An organosilicon photocurable resin and a high-damping horn UV center adhesive containing the same, along with their preparation method and applications.
By using an interpenetrating network structure composed of silicone UV-curable resin and polyurethane acrylic resin, the problem of poor compatibility between silicone and acrylic resin was solved, enabling rapid curing and wide-temperature-range damping performance of the UV center adhesive for high-damping speakers, thereby improving the acoustic performance and production efficiency of the speakers.
Patent Information
- Application Number
- CN202510166710.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-02-14
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2045-02-14
AI Technical Summary
In existing technologies, silicone and acrylic resin have poor compatibility, leading to adhesive delamination. Furthermore, the hot-press coating process is complex and cannot meet the high damping requirements of a single-layer diaphragm and the need for rapid curing in factories.
An interpenetrating network structure composed of organosilicon photocurable resin, polyurethane acrylic resin, and reactive diluents containing polar groups and large side chains is adopted. Through the synergistic effect of strong hydrogen bonding and microphase separation, the damping performance of the adhesive is improved, and a UV curing process is used.
It significantly improves the damping performance of the adhesive, with a damping value tanδ > 0.3 and a damping temperature range from -50℃ to 120℃. It also achieves rapid curing, thereby improving the acoustic performance and production efficiency of the speaker.
Smart Images

Figure CN119859158B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of ultraviolet light curable adhesive technology, and relates to an organosilicon light-curable resin, a high-damping horn UV center adhesive containing the same, its preparation method, and its application. Background Technology
[0002] With the rapid development of VR, AR, and other electronic products, customers have increasingly higher demands for the audio quality of these products. They require not only high reliability but also speakers with low distortion and support for multi-scene 3D sound fields. Related research shows that adding a wide-temperature-range, high-damping adhesive to the vibration system can significantly reduce distortion in miniature speakers and improve their acoustic performance.
[0003] CN118325574A discloses an acoustic damping adhesive prepared by compounding organosilicon and acrylic resin. This adhesive is physically blended and then coated onto a composite diaphragm by hot pressing to improve the damping effect of the diaphragm. However, this process has two problems. First, pure organosilicon itself has poor compatibility with acrylic resin through simple physical blending, and after simple stirring and mixing, delamination will occur after a period of storage. Second, this adhesive is used in composite diaphragms and is not suitable for single-layer diaphragms. Furthermore, the hot pressing coating process is complex and requires baking at a high temperature of 105°C, which can easily cause diaphragm deformation.
[0004] CN102911634A discloses a central adhesive prepared by modifying polyurethane with organosilicon. The main improvement is the temperature resistance of the adhesive, but it does not improve the damping effect. Moreover, the adhesive is moisture-curing and requires a long curing time, which is difficult to meet the needs of factories for rapid curing production.
[0005] In miniature loudspeakers, the center adhesive is mainly used to bond the diaphragm and voice coil. It not only fixes the voice coil and diaphragm, but also, with its high damping, can greatly improve the electroacoustic performance of the loudspeaker, reduce distortion, and enhance the acoustic performance of the loudspeaker. Summary of the Invention
[0006] To address the shortcomings of existing technologies, the present invention aims to provide an organosilicon photocurable resin, a high-damping UV center adhesive for horns containing the same, its preparation method, and its applications. The organosilicon photocurable resin of this invention, combined with polyurethane acrylic resin, a diluent containing polar groups and large side chains, and a photoinitiator, prepares a high-damping UV adhesive with an interpenetrating polymer network (IPN). Simultaneously, through the synergistic effects of strong hydrogen bonding, high steric hindrance, and microphase separation, the damping of the adhesive is significantly improved. When applied to the center adhesive portion of a horn, it not only meets the high damping requirements of a single-layer diaphragm but also, using a UV curing process, greatly improves factory production efficiency.
[0007] To achieve this objective, the present invention adopts the following technical solution:
[0008] On one hand, the present invention provides an organosilicon photocurable resin, the organosilicon photocurable resin having the following structure:
[0009]
[0010] Where x = 0 to 1.66 (e.g., 0, 0.2, 0.4, 0.6, 0.8, 1.2, 1.4, 1.6 or 1.66), y = 0 to 1.39 (e.g., 0, 0.2, 0.4, 0.6, 0.8, 1.2 or 1.39), and n = 1 to 5 integers (e.g., 1, 2, 3, 4 or 5).
