A method for strong oxidation activation of uranium ore in argillaceous sandstone using persulfate oxidation.

By generating strong oxidizing free radicals and uranyl sulfate ions through persulfate oxidation, the problem of uranium adsorption by clay in argillaceous sandstone uranium deposits was solved, achieving efficient and low-energy uranium leaching and improving uranium leaching rate and resource utilization.

CN120311050BActive Publication Date: 2026-11-10GUANGZHOU INSTITUTE OF GEOCHEMISTRY CHINESE ACADEMY OF SCIENCES
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202510516252.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-04-23
Publication Date
2026-11-10
Estimated Expiration
2045-04-23

AI Technical Summary

Technical Problem

Existing technologies are insufficient to effectively address the adsorption of uranium by clay minerals in argillaceous sandstone uranium deposits, resulting in low uranium leaching rates. Furthermore, traditional methods pose risks of high energy consumption and environmental pollution.

Method used

The persulfate oxidation method is adopted, which involves mixing persulfate solution with iron-containing nano-minerals to generate strong oxidizing free radicals, converting U(Ⅳ) to U(Ⅵ), and utilizing the electrostatic repulsion between uranyl sulfate ions and clay to improve uranium leaching efficiency.

Benefits of technology

It significantly improves uranium leaching rate under mild conditions, reduces clay adsorption of uranium, generates high-concentration uranium leachate, reduces energy consumption and environmental pollution risks, and improves resource utilization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention provides a strong oxidation activation method for uranium ore in argillaceous sandstone using persulfate oxidation, relating to the application of inorganic nanomaterials and uranium purification and conversion. The method includes: mixing a persulfate solution with a slurry of argillaceous sandstone uranium ore, adding iron-containing nano-minerals, and rapidly converting U(Ⅳ) in the argillaceous sandstone uranium ore into the more mobile U(Ⅵ) through an activation reaction between the iron-containing nano-minerals and persulfate. The suspension is then filtered and washed to obtain a high-concentration uranium leaching solution. The uranium ore activation method provided by this invention not only generates strong oxidizing free radicals but also forms a large number of uranyl sulfate ions, increasing the electrostatic repulsion between U(Ⅵ) and clay, thus improving uranium leaching efficiency. The leaching solution obtained by this method has a higher U(Ⅵ) concentration, lower uranium content in the leaching residue, requires a shorter activation time, and has broad applicability, meeting the activation needs of various uranium ores; it is also easy to apply on a large scale.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of inorganic nanomaterial applications and uranium purification and conversion, and relates to a strong oxidation activation method for argillaceous sandstone uranium ore using persulfate oxidation. Background Technology

[0002] Uranium ore in argillaceous sandstone is a common type of uranium deposit, where uranium minerals are often associated with clay minerals, forming a complex mineral structure. The presence of clay minerals significantly impacts uranium leaching efficiency. Clay minerals have strong adsorption capabilities, easily adsorbing and retaining uranium ions during leaching, leading to low uranium leaching rates and consequently affecting uranium resource recovery efficiency. Traditional uranium leaching methods, such as acid leaching or alkaline leaching, are often ineffective in processing argillaceous sandstone uranium ore. These methods involve lengthy leaching processes requiring high acidity and alkalinity, and the adsorption of uranium by clay minerals is difficult to overcome, resulting in uranium loss and resource waste.

[0003] Currently, although some technologies have attempted to improve leaching efficiency through chemical modification or physical methods, these methods have certain limitations. For example, they require high-temperature and strong acid environments, which not only increases energy consumption but may also lead to environmental pollution and equipment corrosion. Furthermore, most existing technologies have failed to effectively address the electrostatic interaction between clay minerals and uranyl anions, thus hindering further improvements in leaching efficiency.

