A green and efficient reinforced wood-based panel and its preparation method
By synergistically designing nanocellulose, hydrophobic fluorosilane materials, and bio-based resins, a high-strength, moisture-proof, and environmentally friendly reinforced engineered wood panel was prepared. This solved the problems of traditional engineered wood panels easily expanding and releasing harmful substances in humid environments, achieving a technological breakthrough in high performance and environmental protection.
Patent Information
- Application Number
- CN202510599286.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-10
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2045-05-10
AI Technical Summary
Traditional engineered wood panels are prone to expansion and strength loss in humid environments, and may release harmful substances. Existing technologies are difficult to apply in high-end applications, and the production process is complex and costly.
By employing a synergistic design of nanocellulose, fluorosilane hydrophobic materials, and bio-based resins, an enhanced hydrophobic mixture is prepared through solution processing, ultrasonic dispersion, and hot pressing to form a dense moisture-proof layer. Combined with a three-dimensional network structure, this avoids harmful additives.
It significantly improves the bending strength and moisture resistance of wood-based panels, reduces water absorption, eliminates the release of toxic substances, simplifies the process, reduces costs, and is suitable for high humidity and temperature difference environments.
Smart Images

Figure CN120382539B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of engineered wood products technology, specifically to a green and efficient reinforced engineered wood product and its preparation method. Background Technology
[0002] As a core material in the construction and home furnishing industries, the performance of engineered wood products directly affects structural safety and lifespan. Traditional engineered wood products are mostly made from wood chips or fibers as the base material, bonded together with synthetic resins. However, these materials are prone to moisture absorption and expansion, as well as strength reduction, when exposed to humid environments for extended periods, severely limiting their application in high-end settings. Furthermore, to improve moisture resistance and mechanical properties, formaldehyde-based resins or fluorinated hydrophobic agents are often added during production, leading to the release of volatile harmful substances that threaten human health and environmental safety.
[0003] In recent years, the industry has attempted to optimize these issues through material modification. For example, nanocellulose has been used as a reinforcing phase, leveraging its high specific surface area and mechanical properties to improve matrix strength. However, adding nanocellulose alone is insufficient to form a stable hydrophobic network, resulting in limited moisture-proof performance. While introducing fluorosilane hydrophobic agents can reduce water absorption, their poor compatibility with the cellulose interface can easily lead to stress concentration, thus weakening the overall strength. On the other hand, some research has shifted towards using bio-based resins (such as starch and soy protein) to replace traditional adhesives, but their bonding strength and water resistance are insufficient to meet high-strength requirements. It is evident that existing technologies largely focus on improving a single performance aspect, lacking a synergistic design for mechanical reinforcement, moisture-proof durability, and environmental friendliness, and the complex processes further increase production costs.
[0004] Therefore, there is an urgent need to develop a wood-based panel manufacturing solution that balances high performance and environmental friendliness. Through material innovation and process optimization, we can break through the bottleneck of balancing strength, moisture resistance, and environmental protection in traditional technologies, and provide new ideas for the sustainable development of the wood-based panel industry. Summary of the Invention
[0005] In view of this, the purpose of this invention is to provide a green and efficient reinforced engineered wood panel and its preparation method, so as to solve the problems of insufficient mechanical properties, easy expansion due to moisture, formaldehyde release and complex process of traditional engineered wood panels.
[0006] To achieve the above objectives, the present invention provides the following technical solution:
[0007] A method for preparing a green and efficient reinforced engineered wood panel includes the following steps:
[0008] S1. Fluorosilane hydrophobic materials are dissolved in aqueous acrylic emulsion using a solution method, while an appropriate amount of bio-based resin is added, and ultrasonic dispersion technology is used to obtain a uniform reinforced hydrophobic mixture.
[0009] S2. Add nanocellulose to the enhanced hydrophobic mixture in step S1 and mix thoroughly to construct a reinforcing matrix and improve the initial uniformity of the material.