[0011] On the other hand, the present invention provides a method for preparing the organosilicon photocurable resin as described above, the method comprising the following steps:
[0012] Diethoxydimethylsilane, phenyltriethoxysilane, and vinyltriethoxysilane undergo a hydrolysis-condensation reaction to obtain the organosilicon photocurable resin.
[0013] In this invention, the reaction formula for preparing the organosilicon photocurable resin is as follows:
[0014]
[0015] Preferably, the molar ratio of diethoxydimethylsilane, phenyltriethoxysilane, and vinyltriethoxysilane is 1:(1-2):(1-3), for example 1:1:1, 1:1:1.5, 1:1:1.8, 1:1:2, 1:1:2.2, 1:1:2.5, 1:1:2.8, 1:1:3, 1:1.2:1, 1:1.2:1.2, 1:1.2:1.5, 1:1.2:1.8, 1:1.2:2, 1:1.2:2.2, 1:1.2:2.4, 1:1.2:2.6, 1:1.2:2.8, 1:1.2:3, 1:1.5:1, 1:1.5:1.2, 1:1.5:1.5, 1 :1.5:1.8, 1:1.5:2, 1:1.5:2.2, 1:1.5:2.4, 1:1.5:2.6, 1:1.5:2.8, 1:1.5:3, 1:1.8:1, 1:1.8:1.2, 1:1.8:1.5, 1:1.8:1.8, 1:1.8:2, 1:1.8:2.2, 1:1.8:2.4, 1:1.8:2.6, 1:1.8:2.8, 1:1.8:3, 1:2:1, 1:2:1.2, 1:2:1.5, 1:2:1.8, 1:2:2, 1:2:2.2, 1:2:2.4, 1:2:2.6, 1:2:2.8, 1:2:3, etc.
[0016] Preferably, the hydrolysis-condensation reaction is carried out under nitrogen protection.
[0017] Preferably, the hydrolysis-condensation reaction is carried out in the presence of an acidic catalyst.
[0018] Preferably, the acidic catalyst is a hydrochloric acid solution.
[0019] Preferably, the hydrolysis-condensation reaction is carried out at room temperature (20-35°C, for example 20°C, 25°C, 28°C, 30°C, 33°C or 35°C) for a reaction time of 48-72 hours, for example 48 hours, 50 hours, 54 hours, 56 hours, 60 hours, 64 hours, 66 hours, 70 hours or 72 hours.
[0020] On the other hand, the present invention provides a high-damping horn UV center adhesive, the high-damping horn UV center adhesive comprising the following components by weight percentage:
[0021]
[0022] In this invention, the organosilicon photocurable resin has carbon-carbon double bonds on its side chains, which can crosslink with acrylic prepolymer resin, reactive diluents, etc. Simultaneously, its side chains contain polar hydroxyl groups and large phenyl groups. The numerous polar groups can form strong hydrogen bonds with reactive diluents, reducing molecular chain movement. The large phenyl groups, due to steric hindrance, reduce the flexibility of the molecular chain, increasing frictional resistance to chain movement and improving energy dissipation, thereby enhancing the damping performance of the adhesive.
[0023] The content of the organosilicon photocurable resin in the high-damping horn UV center adhesive of the present invention can be 10%, 13%, 15%, 18%, 20%, 23%, 25%, 28%, 30%, 33%, 35%, 38%, or 40%. More preferably, it is 15% to 30%.
[0024] The content of the acrylic prepolymer resin in the high-damping horn UV center adhesive of the present invention can be 25%, 26%, 27%, 28%, 29% or 30%.
[0025] The content of the reactive diluent in the high-damping horn UV center adhesive of the present invention can be 30%, 33%, 35%, 38%, 40%, 42%, 44% or 45%, preferably 30% to 40%.
[0026] The content of the photoinitiator in the high-damping horn UV center adhesive of the present invention can be 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5% or 7%, preferably 3% to 5%.