[0004] Therefore, how to improve the leaching efficiency of uranium ore in argillaceous sandstone, especially while avoiding the adsorption of uranium by clay minerals, and still ensuring efficient leaching, is a technical problem that urgently needs to be solved in the field of uranium leaching. Summary of the Invention

[0005] In view of this, in order to solve the above-mentioned technical problems, the purpose of this invention is to provide a strong oxidation activation method for uranium ore in argillaceous sandstone using persulfate oxidation, relating to the field of uranium resource development technology; the method includes: mixing a persulfate solution with a slurry of argillaceous sandstone uranium ore, adding iron-containing nano-minerals, generating a large number of strongly oxidizing free radicals through the activation reaction between the iron-containing nano-minerals and persulfate, rapidly converting U(Ⅳ) in the argillaceous sandstone uranium ore into the more mobile U(Ⅵ), and then filtering and washing the suspension to obtain a high-concentration uranium leaching solution; The activation method for uranium ore in argillaceous sandstone provided by this invention not only generates strong oxidizing free radicals, but also forms a large number of uranyl sulfate ions, increasing the electrostatic repulsion between U(VI) and clay. This effectively reduces the adsorption of uranium by clay minerals, avoids uranium loss, and improves uranium leaching efficiency. The leaching solution obtained by this method has a higher U(VI) concentration and a lower uranium content in the leaching residue. Compared with traditional leaching methods, this invention improves the uranium leaching resistance of clay under mild reaction conditions, thereby increasing uranium leaching efficiency. It has the advantages of simple operation, low energy consumption, and environmental friendliness.

[0006] Currently, traditional uranium leaching methods often require the use of strong acids or oxidants, which not only poses a serious threat to the ecological environment, but also hinders uranium leaching due to the presence of clay in argillaceous sandstone uranium ore. Therefore, this invention proposes a novel method for activating uranium in argillaceous sandstone uranium ore, comprising: mixing a persulfate solution, iron-containing nanominerals, and an argillaceous sandstone uranium ore slurry; utilizing the reaction between iron ions, persulfate molecules, oxygen, and water molecules to generate various active free radicals (Equations 1-4) to oxidize U(Ⅳ) to U(Ⅵ); and utilizing the electrostatic repulsion between uranyl sulfate anions and clay to improve uranium leaching efficiency. The entire reaction process avoids the use of strong acids, achieving faster uranium leaching without increasing the leaching process steps.

[0007] S2O8 2− +2Fe 3+ →2Fe 2+ +2SO4 2− (1) S2O8 2− +Fe 2+ →Fe 3+ +SO4 •− +SO4 2− (2) SO4 •− +H2O→ • OH + HSO4 − (3) O2+Fe 2+ →Fe 3+ +O2 •− (4) To achieve the above objectives, the following technical solution is adopted: A method for strong oxidation activation of uranium ore in argillaceous sandstone using persulfate oxidation includes: After directly mixing persulfate solution, iron-containing nano-minerals, and uranium ore slurry, an activation reaction occurs under stirring. After the reaction is completed, the leachate and leaching residue are obtained by filtration.

[0008] Furthermore, the original concentration of the persulfate solution is 1~40 mmol / L; the persulfate includes at least one of ammonium persulfate, potassium persulfate, sodium persulfate, and potassium peroxymonosulfate.

[0009] Furthermore, the original concentration of the persulfate solution is 10-30 mmol / L; the uranium ore includes argillaceous sandstone uranium ore.

[0010] Furthermore, the activation method is as follows: First, the persulfate solution and uranium ore slurry are mixed, and then iron-containing nano-minerals are added under stirring. An activation reaction occurs under stirring. After the reaction is completed, the leachate and leaching residue are obtained by filtration.

[0011] Furthermore, the solid content of the uranium ore slurry is 1% to 50%; the stirring speed is 300 to 700 rpm.

[0012] Furthermore, the solid content of the uranium ore pulp is 5%–10%; the concentration of persulfate in the uranium ore pulp is 0.1–1.0 mmol / L; the iron-containing nanominerals include at least one of pyrite, magnetite, hematite, and ferrihydrite. A small amount of iron compound is added to provide Fe. 2+ / Fe 3+ The activation process is carried out under continuous stirring.

[0013] Furthermore, the concentration of persulfate in the uranium ore slurry is 0.3~0.8 mmol / L; the amount of iron-containing nano-minerals used is 0.05~0.5 g / L; and the activation reaction time is 30~60 min.

[0014] Furthermore, the amount of iron-containing nano-minerals used is 0.1~0.3 g / L.

