Solid iron-containing waste treatment system and application method thereof
Through the solid iron-containing waste treatment system, the combined process of blocking, crushing and reducing and reconstruction electric furnaces is used to solve the problem of processing high-iron powder such as steel slag and red mud, and achieve high-value and low-energy consumption production results.
Patent Information
- Application Number
- CN202510698358.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-28
- Publication Date
- 2025-07-18
AI Technical Summary
In the prior art, the treatment process of high-iron powder such as steel slag and red mud has not been reported, resulting in problems with finished product quality and energy consumption, and a lack of high-value and low-energy treatment methods.
It provides a solid iron-containing waste treatment system, including a blocking device, a crushing device, a silo and a reduction and reconstruction electric furnace. Through fuel addition technology and thermal crushing into the furnace, the coordinated disposal of steel slag, red mud, etc. is realized. Two reduction and reconstruction electric furnaces are used to operate alternately, maximizing the use of high-temperature heat of the arc to form continuous and low-energy production of inorganic fiber materials.
It realizes high-value disposal of solid iron-containing waste, reduces energy consumption, ensures the quality of finished products, and ensures the continuity and safety of production.
Smart Images

Figure CN120325650A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of waste treatment, and particularly to a solid iron-containing waste treatment system and an application method thereof. Background Art
[0002] Currently, the commonly used inorganic fiber thermal insulation materials are mainly mineral wool, rock wool, ceramic fiber, etc. The production process mainly involves melting basalt, fly ash, tailings or hot blast furnace slag, etc. using an electric furnace, and then performing fiber-forming treatment on the molten slag using a centrifuge or a high-speed jet nozzle. Relatively few are prepared using steel slag, red mud, or the combination of the two. In addition, the existing electric furnace process mainly feeds cold materials or hot slag into the furnace, and there are no relevant reports on the supporting treatment processes and equipment for powders such as steel slag and red mud after iron separation. The above-mentioned processes have a significant impact on the quality and energy consumption of the finished product. Therefore, it is of great significance to develop processes and equipment that can co-dispose of high-iron-containing powders such as steel slag and red mud, and achieve high-value and low-energy consumption disposal of such solid wastes. Summary of the Invention
[0003] The purpose of the present invention is to overcome the defects in the prior art and provide a solid iron-containing waste treatment system and an application method thereof.
[0004] In order to achieve the above-mentioned invention purpose, the present invention provides the following technical solutions:
[0005] The present invention provides a solid iron-containing waste treatment system, which includes the following systems:
[0006] A raw material treatment device and a reduction device;
[0007] The raw material treatment device includes a briquetting device and a crushing device;
[0008] The reduction device includes a silo and a reduction and reconstruction electric furnace.
[0009] Preferably, the crushing device is connected to the silo through a heat-insulating conveying device.
[0010] Preferably, the number of reduction and reconstruction electric furnaces is 2;
[0011] Slag discharging and smelting are carried out in a single reduction and reconstruction electric furnace;
[0012] Slag discharging and smelting in the two reduction and reconstruction electric furnaces are carried out alternately.
[0013] The present invention also provides an application method of the solid iron-containing waste treatment system, which includes the following steps:
[0014] (1) Feeding the solid iron-containing waste raw material into the briquetting device for briquetting treatment to obtain briquettes;
[0015] (2) Feed the bulk materials into a crushing device to obtain crushed raw materials, and then transfer them to a storage bin through a heat-insulating conveying device;
[0016] (3) Add the crushed raw materials in the storage bin into a reduction and reconstruction electric furnace, and add a modifying agent and a reducing agent for smelting to obtain ferrosilicon molten iron and slag, thus completing the treatment.
[0017] Preferably, the solid iron-containing waste raw materials in step (1) include solid iron-containing waste, waste from the non-ferrous industry, and fuel;
[0018] The mass of the fuel ≤ 10% of the mass of the solid iron-containing waste raw materials.
