A high wear-resistant zirconia-coated silicon carbide material and its preparation method

By introducing a zirconium oxide coating and a sheet-like graphene structure into silicon carbide materials, the oxidation and wear problems of silicon carbide ceramics in high-temperature and low-oxygen environments have been solved, thereby improving the long-term wear resistance and oxidation resistance of the materials.

CN120365074BActive Publication Date: 2026-11-17SUZHOU YIBEI HIGH TEMPERATURE TECH MATERIALS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510356667.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-03-25
Publication Date
2026-11-17
Estimated Expiration
2045-03-25

AI Technical Summary

Technical Problem

Silicon carbide ceramics have poor oxidation resistance in high-temperature and low-oxygen environments, which makes them prone to oxidation and wear in chemical high-temperature fluid pipelines, volutes, nozzles and other applications, thus affecting their wear resistance.

Method used

High wear-resistant zirconia-coated silicon carbide material is used. By using silicon carbide and zirconia coatings of different particle sizes in the core layer, combined with sheet graphene and polytetrafluoroethylene, a multi-layer structure is formed to improve the connection strength and wear resistance.

Benefits of technology

It enhances the long-term wear resistance and service life of the material, especially exhibiting excellent oxidation resistance and wear resistance in high-temperature and low-oxygen environments.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This application relates to a high wear-resistant zirconia-coated silicon carbide material and its preparation method, comprising a core layer and a coating. The core layer consists of the following raw materials in parts by weight: 45-85 parts silicon carbide, 1-5 parts alumina, 1-5 parts magnesium oxide, 1-5 parts zirconia, 1-5 parts silicon dioxide, and 1-3 parts additives. The silicon carbide comprises large silicon carbide and small silicon carbide in a mass ratio of (2-2.3):1, with the large silicon carbide having a particle size of 0.1 mm-2 mm and the small silicon carbide having a particle size of 0.01-0.08 mm. The coating uses zirconia as the matrix material. The zirconia-coated silicon carbide material of this application is not easily damaged by heat and oxygen and maintains high wear resistance over a long period, making it suitable for use in chemical fluid pipelines.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of special wear-resistant ceramic materials, and more specifically, it relates to a high wear-resistant zirconia-coated silicon carbide material and its preparation method. Background Technology

[0002] Silicon carbide ceramics possess high hardness, high strength, high wear resistance, and good chemical stability, making them widely used in mechanical seals and wear-resistant components. Examples include silicon carbide ceramic sealing rings, silicon carbide ceramic bearings, and silicon carbide ceramic wear-resistant plates. They are also used in chemical and environmental protection fields, such as silicon carbide ceramic pipes, silicon carbide ceramic filters, and silicon carbide ceramic reactors. These components can withstand harsh environments with strong acids, strong alkalis, and organic solvents, ensuring the continuity and stability of chemical production and contributing to environmental protection and energy conservation. However, silicon carbide ceramics exhibit poor oxidation resistance in high-temperature, low-oxygen environments. When used in high-temperature fluid pipelines, volutes, and nozzles in chemical applications, oxidation leads to slag shedding and cracking, and they quickly break after being eroded by particulate matter in the fluid. Therefore, providing a silicon carbide material suitable for high-temperature, low-oxygen environments that maintains high wear resistance over a long period is of significant economic value. Summary of the Invention

[0003] To address the issue of improving the wear resistance of silicon carbide ceramics under high temperature and low oxygen conditions, this application provides a high wear-resistant zirconia-coated silicon carbide material and its preparation method.

[0004] In a first aspect, this application provides a high wear-resistant zirconia-coated silicon carbide material, comprising a core layer and a coating. The core layer comprises the following raw materials in parts by weight: 45-85 parts silicon carbide, 1-5 parts alumina, 1-5 parts magnesium oxide, 1-5 parts zirconia, 1-5 parts silicon dioxide, and 1-3 parts additives. The silicon carbide comprises large silicon carbide and small silicon carbide in a mass ratio of (2-2.3):1. The large silicon carbide has a particle size of 0.1 mm-2 mm, and the small silicon carbide has a particle size of 0.01-0.08 mm. The coating uses zirconia as the base material.