[0015] Application of any of the above activation methods in uranium extraction by leaching.

[0016] Beneficial effects: The beneficial effects of this invention are reflected in: 1. Improve uranium leaching efficiency: Through the activation reaction of iron-containing nano-minerals and persulfate, strong oxidizing free radicals are generated, which can effectively convert U(Ⅳ) in uranium ore into more mobile U(Ⅵ). On the other hand, the sulfate ions formed during the reaction can form uranyl sulfate anions with U(Ⅵ), which enhances the electrostatic repulsion between uranium and clay minerals in argillaceous sandstone uranium ore, effectively reducing the adsorption of uranium by clay minerals, avoiding uranium loss, and improving uranium recovery rate. 2. Reduced uranium leaching time: Compared with traditional acid leaching or alkaline leaching methods, the method of this invention can complete the oxidation conversion and leaching process of uranium in a shorter time, which greatly shortens the reaction time and improves production efficiency. 3. Low energy consumption and environmental friendliness: The persulfate oxidation technology used in this invention can achieve efficient uranium leaching under relatively mild reaction conditions. It does not require the use of strong acid or high temperature environment, which reduces energy consumption and avoids the environmental pollution and equipment corrosion problems that may be caused by traditional leaching methods. It has high environmental friendliness. 4. High-concentration uranium leaching solution and low-uranium leaching residue: The method of the present invention can generate a high-concentration uranium leaching solution, while the uranium content in the leaching residue is significantly reduced, which greatly improves the utilization rate of resources and reduces the environmental burden of waste residue. This invention provides an efficient, environmentally friendly, and highly operable oxidation and activation method for uranium ore in argillaceous sandstone, offering a new technical path for the development and utilization of uranium resources and suitable for large-scale application. Detailed Implementation

[0017] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are only for explaining the invention and are not intended to limit the invention. Unless otherwise specified, specific conditions in the embodiments are performed under conventional conditions or conditions recommended by the manufacturer. Reagents or instruments used, unless otherwise specified, are all commercially available conventional products.

[0018] Example 1: The test ore was taken from a muddy sandstone uranium deposit in Inner Mongolia (uranium grade of 0.035%). It has fine grains and is associated with a large amount of illite, kaolinite, calcite and potassium feldspar.

[0019] 50 g of uranium ore powder from argillaceous sandstone was added to 1000 mL of aqueous solution and stirred continuously at 300 rpm for 10 min to obtain a homogeneous suspension. Then, 35 mL of 20 mmol / L ammonium persulfate aqueous solution was added to the suspension and stirred continuously for 10 min. Finally, 0.1 g of pyrite was added to the suspension and stirred continuously for 30 min. The leaching system was then filtered, and the leaching residue was digested using a digestion method. The uranium content in the digestion solution was then determined by ICP-OES, and the results showed that the uranium content in the leaching residue was 0.005%.

[0020] Example 2: The test ore was taken from a muddy sandstone uranium deposit in Inner Mongolia (uranium grade of 0.035%). It has fine grains and is associated with a large amount of illite, kaolinite, calcite and potassium feldspar.

[0021] 50 g of uranium ore powder from argillaceous sandstone was added to 1000 mL of aqueous solution and stirred continuously at 300 rpm for 10 min to obtain a homogeneous suspension. Then, 30 mL of a 30 mmol / L potassium persulfate composite salt solution was added to the suspension and stirred continuously for 10 min. Finally, 0.2 g of magnetite was added to the suspension and stirred continuously for 30 min. The leaching system was then filtered, and the leaching residue was digested using a digestion method. The uranium content in the digestion solution was then determined by ICP-OES, and the results showed that the uranium content in the leaching residue was 0.002%.

[0022] Example 3: The test ore was taken from a muddy sandstone uranium deposit in Inner Mongolia (uranium grade of 0.035%). It has fine grains and is associated with a large amount of illite, kaolinite, calcite and potassium feldspar.