[0010] S3. Gradually add the reinforced hydrophobic mixture obtained in step S2 to the treated artificial board raw materials, while uniformly dispersing it to ensure sufficient distribution of the reinforcing agent and hydrophobic material.
[0011] S4. Apply adhesive to the raw materials mixed in step S3, and then form them through a hot pressing process to obtain green and high-efficiency reinforced engineered wood panels.
[0012] As an optional option, the fluorosilane in step S1 is one or more of trifluoropropyltriethoxysilane and hexadecyltriethoxysilane.
[0013] As an optional option, the bio-based resin in step S1 is one or more of soybean protein resin, starch-based resin, or polylactic acid resin.
[0014] As an optional option, the nanocellulose in step S2 is cellulose nanocrystals or cellulose nanofibers obtained by mechanical treatment or enzymatic hydrolysis.
[0015] As an optional option, the mass ratio of fluorosilane, aqueous acrylic emulsion and bio-based resin in step S1 is (1-5):(10-30):(5-20).
[0016] As an optional approach, the ultrasonic dispersion process in step S1 can be performed for 10-20 minutes at a frequency of 20-30 kHz.
[0017] As an optional option, in step S3, the weight ratio of the enhanced hydrophobic mixture to the raw material of the artificial board is (5-20):100.
[0018] As an optional approach, in step S4, the hot pressing temperature of the raw material after sizing is 160-190℃, the pressure is 4-7MPa, and the time is 5-12 minutes.
[0019] As an optional solution, the moisture content of the resulting green and efficient reinforced wood-based panel is controlled below 8%.
[0020] Meanwhile, the present invention also provides a green and efficient reinforced wood-based panel, which is prepared by the above-mentioned method for preparing green and efficient reinforced wood-based panels.
[0021] By adopting the above technical solution, the present invention will have the following beneficial effects:
[0022] First, by constructing a three-dimensional reinforcing network using nanocellulose and optimizing the interface between fluorosilane hydrophobic materials and bio-based resins, the flexural strength and structural stability of engineered wood panels are significantly improved, overcoming the limitations of limited mechanical gain or weak interfacial bonding associated with single reinforcing phases. Second, fluorosilanes and water-based acrylic emulsions form a dense hydrophobic layer, synergistically providing a physical barrier effect with nanocellulose, endowing engineered wood panels with long-lasting moisture resistance without the need for harmful additives, preventing moisture absorption, expansion, and strength degradation. Third, the use of formaldehyde-free water-based acrylic emulsions and renewable bio-based resins eliminates the release of toxic substances; ultrasonic dispersion technology ensures uniform distribution of the reinforcing agent, simplifying the complex multi-step modification process in traditional manufacturing and reducing production costs. Compared with existing technologies, this invention improves mechanical strength while also considering weather resistance and environmental adaptability, making it suitable for harsh environments such as high humidity and fluctuating temperatures, breaking through the limitations of the single-performance characteristics of traditional engineered wood panels. Attached Figure Description
[0023] Figure 1 This is a TEM image of the nanocellulose solution of the present invention after being mixed with fluorosilane, aqueous acrylic emulsion and bio-based resin;
[0024] Figure 2 This is a stress-strain curve of the green and high-efficiency reinforced wood-based panel described in Example 1;
[0025] Figure 3 This is a line graph showing the water absorption rate of the green and high-efficiency reinforced wood-based panel described in Example 1. Detailed Implementation
[0026] The technical solution of the present invention will be further described in detail below through specific embodiments. In the present invention, unless otherwise specified, the raw materials and equipment used can be purchased from the market or are commonly used in the art. Unless otherwise specified, the methods and equipment in the following embodiments are conventional methods and equipment in the art.
[0027] Example 1
[0028] This embodiment provides a method for preparing a green and efficient reinforced wood-based panel, including the following steps:
[0029] 1. Raw material pretreatment:
[0030] Biomass fiber (bamboo fiber) was soaked in a 5% ammonia solution for 12 hours, then delignified with 2M sodium hydroxide and 1M sodium sulfite (treatment temperature 80℃, time 2 hours). After washing until neutral, it was bleached with 3% hydrogen peroxide for 30 minutes to obtain purified cellulose raw material.
