Crown ether modified polyimide and its preparation method, capacitor
By using crown ether modified polyimide to form hydrogen bonds and mechanical interlocks in the dielectric film, the problem of insufficient capacitance performance and thermal stability of polymer dielectric materials at high temperatures is solved, and capacitance performance with low leakage current and high discharge energy density at high temperatures is achieved.
Patent Information
- Application Number
- CN202410135083.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-31
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-01-31
AI Technical Summary
Existing polymer dielectric materials struggle to achieve both excellent capacitance and thermal stability under high-temperature conditions. Commercially available capacitor films suffer from insufficient thermal stability, while heat-resistant polymers experience increased conduction losses under high electric fields.
A dielectric film was prepared by using crown ether modified polyimide, which forms hydrogen bonds with the imine and sub-amino groups of polyimide through ether bonds and combines mechanical interlocking.
It maintains a high glass transition temperature and conductivity at high temperatures, significantly reduces leakage current density, and improves charge and discharge efficiency and discharge energy density.
Smart Images

Figure CN120399224B_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates to the field of polymer materials, and in particular to a crown ether modified polyimide, its preparation method, and a capacitor. Background Technology
[0002] Mainstream dielectric energy storage technologies in many emerging applications, such as renewable energy, electrified transportation, and advanced propulsion systems, typically require operation under high-temperature conditions. However, for current polymer dielectric materials, excellent capacitance and thermal stability are often mutually exclusive.
[0003] Supramolecular polymers not only possess many advantages of traditional polymers but also exhibit numerous unique properties. They can be constructed through self-assembly using various non-covalent interactions. Host-guest interactions, as an important type of non-covalent interaction, have been widely applied in the construction of supramolecular polymers. Summary of the Invention
[0004] This disclosure provides a crown ether modified polyimide, its preparation method, and a capacitor, to address the shortcomings of related technologies.
[0005] According to a first aspect of the present disclosure, a crown ether modified polyimide is provided, wherein the ether bond of the crown ether forms a hydrogen bond with the imino and / or subamino group of the polyimide; the polyimide is a condensation polymer of a diamine and a dianhydride.
[0006] Optionally, the diamine is selected from at least one of α,α'-bis(4-aminophenyl)-1,4-diisopropylbenzene, m-phenylenediamine, p-phenylenediamine, and 4,4'-diaminodiphenyl ether.
[0007] Optionally, the dianhydride is selected from at least one of bisphenol A type diether dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 4,4'-biphenyl ether dianhydride, 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride, and hexafluorodianhydride.
[0008] Optionally, the diamine is selected from α,α'-bis(4-aminophenyl)-1,4-diisopropylbenzene, and the dianhydride is selected from hexafluorodianhydride.
[0009] Optionally, the mass ratio of the crown ether to the polyimide is 0.2% to 1.2%.
[0010] Optionally, the crown ether modified polyimide has a molecular weight of 200–400 kg / mol.
[0011] Optionally, the glass transition temperature of the crown ether modified polyimide is 200℃~400℃.
[0012] According to a second aspect of the present disclosure, a method for preparing crown ether-modified polyimide is provided, the method comprising:
[0013] In an aprotic polar solvent, a diamine is mixed with a crown ether to obtain a mixture solution;
[0014] A dianhydride was added to the mixture solution and polymerized at room temperature to obtain a polyamic acid solution;
[0015] The solvent in the polyamic acid solution is removed by heat treatment to obtain the crown ether modified polyimide.
[0016] The diamine is selected from at least one of α,α'-bis(4-aminophenyl)-1,4-diisopropylbenzene, m-phenylenediamine, p-phenylenediamine and 4,4'-diaminodiphenyl ether;
[0017] The dianhydride is selected from at least one of bisphenol A type diether dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 4,4'-biphenyl ether dianhydride, 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride, and hexafluorodianhydride.
