By using iron powder, sodium sulfide, and lithium sulfate as raw materials, and combining ball milling, calcination, and alcohol solvent washing, the problems of high cost and environmental pollution in lithium sulfide preparation have been solved, achieving low-cost, green and environmentally friendly lithium sulfide preparation, which is suitable for battery materials.

CN120440841BActive Publication Date: 2026-11-17ZHANGJIAGANG HUASHENG CHEM CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202510737232.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-06-04
Publication Date
2026-11-17
Estimated Expiration
2045-06-04

AI Technical Summary

Technical Problem

Existing methods for preparing lithium sulfide suffer from difficulties in industrialization, high costs, serious environmental pollution, and complex processes.

Method used

Lithium sulfide was prepared by ball milling and mixing iron powder, sodium sulfide and lithium sulfate in an inert atmosphere, followed by calcination, washing with alcohol solvent and vacuum distillation, and finally calcination.

Benefits of technology

It achieves low-cost, green and environmentally friendly lithium sulfide preparation, simplifies the process, and is easy to apply industrially.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120440841B_ABST
    Figure CN120440841B_ABST
Patent Text Reader

Abstract

This invention discloses a lithium sulfide and its preparation method. The preparation method includes the following steps: (1) ball milling and mixing iron powder, sodium sulfide and lithium sulfate in a first inert atmosphere to obtain a mixture; (2) calcining the mixture once in a second inert atmosphere to obtain a reaction material; (3) stirring and washing the reaction material with an alcohol solvent in a third inert atmosphere, then filtering to obtain a filtrate and a filter cake, distilling the filtrate under reduced pressure to obtain crude lithium sulfide, and washing the filter cake with deionized water and then filtering to obtain a solid byproduct; (4) calcining the crude lithium sulfide a second time in a fourth inert atmosphere to obtain lithium sulfide. The preparation method of this invention has the advantages of fewer synthesis steps, simple product purification, and being green and environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of materials preparation technology, and in particular to a lithium sulfide and its preparation method. Background Technology

[0002] Lithium sulfide is a white to yellow crystalline solid with an anti-fluorite structure, its molecular formula being Li₂S. It can be used directly as a cathode material in lithium-sulfur batteries and as a key raw material for the synthesis of sulfide solid electrolytes. Recent reports indicate that sulfide solid electrolytes prepared using lithium sulfide as a raw material exhibit high ionic conductivity. Currently, methods for synthesizing lithium sulfide can be broadly categorized into ball milling, solvent extraction, and high-temperature, high-pressure methods.

[0003] The ball milling method refers to the mechanical ball milling reaction of elemental sulfur and metallic lithium / lithium hydride in an inert atmosphere to obtain lithium sulfide. CN201911128024.4 reports that under inert atmosphere protection, silicon sulfide and lithium oxide are added to a sealed ball mill jar and milled for a certain time. The solid product in the jar is then removed, excess silicon sulfide is recovered, and the remaining solid product is separated to obtain lithium sulfide powder. CN202010765232.1 describes the synthesis of high-purity lithium sulfide powder using lithium-containing compounds, elemental sulfur, and hydrogen as raw materials through simple mechanical ball milling. This method is simple and environmentally friendly, but the reaction time is long, the conversion rate is low, and the obtained product contains impurities.

[0004] Lithium sulfide is prepared by reacting lithium / lithium compounds and sulfur / sulfur compounds in a solvent medium using a solvent method. CN202011457808.4 describes a process where, under an inert atmosphere, lithium source compounds and sulfur source compounds are weighed and their alcohol solutions are prepared separately. The alcohol solution of the lithium source compound is then added to the alcohol solution of the sulfur source compound. After magnetic stirring, the fully reacted product is centrifuged, and the supernatant is collected. This supernatant is then transferred to a tube furnace for heating and crystallization to obtain crude lithium sulfide. After further processing, high-purity lithium sulfide is obtained. This reaction is complete in the liquid phase, leaving little residue, and the product is easy to purify. However, it suffers from problems such as the flammability, explosiveness, volatility, and serious environmental pollution caused by the organic solvents.