[0005] By adopting the above technical solution, large-diameter silicon carbide and small-diameter silicon carbide are used together. The small-diameter silicon carbide achieves better filling within the matrix, resulting in a denser core layer that is less susceptible to oxygen intrusion. After uniform mixing, the large-diameter silicon carbide on the surface has certain protrusions, increasing the adhesion strength of the coating and providing better protection for the core layer with the zirconium oxide coating. By adding a certain mass of alumina, magnesium oxide, zirconium oxide, and silicon dioxide, the resulting core layer exhibits more balanced performance and good wear resistance under stress. By adding a certain mass of additives, especially tricresyl phosphate, the mixed core layer material has good ductility and flexibility, and the particles are more tightly formed during subsequent preparation and pressing, further improving the material's density and preventing heat and oxygen intrusion. By limiting the particle size and mass ratio of large and small silicon carbide, it is found that excessively large particle sizes lead to insufficient stacking of the core layer material, while excessively small particle sizes result in insufficient surface roughness. Through repeated experiments, the applicant discovered a particle size combination with good performance under this formulation.

[0006] Preferably, the silicon carbide comprises large silicon carbide and small silicon carbide in a mass ratio of (2.1-2.2):1, wherein the large silicon carbide has a particle size of 0.2 mm-1 mm and the small silicon carbide has a particle size of 0.01-0.05 mm.

[0007] In one specific implementation, the coating comprises a first coating close to the core layer and a second coating away from the core layer. The first coating comprises the following raw materials in parts by weight: 20-40 parts zirconium oxide, 15-20 parts small silicon carbide, and 5-12 parts sheet graphene. The second coating comprises the following raw materials in parts by weight: 40-50 parts zirconium oxide, 25-35 parts polytetrafluoroethylene, and 5-12 parts sheet graphene.

[0008] By adopting the above technical solution, the first coating near the core layer contains a certain mass of silicon carbide, which allows for better bonding with the core layer. A certain mass of sheet-like graphene is added to both the first and second coatings. The multi-layered stacking of sheet-like graphene provides shielding, extending the path for thermal and oxygen intrusion and further protecting the core layer, thus extending the service life of the prepared material. Simultaneously, the interlayered sheet-like graphene may achieve a certain degree of mechanical interpenetration, resulting in better short-term wear resistance of the prepared silicon carbide material. Adding a certain mass of polytetrafluoroethylene to the second coating reduces fluid adhesion and retention, further minimizing damage to the prepared material.

[0009] Secondly, this application provides a method for preparing a high wear-resistant zirconia-coated silicon carbide material, comprising the following steps: mixing core layer raw materials uniformly, drying, pressing and molding, and sintering at high temperature to obtain a core layer; mixing first coating and second coating raw materials uniformly and sequentially hot-melting them onto the surface of the core layer to obtain a zirconia-coated silicon carbide material.

[0010] By adopting the above technical solution, the preparation method is simple. At the same time, since the core layer also has a small amount of zirconium oxide as raw material, the first coating can melt a layer of zirconium oxide on the surface of the core layer after high-temperature spraying, so as to achieve better connection between the coating and the core layer. Since the core layer contains silicon carbide with different particle sizes, the surface has a certain roughness, and the coating raw material is more likely to be stably connected after being sprayed onto the surface of the core layer. By setting the zirconium oxide in the core layer and silicon carbide with different particle sizes, it is suitable for the high-temperature spraying preparation method, and the connection strength between the coating and the core layer is high.

[0011] In one specific feasible implementation, the thickness of the first coating is 0.1-10 mm, and the thickness of the second coating is 0.1-3 mm.

[0012] In one specific implementation scheme, the first coating of sheet graphene is dodecylsilane coupling agent modified sheet graphene, and the second coating of sheet graphene is octadecylsilane coupling agent modified sheet graphene.

[0013] By adopting the above technical solutions, the modified sheet graphene achieved better dispersion and orientation. Simultaneously, possibly due to the different masses of the modified sheet graphene resulting in different accelerations during the high-temperature melting process, the octadecylsilane coupling agent-modified sheet graphene and dodecylsilane coupling agent-modified sheet graphene were more densely distributed near the interface connecting the first and second coatings after high-temperature melting. This led to a denser distribution of silicon carbide raw material in the first coating near the core surface. The similar materials achieved a tighter connection, and the modified sheet graphene formed better interpenetration at the interface connecting the first and second coatings. Through modified graphene interpenetration and interlayer silicon carbide melting, the resulting zirconia-coated silicon carbide material has a dense structure, is not easily invaded by heat and oxygen, and exhibits good long-term wear resistance.

