating for the outer layer of a partially crystalline optical fiber as described in claim 1, characterized in that, The polymerization inhibitor is one of hydroquinone and p-hydroxyanisole; the amount used is 0.1wt% to 1wt% of the total mass of polyol, isocyanate and (meth)acrylate hydroxy ester.
7. The coating for the outer layer of a partially crystalline optical fiber as described in claim 1, characterized in that, The acrylate reactive monomer diluent is any one or a mixture of tripropylene glycol diacrylate, tripropylene glycol dimethacrylate, triethylene glycol dimethacrylate, diethylene glycol dimethacrylate, 1,4-butanediol dimethacrylate, tricyclodecanediethanol diacrylate, dioxanediol diacrylate, ethylene glycol dimethacrylate, isobornyl acrylate, isobornyl methacrylate, cyclohexyl methacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, ethoxylated trimethylolpropane triacrylate, propionyl trimethylolpropane triacrylate, propionyl glycerol triacrylate, trimethylolpropane trimethacrylate, ethoxylated trimethylolpropane trimethacrylate, pentaerythritol tetraacrylate, and bis(trimethylolpropane tetraacrylate).
8. The coating for the outer layer of a partially crystalline optical fiber as described in claim 1, characterized in that... The photoinitiator is one or a mixture of two or more of the following: 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 2-hydroxy-2-methyl-1-phenylpropanone, 1-hydroxycyclohexylbenzophenone, benzoin dimethyl ether, phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, and 2-methyl-1-(4-methylthiophenyl)-2-morpholine-1-propanone.
9. The coating for the outer layer of a partially crystalline optical fiber as described in claim 1, characterized in that... The additives include any one or any combination of defoamers, leveling agents, antioxidants, and stabilizers.
10. A method for preparing an outer coating of partially crystalline optical fiber, comprising simultaneously preparing an optical fiber surface coating during an optical fiber drawing process; wherein the surface coating adopts the outer coating of partially crystalline optical fiber as described in claim 1; wherein the drawing speed in the optical fiber drawing process is 500-2000 m / min, the curing temperature is 35-55℃, and the power of the ultraviolet curing lamp is 300-700W.
Citation Information
Patent Citations
Moisture-curable polyurethane hot melt resin composition, adhesive and article
CN104245769A
Polyurethane acrylate oligomer, preparation method thereof, coating composition and application of coating composition
CN112812265A