[0005] The high-temperature, high-pressure method refers to the preparation of lithium sulfide by reacting lithium / lithium compounds and sulfur / sulfur compounds under high temperature and pressure in an inert / reducing protective atmosphere through reduction or gas-phase reactions. CN201910993364.7 describes a method that uses a lithium sulfide precursor (one or more of lithium sulfate, lithium sulfite, lithium hydrogen sulfate, and lithium dithionate) with a relevant reducing agent at high temperature to prepare a lithium sulfide-containing substance. The lithium sulfide in this mixture is then leached and purified, and finally spray-dried to obtain a lithium sulfide product with a purity of over 99.9% and a controllable morphology. This method has a simple process flow, produces no harmful gases, and effectively utilizes the advantages of a high-temperature, high-pressure, and closed-loop reaction to avoid leakage of harmful solvents. However, the high temperature and pressure can lead to difficulties in controlling the operating conditions.

[0006] In summary, the drawbacks of different methods for preparing lithium sulfide lead to difficulties in industrialization and persistently high costs. Therefore, the continuous development of inexpensive, efficient, and green lithium sulfide preparation methods is of great significance to the sustainable development of batteries. Summary of the Invention

[0007] In view of the above problems, the purpose of this invention is to provide lithium sulfide and its preparation method, which has the advantages of low raw material cost, fewer synthesis steps, simple product purification, and green environmental protection.

[0008] To achieve the above objectives, the present invention provides a method for preparing lithium sulfide, comprising the steps of: (1) Iron powder, sodium sulfide and lithium sulfate are ball-milled and mixed in a first inert atmosphere to obtain a mixture; (2) The mixture is calcined once in a second inert atmosphere to obtain the reaction material; (3) The reactants were stirred and washed with alcohol solvent in a third inert atmosphere and then filtered to obtain filtrate and filter cake. The filtrate was distilled under reduced pressure to obtain crude lithium sulfide. The filter cake was washed with deionized water and then filtered to obtain solid byproducts. (4) Lithium sulfide crude product is calcined twice in a fourth inert atmosphere to obtain lithium sulfide.

[0009] Compared with existing technologies, this invention uses iron powder, sodium sulfide, and lithium sulfate as raw materials to prepare lithium sulfide. Among them, iron powder has a low cost and valuable solid byproducts iron oxide and iron(II,III) oxide are obtained in the preparation process. Sodium sulfide can be used as a reducing agent and can also increase the source of sulfur in the reaction system. Moreover, the purification method of this invention is simple, the solvent can be recovered and reused in the purification process, which is green and environmentally friendly. At the same time, the preparation method of this invention is simple, environmentally friendly, and easy to industrialize.

[0010] Further, the molar ratio of lithium sulfate, sodium sulfide, and iron powder in this invention is 1:0.5~2:3~8, preferably 1:0.5~1:3~5. As an example, the molar ratio of lithium sulfate, sodium sulfide, and iron powder can be, but is not limited to, 1:0.5:3, 1:0.5:3.5, 1:0.5:4, 1:0.5:4.5, 1:0.5:5, 1:0.5:5.5, 1:0.5:6, 1:0.5:6.5, 1:0.5:7, 1:0.5:7.5, 1:0.5:8, 1:1:3, 1:1:3.5. 1:1:4, 1:1:4.5, 1:1:5, 1:1:5.5, 1:1:6, 1:1:6.5, 1:1:7, 1:1:7.5, 1:1:8, 1:2:3, 1:2:3.5, 1:2:4, 1:2:4.5, 1:2:5, 1:2:5.5, 1:2:6, 1:2:6.5, 1:2:7, 1:2:7.5, 1:2:8.

[0011] Furthermore, the rotational speed of the ball mill in this invention is 400 rpm to 700 rpm. As an example, the rotational speed of the ball mill can be, but is not limited to, 400 rpm, 450 rpm, 500 rpm, 550 rpm, 600 rpm, 650 rpm, or 700 rpm.

[0012] Furthermore, the ball milling time of this invention is 1 hour to 10 hours, preferably 2 hours to 5 hours. As an example, the ball milling time can be, but is not limited to, 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, or 10 hours. By controlling the ball milling speed and time within this range, the particle size of iron powder and lithium sulfate is effectively reduced and the uniformity of mixing is improved, thereby ensuring the conversion rate of the subsequent reduction reaction.

[0013] Furthermore, the calcination temperature of the first calcination in this invention is 500℃~850℃, preferably 650℃~820℃. As an example, the calcination temperature can be, but is not limited to, 500℃, 550℃, 600℃, 650℃, 700℃, 750℃, 800℃, or 850℃.

[0014] Furthermore, the calcination time for one calcination in this invention is 1 hour to 10 hours, preferably 2 hours to 4 hours. As an example, the calcination time can be, but is not limited to, 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, or 10 hours.