[0014] In one specific feasible implementation, the mass ratio of dodecylsilane coupling agent modified sheet graphene to octadecylsilane coupling agent modified sheet graphene is 1:(1-1.1).

[0015] By adopting the above technical solutions, at this mass ratio, the interpenetration of sheet graphene and the shielding effect on the core layer are good, and the resulting zirconia-coated silicon carbide material exhibits good long-term wear resistance.

[0016] In one specific feasible implementation, high-temperature sintering includes the following steps: holding at 800-1000℃ for 3-3.5 hours, then raising the temperature to 2000-2200℃ and holding for 3-4 hours.

[0017] By adopting the above technical solutions, sintering is complete, and the resulting material has high strength and good wear resistance.

[0018] In one specific feasible implementation, the high-temperature spraying current is 400A and the voltage is 65V.

[0019] By adopting the above technical solutions, the melting and spraying effect is good, the resulting coating is smooth and dense, the interlayer bonding strength is high, and the wear resistance is good.

[0020] In one specific feasible implementation, the powder feed rate of high-temperature melt spraying is 3-4 r / min, and the powder feed air pressure is 6.5-7 atm.

[0021] Preferably, the powder feeding speed of high-temperature melt spraying is 3.6-3.7 r / min, and the powder feeding air pressure is 6.6-6.7 atm.

[0022] By adopting the above technical solution, the melting and spraying effect is good, the resulting coating is smooth and dense, and the interlayer bonding strength is high. At the same time, it is possible that under this powder feeding speed and air pressure, the modified sheet graphene not only forms a more reasonable distribution on the surface of the material due to different acceleration magnitudes during the melting and spraying process, but also forms a certain orientation arrangement. The modified sheet graphene thus achieves better protection for the core material and further improves the long-term wear resistance of the material.

[0023] In summary, this application has the following beneficial effects: 1. This application achieves better interlayer compatibility and improves connection strength by sequentially defining the raw material settings of the core layer, the first surface layer, and the second surface layer and performing high-temperature melting and spraying. The raw material settings increase the surface roughness of the core layer and allow the interlayer sheet graphene to interpenetrate, resulting in good protection of the core layer by the surface layer. The resulting material has good long-term wear resistance.

[0024] 2. This application modifies the sheet graphene of the first and second coatings with dodecylsilane coupling agents and octadecylsilane coupling agents respectively, and limits the mass ratio, powder feeding speed and powder feeding pressure of high-temperature melting spray, thereby better adjusting the distribution of raw materials on the shelf and the orientation of sheet graphene, further improving the protection effect on the core layer and extending the service life of the prepared material. Detailed Implementation

[0025] To further aid in understanding the technical solution of the present invention, several specific embodiments are provided to describe the technical solution of the present invention in more detail. All described embodiments are only some embodiments of the present invention, not all of them; embodiments can be combined with each other, and the same or similar concepts or processes may not be repeated in some embodiments. The following embodiments are further illustrations of the present invention, but the present invention is not limited thereto.

[0026] The components used in the preparation examples in this application refer to those obtained through the preparation methods described. Unless otherwise specified, all experimental reagents are from commercially available brands or obtained through conventional preparation processes. Specifically, the dodecylsilane coupling agent has the CAS number 3069-21-4, the octadecylsilane coupling agent has the CAS number 3069-42-9, the epoxysilane has the CAS number 2530-83-8, the large silicon carbide has an average particle size of 1 mm, and the small silicon carbide has an average particle size of 0.05 mm.

[0027] Preparation Example Preparation Example 1: Dodecylsilane Coupling Agent Modified Sheet Graphene S1: Add 5g of sheet graphene and 3g of dodecylsilane coupling agent to 200g of 50vt% ethanol aqueous solution, stir evenly, adjust pH to 6, heat to 75℃ and stir for 2 hours, centrifuge, wash with ethanol and deionized water three times in sequence, and dry to obtain dodecylsilane coupling agent modified sheet graphene.

[0028] Preparation Example 2: Octadecylsilane Coupling Agent Modified Sheet Graphene S1: Add 5g of sheet graphene and 3g of octadecylsilane coupling agent to 200g of 50vt% ethanol aqueous solution, stir evenly, adjust pH to 6, heat to 75℃ and stir for 2 hours, centrifuge, wash with ethanol and deionized water three times in sequence, and dry to obtain octadecylsilane coupling agent modified sheet graphene.