[0019] Preferably, the briquetting treatment in step (1) is cold-state forming or hot-state forming;
[0020] The pressure for the cold-state forming is 10 - 40 MPa;
[0021] The temperature for the hot-state forming ≤ 1500 °C, and the time ≤ 60 min;
[0022] The mass proportion of FeO in the bulk materials ≥ 5%.
[0023] Preferably, the working temperature of the crushing device in step (2) ≤ 1100 °C;
[0024] The particle size of the crushed raw materials is 5 - 60 mm.
[0025] Preferably, the working temperature of the heat-insulating conveying device in step (2) ≥ 500 °C.
[0026] Preferably, the reducing agent in step (3) includes coke; the modifying agent includes one or several of iron tailings, fly ash, waste refractory containing alumina, waste refractory containing silica, waste refractory containing magnesia, and waste refractory containing calcium oxide;
[0027] The particle size of the reducing agent is 5 - 20 mm, and the particle size of the modifying agent is 3 - 15 mm;
[0028] The mass ratio of the crushed raw materials, the reducing agent, and the modifying agent is 10:1 - 5:1 - 5.
[0029] Preferably, the temperature for the smelting in step (3) ≤ 2500 °C, and the time ≤ 2 h.
[0030] The present invention provides a solid iron-containing waste treatment system, which includes the following systems: a raw material treatment device and a reduction device; the raw material treatment device includes a briquetting device and a crushing device; the reduction device includes a silo and a reduction and reconstruction electric furnace. The present invention also provides an application method of the solid iron-containing waste treatment system, which includes the following steps: (1) feeding the solid iron-containing waste raw material into the briquetting device for briquetting treatment to obtain briquettes; (2) feeding the briquettes into the crushing device to obtain crushed raw materials, and then transferring them to the silo through a heat-insulating conveying device; (3) adding the crushed raw materials in the silo into the reduction and reconstruction electric furnace, and adding a modifier and a reducing agent for smelting to obtain silicon-containing molten iron and slag, thus completing the treatment.
[0031] In the present invention, solid wastes from the steel industry, non-ferrous industry wastes, fuels, etc. are mixed, subjected to artificial briquetting treatment, and raw materials with qualified particle sizes are obtained through crushing and hot screening processes. Then, they are transferred to the upper silo of the reduction and reconstruction electric furnace through a heat-insulating conveying device, and the raw materials are added into the reduction and reconstruction electric furnace through a feeding pipeline. After smelting, silicon-containing molten iron and high-temperature slag are obtained. The silicon-containing molten iron can be returned to the steel production process or used to produce pig iron, and the high-temperature slag is used to prepare inorganic fiber materials by centrifugation or injection.
[0032] The present invention mainly aims at comprehensively utilizing solid wastes generated or stored in the steel and non-ferrous industries. Different from the prior art of feeding cold materials into the furnace, in the present invention, through the technology of separate addition of fuel, fuel is first added to the solid iron-containing waste raw material, which facilitates subsequent temperature-raising smelting. Through hot crushing, screening and hot charging into the furnace, the heat-generating agent function of the fuel is maximized, heat loss is prevented, costs are reduced, and energy consumption in subsequent smelting processes is saved. At the same time, this process uses two reduction and reconstruction electric furnaces to alternately produce by submerged arc smelting and electrode injection-assisted feeding methods, making the most of the high-temperature heat of the electric arc, strengthening the formation and homogenization of the molten pool, and realizing continuous low-energy consumption production of inorganic fiber materials.