[0027] The content of the adhesion promoter in the high-damping horn UV center adhesive of the present invention can be 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5% or 8%.
[0028] Preferably, the acrylic prepolymer resin is selected from polyurethane acrylic resin.
[0029] Preferably, the polyurethane acrylic resin includes one or a combination of at least two of the following: Taiwan Changxing Materials 61363, Taiwan Changxing Materials 61396, Songda SD810, Songda SD871, Sartoma CN9001, or Sartoma CN8003.
[0030] Preferably, the reactive diluent is selected from any one or a combination of at least two of the following: monomers containing oxygen heterocycles, monomers containing polar groups, or monomers containing long-chain structures.
[0031] Preferably, the monomer containing an oxygen heterocycle is selected from any one or a combination of at least two of isobornyl acrylate, acrylmorpholine, or tetrahydrofurfuryl acrylate.
[0032] Preferably, the monomer containing the polar group is selected from any one or a combination of at least two of 2-hydroxyethyl acrylate, acrylic acid, 4-hydroxybutyl acrylate or 2-hydroxypropyl acrylate.
[0033] Preferably, the monomer containing the long-chain structure is selected from any one or a combination of at least two of isooctyl acrylate, butyl acrylate, laurate, isodecyl acrylate, or isononyl acrylate.
[0034] Preferably, the photoinitiator is a free radical photoinitiator.
[0035] Preferably, the photoinitiator is selected from any one or a combination of at least two of (2,4,6-trimethylbenzoyl)bis(p-tolyl)phosphine oxide, diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, 1-hydroxycyclohexylphenyl ketone, 2-hydroxy-2-methyl-1-phenylpropanone, benzoin methyl ether, and ethyl 2,4,6-trimethylbenzoylphosphonate. When the initiator is a combination, it can be a mixture in any proportion.
[0036] Preferably, the adhesion promoter is selected from any one or a combination of at least two of 2-hydroxyethyl methacrylate, acrylic acid, γ-aminopropyltrimethoxysilane, and β-acryloyloxypropionic acid. When the adhesion promoter is a combination, it can be a mixture in any proportion.
[0037] On the other hand, the present invention provides a method for preparing the high-damping horn UV center adhesive as described above, the method comprising the following steps:
[0038] The high-damping horn UV center adhesive is obtained by uniformly mixing the photocurable silicone resin, acrylic prepolymer, reactive diluent, photoinitiator and adhesion promoter.
[0039] Preferably, the mixing is carried out under stirring at 20-70°C (e.g., 20°C, 25°C, 28°C, 30°C, 33°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C or 70°C).
[0040] Preferably, the mixing time is 30 min to 3 h, for example, 30 min, 40 min, 50 min, 1 h, 1.3 h, 1.5 h, 1.8 h, 2 h, 2.5 h, 2.8 h or 3 h.
[0041] Preferably, the stirring speed is 800 to 1000 rpm, for example 800 rpm, 830 rpm, 850 rpm, 880 rpm, 900 rpm, 930 rpm, 950 rpm, 980 rpm or 1000 rpm.
[0042] Preferably, the preparation method is carried out in a reaction vessel.
[0043] Preferably, the preparation method specifically includes the following steps: First, add the organosilicon photocurable resin, acrylic prepolymer resin, and reactive diluent to a reaction vessel, heat to 40-70℃ and stir for 20-50 minutes, with the stirring speed controlled at 800-1000 rpm. After the acrylic prepolymer resin dissolves, add the photoinitiator and adhesion promoter, continue stirring for 2 hours until the liquid is evenly mixed, and finally vacuum degassing and stirring for 10-30 minutes to obtain the high-damping horn UV center adhesive.
[0044] On the other hand, the present invention provides, for example, the application of high-damping horn UV center adhesive as described above in horns.
[0045] In this invention, high damping refers to a damping value tanδ > 0.3, such as 0.35, 0.38, 0.4, 0.42, 0.45, 0.5, 0.6, 0.7, 0.8, 0.9, etc.
