A SEBS elastomer composite material with strong cold resistance and its preparation method

By improving the SEBS elastomer composite material formulation and preparation process, the problem of insufficient cold resistance of SEBS has been solved, enabling the material to maintain flexibility and elasticity at extremely low temperatures, thereby improving the material's stability and service life.

CN120504930BActive Publication Date: 2026-11-17QUANZHOU PEAK SHOES
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510805242.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-06-17
Publication Date
2026-11-17
Estimated Expiration
2045-06-17

AI Technical Summary

Technical Problem

Existing SEBS elastomers have unsatisfactory cold resistance, and alternative materials are expensive and dependent on imports, leading to increased product development costs and the risk of supply shortages.

Method used

By using components such as linear SEBS, star-shaped SEBS, maleic anhydride-grafted SEBS, polyether ester plasticizer, and nano-fumed silica, combined with specific mixing and melt blending processes, a SEBS elastomer composite material with strong cold resistance was prepared.

Benefits of technology

Maintaining excellent flexibility and elasticity at extremely low temperatures, the material exhibits improved hardness and low-temperature performance stability, reduces plasticizer migration and exudation, extends service life, and lowers the risk of environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to the field of shoe sole material technology, and in particular to a SEBS elastomer composite material with strong cold resistance and its preparation method, comprising the following materials in parts by weight: 100 parts linear SEBS, 60-130 parts plasticizer, 10-25 parts reactive compatibilizer, 0.5-2 parts antioxidant, 10-30 parts star-shaped SEBS, and 5-15 parts nano-fumed silica.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of shoe sole material formulation technology, and in particular to a SEBS elastomer composite material with strong cold resistance and its preparation method. Background Technology

[0002] Traditional shoe material elastomers mainly include EVA, POE, EPDM, OBC, and SEBS. SEBS is a new type of multi-purpose thermoplastic elastomer, but the cold resistance of commercially available SEBS is not ideal. Therefore, some manufacturers use OBC and EPDM, which have relatively better cold resistance, as substitutes. However, the hardness increases significantly below -15℃, and OBC and EPDM are all imported, with prices more than 30% higher than SEBS. This results in higher costs, greater risk of stockouts, and is not conducive to product development. Summary of the Invention

[0003] Therefore, in view of the above problems, this invention proposes a SEBS elastomer composite material with strong cold resistance and its preparation method.

[0004] To achieve the above objectives, the technical solution of the present invention is to provide a SEBS elastomer composite material with strong cold resistance, comprising the following parts by weight: 100 parts linear SEBS, 60-130 parts plasticizer, 10-25 parts reactive compatibilizer, 0.5-2 parts antioxidant, 10-30 parts star-shaped SEBS, and 5-15 parts nano-fumed silica.

[0005] A further improvement is that the reactive compatibilizer is maleic anhydride-grafted SEBS.

[0006] A further improvement is that the plasticizer is a polyether ester plasticizer with a molecular weight of 2000-6000 g / mol.

[0007] Further improvements include: 0.5-5 parts of a branching structure promoter.

[0008] A further improvement is that the branching accelerator is pentaerythritol, pyromellitic acid, or trimethylolpropane triacrylate.

[0009] A further improvement is that the surface modification treatment of the nano-fumed silica has a specific surface area of ​​180-250 m² / g.

[0010] A method for preparing a SEBS elastomer composite material with strong cold resistance includes the following steps: S1 Premix: Linear SEBS, star-shaped SEBS, and maleic anhydride-grafted SEBS are mixed uniformly in a certain proportion; S2 Plasticizer: Add polyether ester plasticizer and stir to penetrate for 30 minutes; S3 Enhancement: High-speed dispersion with the addition of nano-fumed silica and antioxidants; S4 melt blending: Melt blending is carried out at 160℃ - 220℃.

[0011] S5 extrusion granulation: The melt-blended material is extruded, cooled, and pelletized to obtain composite material granules. A further improvement is that the premixing temperature is 60-80℃.

[0012] A further improvement is that the melt blending is carried out in a twin-screw extruder with a screw speed of 200-400 rpm.

[0013] The advantages and beneficial effects of this invention are as follows: 1. Compared with mineral oil-plasticized SEBS, it has superior cold resistance, maintaining excellent flexibility and elasticity at extremely low temperatures (such as -40℃, -50℃), and is not easily brittle. Its impact strength at low temperatures (such as -30℃ or lower) is significantly improved.

[0014] 2. Through the inherent low migration of high molecular weight polyester plasticizer and the strong anchoring effect of reactive compatibilizer, the migration and exudation of plasticizer are fundamentally suppressed. After long-term use or under high temperature environment (such as after aging at 70-100℃), there is no oily exudate on the material surface, it is not sticky, and it does not contaminate the contact objects. The stability of the material's hardness, low temperature performance and other properties with time and environmental changes is significantly improved.

[0015] 3. Excellent durability: Combined with low migration and a good antioxidant system, the material has a longer service life and is particularly suitable for applications that require high low-temperature performance and long-term stability. The low migration also reduces the risk of environmental pollution. Detailed Implementation

[0016] The specific embodiments of the present invention will be further described below with reference to examples. These examples are only used to more clearly illustrate the technical solutions of the present invention and should not be construed as limiting the scope of protection of the present invention. Example 1

[0017] A SEBS elastomer composite material with strong cold resistance comprises the following materials in parts by weight: 100 parts linear SEBS, 60-130 parts plasticizer, 10-25 parts reactive compatibilizer, 0.5-2 parts antioxidant, 10-30 parts star-shaped SEBS, and 5-15 parts nano-fumed silica.