[0029] Preparation Example 3: Epoxy Silane Coupling Agent Modified Sheet Graphene S1: Add 5g of sheet graphene and 3g of epoxy silane coupling agent to 200g of 50vt% ethanol aqueous solution, stir evenly, adjust pH to 6, heat to 75℃ and stir for 2 hours, centrifuge, wash with ethanol and deionized water three times in sequence, and dry to obtain epoxy silane coupling agent modified sheet graphene.

[0030] Preparation Example 4: Large Silicon Carbide Modified with Dodecylsilane Coupling Agent S1: Add 5g of large silicon carbide and 3g of dodecylsilane coupling agent to 200g of 50vt% ethanol aqueous solution, stir evenly, adjust pH to 6, heat to 75℃ and stir for 2 hours, centrifuge, wash with ethanol and deionized water three times in sequence, and dry to obtain dodecylsilane coupling agent modified large silicon carbide. Example

[0031] Example 1: This embodiment contains the following raw materials by weight: Core layer: 300g large silicon carbide, 150g small silicon carbide, 10g alumina, 50g magnesium oxide, 50g zirconium oxide, 30g silicon dioxide, 20g tricresyl phosphate; The first coating comprises the following raw materials by weight: 400g zirconium oxide, 150g small silicon carbide, and 50g sheet graphene. The second coating comprises the following raw materials by weight: 400g zirconium oxide, 250g polytetrafluoroethylene, and 120g sheet graphene.

[0032] The preparation includes the following steps: The core layer raw materials are mixed evenly, dried, pressed into shape, and held at 900℃ for 3 hours. Then, the temperature is raised to 2100℃ and sintered for 3 hours to obtain the core layer. The raw materials for the first and second coatings are mixed evenly and then sequentially sprayed onto the surface of the core layer at high temperature. The current is 400A, the voltage is 65V, the powder feeding speed is 3r / min, and the powder feeding pressure is 7atm. The thickness of the first coating is 3mm and the thickness of the second coating is 1.5mm, resulting in a high wear-resistant zirconia-coated silicon carbide material.

[0033] Example 2: This embodiment contains the following raw materials by weight: Core layer: 460g large silicon carbide, 200g small silicon carbide, 10g alumina, 50g magnesium oxide, 50g zirconium oxide, 30g silicon dioxide, 10g tricresyl phosphate; The first coating comprises the following raw materials by weight: 400g zirconium oxide, 150g large silicon carbide, and 120g sheet graphene; The second coating comprises the following raw materials by weight: 400g zirconium oxide, 250g polytetrafluoroethylene, and 50g sheet graphene.

[0034] The preparation includes the following steps: The core layer raw materials are mixed evenly, dried, pressed into shape, and held at 900℃ for 3 hours. Then, the temperature is raised to 2100℃ and sintered for 3 hours to obtain the core layer. The raw materials for the first and second coatings are mixed evenly and then sequentially sprayed onto the surface of the core layer at high temperature. The current is 400A, the voltage is 65V, the powder feeding speed is 3r / min, and the powder feeding pressure is 7atm. The thickness of the first coating is 3mm and the thickness of the second coating is 1.5mm, resulting in a high wear-resistant zirconia-coated silicon carbide material.

[0035] Example 3: This embodiment contains the following raw materials by weight: Core layer: 420g large silicon carbide, 200g small silicon carbide, 30g alumina, 30g magnesium oxide, 30g zirconium oxide, 30g silicon dioxide, 20g tricresyl phosphate; The first coating comprises the following raw materials by weight: 300g zirconium oxide, 170g small silicon carbide, and 80g sheet graphene; The second coating comprises the following raw materials by weight: 450g zirconium oxide, 300g polytetrafluoroethylene, and 120g sheet graphene.

[0036] The preparation includes the following steps: The core layer raw materials are mixed evenly, dried, pressed into shape, and held at 900℃ for 3 hours. Then, the temperature is raised to 2100℃ and sintered for 3 hours to obtain the core layer. The raw materials for the first and second coatings are mixed evenly and then sequentially sprayed onto the surface of the core layer at high temperature. The current is 400A, the voltage is 65V, the powder feeding speed is 3r / min, and the powder feeding pressure is 7atm. The thickness of the first coating is 3mm and the thickness of the second coating is 1.5mm, resulting in a high wear-resistant zirconia-coated silicon carbide material.