[0033] Through artificial briquetting pretreatment and supplemented by the technology of separate addition of fuel, the present invention realizes the co-disposal of solid wastes. During the operation process, under the support of the technology of separate addition of fuel and the corresponding briquetting process, the raw materials are gradually heated up and finally hot charged into the furnace, making the most possible use of the chemical energy and heat energy of the fuel, and realizing the energy conservation and safe operation of the overall process. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 is a schematic diagram of the solid iron-containing waste treatment system of the present invention;
[0035] Figure 2 is a schematic diagram of the application process of the solid iron-containing waste treatment system of the present invention. DETAILED DESCRIPTION OF THE INVENTION
[0036] The present invention provides a solid iron-containing waste treatment system, which comprises the following systems:
[0037] A raw material treatment device and a reduction device;
[0038] The raw material treatment device comprises a briquetting device and a crushing device;
[0039] The reduction device comprises a silo and a reduction and reconstruction electric furnace.
[0040] In the present invention, the crushing device is connected to the silo through a heat-insulating conveying device.
[0041] In the present invention, the number of the reduction and reconstruction electric furnaces is 2.
[0042] In the present invention, the reduction and reconstruction electric furnace is provided with a tapping hole and a slag tapping hole, the slag tapping hole is on the upper side, and the tapping hole is on the lower side.
[0043] In the present invention, slag tapping and smelting are carried out in a single reduction and reconstruction electric furnace.
[0044] In the present invention, slag tapping and smelting in the two reduction and reconstruction electric furnaces are carried out alternately.
[0045] In the present invention, during the operation of the two reduction and reconstruction electric furnaces, charging and smelting cannot be carried out simultaneously. When one electric furnace is tapping slag, the other electric furnace must be smelting. The slag tapping cycle and the smelting cycle are kept consistent in time. The present invention adopts two electric furnaces to carry out alternately, so that slag tapping can be carried out continuously, thereby ensuring the continuous operation of the fiber-forming system.
[0046] The schematic diagram of the solid iron-containing waste treatment system of the present invention is as Figure 1 shown.
[0047] Figure 1 In the figure, 1 is a briquetting device, 2 is a crushing device, 3 is a heat-insulating conveying device, 4 is a silo, 5 is a reduction and reconstruction electric furnace 1, and 6 is a reduction and reconstruction electric furnace 2.
[0048] The present invention provides an application method of the solid iron-containing waste treatment system, which comprises the following steps:
[0049] (1) Feeding the solid iron-containing waste raw material into the briquetting device for briquetting treatment to obtain briquettes;
[0050] (2) Feeding the briquettes into the crushing device to obtain crushed raw materials, and then transferring them to the silo through the heat-insulating conveying device;
[0051] (3) Adding the crushed raw materials in the silo into the reduction and reconstruction electric furnace, and adding a modifying agent and a reducing agent for smelting to obtain silicon-containing molten iron and molten slag, thus completing the treatment.
[0052] In the present invention, the solid iron-containing waste raw material in step (1) includes solid iron-containing waste, non-ferrous industry waste, and fuel.
[0053] In the present invention, the solid iron-containing waste includes one or more of steel slag, refining slag, blast furnace slag, blast furnace dust, converter dust, and electric furnace dust.
[0054] In the present invention, the non-ferrous industry waste includes copper slag, nickel slag, tin slag, red mud, or other solid wastes containing elements such as aluminum, silicon, iron, and calcium.
[0055] In the present invention, the fuel includes pulverized coal, coke, or biomass fuel.
[0056] In the present invention, the mass of the fuel is preferably ≤ 10% of the mass of the solid iron-containing waste raw material, more preferably ≤ 8% of the mass of the solid iron-containing waste raw material, and even more preferably ≤ 5% of the mass of the solid iron-containing waste raw material.
[0057] In the present invention, the water content of the solid iron-containing waste raw material is preferably ≤ 10%, more preferably ≤ 6%, and even more preferably ≤ 4%.
[0058] In the present invention, the pelletizing treatment in step (1) is cold forming or hot forming.