[0031] 2. Preparation of nanocellulose:
[0032] 2g of purified cellulose was dispersed in 100ml of deionized water and treated with an ultrasonic disruptor (frequency 25kHz, temperature 30℃) for 15 minutes to obtain a uniform cellulose nanofiber suspension.
[0033] 3. Enhanced preparation of hydrophobic mixtures:
[0034] A mixture of fluorosilane: aqueous acrylic emulsion: bio-based resin in a mass ratio of 3:20:10 was prepared by adding 3g of hexadecyltriethoxysilane, 20g of formaldehyde-free aqueous acrylic emulsion, and 10g of soybean protein resin to a cellulose suspension. The mixture was then treated with an ultrasonic vibrator (30kHz, 35℃) for 15 minutes to obtain a homogeneous enhanced hydrophobic mixture. TEM images (...) Figure 1 As can be seen, the reinforcing agent is evenly distributed and firmly bonded to the cellulose surface.
[0035] 4. Mixing and sizing:
[0036] The enhanced hydrophobic mixture was added to 1300g of pretreated engineered wood product raw material (wood chips and starch-based adhesive mixed at a ratio of 7:3) at a weight ratio of 15:100, and then dispersed evenly by mechanical stirring. The mixture was then dried at 60°C until the moisture content was ≤8%.
[0037] 5. Hot pressing:
[0038] After gluing, the raw materials are hot-pressed in a hot press at 5MPa pressure and 180℃ for 10 minutes to produce green and high-efficiency reinforced wood-based panels.
[0039] This embodiment also provides a green and high-efficiency reinforced engineered wood panel prepared by the above method, and its performance is tested. The results are as follows:
[0040] like Figure 2 As shown, the green and high-efficiency reinforced engineered wood panel provided in this embodiment has a bending strength of 48 MPa, which is far higher than the bending strength of traditional engineered wood panels (28.5 MPa). Figure 3 As shown, the water absorption rate (24h) of the green and high-efficiency reinforced wood-based panel provided in this embodiment is 4%, which is much lower than the water absorption rate (24h) of traditional wood-based panels: 14.2%.
[0041] Example 2
[0042] This embodiment provides a method for preparing a green and efficient reinforced wood-based panel, including the following steps:
[0043] 1. Raw material pretreatment:
[0044] Biomass fiber (wood fiber) was soaked in ammonia water for 24 hours, then delignified with 5M sodium hydroxide and 2.5M sodium sulfite (treatment temperature 90℃, time 3 hours), washed until neutral, and then bleached to obtain purified cellulose.
[0045] 2. Preparation of nanocellulose:
[0046] 4g of purified wood fiber was dispersed in an acetate buffer solution at pH 4.8, and cellulase (enzyme activity 15U / g) was added. The mixture was reacted at 50℃ for 24 hours. Undegraded components were removed by centrifugation to obtain a cellulose nanocrystal suspension.
[0047] 3. Enhanced preparation of hydrophobic mixtures:
[0048] According to the mass ratio of fluorosilane: aqueous acrylic emulsion: bio-based resin = 5:30:15, 5g of trifluoropropyltriethoxysilane, 30g of aqueous acrylic emulsion, and 15g of polylactic acid resin were added to the cellulose suspension and treated with an ultrasonic vibrator (frequency 25kHz, temperature 30℃) for 20 minutes to obtain a uniform reinforced hydrophobic mixture.
[0049] 4. Mixing and sizing:
[0050] The enhanced hydrophobic mixture was added to 1300g of pretreated engineered wood product raw material (wood chips and starch-based adhesive mixed at a ratio of 6:4) at a weight ratio of 20:100, and then dispersed evenly by mechanical stirring. The mixture was then dried at 50°C to a moisture content of 7.5%.
[0051] 5. Hot pressing:
[0052] After gluing, the raw materials are hot-pressed in a hot press at 7MPa pressure and 190℃ for 8 minutes to produce green and high-efficiency reinforced wood-based panels.