[0018] Optionally, the crown ether is selected from 18-crown ether-6, 12-crown ether-4, aza-18-crown ether, benzo-18-crown ether-6, benzo-15-crown ether-5, diaza-18-crown ether-6, benzo-12-crown ether-4, 4-acyl-18-crown ether, dibenzo-18-crown ether-6, dibenzo-24-crown ether-8, dibenzo-18-crown ether-6, dicyclohexyl-18-crown ether-6, 2,3-naphtho-15-crown ether-5, 2- The hydroxymethyl-15-crown-5, 4'-aminobenzo-18-crown-6, 4,4'-dibromodibenzo-18-crown-6, (+)-(18-crown-6)-2,3,11,12-tetracarboxylic acid, 24-crown-8-ether, 4'-acetylbenzo-18-crown-6-ether, 4'-formylbenzo-18-crown-6-ether, bis(1,4-phenylene)-34-crown-10-ether, and dibenzo-30-crown-10.
[0019] Optionally, the crown ether is selected from 18-crown ether-6, dibenzo-18-crown ether-6, dibenzo-24-crown ether-8, 24-crown 8-ether, or bis(1,4-phenylene)-34-crown 10-ether.
[0020] Optionally, the mass ratio of the crown ether to the polyimide is 0.2% to 1.2%.
[0021] Optionally, the molar ratio of the diamine to the crown ether is (50-500):1.
[0022] Optionally, the molar ratio of the diamine to the dianhydride is selected from 1:(0.98 to 1.02).
[0023] Optionally, the mass ratio of the polyimide to the aprotic polar solvent is selected from (3-5):100.
[0024] According to a third aspect of the present disclosure, a capacitor is provided, wherein the dielectric film in the capacitor is the aforementioned crown ether modified polyimide, or is a crown ether modified polyimide prepared by the aforementioned preparation method.
[0025] As can be seen from the above embodiments, this disclosure provides a polymer that has both superior glass transition temperature and electrical conductivity.
[0026] It should be understood that the above general description and the following detailed description are exemplary and explanatory only, and are not intended to limit this disclosure. Attached Figure Description
[0027] The accompanying drawings, which are incorporated in and form a part of this specification, illustrate embodiments consistent with this disclosure and, together with the description, serve to explain the principles of this disclosure.
[0028] Figure 1 This is a schematic diagram of the structure of crown ether modified polyimide according to an exemplary embodiment.
[0029] Figure 2 This is a schematic diagram illustrating, according to an exemplary embodiment, the formation of a crown ether-modified polyimide by a crown ether and a polyimide.
[0030] Figure 3 This is a proton nuclear magnetic resonance spectrum shown according to an exemplary embodiment.
[0031] Figure 4 This is a schematic diagram illustrating a glass transition temperature test according to an exemplary embodiment.
[0032] Figure 5 This is a schematic diagram illustrating a leakage current test according to an exemplary embodiment.
[0033] Figure 6 This is a schematic diagram illustrating a discharge energy density test according to an exemplary embodiment. Detailed Implementation
[0034] Exemplary embodiments will now be described in detail, examples of which are illustrated in the accompanying drawings. When the following description relates to the drawings, unless otherwise indicated, the same numerals in different drawings denote the same or similar elements. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with this disclosure. Rather, they are merely examples of apparatuses and methods consistent with some aspects of this disclosure as detailed in the appended claims.
[0035] The terminology used in this disclosure is for the purpose of describing particular embodiments only and is not intended to be limiting of the disclosure. The singular forms “a,” “the,” and “the” as used in this disclosure and the appended claims are also intended to include the plural forms unless the context clearly indicates otherwise. It should also be understood that the term “and / or” as used herein refers to and includes any and all possible combinations of one or more of the associated listed items.