[0059] In the present invention, when cold forming is used, a binder needs to be added. The binder is a conventional choice for those skilled in the art, but it cannot contain alkali metal elements; the cold forming pressure is preferably 10 - 40 MPa, more preferably 15 - 35 MPa, and even more preferably 20 - 30 MPa; after cold forming, heat treatment is carried out. The temperature of the heat treatment is preferably ≤ 900 °C, more preferably ≤ 800 °C, and even more preferably ≤ 700 °C; the time is preferably 10 - 60 min, more preferably 20 - 50 min, and even more preferably 30 - 40 min.
[0060] In the present invention, the temperature of the hot forming is preferably ≤ 1500 °C, more preferably ≤ 800 °C, and even more preferably ≤ 700 °C; the time is preferably ≤ 60 min, more preferably ≤ 50 min, and even more preferably ≤ 40 min.
[0061] In the present invention, the mass ratio of FeO in the lump material is preferably ≥ 5%, more preferably ≥ 7%, and even more preferably ≥ 9%.
[0062] In the present invention, the working temperature of the crushing device in step (2) is preferably ≤ 1100 °C, more preferably ≤ 1000 °C, and even more preferably ≤ 900 °C.
[0063] In the present invention, the particle size of the crushed raw material is preferably 5 - 60 mm, more preferably 10 - 50 mm, and still more preferably 20 - 40 mm.
[0064] In the present invention, the operating temperature of the heat preservation and transportation device in step (2) is preferably ≥500 °C, more preferably ≥600 °C, and still more preferably ≥700 °C.
[0065] In the present invention, the reducing agent in step (3) contains coke; the modifying agent contains one or several of iron tailings, fly ash, waste refractories containing alumina, waste refractories containing silica, waste refractories containing magnesia, and waste refractories containing calcium oxide.
[0066] In the present invention, the particle size of the reducing agent is preferably 5 - 20 mm, more preferably 10 - 15 mm, and still more preferably 12 - 13 mm; the particle size of the modifying agent is preferably 3 - 15 mm, more preferably 5 - 10 mm, and still more preferably 7 - 8 mm.
[0067] In the present invention, the mass ratio of the crushed raw material, the reducing agent, and the modifying agent is preferably 10:1 - 5:1 - 5, more preferably 10:1.5 - 4.5:1.5 - 4.5, and still more preferably 10:2 - 3:2 - 3.
[0068] In the present invention, the conditioning agent is blown into the furnace through the pores of the hollow electrode by means of electrode injection with a carrier gas.
[0069] In the present invention, the temperature of the smelting in step (3) is preferably ≤2500 °C, more preferably ≤2300 °C, and still more preferably ≤2000 °C; the time is preferably ≤2 h, more preferably ≤1.8 h, and still more preferably ≤1.5 h.
[0070] In the present invention, argon is transported through the hollow electrode during the smelting process in step (3), and the flow rate of the argon is preferably 5 - 20 m 3 / h, more preferably 10 - 15 m 3 / h, and still more preferably 12 - 13 m 3 / h.
[0071] In the present invention, the function of argon is to reduce the radial temperature gradient from the center to the furnace wall in the furnace, and at the same time, it can also accelerate the flow rate of the molten slag in the furnace, accelerating the homogenization and temperature uniformity of the molten slag.
[0072] The application flow schematic diagram of the solid iron-containing waste treatment system of the present invention is as Figure 2 shown.
[0073] The technical solutions provided by the present invention will be described in detail below with reference to the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0074] Example 1
[0075] Build a solid iron-containing waste treatment system. Specifically, the briquetting device is connected to the crushing device. The crushing device is connected to the silo through a heat-insulating conveying device. The silo is connected to two reduction and reconstruction electric furnaces. In the reduction and reconstruction electric furnaces, the slag outlet is at the top and the iron outlet is at the bottom.