[0015] Furthermore, in the first calcination of this invention, the reaction between iron powder and lithium sulfate is as follows: 2Li2SO4 + Na2S + Fe = 2Li₂S + Na₂SO₄ + Fe2O3 2Li2SO4+ Na2S + 3Fe = Li2S + Na2SO4+ Fe3O4 Furthermore, the mass ratio of the alcohol solvent to the reactants in this invention is 30 to 100:1. As an example, the mass ratio of the alcohol solvent to the reactants in this invention can be, but is not limited to, 30:1, 35:1, 40:1, 45:1, 50:1, 55:1, 60:1, 65:1, 70:1, 75:1, 80:1, 85:1, 90:1, 95:1, or 100:1. Controlling the mass ratio of the alcohol solvent to the reactants within this range allows for the maximum retention of crude lithium sulfide while effectively removing solid by-product impurities.

[0016] Furthermore, the alcohol solvent of the present invention is selected from at least one of methanol, ethanol, ethylene glycol, n-propanol, and n-butanol. Preferably, the alcohol solvent of the present invention is selected from ethanol.

[0017] Furthermore, the stirring and washing time of the present invention is 5 min to 30 min. As an example, the stirring and washing time of the present invention is 5 min, 10 min, 15 min, 20 min, 25 min, and 30 min.

[0018] Furthermore, the vacuum distillation temperature of the present invention is 45℃~55℃. Preferably, the vacuum distillation temperature is 50℃. As an example, the vacuum distillation temperature can be, but is not limited to, 45℃, 46℃, 47℃, 48℃, 49℃, 50℃, 51℃, 52℃, 53℃, 54℃, or 55℃.

[0019] Furthermore, the secondary calcination temperature of the present invention is 200℃~500℃, preferably 200℃~350℃. As an example, the secondary calcination temperature of the present invention can be, but is not limited to, 200℃, 220℃, 240℃, 250℃, 260℃, 280℃, 300℃, 320℃, 340℃, 350℃, 360℃, 380℃, 400℃, 420℃, 440℃, 450℃, 460℃, 480℃, or 500℃. At this temperature, residual solvent in the crude lithium sulfide can be effectively removed, improving the purity of lithium sulfide.

[0020] Furthermore, the secondary calcination time of the present invention is 1h to 10h, preferably 2h to 4h. As an example, the secondary calcination time of the present invention can be, but is not limited to, 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, or 10h.

[0021] Furthermore, the first inert atmosphere, the second inert atmosphere, the third inert atmosphere and the fourth inert atmosphere of the present invention are each independently selected from at least one of nitrogen and argon.

[0022] In another aspect, this invention provides a lithium sulfide prepared using the aforementioned method. The lithium sulfide prepared by the method of this invention is battery-grade lithium sulfide and can be directly used in batteries. Attached Figure Description

[0023] Figure 1 The image shows the XRD pattern of lithium sulfide prepared in Example 1 of this invention. Detailed Implementation

[0024] To better illustrate the purpose, technical solution, and beneficial effects of this invention, the invention will be further described below with reference to specific embodiments. It should be noted that the methods described below are further explanations of this invention and should not be construed as limiting it.

[0025] Example 1 This embodiment provides a method for preparing lithium sulfide, including the following steps: (1) 7.65g iron powder, 5g lithium sulfate, 2g sodium sulfide and 250g zirconium oxide grinding balls were placed in a ball milling jar and ball milled under argon atmosphere protection to obtain a mixture. The ball milling speed was 600 rpm and the ball milling time was 2h.

[0026] (2) The mixture was placed in a tube furnace and calcined at 750°C for 3 hours under an argon atmosphere to obtain 1.2g of reaction material; (3) Under nitrogen protection, 60g of anhydrous ethanol was added to the reaction mixture and stirred and washed for 20min. The mixture was filtered to obtain filtrate and filter cake. The filtrate was subjected to vacuum distillation to obtain crude lithium sulfide. The vacuum distillation temperature was 50℃. The filter cake was washed with deionized water and then filtered to obtain solid byproducts iron oxide and iron(II,III) oxide.

[0027] (4) The crude lithium sulfide was transferred to a tube furnace and calcined at 250°C for 3 hours under argon atmosphere protection to obtain 1.07 g of lithium sulfide.

[0028] Figure 1 The image shows the XRD pattern of lithium sulfide obtained in Example 1, proving that lithium sulfide was prepared by the preparation method of the present invention.