[0046] Compared with the prior art, the present invention has the following beneficial effects:
[0047] The organosilicon photocurable resin of this invention contains carbon-carbon double bonds on its side chains, which can crosslink with UV acrylic resins, reactive diluents, etc. Simultaneously, its side chains contain polar hydroxyl groups and large phenyl groups. The numerous polar groups can form strong hydrogen bonds with acrylate monomers, reducing molecular chain movement. The large phenyl groups, due to steric hindrance, can reduce the flexibility of the molecular chain, increasing the frictional resistance of molecular chain movement and improving energy dissipation, thereby enhancing the damping performance of the adhesive.
[0048] The high-damping horn UV center adhesive of this invention utilizes the weak compatibility between organosilicon photocurable resin and acrylic prepolymer resin to achieve microphase separation after curing. Simultaneously, the hydroxyl and phenyl groups of the organosilicon photocurable resin further increase the molecular chain forces of the adhesive, thereby significantly improving the damping temperature range and maximum damping value. Test results show that the highest damping value of this adhesive can reach 0.98, and the damping temperature range (damping value > 0.3) can range from -50℃ to 120℃. Furthermore, by introducing carbon-carbon double bonds into the organosilicon, this adhesive exhibits rapid curing characteristics, greatly improving the efficiency of practical use and far exceeding that of solvent-based damping adhesives currently on the market. Attached Figure Description
[0049] Figure 1 The infrared spectrum of the organosilicon photocurable resin PSI prepared in Example 1.
[0050] Figure 2 The organosilicon photocurable resin PSI prepared in Example 1 is... 1 H-NMR spectrum.
[0051] Figure 3 The figures show the damping test results for Example 1, Comparative Example 1, Comparative Example 3, and Comparative Example 4. Detailed Implementation
[0052] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.
[0053] Preparation Example 1
[0054] A photocurable silicone resin is prepared by means of the following steps:
[0055] (1) At room temperature, under nitrogen protection, 100g of diethoxydimethylsilane, phenyltriethoxysilane, and vinyltriethoxysilane in a molar ratio of 1:1:3 and 10ml of a 37% hydrochloric acid solution were added to a reactor containing 20ml of distilled water.
[0056] (2) The mixture was stirred for 48 hours to complete the hydrolysis and condensation reaction. Then, it was filtered using a Buchner funnel to remove the gel from the mixture. The remaining solution was poured into a separatory funnel, diluted with distilled water, and then added dropwise to a large amount of cold methanol to obtain a precipitate. After filtering and separating the precipitate, it was washed three times with methanol and then dried in a vacuum at 45°C for 24 hours to obtain organosilicon photocurable resin PSI.
[0057] The prepared organosilicon photocurable resin PSI was characterized using a Fourier transform infrared spectroscopy (Nicolet 6700, Thermo Fisher Scientific, USA). Figure 1 As shown, 3300cm -1 Yes, it is the -OH vibration absorption peak, 3030~2860cm. -1 It is the absorption peak of -CH3 and -CH2, at 1600 cm⁻¹. -1 It is a characteristic absorption peak of the benzene ring, at 1018 cm⁻¹. -1 The peak at 810 cm⁻¹ is the characteristic absorption peak of -Si-O-Si, and the peak at 810 cm⁻¹ is the infrared absorption peak of -C=C-.
[0058] The prepared organosilicon photocurable resin PSI was analyzed using a Bruker AV400 nuclear magnetic resonance spectrometer (Germany). 1 Characterized by 1H-NMR, and determined using CDCl3 as the solvent. 1 H-NMR (400MHz) spectrum as follows Figure 2 As shown, the C-H3 absorption peak at 0.2 ppm is the methyl hydrogen 1 position, the absorption peaks at 5.8–6.1 ppm are the CH=CH22,3 positions on the vinyl group, and the absorption peaks at 7.1–7.8 ppm are the phenyl hydrogen positions 4, 5, and 6 as shown in the diagram. 1 H-NMR integration yields signal intensity ratios of vinyl hydrogen to methyl hydrogen and phenyl hydrogen in the polymer of 1:1.44:2.00, respectively. This leads to the conclusion that the ratio of polydimethylsiloxane, phenylsiloxane, and vinylsiloxane is 1:1.66:1.39. Therefore, x ranges from 0 to 1.66, and y ranges from 0 to 1.39.