[0076] Using steel slag, red mud and coke as raw materials, the proportion of coke is 5% of the raw materials, the moisture content of the solid iron-containing waste raw materials is 8%, and the ratio of (calcium oxide mass + magnesium oxide mass) / (silicon dioxide mass + aluminum oxide mass) in the mixture is 1.6. After moderately granulating the above mixture with a rotary drum, it is arranged in the briquetting device through a feeding device, and then ignited for moderate sintering at a temperature of 900 °C for 50 min to control the formation of artificial lump ore with a certain strength in the mixture (where the mass proportion of FeO is 6.5%), and at the same time ensure that there is no unburned fuel in the artificial lump ore. Then, after hot crushing (at a temperature of 1000 °C) and hot screening treatment, broken raw materials with a particle size of 40 mm are obtained and transported into the silo through a heat-insulating conveying device (at a temperature of 550 °C). Then, the broken raw materials, coke and iron tailings are proportioned according to a mass ratio of 10:2:3. The particle size of the coke is 10 mm, and the particle size of the iron tailings is 10 mm. The conditioning agent is blown into the furnace through the holes of the hollow electrode by carrier gas in the way of electrode injection. After all the raw materials are added to the electric furnace, it is heated by electricity, and argon is introduced at a flow rate of 8 m 3 / h at a temperature of 1800 °C for 2 h; when a furnace finishes smelting and the slag and iron are liquid-layered in the furnace, open the slag outlet at the upper part for slag discharging and fiber-forming operation. When the slag discharging of the first furnace is about to end, ensure that the second furnace also finishes smelting and the slag and iron in the furnace are liquid-layered, and then open the second furnace for the same slag discharging to ensure the continuous operation of the fiber-forming device. When the liquid iron level in the furnace exceeds the iron outlet, carry out the iron discharging operation, and the discharged molten iron is transported to the steel production process through an iron ladle. Then, the subsequent operations are carried out in a cyclic manner by analogy.
[0077] Example 2
[0078] Using the processing system in Example 1, with steel slag, copper slag, and coke as raw materials, the proportion of coke is 5% of the raw materials, the moisture content of the solid iron-containing waste raw material is 9%, the ratio of (calcium oxide mass + magnesium oxide mass) / (silica mass + aluminum oxide mass) in the mixture is 1.5. After moderately granulating the above mixture using a rotary drum, it is arranged into a briquetting device through a feeding device, and then ignited for moderate sintering at a temperature of 800°C for 50 minutes to control the formation of artificial lump ore with a certain strength in the mixture (where the mass proportion of FeO is 5.7%), while ensuring that there is no unburned fuel in the artificial lump ore. Then, after hot crushing (at a temperature of 1100°C) and hot screening treatment, broken raw materials with a particle size of 30 mm are obtained, and are transported into the feed bin through a heat-insulating conveying device (at a temperature of 600°C). Then, the broken raw materials, coke, and fly ash are proportioned according to a mass ratio of 10:3:2. The particle size of the coke is 6 mm, and the particle size of the fly ash is 4 mm. The conditioning agent is blown into the furnace through the holes of the hollow electrode by means of electrode injection with a carrier gas. After all the raw materials are added to the electric furnace, it is electrically heated, and argon is introduced at a flow rate of 10 m 3 / h at a temperature of 2000°C for 1.8 h. When a smelting in an electric furnace is completed and the slag and iron are liquid-layered in the furnace, the upper slag tapping hole is opened for slag tapping and fiber-forming operations. When the slag tapping of the first electric furnace is about to end, ensure that the second electric furnace has also completed smelting and the slag and iron in the furnace are liquid-layered, and then open the second electric furnace for the same slag tapping to ensure the continuous operation of the fiber-forming device. When the liquid iron level in the furnace exceeds the iron notch, iron tapping operations are carried out, and the tapped molten iron is transported to the steel production process through a ladle. Subsequently, the cycle operation is carried out by analogy.