[0037] Example 4: This embodiment contains the following raw materials by weight: Core layer: 420g large silicon carbide, 200g small silicon carbide, 30g alumina, 30g magnesium oxide, 30g zirconium oxide, 30g silicon dioxide, 20g tricresyl phosphate; The first coating comprises the following raw materials by weight: 300g zirconium oxide, 170g small silicon carbide, and 80g sheet graphene; The second coating comprises the following raw materials by weight: 300g zirconium oxide, 170g small silicon carbide, and 80g sheet graphene.

[0038] The preparation includes the following steps: The core layer raw materials are mixed evenly, dried, pressed into shape, and held at 900℃ for 3 hours. Then, the temperature is raised to 2100℃ and sintered for 3 hours to obtain the core layer. The raw materials for the first and second coatings are mixed evenly and then sequentially sprayed onto the surface of the core layer at high temperature. The current is 400A, the voltage is 65V, the powder feeding speed is 3r / min, and the powder feeding pressure is 7atm. The thickness of the first coating is 3mm and the thickness of the second coating is 1.5mm, resulting in a high wear-resistant zirconia-coated silicon carbide material.

[0039] Example 5: This embodiment contains the following raw materials by weight: Core layer: 420g large silicon carbide, 200g small silicon carbide, 30g alumina, 30g magnesium oxide, 30g zirconium oxide, 30g silicon dioxide, 20g tricresyl phosphate; The first coating comprises the following raw materials by weight: 300g zirconium oxide, 170g silicon carbide, and 80g sheet graphene. The second coating comprises the following raw materials by weight: 450g zirconium oxide, 300g polytetrafluoroethylene, and 120g sheet graphene.

[0040] The preparation includes the following steps: The core layer raw materials are mixed evenly, dried, pressed into shape, and held at 900℃ for 3 hours. Then, the temperature is raised to 2100℃ and sintered for 3 hours to obtain the core layer. The raw materials for the first and second coatings are mixed evenly and then sequentially sprayed onto the surface of the core layer at high temperature. The current is 400A, the voltage is 65V, the powder feeding speed is 3r / min, and the powder feeding pressure is 7atm. The thickness of the first coating is 3mm and the thickness of the second coating is 1.5mm, resulting in a high wear-resistant zirconia-coated silicon carbide material.

[0041] Example 6: This embodiment contains the following raw materials by weight: Core layer: 420g large silicon carbide, 200g small silicon carbide, 30g alumina, 30g magnesium oxide, 30g zirconium oxide, 30g silicon dioxide, 20g tricresyl phosphate; The first coating comprises the following raw materials by weight: 300g of zirconium oxide, 170g of small silicon carbide, and 80g of dodecylsilane coupling agent modified sheet graphene obtained in Preparation Example 1. The second coating comprises the following raw materials by weight: 450g of zirconium oxide, 300g of polytetrafluoroethylene, and 120g of octadecylsilane coupling agent modified sheet graphene obtained in Preparation Example 2.

[0042] The preparation includes the following steps: The core layer raw materials are mixed evenly, dried, pressed into shape, and held at 900℃ for 3 hours. Then, the temperature is raised to 2100℃ and sintered for 3 hours to obtain the core layer. The raw materials for the first and second coatings are mixed evenly and then sequentially sprayed onto the surface of the core layer at high temperature. The current is 400A, the voltage is 65V, the powder feeding speed is 3r / min, and the powder feeding pressure is 7atm. The thickness of the first coating is 3mm and the thickness of the second coating is 1.5mm, resulting in a high wear-resistant zirconia-coated silicon carbide material.

[0043] Example 7: This embodiment contains the following raw materials by weight: Core layer: 420g large silicon carbide, 200g small silicon carbide, 30g alumina, 30g magnesium oxide, 30g zirconium oxide, 30g silicon dioxide, 20g tricresyl phosphate; The first coating comprises the following raw materials by weight: 300g of zirconium oxide, 170g of small silicon carbide, and 100g of dodecylsilane coupling agent modified sheet graphene obtained in Preparation Example 1. The second coating comprises the following raw materials by weight: 450g of zirconium oxide, 300g of polytetrafluoroethylene, and 100g of octadecylsilane coupling agent modified sheet graphene obtained in Preparation Example 2.