[0059] Preparation Example 2
[0060] The difference from Preparation Example 1 is that the molar ratio of diethoxydimethylsilane, phenyltriethoxysilane, and vinyltriethoxysilane is 1:1:1.
[0061] Preparation Example 3
[0062] The difference from Preparation Example 1 is that the molar ratio of diethoxydimethylsilane, phenyltriethoxysilane, and vinyltriethoxysilane is 1:2:2.
[0063] Comparative Preparation Example 1
[0064] (1) At room temperature, under nitrogen protection, diethoxydimethylsilane and phenyltriethoxysilane are added to a reaction vessel containing an appropriate amount of distilled water in a 1:1 molar ratio and an appropriate amount of hydrochloric acid solution.
[0065] (2) The mixture was stirred for 48 hours to complete the hydrolysis-condensation reaction. Then, it was filtered using a Buchner funnel to remove the gel from the mixture. The remaining solution was poured into a separatory funnel, diluted with distilled water, and then added dropwise to a large amount of cold methanol to obtain a precipitate. After filtering and separating the precipitate, it was washed three times with methanol and then dried in a vacuum at 45°C for 24 hours to obtain organosilicon resin A.
[0066] Example 1
[0067] This embodiment provides a high-damping horn UV center adhesive, which comprises the following components by weight percentage:
[0068]
[0069] The preparation method includes the following steps: The silicone photocurable resin and polyurethane acrylate resin SD871 prepared in Example 1 are added to the stirring container of a non-invasive homogenizer. Then, an active diluent (including 10% 2-hydroxyethyl acrylate, 10% isooctyl acrylate, and 20% isobornyl acrylate) is added. Next, a photoinitiator (2,4,6-trimethylbenzoyl) bis(p-tolyl)phosphine oxide and an adhesion promoter β-acryloyloxypropionic acid are added. The stirring temperature is 25°C, the stirring environment is a vacuum environment, the stirring speed is set to revolution:rotation = 1000:600, and the stirring time is 10 minutes. The final UV adhesive is obtained.
[0070] Example 2
[0071] This embodiment provides a high-damping horn UV center adhesive, which comprises the following components by weight percentage:
[0072]
[0073] The preparation method includes the following steps: The silicone photocurable resin prepared in Preparation Example 1 and polyurethane acrylate resin SD871 prepared in Preparation Example 1 are added to the stirring container of a non-invasive homogenizer. Then, an active diluent (including 10% 2-hydroxyethyl acrylate and 30% butyl acrylate) is added, followed by a photoinitiator (2,4,6-trimethylbenzoyl)phosphine bis(p-tolyl)oxide and an adhesion promoter, acrylic acid. The stirring temperature is 25°C, the stirring environment is a vacuum environment, the stirring speed is set to revolution:rotation = 1000:600, and the stirring time is 10 minutes. The final UV adhesive is obtained.
[0074] Example 3
[0075] This embodiment provides a high-damping horn UV center adhesive, which comprises the following components by weight percentage:
[0076]
[0077] The preparation method includes the following steps: The organosilicon photocurable resin prepared in Preparation Example 1 and polyurethane acrylate resin 61363 prepared in Preparation Example 1 are added to the stirring container of a non-invasive homogenizer. Then, an active diluent (including 20% 4-hydroxybutyl acrylate and 20% acryloylmorpholine) is added, followed by the addition of a photoinitiator (2,4,6-trimethylbenzoyl)phosphine bis(p-tolyl)oxide and an adhesion promoter β-acryloyloxypropionic acid. The stirring temperature is 25°C, the stirring environment is a vacuum environment, the stirring speed is set to revolution:rotation = 1000:600, and the stirring time is 10 min. The UV adhesive is finally obtained.
[0078] Example 4
[0079] This embodiment provides a high-damping horn UV center adhesive, which comprises the following components by weight percentage:
[0080]
[0081] The preparation method includes the following steps: The organosilicon photocurable resin and polyurethane acrylate resin CN9001 prepared in Preparation Example 1 are added to the stirring container of a non-invasive homogenizer. Then, the reactive diluent isobornyl acrylate is added, followed by the photoinitiator (2,4,6-trimethylbenzoyl)phosphine bis(p-tolyl)oxide and the adhesion promoter β-acryloyloxypropionic acid. The stirring temperature is 40℃, the stirring environment is a vacuum environment, the stirring speed is set to revolution:rotation = 1000:600, and the stirring time is 10 min. The UV adhesive is finally obtained.