[0029] Example 2 This embodiment provides a method for preparing lithium sulfide, including the following steps: (1) 10.2g iron powder, 5g lithium sulfate, 2g sodium sulfide and 300g zirconium oxide grinding balls were placed in a ball milling jar and ball milled under argon atmosphere protection to obtain a mixture. The ball milling speed was 600 rpm and the ball milling time was 2h.

[0030] (2) The mixture was placed in a tube furnace and calcined at 750°C for 3 hours under an argon atmosphere to obtain 1.06 g of reaction material; (3) Under nitrogen protection, 60g of anhydrous ethanol was added to the reaction mixture and stirred and washed for 30min. The mixture was filtered to obtain filtrate and filter cake. The filtrate was subjected to vacuum distillation to obtain crude lithium sulfide. The vacuum distillation temperature was 50℃. The filter cake was washed with deionized water and then filtered to obtain solid byproducts iron oxide and iron(II,III) oxide.

[0031] (4) The crude lithium sulfide was transferred to a tube furnace and calcined at 250°C for 3 hours under argon atmosphere protection to obtain 0.95 g of lithium sulfide.

[0032] Example 3 This embodiment provides a method for preparing lithium sulfide, including the following steps: (1) 12.75g iron powder, 5g lithium sulfate, 3.5g sodium sulfide and 350g zirconium oxide grinding balls were placed in a ball milling jar and ball milled under argon atmosphere protection to obtain a mixture. The ball milling speed was 700 rpm and the ball milling time was 1 h.

[0033] (2) The mixture was placed in a tube furnace and calcined at 750°C for 3 hours under an argon atmosphere to obtain 1.14 g of reaction material; (3) Under nitrogen protection, 60g of anhydrous ethanol was added to the reaction mixture and stirred and washed for 20min. The mixture was filtered to obtain filtrate and filter cake. The filtrate was subjected to vacuum distillation to obtain crude lithium sulfide. The vacuum distillation temperature was 50℃. The filter cake was washed with deionized water and then filtered to obtain solid byproducts iron oxide and iron(II,III) oxide.

[0034] (4) The crude lithium sulfide was transferred to a tube furnace and calcined at 250°C for 3 hours under argon atmosphere protection to obtain 1g of lithium sulfide.

[0035] Example 4 This embodiment provides a method for preparing lithium sulfide, including the following steps: (1) 7.65g iron powder, 5g lithium sulfate, 2g sodium sulfide and 250g zirconium oxide grinding balls were placed in a ball milling jar and ball milled under argon atmosphere protection to obtain a mixture. The ball milling speed was 700 rpm and the ball milling time was 2h.

[0036] (2) The mixture was placed in a tube furnace and calcined at 820°C for 3 hours under an argon atmosphere to obtain 1.4g of reaction material; (3) Under nitrogen protection, 45g of anhydrous ethanol was added to the reaction mixture and stirred and washed for 20min. The mixture was filtered to obtain filtrate and filter cake. The filtrate was subjected to vacuum distillation to obtain crude lithium sulfide. The vacuum distillation temperature was 50℃. The filter cake was washed with deionized water and then filtered to obtain solid byproducts iron oxide and iron(II,III) oxide.

[0037] (4) The crude lithium sulfide was transferred to a tube furnace and calcined at 250°C for 3 hours under argon atmosphere protection to obtain 1.23 g of lithium sulfide.

[0038] Example 5 This embodiment provides a method for preparing lithium sulfide, including the following steps: (1) 7.65g iron powder, 5g lithium sulfate, 2g sodium sulfide and 250g zirconium oxide grinding balls were placed in a ball milling jar and ball milled under argon atmosphere protection to obtain a mixture. The ball milling speed was 700 rpm and the ball milling time was 1 h.

[0039] (2) The mixture was placed in a tube furnace and calcined at 750°C for 4 hours under an argon atmosphere to obtain 1.08 g of reaction material; (3) Under nitrogen protection, 60g of anhydrous ethanol was added to the reaction mixture and stirred and washed for 10min. The mixture was filtered to obtain filtrate and filter cake. The filtrate was subjected to vacuum distillation to obtain crude lithium sulfide. The vacuum distillation temperature was 50℃. The filter cake was washed with deionized water and then filtered to obtain solid byproducts iron oxide and iron(II,III) oxide.

[0040] (4) The crude lithium sulfide was transferred to a tube furnace and calcined at 250°C for 3 hours under argon atmosphere protection to obtain 0.87 g of lithium sulfide.