[0023] 50 g of uranium ore powder from argillaceous sandstone was added to 1000 mL of aqueous solution and stirred continuously at 300 rpm for 10 min to obtain a homogeneous suspension. Then, 25 mL of a 25 mmol / L potassium persulfate aqueous solution was added to the suspension and stirred continuously for 10 min. Finally, 0.15 g of hematite was added to the suspension and stirred continuously for 30 min. The leaching system was then filtered, and the leaching residue was digested using a digestion method. The uranium content in the digestion solution was then determined by ICP-OES, and the results showed that the uranium content in the leaching residue was 0.004%.

[0024] Example 4: The test ore was taken from a muddy sandstone uranium deposit in Inner Mongolia (uranium grade of 0.035%). It has fine grains and is associated with a large amount of illite, kaolinite, calcite and potassium feldspar.

[0025] 50 g of uranium ore powder from argillaceous sandstone was added to 1000 mL of aqueous solution and stirred continuously at 300 rpm for 10 min to obtain a homogeneous suspension. Then, 50 mL of a 10 mmol / L sodium persulfate aqueous solution was added to the suspension and stirred continuously for 10 min. Finally, 0.35 g of ferrohydrate was added to the suspension and stirred continuously for 30 min. The leaching system was then filtered, and the leaching residue was digested using a digestion method. The uranium content in the digestion solution was then determined by ICP-OES, and the results showed that the uranium content in the leaching residue was 0.005%.

[0026] Comparative Example 1: The test ore was taken from a muddy sandstone uranium deposit in Inner Mongolia (uranium grade of 0.035%). It has fine grains and is associated with a large amount of illite, kaolinite, calcite and potassium feldspar.

[0027] 50 g of uranium ore powder from argillaceous sandstone was added to 1000 mL of aqueous solution and stirred continuously at 300 rpm for 10 min to obtain a homogeneous suspension. Then, 50 mL of sulfuric acid solution was added to the suspension and stirred continuously for 30 min. Finally, the leaching system was filtered, and the leaching residue was digested using a digestion method. The uranium content in the digestion solution was then determined using ICP-OES, and the calculated content in the leaching residue was 0.016%.

[0028] Comparative Example 2: The test ore was taken from a muddy sandstone uranium deposit in Inner Mongolia (uranium grade of 0.035%). It has fine grains and is associated with a large amount of illite, kaolinite, calcite and potassium feldspar.

[0029] 50 g of uranium ore powder from argillaceous sandstone was added to 1000 mL of aqueous solution and stirred continuously at 300 rpm for 10 min to obtain a homogeneous suspension. Then, 20 mL of potassium permanganate solution was added to the suspension, and stirring continued for 30 min. Finally, the leaching system was filtered, and the leaching residue was digested. The uranium content in the digestion solution was then determined using ICP-OES, and the calculated content in the leaching residue was 0.009%.

[0030] Comparative Example 3: The test ore was taken from a muddy sandstone uranium deposit in Inner Mongolia (uranium grade of 0.035%). It has fine grains and is associated with a large amount of illite, kaolinite, calcite and potassium feldspar.

[0031] 50 g of uranium ore powder from argillaceous sandstone was added to 1000 mL of aqueous solution and stirred continuously at 300 rpm for 10 min to obtain a homogeneous suspension. Then, 35 mL of a 20 mmol / L ammonium persulfate aqueous solution was added to the suspension and stirred continuously for 40 min. The leaching system was then filtered, and the leaching residue was digested using a digestion method. The uranium content in the digestion solution was then determined by ICP-OES, and the results showed that the uranium content in the leaching residue was 0.029%.

[0032] Comparative Example 4: The test ore was taken from a muddy sandstone uranium deposit in Inner Mongolia (uranium grade of 0.035%). It has fine grains and is associated with a large amount of illite, kaolinite, calcite and potassium feldspar.

[0033] 50 g of uranium ore powder from argillaceous sandstone was added to 1000 mL of aqueous solution and stirred continuously at 300 rpm for 10 min to obtain a homogeneous suspension. 0.1 g of pyrite was added to the suspension and stirred continuously for 40 min. The leaching system was then filtered, and the leaching residue was digested using a digestion method. The uranium content in the digestion solution was then determined by ICP-OES, and the results showed that the uranium content in the leaching residue was 0.032%.