[0082] Example 5
[0083] This embodiment provides a high-damping horn UV center adhesive, which comprises the following components by weight percentage:
[0084]
[0085] The preparation method includes the following steps: The organosilicon photocurable resin prepared in Preparation Example 1 and polyurethane acrylate resin SD810 are added to the stirring container of a non-invasive homogenizer. Then, the reactive diluent 4-hydroxybutyl acrylate is added, followed by the photoinitiator (2,4,6-trimethylbenzoyl)phosphine bis(p-tolyl)oxide and the adhesion promoter β-acryloyloxypropionic acid. The stirring temperature is 70°C, the stirring environment is a vacuum environment, the stirring speed is set to revolution:rotation = 1000:600, and the stirring time is 10 min. The UV adhesive is finally obtained.
[0086] Example 6
[0087] This embodiment provides a high-damping horn UV center adhesive, which comprises the following components by weight percentage:
[0088]
[0089]
[0090] The preparation method includes the following steps: The organosilicon photocurable resin prepared in Preparation Example 2 and polyurethane acrylate resin CN8003 are added to the stirring container of a non-invasive homogenizer. Then, the reactive diluent isodecyl acrylate is added, followed by the photoinitiator diphenyl (2,4,6-trimethylbenzoyl)phosphine oxide and the adhesion promoter 2-hydroxyethyl methacrylate phosphate. The stirring temperature is 50°C, the stirring environment is a vacuum environment, the stirring speed is set to revolution:rotation = 1000:600, and the stirring time is 10 min. The UV adhesive is finally obtained.
[0091] Example 7
[0092] This embodiment provides a high-damping horn UV center adhesive, which comprises the following components by weight percentage:
[0093]
[0094] The preparation method includes the following steps: The organosilicon photocurable resin prepared in Preparation Example 3 and polyurethane acrylate resin CN8003 prepared in the stirring container of a non-invasive homogenizer are added, followed by the addition of the reactive diluent isodecyl acrylate, then the photoinitiator diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide and the adhesion promoter 2-hydroxyethyl methacrylate phosphate. The stirring temperature is 30°C, the stirring environment is a vacuum environment, the stirring speed is set to revolution:rotation = 1000:600, and the stirring time is 10 min. The UV adhesive is finally obtained.
[0095] Comparative Example 1
[0096] Commercially available UV adhesive 1, DELO 4086 UV adhesive from Germany, is specifically used as a center adhesive for the sound diaphragm of miniature loudspeakers. The MSDS (Material Safety Data Sheet) indicates that this UV adhesive contains polyurethane acrylic resin, N,N-dimethylacrylamide, 3,3,5-trimethylcyclohexyl acrylate, ethoxyethoxyethyl acrylate, acrylic acid, etc.
[0097] Comparative Example 2
[0098] Commercially available UV adhesive 2, Kyoritsu Chemical Co., Ltd. of Japan, product 5305R UV adhesive, is specifically designed for use as the center adhesive for speaker cones up to 10 watts. The MSDS (Material Safety Data Sheet) indicates that this UV adhesive contains polyurethane acrylate resin, isoborneol acrylate, N,N-dimethylacrylamide, hydroxyethyl methacrylate, etc.
[0099] Comparative Example 3
[0100] The only difference from Example 1 is that the silicone photocurable resin is replaced with phenyl vinyl silicone oil AM-3050 (Klamar).
[0101] Comparative Example 4
[0102] The only difference from Example 1 is that the organosilicon photocurable resin is replaced with organosilicon resin A prepared in Comparative Example 1.
[0103] The comprehensive performance comparison parameters of Examples 1-6 and Comparative Examples 1-4 are shown in Tables 1 and 2.