[0053] This embodiment also provides a green and high-efficiency reinforced engineered wood panel prepared by the above method, and its performance is tested. The results are as follows:
[0054] The bending strength is 52.5 MPa, which is much higher than the bending strength of traditional wood-based panels (28.5 MPa); the water absorption rate (24h) is 3.2%, which is much lower than the water absorption rate (24h) of traditional wood-based panels (14.2%).
[0055] The technical effects of this invention will be demonstrated through comparative experiments below:
[0056] (I) Control group setup:
[0057] 1. Traditional engineered wood panels: No reinforcing agents (nanocellulose, fluorosilanes, bio-based resins) are added; only basic materials and ordinary processes are used.
[0058] 2. Single reinforcing agent group: Nanocellulose, fluorosilane or bio-based resin were added separately to verify the independent effect of each component.
[0059] 3. Partial combination groups: for example, nanocellulose + fluorosilane (without bio-based resin), or fluorosilane + bio-based resin (without nanocellulose), to analyze synergistic effects.
[0060] Test metrics:
[0061] Mechanical properties: bending strength, elastic modulus.
[0062] Moisture-proof performance: water absorption rate (24 hours), wet expansion rate.
[0063] Environmental friendliness: formaldehyde emission and VOC content.
[0064] Durability: Performance retention rate after damp heat cycling, weather resistance testing (such as UV aging).
[0065] Standardization of experimental conditions:
[0066] All experimental and control groups used the same raw material sources and pretreatment processes.
[0067] The test methods must comply with national standards (such as GB / T 17657), and the experimental parameters (such as test temperature, humidity, and instrument model) must be recorded in detail.
[0068] (II) Test Results
[0069] Table 1: Comparison of flexural strength and water absorption rate
[0070]
[0071] Table 2: Comparison of Durability and Environmental Friendliness Data
[0072]
[0073] (III) Data Analysis and Explanation
[0074] 1. Bending strength
[0075] Traditional engineered wood panels have a bending strength of only 28.5 MPa. Adding nanocellulose or fluorosilane alone can increase this to 34-36 MPa, but the effect is limited. Examples 1 and 2 of this invention, through the synergistic effect of the three components, achieve bending strengths of 48 MPa and 52.5 MPa respectively, representing an improvement of approximately 33%-55% compared to traditional panels.
[0076] 2. Water absorption rate and wet expansion rate
[0077] Traditional engineered wood panels have a water absorption rate as high as 14.2% and a moisture expansion rate of 1.8%, making them prone to deformation when exposed to moisture. Fluorosilanes alone can reduce the water absorption rate to 7.3%, but when combined with a dense network of nanocellulose (Example 1), the water absorption rate is further reduced to 3.2%, and the moisture expansion rate is only 0.4%.
[0078] 3. Environmental performance
[0079] Traditional engineered wood panels release 0.15 mg / m³ of formaldehyde. 3 The concentration exceeds the environmental protection standard (GB / T 17657-2013 requirement of ≤0.05mg / m³). 3 Examples 1 and 2 of this invention use formaldehyde-free waterborne acrylic emulsion and bio-based resin, with formaldehyde release levels below 0.01 mg / m³. 3 Total VOC release ≤50μg / m³ 3 It meets the requirements for green building materials certification.
[0080] 4. Durability
[0081] Traditional engineered wood panels retain only 65% of their strength after humid heat cycling, while Examples 1 and 2 of this invention achieve 93% and 96% respectively, indicating excellent stability of the material in high-humidity environments. QUV aging tests show that the engineered wood panels of this invention exhibit no cracking or discoloration on the surface, demonstrating significantly better weather resistance than the control group.
[0082] (iv) Explanation of Technical Mechanism
[0083] The reinforcing effect of nanocellulose: Nanocellulose forms a three-dimensional network structure through hydrogen bonding and mechanical interlocking effects, which effectively disperses stress and improves flexural strength and elastic modulus.