[0044] The preparation includes the following steps: The core layer raw materials are mixed evenly, dried, pressed into shape, and held at 900℃ for 3 hours. Then, the temperature is raised to 2100℃ and sintered for 3 hours to obtain the core layer. The raw materials for the first and second coatings are mixed evenly and then sequentially sprayed onto the surface of the core layer at high temperature. The current is 400A, the voltage is 65V, the powder feeding speed is 3r / min, and the powder feeding pressure is 7atm. The thickness of the first coating is 3mm and the thickness of the second coating is 1.5mm, resulting in a high wear-resistant zirconia-coated silicon carbide material.

[0045] Example 8: This embodiment contains the following raw materials by weight: Core layer: 420g large silicon carbide, 200g small silicon carbide, 30g alumina, 30g magnesium oxide, 30g zirconium oxide, 30g silicon dioxide, 20g tricresyl phosphate; The first coating comprises the following raw materials by weight: 300g of zirconium oxide, 170g of small silicon carbide, and 80g of octadecylsilane coupling agent modified sheet graphene obtained in Preparation Example 2. The second coating comprises the following raw materials by weight: 450g of zirconium oxide, 300g of polytetrafluoroethylene, and 120g of dodecylsilane coupling agent modified sheet graphene prepared in Preparation Example 1.

[0046] The preparation includes the following steps: The core layer raw materials are mixed evenly, dried, pressed into shape, and held at 900℃ for 3 hours. Then, the temperature is raised to 2100℃ and sintered for 3 hours to obtain the core layer. The raw materials for the first and second coatings are mixed evenly and then sequentially sprayed onto the surface of the core layer at high temperature. The current is 400A, the voltage is 65V, the powder feeding speed is 3r / min, and the powder feeding pressure is 7atm. The thickness of the first coating is 3mm and the thickness of the second coating is 1.5mm, resulting in a high wear-resistant zirconia-coated silicon carbide material.

[0047] Example 9: This embodiment contains the following raw materials by weight: Core layer: 420g large silicon carbide, 200g small silicon carbide, 30g alumina, 30g magnesium oxide, 30g zirconium oxide, 30g silicon dioxide, 20g tricresyl phosphate; The first coating comprises the following raw materials by weight: 300g of zirconium oxide, 170g of small silicon carbide, and 80g of dodecylsilane coupling agent modified sheet graphene obtained in Preparation Example 1. The second coating comprises the following raw materials by weight: 450g of zirconium oxide, 300g of polytetrafluoroethylene, and 120g of epoxy silane coupling agent modified sheet graphene obtained in Preparation Example 3.

[0048] The preparation includes the following steps: The core layer raw materials are mixed evenly, dried, pressed into shape, and held at 900℃ for 3 hours. Then, the temperature is raised to 2100℃ and sintered for 3 hours to obtain the core layer. The raw materials for the first and second coatings are mixed evenly and then sequentially sprayed onto the surface of the core layer at high temperature. The current is 400A, the voltage is 65V, the powder feeding speed is 3r / min, and the powder feeding pressure is 7atm. The thickness of the first coating is 3mm and the thickness of the second coating is 1.5mm, resulting in a high wear-resistant zirconia-coated silicon carbide material.

[0049] Example 10: This embodiment contains the following raw materials by weight: Core layer: 420g large silicon carbide, 200g small silicon carbide, 30g alumina, 30g magnesium oxide, 30g zirconium oxide, 30g silicon dioxide, 20g tricresyl phosphate; The first coating comprises the following raw materials by weight: 300g of zirconium oxide, 170g of small silicon carbide, and 80g of dodecylsilane coupling agent modified sheet graphene obtained in Preparation Example 1. The second coating comprises the following raw materials by weight: 450g of zirconium oxide, 300g of polytetrafluoroethylene, and 120g of dodecylsilane coupling agent modified silicon carbide obtained in Preparation Example 4.

[0050] The preparation includes the following steps: The core layer raw materials are mixed evenly, dried, pressed into shape, and held at 900℃ for 3 hours. Then, the temperature is raised to 2100℃ and sintered for 3 hours to obtain the core layer. The raw materials for the first and second coatings are mixed evenly and then sequentially sprayed onto the surface of the core layer at high temperature. The current is 400A, the voltage is 65V, the powder feeding speed is 3r / min, and the powder feeding pressure is 7atm. The thickness of the first coating is 3mm and the thickness of the second coating is 1.5mm, resulting in a high wear-resistant zirconia-coated silicon carbide material.