[0104] Tg, modulus, damping coefficient, and damping temperature range were all tested using a METTLER TOLED0 DMA instrument. The test conditions were tensile mode, sample size: 10.000mm × 2.660mm × 4.020mm, temperature range: -40℃~110℃, heating rate: 5K / min, vibration frequency: 1Hz, amplitude: 5μm, dynamic force: 10.00N, static force: 0.02N, and atmosphere: air.
[0105] Table 1
[0106]
[0107] Table 2
[0108] Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Tg / ℃ 74 49.8 45.9 57.2 Modulus / MPa@25℃ 190 13.76 210 185 Maximum damping coefficient tanδmax 0.678 1.25 0.73 0.74 tanδ>0.3 Damping temperature / ℃ 44.5~92 17.7~103.4 24.9~70.3 32.1~92.9 Damping temperature range / ℃ 47.5 85.7 45.4 60.7
[0109] As can be seen from the data in Table 1, the maximum damping coefficient tanδmax of Examples 1 to 6 all exceeded 0.95, and the damping coefficients of Examples 4 and 5 even showed overdamping phenomena of 1.192 and 1.339, respectively. At the same time, the damping temperature range of Examples 1 to 4 all exceeded 100℃, with Example 1 even showing a high damping temperature range of tanδ>0.3 across the entire working area of 167℃. In contrast, the maximum damping coefficient tanδmax of Comparative Examples 1 to 4 all exceeded 0.75 (except for Comparative Example 2), and the maximum damping temperature range was only 85.7℃, which was much smaller than the damping effect in the Examples.
[0110] A comparative study of Example 1, Comparative Example 3, and Comparative Example 4 reveals that the adhesive with the prepared organosilicon photocurable resin added has a significantly larger damping temperature range and a significantly higher maximum damping coefficient after curing compared to adhesives with other organosilicon or vinyl silicone resins. This indicates that the prepared photocurable organosilicon has a synergistic effect with other monomers and resins. Example 1 shows a double peak at -9.9℃ and 71.3℃, which is due to the phase separation structure between the photocurable organosilicon and the polyurethane acrylate.
[0111] Figure 3 These are the damping test results for Example 1, Comparative Examples 1, 3, and 4.
[0112] The applicant declares that this invention illustrates the organosilicon photocurable resin and the high-damping horn UV center adhesive containing it, as well as their preparation method and application, through the above embodiments. However, this invention is not limited to the above embodiments, that is, it does not mean that this invention must rely on the above embodiments to be implemented. Those skilled in the art should understand that any improvements to this invention, equivalent substitutions of the raw materials used in this invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of this invention.
Claims
1. A high-damping horn UV center adhesive, characterized in that, The high-damping horn UV center adhesive comprises the following components by weight percentage: Organosilicon photocurable resin 10%–40% Acrylic prepolymer resin 25%~30% Reactive diluent 30%–45% Photoinitiator 3%–7% Adhesion promoter 2%–8%; The organosilicon photocurable resin is prepared by the following method, which includes the following steps: Diethoxydimethylsilane, phenyltriethoxysilane and vinyltriethoxysilane undergo a hydrolysis-condensation reaction to obtain the organosilicon photocurable resin; The hydrolysis-condensation reaction was carried out under nitrogen protection; The hydrolysis-condensation reaction is carried out at room temperature for 48-72 hours. The organosilicon photocurable resin has the following structure: Where x is a natural number from 0 to 1.66, y is a natural number from 0 to 1.39, and n is an integer from 1 to 5; The acrylic prepolymer resin is selected from polyurethane acrylic resin; The high-damping horn UV center adhesive can meet the high-damping effect of a single-layer diaphragm.
2. The high-damping horn UV center adhesive according to claim 1, characterized in that, The molar ratio of diethoxydimethylsilane, phenyltriethoxysilane and vinyltriethoxysilane is 1:(1~2):(1~3).
3. The high-damping horn UV center adhesive according to claim 1, characterized in that, The hydrolysis-condensation reaction is carried out in the presence of an acidic catalyst.
4. The high-damping horn UV center adhesive according to claim 3, characterized in that, The acidic catalyst is a hydrochloric acid solution.
5. The high-damping horn UV center adhesive according to claim 1, characterized in that, The content of the organosilicon photocurable resin is 15% to 30%.