[0036] In existing technologies, dielectric capacitors possess the characteristics of rapid charging and discharging, making them crucial energy storage components in modern electronic devices and power systems. Polymer dielectrics are the preferred material for high-voltage dielectric capacitors due to their high voltage resistance and ease of processing. However, these organic materials face significant challenges in emerging applications. For example, in mainstream renewable energy technologies, electrified transportation, and advanced propulsion systems, electronic equipment needs to operate stably under harsh temperature conditions exceeding 150°C to 250°C.
[0037] However, on the one hand, commercially available capacitor films, represented by biaxially oriented polypropylene (BOPP), are designed to have a wide band gap (Eg) and high resistance, but lack thermal stability exceeding 105°C. On the other hand, although heat-resistant polymers such as polyimide (PI) and fluorene polyester (FPE) have good thermal stability (glass transition temperature Tg exceeding 350°C), they contain a large number of highly conjugated structures, and their conduction losses increase exponentially with increasing temperature and electric field.
[0038] In view of this, the present disclosure provides a crown ether modified polyimide, wherein the ether bond of the crown ether forms a hydrogen bond with the imino and / or subamino group of the polyimide.
[0039] like Figure 1 As shown, the crown ether-modified polyimide comprises a molecular axis and cyclic molecules, and the molecular axis and cyclic molecules are linked by mechanical interlocking. In this disclosure, the molecular axis is a polyimide molecular chain, and the cyclic molecules are crown ethers.
[0040] like Figure 3As shown, from top to bottom, the polymer containing a polyimide molecular chain passing through a crown ether ring obtained in the embodiments of this disclosure, a mixture of polyimide and crown ether, and polyimide are shown. It can be seen that the ether bond of the crown ether forms hydrogen bonds with the imino and / or subamino groups in the polyimide, thereby changing the chemical shift.
[0041] In some embodiments of this disclosure, the polyimide is a condensation polymer of a diamine and a dianhydride. The diamine is selected from at least one of α,α'-bis(4-aminophenyl)-1,4-diisopropylbenzene, m-phenylenediamine, p-phenylenediamine, and 4,4'-diaminodiphenyl ether; the dianhydride is selected from at least one of bisphenol A type diether dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 4,4'-biphenyl ether dianhydride, 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride, and hexafluorodianhydride. Optionally, the diamine is selected from α,α'-bis(4-aminophenyl)-1,4-diisopropylbenzene, and the dianhydride is selected from hexafluorodianhydride.
[0042] In some embodiments of this disclosure, the crown ether is selected from 18-crown ether-6, 12-crown ether-4, aza-18-crown ether, benzo-18-crown ether-6, benzo-15-crown ether-5, aza-18-crown ether-6, benzo-12-crown ether-4, 4-acyl-18-crown ether, dibenzo-18-crown ether-6, dibenzo-24-crown ether-8, dibenzo-18-crown ether-6, dicyclohexyl-18-crown ether-6, and 2,3-naphtho-15-crown ether- 5. At least one of 2-hydroxymethyl-15-crown ether-5, 4'-aminobenzo-18-crown ether-6, 4,4'-dibromodibenzo-18-crown ether-6, (+)-(18-crown ether-6)-2,3,11,12-tetracarboxylic acid, 24-crown 8-ether, 4'-acetylbenzo-18-crown-6-ether, 4'-formylbenzo-18-crown-6-ether, bis(1,4-phenylene)-34-crown 10-ether, and dibenzo-30-crown ether-10.
[0043] Optionally, the crown ether is selected from 18-crown ether-6, dibenzo-18-crown ether-6, dibenzo-24-crown ether-8, 24-crown 8-ether, or bis(1,4-phenylene)-34-crown 10-ether; specifically, the crown ether is selected from dibenzo-18-crown ether-6.
[0044] In some embodiments of this disclosure, the aprotic polar solvent may be selected from NMP, DMF or DMAc, specifically, the aprotic polar solvent is NMP.