[0041] Example 6 This embodiment provides a method for preparing lithium sulfide, including the following steps: (1) 7.65g iron powder, 5g lithium sulfate, 3g sodium sulfide and 250g zirconium oxide grinding balls were placed in a ball milling jar and ball milled under argon atmosphere protection to obtain a mixture. The ball milling speed was 500 rpm and the ball milling time was 2h.

[0042] (2) The mixture was placed in a tube furnace and calcined at 820°C for 2 hours under an argon atmosphere to obtain 1.15g of reaction material; (3) Under nitrogen protection, 80g of anhydrous ethanol was added to the reaction mixture and stirred and washed for 20min. The mixture was filtered to obtain filtrate and filter cake. The filtrate was subjected to vacuum distillation to obtain crude lithium sulfide. The vacuum distillation temperature was 50℃. The filter cake was washed with deionized water and then filtered to obtain solid byproducts iron oxide and iron(II,III) oxide.

[0043] (4) The crude lithium sulfide was transferred to a tube furnace and calcined at 300°C for 2 hours under argon atmosphere protection to obtain 1.01 g of lithium sulfide.

[0044] Example 7 This embodiment provides a method for preparing lithium sulfide, including the following steps: (1) 12.75g iron powder, 5g lithium sulfate, 2g sodium sulfide and 350g zirconium oxide grinding balls were placed in a ball milling jar and ball milled under argon atmosphere protection to obtain a mixture. The ball milling speed was 700 rpm and the ball milling time was 4h.

[0045] (2) The mixture was placed in a tube furnace and calcined at 820°C for 4 hours under an argon atmosphere to obtain 1.26 g of reaction material; (3) Under nitrogen protection, 90g of anhydrous ethanol was added to the reaction mixture and stirred and washed for 30min. The mixture was filtered to obtain filtrate and filter cake. The filtrate was subjected to vacuum distillation to obtain crude lithium sulfide. The vacuum distillation temperature was 50℃. The filter cake was washed with deionized water and then filtered to obtain solid byproducts iron oxide and iron(II,III) oxide.

[0046] (4) The crude lithium sulfide was transferred to a tube furnace and calcined at 350°C for 2 hours under argon atmosphere protection to obtain 1.11 g of lithium sulfide.

[0047] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to preferred embodiments, it is not limited to those listed in the embodiments. Those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the essence and scope of the technical solutions of the present invention.

Claims

1. A process for the production of lithium sulfide, characterized in that, Including the following steps: (1) Iron powder, sodium sulfide and lithium sulfate are ball-milled and mixed in a first inert atmosphere to obtain a mixture, wherein the molar ratio of lithium sulfate, sodium sulfide and iron powder is 1:0.5~2:3~8, the ball milling speed is 400rpm~700rpm, and the ball milling time is 1h~10h; (2) The mixture is calcined once in a second inert atmosphere to obtain a reaction material. The temperature of the first calcination is 500℃~850℃ and the time of the first calcination is 1h~10h. (3) The reactants are stirred and washed with alcohol solvent in a third inert atmosphere and then filtered to obtain filtrate and filter cake. The filtrate is distilled under reduced pressure to obtain crude lithium sulfide. The filter cake is washed with deionized water and then filtered to obtain solid byproducts. (4) The crude lithium sulfide is calcined twice in a fourth inert atmosphere to obtain lithium sulfide.

2. The method for preparing lithium sulfide according to claim 1, characterized in that, The mass ratio of the alcohol solvent to the reactant is 30~100:

1.

3. The method for preparing lithium sulfide according to claim 1, characterized in that, The alcohol solvent is selected from at least one of methanol, ethanol, ethylene glycol, n-propanol, and n-butanol.

4. The method for preparing lithium sulfide according to claim 1, characterized in that, The stirring and washing time is 5 min to 30 min, and the vacuum distillation temperature is 45℃ to 55℃.

5. The method for preparing lithium sulfide according to claim 1, characterized in that, The temperature of the secondary calcination is 200℃~500℃, and the time of the secondary calcination is 1h~10h.

6. The method for preparing lithium sulfide according to claim 1, characterized in that, The first inert atmosphere, the second inert atmosphere, the third inert atmosphere, and the fourth inert atmosphere are each independently selected from at least one of nitrogen and argon.

Citation Information

Patent Citations

  • A mechanical ball milling synthesis method for lithium sulfide powder

    CN110790239B

  • A green and efficient preparation method for lithium sulfide

    CN112125322B

  • A method for preparing lithium sulfide, lithium sulfide and its applications

    CN112551491B

  • Preparation method of high-purity lithium sulfide

    CN112678780B

  • Lithium-containing transition metal sulfide compounds

    CN102177094A