6. The high-damping horn UV center adhesive according to claim 1, characterized in that, The content of the active diluent is 30% to 40%.
7. The high-damping horn UV center adhesive according to claim 1, characterized in that, The content of the photoinitiator is 3% to 5%.
8. The high-damping horn UV center adhesive according to claim 1, characterized in that, The polyurethane acrylic resin includes one or a combination of at least two of the following: Taiwan Changxing Materials 61363, Taiwan Changxing Materials 61396, Songda SD810, Songda SD871, Sartoma CN9001, or Sartoma CN8003.
9. The high-damping horn UV center adhesive according to claim 1, characterized in that, The reactive diluent is selected from any one or a combination of at least two of the following: monomers containing oxygen heterocycles, monomers containing polar groups, or monomers containing long-chain structures.
10. The high-damping horn UV center adhesive according to claim 9, characterized in that, The monomer containing the oxygen heterocycle is selected from any one or a combination of at least two of isobornyl acrylate, acrylmorpholine, or tetrahydrofurfuryl acrylate.
11. The high-damping horn UV center adhesive according to claim 9, characterized in that, The monomer containing the polar group is selected from any one or a combination of at least two of 2-hydroxyethyl acrylate, acrylic acid, 4-hydroxybutyl acrylate or 2-hydroxypropyl acrylate.
12. The high-damping horn UV center adhesive according to claim 9, characterized in that, The monomer containing the long-chain structure is selected from any one or a combination of at least two of isooctyl acrylate, butyl acrylate, laurate, isodecyl acrylate, or isononyl acrylate.
13. The high-damping horn UV center adhesive according to claim 1, characterized in that, The photoinitiator is a free radical photoinitiator.
14. The high-damping horn UV center adhesive according to claim 1, characterized in that, The photoinitiator is selected from any one or a combination of at least two of the following: (2,4,6-trimethylbenzoyl)bis(p-tolyl)phosphine oxide, diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, 1-hydroxycyclohexylphenyl ketone, 2-hydroxy-2-methyl-1-phenylpropanone, benzoin methyl ether, and ethyl 2,4,6-trimethylbenzoylphosphonate.
15. The high-damping horn UV center adhesive according to claim 1, characterized in that, The adhesion promoter is selected from any one or a combination of at least two of 2-hydroxyethyl methacrylate phosphate, acrylic acid, γ-aminopropyltrimethoxysilane, and β-acryloyloxypropionic acid.
16. A method for preparing a high-damping horn UV center adhesive as described in any one of claims 1-15, characterized in that, The preparation method includes the following steps: The high-damping horn UV center adhesive is obtained by uniformly mixing the photocurable silicone resin, acrylic prepolymer, reactive diluent, photoinitiator and adhesion promoter.
17. The preparation method according to claim 16, characterized in that, The mixing is carried out under stirring at 20-70℃.
18. The preparation method according to claim 16, characterized in that, The mixing time is 30 min to 3 h.
19. The preparation method according to claim 17, characterized in that, The stirring mechanism has an orbital speed of 800-1000 rpm and a rotational speed of 600-800 rpm.
20. The preparation method according to claim 16, characterized in that, The preparation method is carried out in a reaction vessel.
21. The preparation method according to claim 16, characterized in that, The preparation method specifically includes the following steps: First, add the organosilicon photocurable resin, acrylic prepolymer resin, and reactive diluent to a reaction vessel, heat to 40-70℃ and stir for 20-50 minutes, controlling the stirring speed at 800-1000 rpm. After the acrylic prepolymer resin dissolves, add the photoinitiator and adhesion promoter, continue stirring for 2 hours until the liquid is evenly mixed, and finally vacuum degassing and stirring for 10-30 minutes to obtain the high-damping horn UV center adhesive.
22. The application of a high-damping horn UV center adhesive as described in any one of claims 1-15 in a horn.
Citation Information
Patent Citations
Loudspeaker center adhesive and preparation method thereof
CN102911634A
Preparation method of organosilicone gradient damping polymers
CN108715626A
Organosilicone modified acrylate resin and preparation method thereof and hydrophobic weatherproof slow-release modified acrylic resin coating