[0051] Example 11: This embodiment contains the following raw materials by weight: Core layer: 420g large silicon carbide, 200g small silicon carbide, 30g alumina, 30g magnesium oxide, 30g zirconium oxide, 30g silicon dioxide, 20g tricresyl phosphate; The first coating comprises the following raw materials by weight: 300g of zirconium oxide, 170g of small silicon carbide, and 100g of dodecylsilane coupling agent modified sheet graphene obtained in Preparation Example 1. The second coating comprises the following raw materials by weight: 450g of zirconium oxide, 300g of polytetrafluoroethylene, and 100g of octadecylsilane coupling agent modified sheet graphene obtained in Preparation Example 2.

[0052] The preparation includes the following steps: The core layer raw materials are mixed evenly, dried, pressed into shape, and held at 900℃ for 3 hours. Then, the temperature is raised to 2100℃ and sintered for 3 hours to obtain the core layer. The raw materials for the first and second coatings are mixed evenly and then sequentially sprayed onto the surface of the core layer at high temperature. The current is 400A, the voltage is 65V, the powder feeding speed is 3.6r / min, and the powder feeding pressure is 6.6atm. The thickness of the first coating is 3mm and the thickness of the second coating is 1.5mm, resulting in a high wear-resistant zirconia-coated silicon carbide material.

[0053] Comparative Example Comparative Example 1: This comparative example contains the following raw materials by weight: Core layer: 450g silicon carbide, 10g aluminum oxide, 50g magnesium oxide, 30g silicon dioxide, 20g tricresyl phosphate; The first coating comprises the following raw materials by weight: 400g zirconium oxide, 150g small silicon carbide, and 50g sheet graphene. The second coating comprises the following raw materials by weight: 400g zirconium oxide, 250g polytetrafluoroethylene, and 120g sheet graphene.

[0054] The preparation includes the following steps: The core layer raw materials are mixed evenly, dried, pressed into shape, and held at 900℃ for 3 hours. Then, the temperature is raised to 2100℃ and sintered for 3 hours to obtain the core layer. The raw materials for the first and second coatings are mixed evenly and then sequentially sprayed onto the surface of the core layer at high temperature. The current is 400A, the voltage is 65V, the powder feeding speed is 3r / min, and the powder feeding pressure is 7atm. The thickness of the first coating is 3mm and the thickness of the second coating is 1.5mm, resulting in a high wear-resistant zirconia-coated silicon carbide material.

[0055] Comparative Example 2: This comparative example contains the following raw materials by weight: Core layer: 300g large silicon carbide, 150g small silicon carbide, 10g alumina, 50g magnesium oxide, 50g zirconium oxide, 30g silicon dioxide, 20g tricresyl phosphate; The first coating comprises the following raw materials by weight: 550g of small silicon carbide and 50g of sheet graphene; The second coating comprises the following raw materials by weight: 550g of small silicon carbide and 50g of sheet graphene.

[0056] The preparation includes the following steps: The core layer raw materials are mixed evenly, dried, pressed into shape, and held at 900℃ for 3 hours. Then, the temperature is raised to 2100℃ and sintered for 3 hours to obtain the core layer. The raw materials for the first and second coatings are mixed evenly and then sequentially sprayed onto the surface of the core layer at high temperature. The current is 400A, the voltage is 65V, the powder feeding speed is 3r / min, and the powder feeding pressure is 7atm. The thickness of the first coating is 3mm and the thickness of the second coating is 1.5mm, resulting in a high wear-resistant zirconia-coated silicon carbide material.

[0057] Performance testing Test 1: Refer to standard GB / T 18301-2001: Test method for abrasion resistance of refractory materials at room temperature. The weight loss (g) of the high wear-resistant zirconia-coated silicon carbide materials prepared in each embodiment and comparative example was measured. The test results are summarized in Table 1.

[0058] Test 2: The high wear-resistant zirconia-coated silicon carbide materials prepared in each embodiment and comparative example were immersed in hot water at 100℃ for 120 hours, removed, dried at 100℃, and then the weight loss 2 (g) of the high wear-resistant zirconia-coated silicon carbide materials prepared in each embodiment and comparative example was repeatedly tested according to standard GB / T 18301-2001: Test method for wear resistance of refractory materials at room temperature. The change rate was calculated as (weight loss 2 - weight loss 1) / weight loss 1 × 100%, and the test results are summarized in Table 1.