[0079] Example 3
[0080] Using the processing system in Example 1, with blast furnace slag, red mud and coke as raw materials, the proportion of coke is 6% of the raw materials, the moisture content of the solid iron-containing waste raw material is 9%, the ratio of (calcium oxide mass + magnesium oxide mass) / (silicon dioxide mass + aluminum oxide mass) in the mixed material is 1.5. The mixed material is directly cold-consolidated into pellets by a pair-roll pelletizer under a pressure of 30 MPa. There is no need to use a rotary drum for moderate granulation. The cold-consolidated pellets are subjected to high-temperature roasting operation using a continuous belt drying equipment, ensuring that the temperature of the cold-consolidated pellets is 700 °C and the treatment time is 30 minutes to ensure that there is no unburned fuel in the pellets (where the mass ratio of FeO is 5.5%). Then, after hot crushing (at a temperature of 900 °C) and hot screening, broken raw materials with a particle size of 40 mm are obtained and transported into the feed bin through a heat-insulating conveying device (at a temperature of 650 °C). Then, batching is carried out according to the mass ratio of broken raw materials, coke and fly ash of 10:1:3. The particle size of the coke is 18 mm and the particle size of the fly ash is 6 mm. The conditioning agent is blown into the furnace through the holes of the hollow electrode by means of electrode injection with a carrier gas. After all the raw materials are added to the electric furnace, it is powered on for heating, and argon is introduced at a flow rate of 12 m 3 / h, the temperature is 2400 °C, and the time is 1.5 h; when a smelting in an electric furnace is completed and the slag and iron are liquid-layered in the furnace, the upper slag tapping hole is opened for slag tapping and fiber-forming operation. When the slag tapping of the first electric furnace is about to end, ensure that the second electric furnace has also completed smelting and the slag and iron in the furnace are liquid-layered, and then open the second electric furnace for the same slag tapping to ensure the continuous operation of the fiber-forming device. When the liquid iron level in the furnace exceeds the iron notch, iron tapping operation is carried out, and the tapped molten iron is transported to the steel production process through an iron ladle. Subsequently, the cycle operation is carried out by analogy.
[0081] Example 4
[0082] Using the processing system in Example 1, with blast furnace slag, red mud and coke as raw materials, the proportion of coke is 6% of the raw materials, the moisture content of the solid iron-containing waste raw material is 9%, the ratio of (calcium oxide mass + magnesium oxide mass) / (silicon dioxide mass + aluminum oxide mass) in the mixed material is 1.4. The mixed material is directly cold-consolidated and formed by a pair-roll pelletizer under a pressure of 40 MPa. There is no need to use a rotary drum for moderate granulation. The pellets after cold-consolidated forming are subjected to high-temperature roasting operation by a continuous belt drying equipment, ensuring that the temperature of the cold-consolidated pellets is 800 °C and the treatment time is 40 minutes to ensure that there is no unburned fuel in the pellets (where the mass ratio of FeO is 5.3%). Then, after hot crushing (at a temperature of 1000 °C) and hot screening treatment, crushed raw materials with a particle size of 15 mm are obtained and transported into the feed bin through a heat-insulating conveying device (at a temperature of 700 °C). Then, batching is carried out according to the mass ratio of crushed raw materials, coke and iron tailings of 10:4:5. The particle size of the coke is 8 mm and the particle size of the iron tailings is 5 mm. The conditioning agent is blown into the furnace through the holes of the hollow electrode by means of electrode injection with a carrier gas. After all the raw materials are added to the electric furnace, power is supplied for heating, and argon is introduced at a flow rate of 15 m 3 / h at a temperature of 2500 °C for 2 h; when a smelting in an electric furnace is completed and the slag and iron are liquid-layered in the furnace, the upper slag tapping hole is opened for slag tapping and fiber-forming operation. When the slag tapping of the first electric furnace is about to end, ensure that the second electric furnace has also completed smelting and the slag and iron in the furnace are liquid-layered, and then open the second electric furnace for the same slag tapping to ensure the continuous operation of the fiber-forming device. When the liquid iron level in the furnace exceeds the iron notch, tapping operation is carried out, and the tapped molten iron is transported to the steel production process through a ladle. Subsequently, the cycle operation is carried out by analogy.