[0045] Figure 2 A schematic diagram is shown illustrating the composition of crown ether-modified polyimide from crown ether and polyimide. (See diagram for reference.) Figure 2As shown, the chemical topology of this polymer comprises a polyimide molecular chain and a crown ether, the polyimide molecular chain passing through the ring of the crown ether; wherein the diamine used is selected from α,α'-bis(4-aminophenyl)-1,4-diisopropylbenzene, the dianhydride used is selected from hexafluorodianhydride (also known as 4,4'-(hexafluoroisopropylene)phthalic anhydride, 6FDA), and the crown ether used is selected from dibenzo-18-crown ether-6. Specifically, α,α'-bis(4-aminophenyl)-1,4-diisopropylbenzene and dibenzo-18-crown ether-6 are linked together via hydrogen-bonded self-assembly. Dibenzo-18-crown ether-6 serves as the host compound, and α,α'-bis(4-aminophenyl)-1,4-diisopropylbenzene serves as the guest compound. The isopropyl and hexafluoroisopropyl groups present on the polyimide molecular chain can lock the crown ether, preventing its separation from the chain.
[0046] In some embodiments of this disclosure, the molar ratio of diamine to dianhydride is selected from 1:(0.98 to 1.02); specifically, the molar ratio of diamine to dianhydride can be 1:1.
[0047] In some embodiments of this disclosure, the molar ratio of diamine to crown ether is selected from (50 to 500):1; specifically, the molar ratio of diamine to crown ether can be 50, 63, 95 or 190.
[0048] In some embodiments of this disclosure, the mass ratio of the sum of the diamine and dianhydride to the aprotic polar solvent is selected from (3-5):100; specifically, the mass ratio of the sum of the diamine and dianhydride to the organic solvent is 3:100.
[0049] In some embodiments of this disclosure, the mass ratio of crown ether to polyimide molecular chain is selected from 0.2% to 1.2%; specifically, the mass ratio of crown ether to polyimide molecular chain can be 0.25, 0.5, 0.75 or 1.
[0050] In some embodiments of this disclosure, the glass transition temperature of the obtained polymer is selected from 200°C to 400°C.
[0051] In some embodiments of this disclosure, the obtained polymer has a molecular weight of 200 to 400 kg / mol, specifically, the obtained polymer has a molecular weight of 250 kg / mol.
[0052] This disclosure also provides a dielectric film comprising the aforementioned polymer.
[0053] In some embodiments of this disclosure, the thickness of the dielectric film is selected from 6 to 8 μm.
[0054] In some embodiments of this disclosure, the method for preparing the dielectric film includes the following steps:
[0055] Dissolve the diamine in an aprotic polar solvent. After it is completely dissolved, add the crown ether and stir for 1 to 4 hours.
[0056] Add dianhydride and polymerize at room temperature for 3–5 hours, controlling the stirring speed at 100–800 rpm to obtain a polymer solution;
[0057] After the polymer solution is poured onto a glass plate, the glass plate is heated through a heating process to obtain a polymer film. After the heating is finished and the glass plate is cooled to room temperature, the glass plate is placed in water to peel off the polymer film.
[0058] In some embodiments of this disclosure, the purpose of heating is to evaporate the organic solvent and to carry out the acylation process.
[0059] In some embodiments of this disclosure, the molar amounts of dianhydride and diamine are equal in the method for preparing polyimide.
[0060] In some embodiments of this disclosure, the polymerization time in the method for preparing the polymer film is 4 hours.
[0061] In some embodiments of this disclosure, the method for preparing the polymer film further includes an acylation process after the process of evaporating the organic solvent.
[0062] In some embodiments of this disclosure, the method for preparing the polymer film includes the following steps:
[0063] Dissolve the diamine in NMP organic solvent; after the diamine is completely dissolved, add the crown ether and stir for 2 hours;
[0064] Dianhydride was added to the aforementioned solution, and polymerization was carried out at room temperature for 4 hours with a stirring rate of 100–800 rpm to obtain a polymer solution. Using a syringe with a 200 nm pore size polytetrafluoroethylene filter, 1.5 mL of the polymer solution was extracted and cast onto a pre-cleaned glass plate with an area of 5 cm × 5 cm. Then, the plate was heated at 80 °C for 8 hours to evaporate the NMP solution and obtain a polymer film. The polymer film was then heated and held at 100 °C, 150 °C, and 200 °C for 1 hour, and finally held at 250 °C for 0.5 hours.