[0034] The U content in the leaching residue of each case is shown in Table 1: Table 1. U content in leaching residue from each case In summary, the strong oxidation activation method for uranium ore in argillaceous sandstone using persulfate oxidation provided by this invention is based on the oxidation reaction between persulfate, iron-containing nano-minerals, water and oxygen to generate a variety of free radicals with strong oxidizing properties, thereby realizing the oxidation of U(Ⅳ) in argillaceous sandstone uranium ore, and utilizing the electrostatic repulsion between uranyl sulfate ions and clay to improve the leaching efficiency of uranium elements.

[0035] This invention provides a method for activating uranium ore in argillaceous sandstone based on persulfate oxidation technology. By mixing a persulfate solution with iron-containing nano-minerals and a slurry, highly reactive sulfate radicals, hydroxyl radicals, and superoxide radicals are generated, rapidly oxidizing tetravalent uranium to hexavalent uranium. The electrostatic repulsion between uranyl sulfate and clay reduces the clay's adsorption of uranium. This method does not require a high-temperature, high-pressure environment, avoids the use of strong acids or highly toxic oxidants, reduces environmental pollution, and improves operational safety and environmental friendliness. Compared to traditional methods, this technology has stronger oxidation capacity and shorter activation time. Its green, efficient, and easily scalable characteristics make it of significant application value in uranium resource development, providing a superior technical guarantee for nuclear energy supply.

[0036] The above description is not intended to limit the present invention in any way. Although the present invention has been disclosed through the above embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some changes or modifications to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.

Claims

1. A method for strong oxidation activation of uranium ore in argillaceous sandstone using persulfate oxidation, characterized in that, The activation method includes: After directly mixing persulfate solution, iron-containing nano-minerals and uranium ore slurry, an activation reaction occurs under stirring. After the reaction is completed, the leachate and leaching residue are obtained by filtration. The uranium ore slurry is a slurry of argillaceous sandstone uranium ore that has been crushed and screened, with a particle size of less than 0.74 micrometers, and contains montmorillonite, kaolinite, illite clay; The iron-containing nanominerals include at least one of pyrite, magnetite, hematite, and ferrihydrite.

2. The method for strong oxidation activation of uranium ore in argillaceous sandstone using persulfate oxidation as described in claim 1, characterized in that, The original concentration of the persulfate solution is 1-40 mmol / L; the persulfate includes at least one of ammonium persulfate, potassium persulfate, sodium persulfate, and potassium peroxymonosulfate.

3. The method for strong oxidation activation of uranium ore in argillaceous sandstone using persulfate oxidation as described in claim 1, characterized in that, The original concentration of the persulfate solution was 10-30 mmol / L.

4. The method for strong oxidation activation of uranium ore in argillaceous sandstone using persulfate oxidation as described in claim 1, characterized in that, The activation method is as follows: First, the persulfate solution and uranium ore slurry are mixed, and then iron-containing nano-minerals are added under stirring. An activation reaction occurs under stirring. After the reaction is completed, the leachate and leaching residue are obtained by filtration.

5. The method for strong oxidation activation of uranium ore in argillaceous sandstone using persulfate oxidation as described in claim 1, characterized in that, The solid content of the uranium ore slurry is 1% to 50%; the stirring speed is 300 to 700 rpm.

6. The method for strong oxidation activation of uranium ore in argillaceous sandstone using persulfate oxidation as described in claim 1, characterized in that, The solid content of the uranium ore slurry is 5%~10%; the concentration of persulfate in the uranium ore slurry is 0.1~1.0 mmol / L.

7. The method for strong oxidation activation of uranium ore in argillaceous sandstone using persulfate oxidation as described in claim 1, characterized in that, The concentration of persulfate in the uranium ore slurry is 0.3~0.8 mmol / L; the amount of iron-containing nano-minerals used is 0.05~0.5 g / L; and the activation reaction time is 30~60 min.

8. The method for strong oxidation activation of uranium ore in argillaceous sandstone using persulfate oxidation as described in claim 1, characterized in that, The amount of iron-containing nano-minerals used is 0.1~0.3 g / L.

9. The application of the activation method as described in any one of claims 1-8 in uranium leaching for uranium extraction.

Citation Information

Patent Citations

  • Comprehensive extraction method of complex uranium-molybdenum ore

    CN115852140A