[0059] Table 1 Weight loss per 1g Rate of change (%) Example 1 8.2 21.1 Example 2 8.4 21.3 Example 3 8.0 20.8 Example 4 12.4 23.5 Example 5 10.0 24.2 Example 6 6.1 16.4 Example 7 5.7 13.8 Example 8 7.2 18.4 Example 9 7.7 18.8 Example 10 12.8 26.9 Example 11 4.1 10.1 Comparative Example 1 19.2 33.1 Comparative Example 2 16.7 45.0 In conjunction with Examples 1-5, Comparative Examples 1-2, and Table 1, this application achieves higher interlayer bonding strength, better protection of the core layer, and good long-term wear resistance of the material by sequentially defining the raw material settings of the core layer, the first surface layer, and the second surface layer and performing high-temperature spraying.

[0060] In conjunction with Examples 3 and 6-11 and Table 1, this application modifies the sheet graphene of the first and second coatings with dodecylsilane coupling agents and octadecylsilane coupling agents respectively, and limits the mass ratio, powder feeding speed and powder feeding pressure of high-temperature melting spray. This better regulates the distribution of raw materials on the shelf and the orientation of sheet graphene, further improves the protection effect on the core layer, and extends the service life of the prepared material.

[0061] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of the claims of this application.

Claims

1. A highly wear-resistant zirconia-coated silicon carbide material, characterized in that: The product comprises a core layer and a coating layer. The core layer consists of the following raw materials in parts by weight: 45-85 parts silicon carbide, 1-5 parts alumina, 1-5 parts magnesium oxide, 1-5 parts zirconium oxide, 1-5 parts silicon dioxide, and 1-3 parts additives. The silicon carbide comprises large silicon carbide and small silicon carbide in a mass ratio of (2-2.3):1, wherein the large silicon carbide has a particle size of 0.1mm-2mm and the small silicon carbide has a particle size of 0.01-0.08mm. The coating layer uses zirconium oxide as the base material. The coating comprises a first coating close to the core layer and a second coating away from the core layer. The first coating comprises the following raw materials in parts by weight: 20-40 parts of zirconium oxide, 15-20 parts of small silicon carbide, and 5-12 parts of sheet graphene. The second coating comprises the following raw materials in parts by weight: 40-50 parts of zirconium oxide, 25-35 parts of polytetrafluoroethylene, and 5-12 parts of sheet graphene. The first coating consists of sheet graphene modified with dodecylsilane coupling agent, and the second coating consists of sheet graphene modified with octadecylsilane coupling agent. The coating material is applied to the core surface using a high-temperature spraying method to obtain a zirconia-coated silicon carbide material. The high-temperature spraying current is 400A and the voltage is 65V. The mass ratio of the dodecylsilane coupling agent modified sheet graphene to the octadecylsilane coupling agent modified sheet graphene is 1:(1-1.1); the powder feeding speed of the high-temperature melting spray is 3-4 r / min, and the powder feeding pressure is 6.5-7 atm.

2. A method for preparing a high wear-resistant zirconia-coated silicon carbide material as described in claim 1, characterized in that: Includes the following steps: The core layer is obtained by uniformly mixing, drying, pressing, and high-temperature sintering of the core layer raw materials. The first and second coating materials are uniformly mixed and sequentially sprayed onto the surface of the core layer at high temperature to obtain a zirconia-coated silicon carbide material.

3. The method for preparing the high wear-resistant zirconia-coated silicon carbide material according to claim 2, characterized in that: The thickness of the first coating is 0.1-10 mm, and the thickness of the second coating is 0.1-3 mm.

4. The method for preparing the high wear-resistant zirconia-coated silicon carbide material according to claim 2, characterized in that: The high-temperature sintering includes the following steps: holding at 800-1000℃ for 3-3.5 hours, then raising the temperature to 2000-2200℃ and holding for 3-4 hours.

Citation Information

Patent Citations

  • Preparation method of modified anti-friction, wear-resistant and corrosion-resistant nano-ceramic powder material for additive manufacturing

    CN107500782A

  • Silicon carbide wear-resistant coating for repairing and protecting flow passage component

    CN114437619A