[0065] After heating and cooling to room temperature, the glass plate is placed in water to peel off the polymer film; the polymer film is cleaned with alcohol and vacuum dried in an oven at 100°C for 24 hours.
[0066] This disclosure also provides a capacitor comprising a dielectric film, wherein the dielectric film is the aforementioned polymer film.
[0067] In some embodiments of this disclosure, the dielectric film in the capacitor has a thickness of 6-8 μm, a width of 50 mm, a margin width of 4 mm, and a non-blank pattern on the metal vapor-deposited film. The capacitor element has a capacitance of 100 μF, and the specifications of the capacitor element are defined as those required for a capacitance of 100 μF. However, the specifications of the capacitor are not limited to these in this disclosure.
[0068] In this disclosure, due to the suppression of molecular chain vibration by crown ethers, the phonon-assisted interchain charge transfer is restricted, thus the leakage current density is reduced by 1 to 2 orders of magnitude at high temperatures. Benefiting from the reduced leakage current density, the conductivity loss is suppressed, and the charge and discharge efficiency is significantly improved, thereby enabling higher discharge energy density to be obtained under higher electric fields.
[0069] The present application is further illustrated below with specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the present application.
[0070] Examples and test methods:
[0071] Glass transition temperature (Tg) testing: This includes DSC testing, where the temperature is increased from room temperature to 300°C at a rate of 10°C / min, then decreased to 100°C, and then increased to 300°C again, with both heating and cooling rates at 10°C / min. The curve from the second heating is used to determine Tg.
[0072] Testing of the electric displacement electric field loop and leakage current: The electric displacement electric field (DE) loop was recorded on a modified Sawyer Tower circuit under a 100Hz monopole wave. The electrode diameter used in this test was 3mm. During the DE loop test, the sample was immersed in dimethylsiloxane (DOW CORNING) to prevent surface flashover. The temperature of the silicone oil was controlled by a hot plate and matched with a thermocouple temperature sensor. The leakage current density associated with the electric field was recorded using a Keithley 6517B ammeter with a Stanford PS350 voltage source and an oven for controlling the voltage and temperature. The voltage was held for 5 minutes under each electric field, and the current density was recorded in the last second. The leakage current was tested every 25MV / m of electric field strength, from 25MV / m to 300MV / m.
[0073] Example 1:
[0074] 131 mg (0.38 mmol) of α,α'-bis(4-aminophenyl)-1,4-diisopropylbenzene was dissolved in 10 mL of NMP solution. After complete dissolution, 0.75 mg (0.002 mmol) of dibenzo-18-crown ether-6 was weighed and added to the solution, and the mixture was stirred for 2 hours. Then, an equimolar amount (0.38 mmol, 169 mg) of hexafluorodianhydride (also known as 4,4'-(hexafluoroisopropylidene)phthalic anhydride, 6FDA) was added to the mixture, and polymerization was carried out at room temperature for 4 hours to form a polyamic acid solution (PAA solution). The above steps require maintaining a low stirring rate, controlled at 300–400 rpm.
[0075] Using a syringe with a 200 nm pore size polytetrafluoroethylene filter, extract 1.5 mL of the above PAA solution and cast it onto a pre-cleaned glass plate with an area of 5 cm × 5 cm.
[0076] The NMP solution was evaporated by heating at 80°C for 8 hours, then continuously heated and held at 100°C, 150°C and 200°C for 1 hour, and finally held at 250°C for 0.5 hours. After naturally cooling to room temperature, the glass slide was placed in deionized water to peel off the polymer film. The polymer film was cleaned with alcohol and vacuum dried in an oven at 100°C for 24 hours. The thickness of the polymer film obtained in Example 1 was 6-8 μm.