[0083] The component analysis of the finished fibers and molten iron prepared in Examples 1 to 4 is carried out. The component records of the finished fibers are shown in Table 1, and the component records of the molten iron are shown in Table 2.
[0084] Table 1 Component of Finished Fibers
[0085]
[0086]
[0087] Table 2 Component of Molten Iron
[0088] TFe (%) C(%) Si (%) Ti (%) S(%) Example 1 92.87 4.39 0.32 0.0497 0.419 Example 2 91.33 4.55 0.26 0.0453 0.387 Example 3 93.16 4.21 0.23 0.0488 0.453 Example 4 92.42 4.52 0.37 0.0491 0.441
[0089] The above is only the preferred embodiment of the present invention. It should be noted that for those of ordinary skill in the art, without departing from the principle of the present invention, several improvements and refinements can be made, and these improvements and refinements should also be regarded as the protection scope of the present invention.
Claims
1. A solid iron-containing waste treatment system, characterized in that, The following systems are included: A raw material processing device and a reduction device; The raw material processing device includes a briquetting device and a crushing device; The reduction device includes a silo and a reduction and reconstruction electric furnace.
2. The solid iron-containing waste treatment system according to claim 1, wherein The crushing device is connected to the silo through a heat-insulating conveying device.
3. The solid iron-containing waste treatment system according to claim 2, wherein The number of the reduction and reconstruction electric furnaces is two; Slag discharging and smelting are carried out in a single reduction and reconstruction electric furnace; Slag discharging and smelting in the two reduction and reconstruction electric furnaces are carried out alternately.
4. The application method of the solid iron-containing waste treatment system according to any one of claims 1 to 3, characterized in that, The following steps are included: (1) Feed the solid iron-containing waste raw material into the briquetting device for briquetting treatment to obtain briquettes; (2) Feed the briquettes into the crushing device to obtain crushed raw materials, and then transfer them to the silo through the heat-insulating conveying device; (3) Add the crushed raw materials in the silo into the reduction and reconstruction electric furnace, and add a modifying agent and a reducing agent for smelting to obtain silicon-containing molten iron and molten slag, thus completing the treatment.
5. The application method of the solid iron-containing waste treatment system according to claim 4, characterized in that In step (1), the solid iron-containing waste raw material includes solid iron-containing waste, waste from the non-ferrous industry, and fuel; The mass of the fuel ≤ 10% of the mass of the solid iron-containing waste raw material.
6. The application method of the solid iron-containing waste treatment system according to claim 5, characterized in that The briquetting treatment in step (1) is cold forming or hot forming; The pressure of the cold forming is 10 - 40 MPa; The temperature of the hot forming ≤ 1500 °C, and the time ≤ 60 min; The mass ratio of FeO in the briquettes ≥ 5%.
7. The application method of the solid iron-containing waste treatment system according to claim 6, characterized in that In step (2), the working temperature of the crushing device ≤ 1100 °C; The particle size of the crushed raw materials is 5 - 60 mm.
8. The application method of the solid iron-containing waste treatment system according to claim 7, characterized in that In step (2), the working temperature of the heat-insulating conveying device ≥ 500 °C.
9. The application method of the solid iron-containing waste treatment system according to claim 8, characterized in that In step (3), the reducing agent includes coke; the modifying agent includes one or several of iron tailings, fly ash, waste refractories containing alumina, waste refractories containing silica, waste refractories containing magnesia, and waste refractories containing calcium oxide; The particle size of the reducing agent is 5 - 20 mm, and the particle size of the modifying agent is 3 - 15 mm; The mass ratio of the crushed raw materials, the reducing agent, and the modifying agent is 10:1 - 5:1 - 5.
10. The application method of the solid iron-containing waste treatment system according to claim 9, characterized in that, In step (3), the temperature of the smelting ≤ 2500 °C, and the time ≤ 2 h.