[0018] To enable the plasticizer to bind stably with linear SEBS, the reactive compatibilizer is maleic anhydride-grafted SEBS.

[0019] In order to suppress migration and exudation, provide a long-term stable plasticizing effect, and suppress low-temperature crystallization, the plasticizer is a polyether ester plasticizer with a molecular weight of 2000-6000 g / mol.

[0020] To improve plasticizing efficiency and aid in inhibiting migration, the product also includes 0.5-5 parts of a branching accelerator, wherein the branching accelerator is pentaerythritol, trimesic acid, or trimethylolpropane triacrylate.

[0021] To enhance the friction of the composite material on low-temperature wet and slippery surfaces, the nano-fumed silica undergoes surface modification treatment, and the specific surface area of ​​the nano-fumed silica is 180-250 m² / g. Nano-sized fumed silica was surface-treated using silane coupling agent KH-570.

[0022] A method for preparing a SEBS elastomer composite material with strong cold resistance includes the following steps: S1 Premix: Linear SEBS, star-shaped SEBS, and maleic anhydride-grafted SEBS are mixed evenly in proportion; S2 Plasticizer: Add polyether ester plasticizer and stir to penetrate for 30 minutes; S3 Enhancement: High-speed dispersion with the addition of nano-fumed silica and antioxidants; S4 melt blending: Melt blending is carried out at 160℃ - 220℃.

[0023] S5 extrusion granulation: The melt-blended material is extruded, cooled, and pelletized to obtain composite material granules. To enhance premixing efficiency, the premixing temperature is 60-80℃.

[0024] The melt blending is carried out in a twin-screw extruder with a screw speed of 200-400 rpm.

[0025] Comparative experiment: C1: Mineral oil replaces polyether ester; C2: No star-shaped SEBS added; C3: No surface-treated SiO2.

[0026]

[0027] The data in the table shows that, compared to C1, the material of Example 1 has a better low-temperature resistance and can be used at more extreme temperatures. Compared to C2, it exhibits superior resistance to deformation and strong wear resistance at low temperatures; Compared to C3, it has a superior coefficient of friction on ice surfaces; In summary, this material exhibits superior performance and a longer service life compared to ordinary SEBS materials at low temperatures, making it feasible as a base material or auxiliary modification material for low-temperature shoe soles.

[0028] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions above are merely illustrative of the principles of the present invention. Various changes and modifications can be made to the present invention without departing from its spirit and scope. All such changes and modifications fall within the scope of the present invention as claimed, which is defined by the appended claims and their equivalents.

Claims

1. A SEBS elastomer composite having strong cold resistance performance, characterized in that: The material comprises the following parts by weight: 100 parts linear SEBS, 60-130 parts plasticizer, 10-25 parts reactive compatibilizer, 0.5-2 parts antioxidant, 10-30 parts star-shaped SEBS, and 5-15 parts nano-fumed silica. The plasticizer is a polyether ester plasticizer, and the molecular weight of the polyether ester plasticizer is 2000-6000 g / mol; The surface modification treatment of the nano-fumed silica, wherein the specific surface area of ​​the nano-fumed silica is 180-250 m² / g; The reactive compatibilizer is maleic anhydride-grafted SEBS.

2. The SEBS elastomer composite material with strong cold resistance performance according to claim 1, characterized in that: Also includes: 0.5-5 parts of branching accelerator.

3. The SEBS elastomer composite material with strong cold resistance performance according to claim 2, characterized in that: The branching promoter is pentaerythritol, pyromellitic acid, or trimethylolpropane triacrylate.

4. A process for the preparation of the SEBS elastomeric composite having high cold resistance according to any one of claims 1-3, characterized by the fact that: Includes the following steps: S1 Premix: Linear SEBS, star-shaped SEBS, and maleic anhydride-grafted SEBS are mixed uniformly in proportion. S2 Plasticizer: Add polyether ester plasticizer and stir to penetrate for 30 minutes; S3 Enhancement: High-speed dispersion with the addition of nano-fumed silica, branching structure promoter and antioxidant; S4 melt blending: Melt blending is carried out at 160℃-220℃; S5 extrusion granulation: The melt-blended material is extruded, cooled, and granulated to obtain composite material granules; The branching accelerator is pentaerythritol, pyromellitic acid, or trimethylolpropane triacrylate. The plasticizer is a polyether ester plasticizer, and the molecular weight of the polyether ester plasticizer is 2000-6000 g / mol; The surface modification treatment of the nano-fumed silica has a specific surface area of ​​180-250 m² / g.

5. The method of claim 4, wherein the SEBS elastomer composite is prepared by: The temperature during premixing is 60-80℃.

6. The method for preparing a SEBS elastomer composite material according to claim 4, characterized in that: The melt blending is carried out in a twin-screw extruder with a screw speed of 200-400 rpm.

Citation Information

Patent Citations

  • Thermoplastic elastomer material and preparation method thereof

    CN109796731A

  • Antibacterial TPV (thermoplastic vulcanizate) material for nurse shoes