[0077] Example 2:
[0078] 131 mg (0.38 mmol) of α,α'-bis(4-aminophenyl)-1,4-diisopropylbenzene was dissolved in 10 mL of NMP solution. After complete dissolution, 1.5 mg (0.004 mmol) of dibenzo-18-crown ether-6 was weighed and added to the solution, and the mixture was stirred for 2 hours. Then, an equimolar amount (0.38 mmol, 169 mg) of hexafluorodianhydride (also known as 4,4'-(hexafluoroisopropylidene)phthalic anhydride, 6FDA) was added to the mixture, and polymerization was carried out at room temperature for 4 hours to form a polyamic acid solution (PAA solution). The above steps require maintaining a low stirring rate, controlled at 300–400 rpm.
[0079] Using a syringe with a 200 nm pore size polytetrafluoroethylene filter, extract 1.5 mL of the above PAA solution and cast it onto a pre-cleaned glass plate with an area of 5 cm × 5 cm.
[0080] The NMP solution was evaporated by heating at 80°C for 8 hours, then continuously heated and held at 100°C, 150°C and 200°C for 1 hour, and finally held at 250°C for 0.5 hours. After naturally cooling to room temperature, the glass slide was placed in deionized water to peel off the polymer film. The polymer film was cleaned with alcohol and vacuum dried in an oven at 100°C for 24 hours. The thickness of the polymer film obtained in Example 2 was 6-8 μm.
[0081] Example 3:
[0082] 131 mg (0.38 mmol) of α,α'-bis(4-aminophenyl)-1,4-diisopropylbenzene was dissolved in 10 mL of NMP solution. After complete dissolution, 2.25 mg (0.006 mmol) of dibenzo-18-crown ether-6 was weighed and added to the solution, and the mixture was stirred for 2 hours. Then, an equimolar amount (0.38 mmol, 169 mg) of hexafluorodianhydride (also known as 4,4'-(hexafluoroisopropylidene)phthalic anhydride, 6FDA) was added to the mixture, and polymerization was carried out at room temperature for 4 hours to form a polyamic acid solution (PAA solution). The above steps require maintaining a low stirring rate, controlled at 300–400 rpm.
[0083] Using a syringe with a 200 nm pore size polytetrafluoroethylene filter, extract 1.5 mL of the above PAA solution and cast it onto a pre-cleaned glass plate with an area of 5 cm × 5 cm.
[0084] The NMP solution was evaporated by heating at 80°C for 8 hours, then continuously heated and held at 100°C, 150°C and 200°C for 1 hour, and finally held at 250°C for 0.5 hours. After naturally cooling to room temperature, the glass slide was placed in deionized water to peel off the polymer film. The polymer film was cleaned with alcohol and vacuum dried in an oven at 100°C for 24 hours. The thickness of the polymer film obtained in Example 3 was 6-8 μm.
[0085] Example 4:
[0086] 131 mg (0.38 mmol) of α,α'-bis(4-aminophenyl)-1,4-diisopropylbenzene was dissolved in 10 mL of NMP solution. After complete dissolution, 3 mg (0.008 mmol) of dibenzo-18-crown ether-6 was weighed and added to the solution, and the mixture was stirred for 2 hours. Then, an equimolar amount (0.38 mmol, 169 mg) of hexafluorodianhydride (also known as 4,4'-(hexafluoroisopropylidene) phthalic anhydride, 6FDA) was added to the mixture, and polymerization was carried out at room temperature for 4 hours to form a polyamic acid solution (PAA solution). The above steps require maintaining a low stirring rate, controlled at 300–400 rpm.
[0087] Using a syringe with a 200 nm pore size polytetrafluoroethylene filter, extract 1.5 mL of the above PAA solution and cast it onto a pre-cleaned glass plate with an area of 5 cm × 5 cm.