[0084] The hydrophobic effect of fluorosilanes: Fluorosilanes form a low surface energy protective layer on the material surface, preventing water penetration and reducing water absorption and moisture expansion rate.
[0085] Interface optimization of bio-based resins: Bio-based resins (such as soy protein) can be used as binders to improve the interfacial bonding between nanocellulose and the substrate, reduce defects, and inhibit the aggregation of reinforcing agents.
[0086] (V) Conclusion
[0087] This invention successfully prepares a high-efficiency reinforced engineered wood product with high strength, excellent moisture resistance, and environmentally friendly properties through the synergistic effect of nanocellulose, hydrophobic fluorosilane materials, and bio-based resins. Compared with traditional engineered wood products and single-component improvement schemes, this invention achieves improvements in flexural strength (33%-55%), water absorption (reduced to 4%-3.2%), and formaldehyde emission (≤0.008 mg / m³). 3Significant breakthroughs have been achieved in aspects such as durability (strength retention rate during damp heat cycling ≥95%), while the process is simplified and costs are controllable. Experimental data fully verify the technical advantages of multi-component synergistic design, providing an innovative solution for the high-end and environmentally friendly development of engineered wood panels. It is suitable for high-requirement scenarios such as construction and home furnishing, and has significant prospects for industrial application.
[0088] The foregoing general description of the invention and its specific embodiments should not be construed as limiting the technical solution of the invention. Those skilled in the art, based on the disclosure of this application, can add, reduce, or combine the disclosed technical features in the foregoing general description and / or embodiments without departing from the constituent elements of the invention, to form other technical solutions within the scope of protection of this application.
Claims
1. A method for preparing green and efficient enhanced wood-based panel, characterized in that, Includes the following steps: S1. Fluorosilane hydrophobic material is dissolved in aqueous acrylic emulsion using a solution method, and an appropriate amount of bio-based resin is added. The mixture is then treated with ultrasonic dispersion technology to obtain a uniform reinforced hydrophobic mixture. The mass ratio of fluorosilane, aqueous acrylic emulsion and bio-based resin is (1-5):(10-30):(5-20). The fluorosilane is one or more of trifluoropropyltriethoxysilane and hexadecylfluorohexyltriethoxysilane; the bio-based resin is one or more of soybean protein resin, starch-based resin or polylactic acid resin. S2. Add nanocellulose to the reinforcing hydrophobic mixture in step S1 and mix thoroughly to construct a reinforcing matrix and improve the initial uniformity of the material; the nanocellulose is cellulose nanocrystals or cellulose nanofibers obtained by mechanical treatment or enzymatic hydrolysis. S3. Gradually add the reinforced hydrophobic mixture obtained in step S2 to the treated artificial board raw materials, while uniformly dispersing it to ensure sufficient distribution of the reinforcing agent and hydrophobic material. S4. Apply adhesive to the raw materials mixed in step S3, and then form them through a hot pressing process to obtain green and high-efficiency reinforced engineered wood panels.
2. The method of claim 1, wherein the green high-performance enhanced wood-based panel is prepared by the steps of: The ultrasonic dispersion process in step S1 takes 10-20 minutes and has a frequency of 20-30 kHz. 3. The method for preparing green and high-efficiency reinforced wood-based panels according to claim 1, characterized in that, In step S3, the weight ratio of the enhanced hydrophobic mixture to the raw material of the artificial board is (5-20):
100.
4. The method for preparing green and high-efficiency reinforced wood-based panels according to claim 1, characterized in that, In step S4, the hot pressing temperature of the raw material after sizing is 160-190℃, the pressure is 4-7 MPa, and the time is 5-12 minutes.
5. The method for preparing green and high-efficiency reinforced wood-based panels according to claim 1, characterized in that, The resulting green and efficient reinforced wood-based panels have a moisture content controlled below 8%.
6. A green and efficient enhanced wood-based panel, characterized in that, The green and efficient reinforced wood-based panel is prepared by any one of claims 1 to 5.
Citation Information
Patent Citations
Straw board for floor and manufacturing method and application of straw board
CN111483032A