[0088] The NMP solution was evaporated by heating at 80°C for 8 hours, then continuously heated and held at 100°C, 150°C and 200°C for 1 hour, and finally held at 250°C for 0.5 hours. After naturally cooling to room temperature, the glass slide was placed in deionized water to peel off the polymer film. The polymer film was cleaned with alcohol and vacuum dried in an oven at 100°C for 24 hours. The thickness of the polymer film obtained in Example 4 was 6-8 μm.
[0089] Comparative Example 1:
[0090] 131 mg (0.38 mmol) of α,α'-bis(4-aminophenyl)-1,4-diisopropylbenzene was dissolved in 10 mL of NMP solution. After complete dissolution, an equimolar amount (0.38 mmol, 169 mg) of hexafluorodianhydride (also known as 4,4'-(hexafluoroisopropylidene) phthalic anhydride, 6FDA) was added to the mixture, and polymerization was carried out at room temperature for 4 hours to form a polyamic acid solution (PAA solution). The above steps require maintaining a low stirring rate, controlling the stirring rate at 300-400 rpm.
[0091] Using a syringe with a 200 nm pore size polytetrafluoroethylene filter, extract 1.5 mL of the above PAA solution and cast it onto a pre-cleaned glass plate with an area of 5 cm × 5 cm.
[0092] The NMP solution was evaporated by heating at 80°C for 8 hours, then continuously heated and held at 100°C, 150°C and 200°C for 1 hour, and finally held at 250°C for 0.5 hours. After naturally cooling to room temperature, the glass slide was placed in deionized water to peel off the polymer film. The polymer film was cleaned with alcohol and vacuum dried in an oven at 100°C for 24 hours. The thickness of the polymer film obtained in Comparative Example 1 was 6-8 μm.
[0093] The Tg of the polymer films obtained in Comparative Example 1 and Examples 1-4 were tested, and the results are as follows: Figure 4 As shown, the Tg value gradually decreases as the mass percentage of crown ether increases. The introduction of crown ether generates free volume, and as the free volume increases, the glass transition temperature of the polymer film decreases.
[0094] Preparation Examples 1-5:
[0095] Capacitors were prepared using the polymer films obtained in Examples 1-4 and Comparative Example 1 as dielectric films (Preparation Example 1 used the polymer film of Example 1, Preparation Example 2 used the polymer film of Example 2, Preparation Example 3 used the polymer film of Example 3, Preparation Example 4 used the polymer film prepared in Example 4, and Preparation Example 5 used the polymer film of Comparative Example 1). The thickness of the dielectric film in the capacitor was controlled at 6-8 μm, and the size was a square with a side length of 5 cm.
[0096] Examples 1-5 were tested for electric displacement and electric field loops and leakage current. The results are as follows: Figure 5 and Figure 6 As shown. Combined with Figure 4 and Figure 5 As can be seen, the polymer film prepared in this embodiment can maintain a superior glass transition temperature (>255°C) while significantly improving electrical insulation (50°C to 250°C) compared to Comparative Example 1. Combined with... Figure 5 and Figure 6 As can be seen, the polymer film prepared in this embodiment exhibits better electrical insulation in the temperature range of 50°C to 250°C, and at 200°C, it has a discharge efficiency of over 6 J / cm² while maintaining a discharge efficiency of over 90%. 3 The discharge energy density is still 3 J / cm³ even at 250 degrees Celsius. 3 Its discharge energy density is extremely high, making it a dielectric polymer with exceptionally good high-temperature capacitance performance in the field.
[0097] Because crown ethers suppress molecular chain vibrations, phonon-assisted interchain charge transfer is restricted, resulting in a 1-2 order of magnitude reduction in leakage current density at high temperatures. Benefiting from the reduced leakage current density, conductivity loss is suppressed, thus significantly improving charge and discharge efficiency and enabling higher discharge energy density at higher electric fields.
[0098] Other embodiments of this disclosure will readily occur to those skilled in the art upon consideration of the specification and practice of the disclosure herein. This disclosure is intended to cover any variations, uses, or adaptations of this disclosure that follow the general principles of this disclosure and include common knowledge or customary techniques in the art not disclosed herein. The specification and examples are to be considered exemplary only, and the true scope and spirit of this disclosure are indicated by the following claims.
[0099] It should be understood that this disclosure is not limited to the precise structures described above and shown in the accompanying drawings, and various modifications and changes can be made without departing from its scope. The scope of this disclosure is limited only by the appended claims.
Claims
1. A crown ether modified polyimide, characterized in that, In the crown ether modified polyimide, hydrogen bonds are formed between the ether bonds of the crown ether and the imino and / or subamino groups of the polyimide; the mass ratio of the crown ether to the polyimide is 0.2% to 1.2%. The polyimide is a condensation polymer of a diamine and a dianhydride; The diamine is selected from α,α'-bis(4-aminophenyl)-1,4-diisopropylbenzene; The dianhydride is selected from at least one of bisphenol A type diether dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 4,4'-biphenyl ether dianhydride, 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride, and hexafluorodianhydride.
2. The crown ether modified polyimide according to claim 1, characterized in that, The crown ether modified polyimide has a molecular weight of 200-400 kg / mol.
3. The crown ether modified polyimide according to claim 1, characterized in that, The glass transition temperature of the crown ether modified polyimide is 200℃~400℃.
4. A method for preparing crown ether modified polyimide, characterized in that, include: In an aprotic polar solvent, a diamine is mixed with a crown ether to obtain a mixture solution; A dianhydride was added to the mixture solution and polymerized at room temperature to obtain a polyamic acid solution; The solvent in the polyamic acid solution is removed by heat treatment to obtain the crown ether-modified polyimide; the mass ratio of the crown ether to the polyimide is 0.2%~1.2%. The diamine is selected from α,α'-bis(4-aminophenyl)-1,4-diisopropylbenzene; The dianhydride is selected from at least one of bisphenol A type diether dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 4,4'-biphenyl ether dianhydride, 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride, and hexafluorodianhydride.
5. The preparation method according to claim 4, characterized in that, The crown ether is selected from 18-crown ether-6, 12-crown ether-4, aza-18-crown ether, benzo-18-crown ether-6, benzo-15-crown ether-5, aza-18-crown ether-6, benzo-12-crown ether-4, 4-acyl-18-crown ether, dibenzo-24-crown ether-8, dibenzo-18-crown ether-6, dicyclohexyl-18-crown ether-6, 2,3-naphtho-15-crown ether-5, 2-hydroxymethyl-15- At least one of crown ether-5, 4'-aminobenzo-18-crown ether-6, 4,4'-dibromodibenzo-18-crown ether-6, (+)-(18-crown ether-6)-2,3,11,12-tetracarboxylic acid, 24-crown 8-ether, 4'-acetylbenzo-18-crown-6-ether, 4'-formylbenzo-18-crown-6-ether, bis(1,4-phenylene)-34-crown 10-ether, and dibenzo-30-crown ether-10.
6. The preparation method according to claim 5, characterized in that, The crown ether is selected from 18-crown ether-6, dibenzo-18-crown ether-6, dibenzo-24-crown ether-8, 24-crown 8-ether, or bis(1,4-phenylene)-34-crown 10-ether.
7. The preparation method according to claim 4, characterized in that, The molar ratio of the diamine to the crown ether is (50~500):
1.
8. A capacitor, characterized in that, The dielectric film in the capacitor is a crown ether modified polyimide according to any one of claims 1 to 3, or a crown ether modified polyimide prepared by the preparation method according to any one of claims 4 to 7.
Citation Information
Patent Citations
Crown ether modified polyimide hybrid membrane and preparation method thereof
CN104356647A
Polyimide resin, polyimide film, preparation method and flexible equipment
CN116199883A